JPH0677448B2 - Non-aqueous electrolyte battery - Google Patents

Non-aqueous electrolyte battery

Info

Publication number
JPH0677448B2
JPH0677448B2 JP61069090A JP6909086A JPH0677448B2 JP H0677448 B2 JPH0677448 B2 JP H0677448B2 JP 61069090 A JP61069090 A JP 61069090A JP 6909086 A JP6909086 A JP 6909086A JP H0677448 B2 JPH0677448 B2 JP H0677448B2
Authority
JP
Japan
Prior art keywords
positive electrode
aqueous electrolyte
mixture
electrolyte battery
active material
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP61069090A
Other languages
Japanese (ja)
Other versions
JPS62226564A (en
Inventor
義久 日野
博之 高柳
吾恵 吉岡
Original Assignee
富士電気化学株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 富士電気化学株式会社 filed Critical 富士電気化学株式会社
Priority to JP61069090A priority Critical patent/JPH0677448B2/en
Publication of JPS62226564A publication Critical patent/JPS62226564A/en
Publication of JPH0677448B2 publication Critical patent/JPH0677448B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】 〈産業上の利用分野〉 この発明は非水電解液電池に関し、詳しくは、三酸化モ
リブデンMoO3を正極活物質とする非水電解液電池に関す
るものである。
The present invention relates to a non-aqueous electrolyte battery, and more particularly to a non-aqueous electrolyte battery using molybdenum trioxide MoO 3 as a positive electrode active material.

〈従来の技術〉 上記のような非水電解液電池では、リチウムやナトリウ
ムの如きアルカリ金属あるいはアルカリ土類金属などを
負極活物質とし、非水系の電解液を用いる構成が採られ
ている。
<Prior Art> The above-mentioned non-aqueous electrolyte battery employs a configuration in which an alkali metal such as lithium or sodium or an alkaline earth metal is used as a negative electrode active material and a non-aqueous electrolyte is used.

この非水電解液電池において、三酸化モリブデンを活物
質とする正極は、従来、三酸化モリブデン粉末と黒鉛な
どの導電剤粉末との混合物にバインダーとして四フッ化
エチレン樹脂(PTFE)粉末などを加えた合剤を加圧成形
したものが用いられている。
In this non-aqueous electrolyte battery, the positive electrode using molybdenum trioxide as the active material has conventionally been prepared by adding tetrafluoroethylene resin (PTFE) powder as a binder to a mixture of molybdenum trioxide powder and conductive agent powder such as graphite. A mixture obtained by pressing the mixture is used.

〈発明が解決しようとする問題点〉 ところで、この種の電池において正極の性状を改良して
放電特性の向上を図る場合、正極中の活物質である三酸
化モリブデンの表面積を増加させると共に正極合剤単位
体積中における外部と連通した気孔の割合(気孔率)を
高くして正極に電解液を充分に含浸・保持させることが
必要となる。そして、上記従来の正極では粉体(三酸化
モリブデン粉末,導電剤粉末,バインダー粉末など)混
合物を加圧成形しており、この正極を用いて活物質表面
積増加及び気孔率の向上を図るには、成形圧力を極端に
下げると共に活物質粒子を微粉化することが必要とな
る。
<Problems to be Solved by the Invention> By the way, in the case of improving the discharge characteristics by improving the properties of the positive electrode in this type of battery, the surface area of molybdenum trioxide, which is the active material in the positive electrode, is increased and the positive electrode mixture is increased. It is necessary to increase the ratio of pores communicating with the outside (porosity) in the unit volume of the agent to sufficiently impregnate and retain the electrolytic solution in the positive electrode. In the above-mentioned conventional positive electrode, a mixture of powders (molybdenum trioxide powder, conductive agent powder, binder powder, etc.) is pressure-molded. In order to increase the active material surface area and the porosity by using this positive electrode, However, it is necessary to reduce the molding pressure extremely and to make the active material particles fine.

