JPH0657018A - Biaxially oriented polyester film - Google Patents

Biaxially oriented polyester film

Info

Publication number
JPH0657018A
JPH0657018A JP13246592A JP13246592A JPH0657018A JP H0657018 A JPH0657018 A JP H0657018A JP 13246592 A JP13246592 A JP 13246592A JP 13246592 A JP13246592 A JP 13246592A JP H0657018 A JPH0657018 A JP H0657018A
Authority
JP
Japan
Prior art keywords
film
polyester
acid
biaxially stretched
polyester film
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP13246592A
Other languages
Japanese (ja)
Other versions
JP3185355B2 (en
JPH0657018A5 (en
Inventor
Nobuyuki Kagami
信行 鏡味
Yuzo Shimizu
有三 清水
Masaru Suzuki
勝 鈴木
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toray Industries Inc
Original Assignee
Toray Industries Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toray Industries Inc filed Critical Toray Industries Inc
Priority to JP13246592A priority Critical patent/JP3185355B2/en
Publication of JPH0657018A publication Critical patent/JPH0657018A/en
Publication of JPH0657018A5 publication Critical patent/JPH0657018A5/ja
Application granted granted Critical
Publication of JP3185355B2 publication Critical patent/JP3185355B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

(57)【要約】 【構成】分子内に3個以上のエステル形成性官能基を有
する化合物を0.05〜3.0モル%含み、極限粘度が
0.64〜1.1のポリエステルからなり、ヤング率が
410kg/mm2 以上であることを特徴とする二軸延
伸ポリエステルフィルム。 【効果】本発明の二軸延伸ポリエステルフィルムは高強
力、高弾性という優れた機械的特性を有し、薄膜化して
も低コストでかつ安定な製膜が可能であり、磁気テープ
用、コンデンサー用、感熱転写用等の用途、特に磁気テ
ープ用途に好適に使用される。
(57) [Summary] [Structure] A polyester containing 0.05 to 3.0 mol% of a compound having three or more ester-forming functional groups in its molecule and having an intrinsic viscosity of 0.64 to 1.1. A biaxially stretched polyester film having a Young's modulus of 410 kg / mm 2 or more. [Effect] The biaxially stretched polyester film of the present invention has excellent mechanical properties such as high strength and high elasticity, and can be formed into a thin film at low cost and stable even if it is thinned. It is preferably used for applications such as heat-sensitive transfer, especially for magnetic tape applications.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は優れた機械的特性を有す
る二軸延伸ポリエステルフィルムに関するものである。
詳しくは高強力、高弾性を有する二軸延伸ポリエステル
フィルム、更に詳しくは磁気テープ用途、コンデンサー
用途、感熱転写用途等、特に磁気テープ用途に好適な高
強力、高弾性二軸延伸ポリエステルフィルムに関するも
のである。
FIELD OF THE INVENTION The present invention relates to a biaxially stretched polyester film having excellent mechanical properties.
More specifically, it relates to a biaxially stretched polyester film having high strength and high elasticity, more specifically to a high strength and high elasticity biaxially stretched polyester film suitable for magnetic tape applications, condenser applications, thermal transfer applications and the like. is there.

【0002】[0002]

【従来の技術】芳香族ジカルボン酸とグリコールからな
るポリエステル、特にポリエチレンテレフタレートは優
れた機械的特性、電気的特性、耐熱性、寸法安定性、耐
薬品性を有していることから、磁気テープ、コンデンサ
ー、感熱転写用フィルム、包装用フィルム、磁気カー
ド、タイヤコード、繊維、ボトル等工業的に広く用いら
れている。しかしながら、近年ポリエチレンテレフタレ
ートフィルムの利用分野、例えば磁気テープ用途におい
ては長録画時間化、小型化の要求が強まり、このために
フィルムを薄膜化することが必要となってきている。し
かし、従来のポリエチレンテレフタレートフィルムでは
強度、弾性率等の機械特性が不足するため薄膜化を達成
することができないという問題点があった。
2. Description of the Related Art Polyesters composed of aromatic dicarboxylic acids and glycols, particularly polyethylene terephthalate, have excellent mechanical properties, electrical properties, heat resistance, dimensional stability, and chemical resistance. It is widely used industrially such as capacitors, heat-sensitive transfer films, packaging films, magnetic cards, tire cords, fibers and bottles. However, in recent years, in the field of use of polyethylene terephthalate film, for example, magnetic tape applications, there is an increasing demand for longer recording time and downsizing, and for this reason, it has become necessary to make the film thinner. However, the conventional polyethylene terephthalate film has a problem that it cannot be made thin because mechanical properties such as strength and elastic modulus are insufficient.