しかしながら、このように成形圧力の低下並びに粒子微
粉化をした場合は圧粉体である正極の機械的強度の低下
を招く。また微粉化にも製法上制約があり、平均粒径3
μ程度が限度であって機械的にそれ以上細かくすること
は困難である。更に、余り細かくしても粒子が独立しが
ちとなって電子電導不足を招くので個々の活物質粒子が
有効に利用されなくなる等といった問題があることか
ら、上記放電特性の向上を図ることは従来技術では困難
であった。
However, when the molding pressure is reduced and the particles are pulverized in this manner, the mechanical strength of the positive electrode, which is a green compact, is reduced. In addition, there are restrictions on the pulverization due to the manufacturing method, and the average particle size is 3
There is a limit of about μ, and it is difficult to make it mechanically finer. Furthermore, even if it is made too fine, particles tend to become independent and lead to electron conduction deficiency, so that there is a problem that individual active material particles cannot be effectively used. It was difficult with technology.

〈問題点を解決するための手段〉 この発明の非水電解液電池は、モリブデン酸H2MoO4を含
んでなる合剤を成形後に加熱脱水処理してなる正極を備
えたことを要旨とする。
<Means for Solving Problems> The non-aqueous electrolyte battery of the present invention is characterized in that it is provided with a positive electrode formed by heat-dehydrating a mixture containing molybdate H 2 MoO 4 after molding. .

上記のような加熱脱水処理は、成形合剤を約150℃以上
の温度で加熱することで達成される。加熱温度が150℃
以下だとモリブデン酸の熱分解並びに脱水が不十分とな
る。また、加熱温度が800℃以上になると生成した三酸
化モリブデン(融点約795℃)が融解あるいは昇華して
しまうので、上限温度は800℃にする必要がある。尚、
加熱後に公知の脱水処理(例えば真空乾燥処理)を別途
行なって脱水の完全化を図るようにしてもよい。
The heat dehydration treatment as described above is achieved by heating the molding mixture at a temperature of about 150 ° C. or higher. Heating temperature is 150 ℃
If it is below, thermal decomposition and dehydration of molybdic acid will be insufficient. In addition, since the generated molybdenum trioxide (melting point: about 795 ° C) melts or sublimes when the heating temperature is 800 ° C or higher, the upper limit temperature needs to be 800 ° C. still,
A known dehydration treatment (for example, vacuum drying treatment) may be separately performed after heating to complete dehydration.

〈作用〉 上記のようにモリブデン酸H2MoO4を含んだ合剤を成形後
に加熱脱水処理することにより、次式で示したように合
剤中のモリブデン酸は三酸化モリブデンと水に熱分解す
ると共に成形合剤中の生成水分の外部飛散によって成形
合剤中に新たな気孔(外部と連通した気孔)が多数でき
て合剤の気孔率が増大し、合剤単位体積当りの三酸化モ
リブデンの表面積が著しく増大する。
<Function> As described above, by heat-dehydrating the mixture containing molybdate H 2 MoO 4 after molding, the molybdic acid in the mixture is thermally decomposed into molybdenum trioxide and water as shown in the following formula. At the same time, due to the external scattering of the generated water in the molding mixture, many new pores (pores communicating with the outside) are formed in the molding mixture, increasing the porosity of the mixture, and molybdenum trioxide per unit volume of the mixture. Significantly increases the surface area of.

H2MoO4→MoO3+H2O↑ よって、このように加熱脱水処理した成形合剤を正極と
して用いることで、気孔増大分だけ正極の含電解液量が
増量できると共に、正極活物質の有効表面積が増大す
る。
H 2 MoO 4 → MoO 3 + H 2 O ↑ Therefore, by using the heat-dehydrated molding mixture as the positive electrode, the amount of electrolyte solution in the positive electrode can be increased by the amount of increased pores, and the positive electrode active material can be effectively used. Increased surface area.

〈実施例〉 以下、この発明を偏平形リチウム電池に適用した実施例
について説明する。
<Example> An example in which the present invention is applied to a flat lithium battery will be described below.