【0003】一方、ポリエチレンテレフタレートの強
度、ヤング率等の機械特性を向上させようとする試みは
数多く行われており、例えば特開平1−217033号
公報では芳香族化合物を共重合する試みがなされてい
る。しかしながらこのような共重合成分を導入する方法
では、モノマの製造コスト高がフィルム製造コストに影
響してしまうという問題がある。また別の方法として多
官能化合物を共重合する方法があり、例えば特開昭50
−37893号公報には、ポリエチレンテレフタレート
にポリオキシアルキレングリコール及び多官能化合物を
共重合した、繊維用ポリエステルの製造方法が開示され
ている。しかし、このようなポリエステルでは高強力、
高弾性フィルムには適当ではない。また、例えば特開平
2−47038号公報にはフィルムの手切れ性を付与す
るために多官能化合物をポリエステルに共重合する提案
が、特開昭49−68066号公報には繊維の抗ピル性
を付与するために多官能化合物をポリエステルに共重合
する提案がなされている。しかし、これらの提案は低分
子量ポリエステルに多官能化合物を共重合し、ポリエス
テルの成型性改善しようとするものであり、本発明が目
的としている機械特性向上を達成することはできない。
一方特開昭55−34245号公報には、ポリエステル
フィルムに紫外線照射による架橋を行い高強力化を図る
提案がなされている。しかしこの方法においては、フィ
ルムの架橋度を高めるために長時間の紫外線照射や増感
剤等の添加剤が必要であり、生産性が著しく低下したり
コスト高になってしまうという問題点がある。
On the other hand, many attempts have been made to improve mechanical properties such as strength and Young's modulus of polyethylene terephthalate. For example, Japanese Patent Laid-Open No. 1-217033 makes an attempt to copolymerize an aromatic compound. There is. However, in the method of introducing such a copolymerization component, there is a problem that the high production cost of the monomer affects the production cost of the film. As another method, there is a method of copolymerizing a polyfunctional compound.
JP-A-37893 discloses a method for producing a polyester for fibers, which is obtained by copolymerizing polyethylene terephthalate with polyoxyalkylene glycol and a polyfunctional compound. However, with such polyester, high strength,
Not suitable for high elasticity films. Further, for example, Japanese Patent Application Laid-Open No. 2-47038 proposes copolymerization of a polyfunctional compound with polyester in order to impart hand-cutting properties to the film, and Japanese Patent Application Laid-Open No. 49-68066 discloses anti-pill property of fibers. Proposals have been made to copolymerize polyfunctional compounds with polyesters for application. However, these proposals are intended to improve the moldability of the polyester by copolymerizing a polyfunctional compound with a low molecular weight polyester, and the improvement in mechanical properties aimed at by the present invention cannot be achieved.
On the other hand, JP-A-55-34245 proposes to increase the strength by cross-linking a polyester film by irradiating it with ultraviolet rays. However, in this method, long-term ultraviolet irradiation and additives such as a sensitizer are required to increase the degree of cross-linking of the film, and there is a problem that productivity is significantly reduced or cost is increased. .

【0004】[0004]

【発明が解決しようとする課題】本発明の目的は上記し
た従来技術における問題点を解消することにあり、高強
力、高弾性であり、かつ低コストで生産性に優れる二軸
延伸ポリエステルフィルムを提供することにある。
SUMMARY OF THE INVENTION An object of the present invention is to solve the above problems in the prior art, and to provide a biaxially stretched polyester film having high strength, high elasticity, low cost and excellent productivity. To provide.

【0005】[0005]

【課題を解決するための手段】前記した本発明の目的
は、分子内に3個以上のエステル形成性官能基を有する
化合物を0.05〜3.0モル%含み、極限粘度が0.
64〜1.1のポリエステルからなり、ヤング率が41
0kg/mm2 以上であることを特徴とする二軸延伸ポ
リエステルフィルムによって達成することができる。
The above-mentioned object of the present invention contains 0.05 to 3.0 mol% of a compound having three or more ester-forming functional groups in the molecule and has an intrinsic viscosity of 0.
Made of 64 to 1.1 polyester, Young's modulus is 41
It can be achieved by a biaxially stretched polyester film characterized by being 0 kg / mm 2 or more.

【0006】本発明におけるポリエステルとは、芳香族
ジカルボン酸とグリコールを主たる構成成分とする。芳
香族ジカルボン酸としては例えばテレフタル酸、イソフ
タル酸、2,6−ナフタレンジカルボン酸、2,7−ナ
フタレンジカルボン酸、ジフェニルジカルボン酸、ジフ
ェニルスルホンジカルボン酸、ジフェノキシエタンジカ
ルボン酸、ジフェニルエーテルジカルボン酸、5−スル
ホイソフタル酸、フタル酸等を挙げることができる。こ
れらの酸成分のうちテレフタル酸、ナフタレンジカルボ
ン酸が好ましく、特にテレフタル酸が好ましい。これら
の酸成分は1種のみ用いてもよく、2種以上併用しても
よい。また、芳香族ジカルボン酸のほかにシュウ酸、コ
ハク酸、アジピン酸、セバシン酸、ダイマー酸、マレイ
ン酸、フマル酸等の脂肪族ジカルボン酸、シクロヘキサ
ンジカルボン酸等の脂環族ジカルボン酸、p−オキシ安
息香酸等のオキシカルボン酸を共重合してもよい。グリ
コール成分としては例えばエチレングリコール、1,2
−プロパンジオール、1,3−プロパンジオール、1,
3−ブタンジオール、1,4−ブタンジオール、1,5
−ペンタンジオール、1,6−ヘキサンジオール、ジエ
チレングリコール、トリエチレングリコール、ポリエチ
レングリコール、ネオペンチルグリコール等の脂肪族グ
リコール、ビスフェノールA、ビスフェノールS等の芳
香族グリコール、1,2−シクロヘキサンジメタノー
ル、1,3−シクロヘキサンジメタノール、1,4−シ
クロヘキサンジメタノール等の脂環族グリコール等が挙
げられる。これらのグリコール成分のうちエチレングリ
コール、1,4−ブタンジオール、1,6−ヘキサンジ
オールが好ましく、特にエチレングリコールが好まし
い。これらグリコール成分は1種のみ用いても、2種以
上を併用してもよい。上記の芳香族ジカルボン酸成分と
グリコール成分からなるポリエステルとしては、例えば
ポリエチレンテレフタレート、ポリブチレンテレフタレ
ート、ポリヘキサメチレンテレフタレート、ポリエチレ
ンナフタレート等を挙げることができる。これらのポリ
エステルのうちポリエチレンテレフタレートが特に好ま
しい。
The polyester in the present invention comprises aromatic dicarboxylic acid and glycol as main constituent components. Examples of the aromatic dicarboxylic acid include terephthalic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, diphenyldicarboxylic acid, diphenylsulfonedicarboxylic acid, diphenoxyethanedicarboxylic acid, diphenyletherdicarboxylic acid, 5- Examples thereof include sulfoisophthalic acid and phthalic acid. Of these acid components, terephthalic acid and naphthalenedicarboxylic acid are preferable, and terephthalic acid is particularly preferable. These acid components may be used alone or in combination of two or more. In addition to aromatic dicarboxylic acids, oxalic acid, succinic acid, adipic acid, sebacic acid, dimer acid, maleic acid, fumaric acid and other aliphatic dicarboxylic acids, cyclohexanedicarboxylic acid and other alicyclic dicarboxylic acids, p-oxy An oxycarboxylic acid such as benzoic acid may be copolymerized. Examples of the glycol component include ethylene glycol, 1,2
-Propanediol, 1,3-propanediol, 1,
3-butanediol, 1,4-butanediol, 1,5
-Aliphatic glycols such as pentanediol, 1,6-hexanediol, diethylene glycol, triethylene glycol, polyethylene glycol and neopentyl glycol, aromatic glycols such as bisphenol A and bisphenol S, 1,2-cyclohexanedimethanol, 1, Examples thereof include alicyclic glycols such as 3-cyclohexanedimethanol and 1,4-cyclohexanedimethanol. Among these glycol components, ethylene glycol, 1,4-butanediol and 1,6-hexanediol are preferable, and ethylene glycol is particularly preferable. These glycol components may be used alone or in combination of two or more. Examples of the polyester composed of the aromatic dicarboxylic acid component and the glycol component include polyethylene terephthalate, polybutylene terephthalate, polyhexamethylene terephthalate and polyethylene naphthalate. Of these polyesters, polyethylene terephthalate is particularly preferable.

【0007】本発明におけるポリエステルでは、上記し
た芳香族ジカルボン酸成分及びグリコール成分のほかに
共重合成分として、分子内に3個以上のエステル形成性
官能基を有する化合物を含有させることが必要である。
エステル形成性多官能化合物における官能基数は3個以
上であれば任意とすることができるが、好ましくは3〜
4個、更に好ましくは3個である。本発明におけるエス
テル形成性多官能化合物は分子内にエステル形成性官能
基を3個以上有している化合物であれば脂肪族、脂環
族、芳香族等いずれであってもよい。エステル形成性官
能基としてはヒドロキシル基、カルボキシル基、メトキ
シ基等が挙げられ、またこれら官能基は炭素数1〜6の
低級アルキルエステル等であってもよい。分子内に3個
以上のエステル形成性官能基を有する化合物中における
エステル形成性官能基は各々異なっていてもよいが、同
種であることが好ましい。このようなエステル形成性多
官能化合物として例えば、トリメリット酸、トリメシン
酸、ヘミメリット酸、ピロメリット酸、プレニット酸、
ジヒドロキシテレフタル酸、ジヒドロキシイソフタル
酸、トリメチロールエタン、トリメチロールプロパン、
トリメチロールブタン、トリメチロールベンゼン、トリ
エチロールベンゼン、トリブチロールベンゼン、ヘキサ
ントリオール、テトラメチロールシクロヘキサノール、
ペンタエリスリトール、グリセロール等を挙げることが
できる。これらのうちトリメリット酸、トリメシン酸、
トリメチロールプロパンが好ましい。これらの化合物は
1種のみ用いても、2種以上を併用してもよい。エテル
形成性多官能化合物のポリエステルへの添加量は、ポリ
エステルを構成する酸成分またはグリコール成分に対し
て0.05〜3.0モル%であることが必要であり、好
ましくは0.1〜2.0モル%、更に好ましくは0.3
〜1.0モル%である。0.05モル%未満であると本
発明の目的とするフィルムの機械的特性の向上の効果が
十分でなく、また3.0モル%を越えるとポリエステル
の重縮合反応時にゲル化が生じやすくなったり、ポリマ
の吐出性が悪化したりするので好ましくない。
In the polyester of the present invention, in addition to the above-mentioned aromatic dicarboxylic acid component and glycol component, it is necessary to contain a compound having three or more ester-forming functional groups in the molecule as a copolymerization component. .
The number of functional groups in the ester-forming polyfunctional compound can be arbitrary as long as it is 3 or more, but preferably 3 to
It is four, and more preferably three. The ester-forming polyfunctional compound in the present invention may be aliphatic, alicyclic, aromatic or the like as long as it is a compound having three or more ester-forming functional groups in the molecule. Examples of the ester-forming functional group include a hydroxyl group, a carboxyl group and a methoxy group, and these functional groups may be a lower alkyl ester having 1 to 6 carbon atoms. The ester-forming functional groups in the compound having three or more ester-forming functional groups in the molecule may be different, but are preferably the same type. Examples of such ester-forming polyfunctional compounds include trimellitic acid, trimesic acid, hemimellitic acid, pyromellitic acid, prenittic acid,
Dihydroxyterephthalic acid, dihydroxyisophthalic acid, trimethylolethane, trimethylolpropane,
Trimethylol butane, trimethylol benzene, trimethylol benzene, tributyrole benzene, hexane triol, tetramethylol cyclohexanol,
Pentaerythritol, glycerol, etc. can be mentioned. Of these, trimellitic acid, trimesic acid,
Trimethylolpropane is preferred. These compounds may be used alone or in combination of two or more. The amount of the ether-forming polyfunctional compound added to the polyester needs to be 0.05 to 3.0 mol%, preferably 0.1 to 2 with respect to the acid component or glycol component constituting the polyester. 0.0 mol%, more preferably 0.3
Is about 1.0 mol%. If it is less than 0.05 mol%, the effect of improving the mechanical properties of the film, which is the object of the present invention, is not sufficient, and if it exceeds 3.0 mol%, gelation tends to occur during the polycondensation reaction of the polyester. And the dischargeability of the polymer deteriorates, which is not preferable.