平均粒径3μのモリブデン酸粉末と黒鉛粉末とPTFE粉末
とを重量比で4:1:0.4の割合で混合した。次いで、ステ
ンレスネット製の正極集電体を内底面中央にスポット溶
接して固着した正極缶の内底面に金型を用いて上記で得
た混合物を直接盛込み、1.5ton/cm2の圧力でこの混合物
をディスク状に加圧成形すると共に、この成形体を上記
正極集電体を介して正極缶内底面に圧着した。加圧成形
後、これらを真空中で温度250℃で15時間加熱した。こ
の加熱により上記成形体中のモリブデン酸が三酸化モリ
ブデンと水に分解すると共に生成した水分が成形体から
飛散して成形体の脱水が行なえた。
Molybdic acid powder having an average particle diameter of 3μ, graphite powder and PTFE powder were mixed at a weight ratio of 4: 1: 0.4. Next, a positive electrode current collector made of stainless steel net was spot-welded to the center of the inner bottom surface and fixed to the inner bottom surface of the positive electrode can using a mold to directly pour the mixture obtained above into a positive pressure of 1.5 ton / cm 2. The mixture was pressure-molded into a disk shape, and the molded body was pressure-bonded to the inner bottom surface of the positive electrode can via the positive electrode current collector. After pressure molding, these were heated in vacuum at a temperature of 250 ° C. for 15 hours. By this heating, the molybdic acid in the molded body was decomposed into molybdenum trioxide and water, and the generated water was scattered from the molded body, so that the molded body could be dehydrated.

そして、以上のような加熱脱水処理をした成形体を正極
とし、この正極に飽和吸液量の電解液を含浸・吸液さ
せ、第1図に示したように、正極1、正極缶2、並びに
正極集電体3とからなる正極部分と、ステンレス製の負
極缶4の内底面にスポット溶接したステンレスネットか
らなる負極集電体5を介して金属リチウム製の負極6を
負極缶内底面に圧着してなる負極部分とを、ポリプロピ
レン不織布製のセパレータ7を介して対向させ、またポ
リプロピレン製のガスケット8を周縁部に組合せ、公知
の方法によって2016形のコイン形リチウム電池(本発明
品A)を作った。尚、上記の電解液としては、プロピレ
ンカーボネート(PC)と2-メチル‐テトラヒドロフラン
とを容量比で1:1で混合した溶媒に、6フッ化リン酸リ
チウムLiPF6を溶質として1モル濃度混ぜたものを用い
た。
Then, the molded body that has been subjected to the heat dehydration treatment as described above is used as a positive electrode, and this positive electrode is impregnated and absorbed with an electrolyte solution having a saturated absorption amount, and as shown in FIG. 1, the positive electrode 1, the positive electrode can 2, In addition, a negative electrode 6 made of metallic lithium is placed on the inner bottom surface of the negative electrode can via a positive electrode portion made up of the positive electrode current collector 3 and a negative electrode current collector 5 made of stainless net spot-welded to the inner bottom surface of the negative electrode can 4 made of stainless steel. A 2016 type coin-shaped lithium battery (the present invention product A) is made to face the pressure-bonded negative electrode portion with a polypropylene nonwoven fabric separator 7 in between, and a polypropylene gasket 8 is combined with the peripheral portion, by a known method. made. As the above-mentioned electrolytic solution, 1 molar concentration of lithium hexafluorophosphate LiPF 6 was mixed as a solute in a solvent in which propylene carbonate (PC) and 2-methyl-tetrahydrofuran were mixed at a volume ratio of 1: 1. I used one.