【0008】本発明においてポリエステルの極限粘度は
0.64〜1.1とすることが必要であり、好ましくは
0.66〜1.0、更に好ましくは0.68〜0.9で
ある。極限粘度が0.64未満の場合にはフィルムの強
度、弾性率に劣り、また1.1を越えると、フィルムの
製膜時に膜破れや延伸困難になるなど製膜安定性に劣る
ので好ましくない。
In the present invention, the intrinsic viscosity of the polyester must be 0.64 to 1.1, preferably 0.66 to 1.0, and more preferably 0.68 to 0.9. When the intrinsic viscosity is less than 0.64, the strength and elastic modulus of the film are poor, and when the intrinsic viscosity is more than 1.1, the film stability is poor such as film breakage or stretching during film production, which is not preferable. .

【0009】本発明におけるポリエステルを製造するに
際しては、従来公知の任意の方法を採用することができ
る。例えば、分子内に3個以上のエステル形成性官能基
を有する化合物としてトリメリット酸トリメチルをポリ
エチレンテレフタレートに共重合する場合で説明する
と、テレフタル酸ジメチル、エチレングリコール、トリ
メリット酸トリメチルを触媒の存在下でメタノールを反
応系外に留出させながらエステル交換反応を行い、続い
て触媒の存在下で高温、減圧にしてエチレングリコール
を反応系外から留出させ重縮合する方法が挙げられる。
また、テレフタル酸、トリメリット酸、エチレングリコ
ールから直接エステル化反応させ、続いて触媒の存在下
で重縮合反応させる方法を採用することもできる。ま
た、エステル交換またはエステル化反応後に一定の重合
度になるまで重縮合し、ついで得られた重合体をその融
点より低い温度において減圧下または不活性ガス気流下
において更に重縮合反応させる固相重合法を用いてもよ
い。
In producing the polyester in the present invention, any conventionally known method can be adopted. For example, in the case of copolymerizing trimethyl trimellitate with polyethylene terephthalate as a compound having three or more ester-forming functional groups in the molecule, dimethyl terephthalate, ethylene glycol, trimethyl trimellitate in the presence of a catalyst will be described. A method in which the ester exchange reaction is carried out while distilling methanol out of the reaction system in the following, and then ethylene glycol is distilled out of the reaction system at high temperature and reduced pressure in the presence of a catalyst to carry out polycondensation.
It is also possible to employ a method in which terephthalic acid, trimellitic acid and ethylene glycol are directly subjected to an esterification reaction, followed by a polycondensation reaction in the presence of a catalyst. In addition, solid-state polycondensation is performed after the transesterification or esterification reaction until polycondensation reaches a certain degree of polymerization, and then the obtained polymer is further polycondensed at a temperature lower than its melting point under reduced pressure or under an inert gas stream. Legal may be used.

【0010】本発明に用いるポリエステルを製造するに
あたり、従来公知の任意の触媒を使用することができ
る。かかる触媒としては例えば、アルカリ金属化合物、
アルカリ土類金属化合物、亜鉛化合物、鉛化合物、マン
ガン化合物、マグネシウム化合物、アルミニウム化合
物、アンチモン化合物、ゲルマニウム化合物、チタン化
合物等を挙げることができる。
In producing the polyester used in the present invention, any conventionally known catalyst can be used. Examples of such catalysts include alkali metal compounds,
Examples thereof include alkaline earth metal compounds, zinc compounds, lead compounds, manganese compounds, magnesium compounds, aluminum compounds, antimony compounds, germanium compounds, titanium compounds and the like.

【0011】本発明における二軸延伸ポリエステルフィ
ルムは、従来公知の任意の方法を用いて製膜することが
できる。例えば、前記したポリエステルを十分に乾燥さ
せた後押出し機に供給し、キャスティングドラムに溶融
押出して未延伸フィルムとし、次いでこの未延伸フィル
ムを同時あるいは逐次に二軸延伸する方法が挙げられ
る。また逐次二軸延伸の場合、その延伸順序はフィルム
を長手方向、幅方向の順、あるいはこの逆としてもよ
い。更に同時二軸あるいは逐次二軸延伸において、長手
方向あるいは幅方向の延伸を2回以上行うことも可能で
ある。フィルムの長手方向及び幅方向の延伸倍率は目的
とする強度、弾性率等の機械特性に応じて任意とするこ
とができるが、機械特性を十分に発現させるために好ま
しくは2.5〜6.0倍、更に好ましくは3.0〜5.
0倍である。長手方向、幅方向の延伸倍率はどちらを大
きくしてもよく、同一としてもよい。また、延伸温度は
ポリエステルのガラス転移温度以上、結晶化温度以下の
範囲であれば任意の温度とすることができるが、通常は
80〜140℃が好ましい。更に二軸延伸の後にフィル
ムの熱処理を行うことができる。この熱処理はオーブン
中、加熱されたロール上等、従来公知の任意の方法で行
うことができる。熱処理温度はポリエステルの結晶化温
度以上、軟化点以下の任意の温度とすることができる
が、好ましくは180〜250℃、更に好ましくは19
0〜230℃である。また熱処理時間は任意とすること
ができるが、通常1〜60秒間行うのが好ましい。熱処
理はフィルムをその長手方向及び/または幅方向に弛緩
させつつ行ってもよい。
The biaxially stretched polyester film of the present invention can be formed by any conventionally known method. For example, there may be mentioned a method in which the above-mentioned polyester is sufficiently dried, then supplied to an extruder, melt-extruded into a casting drum to obtain an unstretched film, and then the unstretched film is biaxially stretched simultaneously or sequentially. In the case of sequential biaxial stretching, the stretching order may be the longitudinal direction of the film, the transverse direction of the film, or vice versa. Further, in simultaneous biaxial or sequential biaxial stretching, it is possible to carry out stretching in the longitudinal direction or the width direction twice or more. The stretching ratios in the longitudinal direction and the width direction of the film can be arbitrarily set according to the desired mechanical properties such as strength and elastic modulus, but are preferably 2.5 to 6 in order to sufficiently express the mechanical properties. 0 times, more preferably 3.0 to 5.
It is 0 times. Either the stretching ratio in the longitudinal direction or the stretching ratio in the width direction may be increased or may be the same. The stretching temperature may be any temperature in the range of not less than the glass transition temperature of polyester and not more than the crystallization temperature, but it is usually preferably 80 to 140 ° C. Further, the film can be heat-treated after the biaxial stretching. This heat treatment can be performed by any conventionally known method such as in an oven or on a heated roll. The heat treatment temperature may be any temperature not lower than the crystallization temperature of the polyester and not higher than the softening point, preferably 180 to 250 ° C., more preferably 19.
It is 0-230 degreeC. The heat treatment time may be arbitrary, but it is usually preferably 1 to 60 seconds. The heat treatment may be performed while relaxing the film in the longitudinal direction and / or the width direction.

【0012】このようにして得られた本発明における二
軸延伸ポリエステルフィルムのヤング率は410kg/
mm2 以上であることが必要であり、好ましくは420
kg/mm2 以上、更に好ましくは430kg/mm2
以上である。ヤング率が410kg/mm2 未満の場合
には、ポリエステルフィルムの各種利用分野に要求され
ている薄膜化を達成することが難しくなるので好ましく
ない。二軸延伸ポリエステルフィルムのヤング率はフィ
ルムの長手方向または幅方向ともに410kg/mm2
以上としてもよいし、あるいは長手方向または幅方向い
ずれかが410kg/mm2 以上であってもよい。
The Young's modulus of the biaxially stretched polyester film of the present invention thus obtained is 410 kg /
It is necessary to be at least 2 mm 2 , preferably 420
kg / mm 2 or more, more preferably 430 kg / mm 2
That is all. When the Young's modulus is less than 410 kg / mm 2 , it is difficult to achieve the thinning required for various fields of use of the polyester film, which is not preferable. The Young's modulus of the biaxially stretched polyester film is 410 kg / mm 2 in the longitudinal direction or the width direction of the film.
Alternatively, it may be 410 kg / mm 2 or more in either the longitudinal direction or the width direction.