一方、従来電池に用いられる三酸化モリブデン粉末(平
均粒径3μ)と黒鉛粉末とPTFE粉末とを重量比で4:1:0.
4の割合で混合後1.5ton/cm2の圧力でコイン状に加圧成
形し、次いで温度120℃で5時間真空乾燥したものを正
極とした以外は同様にして、2016形のコイン形リチウム
電池(従来品B)を作った。尚、両電池に組込む正極の
成形厚を調節して本発明品Aと従来品Bとの理論放電容
量を共に30mAHに揃えた。
On the other hand, the weight ratio of molybdenum trioxide powder (average particle size 3μ), graphite powder and PTFE powder used in conventional batteries is 4: 1: 0.
2016 type coin-type lithium battery except that the mixture was mixed at a ratio of 4 and pressure-molded into a coin shape at a pressure of 1.5 ton / cm 2 and then vacuum dried at a temperature of 120 ° C. for 5 hours to obtain a positive electrode. (Conventional product B) was made. The theoretical discharge capacities of the product A of the present invention and the product B of the prior art were both adjusted to 30 mAH by adjusting the molding thickness of the positive electrode incorporated in both batteries.

以上の2つの電池について、2mAの定電流で放電させた
場合の電池の端子電圧(V)の経時変化を調べた。
With respect to the above two batteries, the change with time of the terminal voltage (V) of the batteries when discharged at a constant current of 2 mA was examined.

結果は第2図に示す通りであり、放電終止電圧を1.7
(V)とした場合、本発明品Aの放電時間は従来品Bの
1.2倍であり、その分放電容量が増大している。これは
本発明品Aで用いた正極が従来品Bのものに較べて気孔
率が高いので正極の吸液(吸電解液)量が多く、また活
物質である三酸化モリブデンの表面積が大きいので活物
質利用率が高いことによるものと考えられる。
The results are shown in Fig. 2, and the discharge end voltage was 1.7.
In the case of (V), the discharge time of the product A of the present invention is
It is 1.2 times, and the discharge capacity is increased accordingly. This is because the positive electrode used in the product A of the present invention has a higher porosity than that of the conventional product B, so that the amount of liquid absorption (electrolyte absorption liquid) of the positive electrode is large and the surface area of molybdenum trioxide which is an active material is large. It is thought that this is because the active material utilization rate is high.

また、両電池の正極の気孔率(%)を調べた結果を参考
のため第1表に示した。
The results of examining the porosity (%) of the positive electrodes of both batteries are shown in Table 1 for reference.

尚、この発明を非水電解液一次電池及び二次電池の双方
に適用できることは言うまでもない。
It goes without saying that the present invention can be applied to both non-aqueous electrolyte primary batteries and secondary batteries.

〈発明の効果〉 以上のように構成されるこの発明の非水電解液電池によ
れば、正極の気孔率を高めることができて正極に電解液
を充分に含浸・吸液させることができると共に、正極中
の活物質である三酸化モリブデンの有効表面積が増大し
て正極での活物質利用率が高まる結果、電池放電特性の
向上を図ることができるという効果を奏する。
<Effects of the Invention> According to the non-aqueous electrolyte battery of the present invention configured as described above, the porosity of the positive electrode can be increased, and the positive electrode can be sufficiently impregnated with and absorb the electrolytic solution. As a result of increasing the effective surface area of molybdenum trioxide, which is the active material in the positive electrode, and increasing the utilization rate of the active material in the positive electrode, it is possible to improve the battery discharge characteristics.

【図面の簡単な説明】[Brief description of drawings]

第1図は本発明の実施例の電池構造を示した断面図、第
2図は本発明品と従来品との放電時の端子電圧の変化を
示したグラフである。 1……正極、2……正極缶、4……負極缶、6……負
極。
FIG. 1 is a cross-sectional view showing a battery structure of an embodiment of the present invention, and FIG. 2 is a graph showing changes in the terminal voltage during discharge of the product of the present invention and the conventional product. 1 ... Positive electrode, 2 ... Positive electrode can, 4 ... Negative electrode can, 6 ... Negative electrode.

Claims (1)

【特許請求の範囲】[Claims] 【請求項1】モリブデン酸を含んでなる合剤を成形後に
加熱脱水処理してなる正極を備えたことを特徴とする非
水電解液電池。
1. A non-aqueous electrolyte battery comprising a positive electrode obtained by subjecting a mixture containing molybdic acid to heat treatment and dehydration after molding.
JP61069090A 1986-03-27 1986-03-27 Non-aqueous electrolyte battery Expired - Fee Related JPH0677448B2 (en)