【0013】本発明のポリエステルフィルムの厚さはそ
の用途により任意とすることができ、例えば磁気テープ
用途では5〜10μmとすれば、磁気テープの長録画時
間化、小型化が可能となり好ましい。またフィルムに離
型性、接着性、ヒートシール性、滑り性、平滑性等を付
与するために積層フィルムとしてもよいし、溶剤コーテ
ィング処理、コロナ放電処理等を施してもよい。
The thickness of the polyester film of the present invention can be arbitrarily set according to its use. For example, in the case of a magnetic tape application, it is preferable that the thickness is 5 to 10 μm because the recording time of the magnetic tape can be made longer and the size can be reduced. Further, in order to impart releasability, adhesiveness, heat sealability, slipperiness, smoothness, etc. to the film, it may be a laminated film, or may be subjected to solvent coating treatment, corona discharge treatment or the like.

【0014】本発明におけるポリエステルおよび二軸配
向ポリエステルフィルムを製造するにあたり、必要によ
り酸化防止剤、可塑剤、帯電防止剤、耐候剤、末端封鎖
剤等の添加剤を適宜使用することができる。また、フィ
ルムに滑り性を付与するためにポリエステルに無機微細
粒子及び/または有機微細粒子を含有させてもよい。か
かる微細粒子としては例えば、リン酸リチウム、リン酸
カルシウム、リン酸マグネシウム、カオリン、タルク、
炭酸マグネシウム、炭酸カルシウム、炭酸バリウム、硫
酸カルシウム、酸化アルミニウム、酸化ジルコニウム、
酸化ケイ素、酸化チタン、フッ化リチウム、カーボンブ
ラック、ポリスチレン粒子等を挙げることができる。こ
れら微細粒子の平均粒径は0.005〜5.0μmが好
ましく、更には0.01〜3.0μmが好ましい。また
添加量はポリエステルに対して0.05〜5.0重量%
が好ましく、更には0.1〜3.0重量%が好ましい。
微細粒子の形状は球状、塊状、偏平状等任意でよく、硬
度、比重、比表面積等も任意とすることができる。
In producing the polyester and the biaxially oriented polyester film of the present invention, if necessary, additives such as an antioxidant, a plasticizer, an antistatic agent, a weatherproofing agent and a terminal blocking agent can be appropriately used. In addition, the polyester may contain inorganic fine particles and / or organic fine particles in order to impart slipperiness to the film. Examples of such fine particles include lithium phosphate, calcium phosphate, magnesium phosphate, kaolin, talc,
Magnesium carbonate, calcium carbonate, barium carbonate, calcium sulfate, aluminum oxide, zirconium oxide,
Examples thereof include silicon oxide, titanium oxide, lithium fluoride, carbon black and polystyrene particles. The average particle size of these fine particles is preferably 0.005 to 5.0 μm, and more preferably 0.01 to 3.0 μm. The addition amount is 0.05 to 5.0% by weight with respect to the polyester.
Is more preferable, and 0.1 to 3.0% by weight is more preferable.
The shape of the fine particles may be spherical, lumpy, flattened, etc., and hardness, specific gravity, specific surface area, etc. may also be arbitrary.

【0015】[0015]

【実施例】以下実施例によって本発明を詳説する。なお
ポリエステル及びフィルムの特性は以下の方法により測
定した。
The present invention will be described in detail with reference to the following examples. The properties of polyester and film were measured by the following methods.

【0016】(1)ポリエステルの極限粘度 ポリエステルをオルソクロロフェノールに溶解し、25
℃において測定した。
(1) Intrinsic viscosity of polyester Dissolve polyester in orthochlorophenol and prepare 25
It was measured at ° C.

【0017】(2)フィルムの延伸性 乾燥したポリエステルチップを押出し機により押出し、
厚さ100μmの未延伸フィルムとした。この未延伸シ
ートを同時二軸延伸装置を用いて、90℃で3000m
m/minの延伸速度で4倍に同時二軸延伸した。上記
延伸を10回行い、フィルムの延伸性を以下の基準で評
価し、2級以上を合格とした。 1級 …… 8回以上破れることなく、二軸延伸できた
もの 2級 …… 6回以上8回未満破れることなく、二軸延
伸できたもの 3級 …… 二軸延伸できたものが6回未満であるもの
(2) Stretchability of film Dry polyester chips are extruded by an extruder,
The film was an unstretched film having a thickness of 100 μm. This unstretched sheet is 3000 m at 90 ° C. using a simultaneous biaxial stretching device.
Simultaneous biaxial stretching was performed 4 times at a stretching speed of m / min. The above stretching was carried out 10 times, the stretchability of the film was evaluated according to the following criteria, and grade 2 or higher was passed. 1st grade …… 8 times or more that can be biaxially stretched without tearing 2nd grade …… 6 times or more but less than 8 times that can be biaxially stretched without tearing 3rd grade …… 6 times that can be biaxially stretched Less than

【0018】(3)ヤング率、破断強度、破断伸度 二軸延伸フィルムから長さ150mm、幅10mmの試
料を切り出し、この試料をオリエンテック社製引っ張り
試験機を用い、初期長100mm、引っ張り速度300
mm/minの条件で引っ張り、得られた荷重−歪曲線
からヤング率、破断強度、破断伸度を求めた。なお、二
軸延伸フィルムの長手方向及び幅方向の測定値は、各方
向を試料の長さ方向として切り出した試料について測定
したものである。
(3) Young's modulus, breaking strength, breaking elongation A sample having a length of 150 mm and a width of 10 mm was cut out from the biaxially stretched film, and the sample was used with a tensile tester manufactured by Orientec Co., Ltd. to have an initial length of 100 mm and a pulling speed. 300
The Young's modulus, the breaking strength and the breaking elongation were obtained from the load-strain curve obtained by pulling under the condition of mm / min. The measured values in the longitudinal direction and the width direction of the biaxially stretched film are measured for a sample cut out with each direction taken as the length direction of the sample.

【0019】実施例1 テレフタル酸ジメチル150重量部、トリメリット酸ト
リメチル0.98重量部(ポリエステルの酸成分に対し
て0.5モル%)、エチレングリコール96.4重量
部、酢酸カルシウム0.14重量部を精留塔、留出コン
デンサを備えたフラスコに仕込み、攪拌しながら150
〜240℃に加熱しメタノールを留出させエステル交換
反応を行った。ほぼ理論量のメタノールが留出した後リ
ン酸トリメチル0.06重量部、三酸化アンチモン0.
05重量部を添加し、反応物を留出コンデンサを備えた
反応器に移した。ついで攪拌しながら反応器内を徐々に
0.5mmHgまで減圧するとともに290℃まで昇温
し重縮合反応を行った。このようにして得られた共重合
ポリエステルの極限粘度は0.75であった。
Example 1 150 parts by weight of dimethyl terephthalate, 0.98 parts by weight of trimethyl trimellitate (0.5 mol% with respect to the acid component of polyester), 96.4 parts by weight of ethylene glycol, and 0.14 of calcium acetate. Part by weight is charged into a flask equipped with a rectification column and a distillation condenser, and stirred to 150
It heated at -240 degreeC, the methanol was distilled off, and the transesterification reaction was performed. After distilling out almost the theoretical amount of methanol, 0.06 part by weight of trimethyl phosphate and 0.
05 parts by weight were added and the reaction mass was transferred to a reactor equipped with a distillation condenser. Then, while stirring, the pressure inside the reactor was gradually reduced to 0.5 mmHg and the temperature was raised to 290 ° C. to carry out a polycondensation reaction. The intrinsic viscosity of the copolymerized polyester thus obtained was 0.75.

【0020】このポリエステルチップを160℃で5時
間減圧乾燥した後、T型口金を備えた押出し機を用いて
キャスティングドラムに溶融押出しして未延伸フィルム
を得た。この未延伸フィルムを90℃の延伸温度で長手
方向に3.5倍に延伸した。続いてこの一軸延伸フィル
ムをステンタを用いて90℃の延伸温度で幅方向に4.
0倍に延伸した。更にこの二軸延伸フィルムを定長下2
00℃で30秒間熱処理し、厚さ約8μmの二軸延伸フ
ィルムを得た。この二軸延伸フィルムの機械特性及び未
延伸フィルムの延伸性を表1に示す。本発明の二軸延伸
ポリエステルフィルムは高い破断強度とヤング率を有し
ており、かつ延伸性も良好であった。
This polyester chip was dried under reduced pressure at 160 ° C. for 5 hours and then melt-extruded into a casting drum using an extruder equipped with a T-type die to obtain an unstretched film. This unstretched film was stretched 3.5 times in the longitudinal direction at a stretching temperature of 90 ° C. Subsequently, this uniaxially stretched film was stretched in the width direction at a stretching temperature of 90 ° C. using a stenter.
It was stretched to 0 times. Furthermore, this biaxially stretched film is
Heat treatment was performed at 00 ° C. for 30 seconds to obtain a biaxially stretched film having a thickness of about 8 μm. The mechanical properties of this biaxially stretched film and the stretchability of the unstretched film are shown in Table 1. The biaxially stretched polyester film of the present invention had high breaking strength and Young's modulus, and also had good stretchability.

【0021】比較実施例1 テレフタル酸ジメチル150重量部、エチレングリコー
ル96重量部からポリエチレンテレフタレートを実施例
1と同様に重合し、二軸延伸フィルムを得た。この二軸
延伸フィルムの強度特性及び未延伸フィルムの延伸性を
表1に示す。この結果から明らかなように、延伸性には
優れているものの、機械特性に劣るものであった。
Comparative Example 1 Polyethylene terephthalate was polymerized from 150 parts by weight of dimethyl terephthalate and 96 parts by weight of ethylene glycol in the same manner as in Example 1 to obtain a biaxially stretched film. Table 1 shows the strength characteristics of the biaxially stretched film and the stretchability of the unstretched film. As is clear from this result, the stretchability was excellent, but the mechanical properties were poor.

【0022】実施例2〜6 共重合成分としてトリメリット酸トリメチルまたはトリ
メチロールプロパンを用い、共重合量、極限粘度を変え
た共重合ポリエステルを実施例1と同様に重合した。こ
のポリエステルを用いて実施例1と同様の条件で二軸延
伸フィルムを得た。この二軸延伸フィルムの機械特性及
び未延伸フィルムの延伸性を表1に示した。実施例2〜
6はいずれも本発明の範囲内のものであり、優れた強
度、ヤング率を有し、また延伸性も良好であった。
Examples 2 to 6 Copolymerized polyesters in which trimethyl trimellitate or trimethylolpropane was used as the copolymerization component and the copolymerization amount and the intrinsic viscosity were changed were polymerized in the same manner as in Example 1. Using this polyester, a biaxially stretched film was obtained under the same conditions as in Example 1. The mechanical properties of this biaxially stretched film and the stretchability of the unstretched film are shown in Table 1. Examples 2 to
All of 6 were within the range of the present invention, and had excellent strength and Young's modulus, and also had good stretchability.

【0023】比較実施例2 実施例1と同様の方法でポリエチレンテレフタレートに
トリメリット酸トリメチルを0.5モル%共重合し、極
限粘度0.58の共重合ポリエステルを得た。このポリ
エステルの二軸延伸フィルムの機械特性及び未延伸フィ
ルムの延伸性の評価結果を表1に示す。比較実施例2は
ポリエステルの極限粘度が本発明の範囲外であり、フィ
ルムの延伸性は良好であったが破断強度、ヤング率に劣
っていた。
Comparative Example 2 Polyethylene terephthalate was copolymerized with 0.5 mol% of trimethyl trimellitate in the same manner as in Example 1 to obtain a copolymerized polyester having an intrinsic viscosity of 0.58. Table 1 shows the evaluation results of the mechanical properties of the biaxially stretched film of this polyester and the stretchability of the unstretched film. In Comparative Example 2, the intrinsic viscosity of the polyester was out of the range of the present invention, and although the stretchability of the film was good, the breaking strength and Young's modulus were poor.

【0024】比較実施例3 実施例1と同様の方法でポリエチレンテレフタレートに
トリメチロールプロパンを1.0モル%共重合し、極限
粘度0.67の共重合ポリエステルを得た。このポリマ
を更に210℃、0.5mmHgで固相重合し、極限粘
度1.20の共重合ポリエステルを得た。このポリエス
テルフィルムの延伸性評価を行なったところ、3級で延
伸性に劣るものであった。また実施例1と同様に二軸延
伸フィルムを製膜したところ、延伸工程で膜破れが多発
し、安定してフィルムを製造することができなかった。
Comparative Example 3 In the same manner as in Example 1, polyethylene terephthalate was copolymerized with 1.0 mol% of trimethylolpropane to obtain a copolymerized polyester having an intrinsic viscosity of 0.67. This polymer was further solid-phase polymerized at 210 ° C. and 0.5 mmHg to obtain a copolyester having an intrinsic viscosity of 1.20. When the stretchability of this polyester film was evaluated, it was grade 3 and the stretchability was poor. When a biaxially stretched film was formed in the same manner as in Example 1, film breakage frequently occurred in the stretching process, and a stable film could not be produced.

【0025】比較実施例4 実施例1と同様にしてポリエチレンテレフタレートにト
リメリット酸トリメチルを3.5モル%共重合し、共重
合ポリエステルを製造したところ、重縮合反応時にポリ
エステルがゲル化し安定してポリマを製造することがで
きなかった。
Comparative Example 4 In the same manner as in Example 1, polyethylene terephthalate was copolymerized with trimethyl trimellitate in an amount of 3.5 mol% to produce a copolymerized polyester. The polyester was gelated and stabilized during the polycondensation reaction. The polymer could not be manufactured.

【0026】[0026]

【表1】 表中の略号は以下の通りである。[Table 1] The abbreviations in the table are as follows.

【0027】MD :フィルムの長手方向 TD :フィルムの幅方向 TMTM:トリメリット酸トリメチル TMP :トリメチロールプロパンMD: longitudinal direction of film TD: width direction of film TMTM: trimethyl trimellitate TMP: trimethylolpropane

【0028】[0028]

【発明の効果】本発明の二軸延伸ポリエステルフィルム
は高強力、高弾性という優れた機械的特性を有し、薄膜
化しても低コストでかつ安定な製膜が可能であり、磁気
テープ用、コンデンサー用、感熱転写用等の用途、特に
磁気テープ用途に好適に使用される。
INDUSTRIAL APPLICABILITY The biaxially stretched polyester film of the present invention has excellent mechanical properties such as high strength and high elasticity, can be formed into a thin film at a low cost and with stable properties, and can be used for magnetic tapes. It is preferably used for applications such as condensers and thermal transfer, especially for magnetic tape applications.

Claims (1)

【特許請求の範囲】[Claims] 【請求項1】 分子内に3個以上のエステル形成性官能
基を有する化合物を0.05〜3.0モル%含み、極限
粘度が0.64〜1.1のポリエステルからなり、ヤン
グ率が410kg/mm2 以上であることを特徴とする
二軸延伸ポリエステルフィルム。
1. A polyester comprising 0.05 to 3.0 mol% of a compound having 3 or more ester-forming functional groups in its molecule and having an intrinsic viscosity of 0.64 to 1.1 and having a Young's modulus of A biaxially stretched polyester film having a weight of 410 kg / mm 2 or more.
JP13246592A 1992-05-25 1992-05-25 Biaxially stretched polyester film Expired - Fee Related JP3185355B2 (en)