JPH07101143A - Ink jet recording method - Google Patents

Ink jet recording method

Info

Publication number
JPH07101143A
JPH07101143A JP5274988A JP27498893A JPH07101143A JP H07101143 A JPH07101143 A JP H07101143A JP 5274988 A JP5274988 A JP 5274988A JP 27498893 A JP27498893 A JP 27498893A JP H07101143 A JPH07101143 A JP H07101143A
Authority
JP
Japan
Prior art keywords
ink
paper
recording
surface tension
ink jet
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP5274988A
Other languages
Japanese (ja)
Other versions
JP3724820B2 (en
Inventor
Takashi Ueno
隆 上野
Yoshio Yoshida
義雄 吉田
Yoshihiro Kuroyama
良弘 黒山
Yoshifumi Iimori
良文 飯森
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Paper Industries Co Ltd
Jujo Paper Co Ltd
Original Assignee
Nippon Paper Industries Co Ltd
Jujo Paper Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Paper Industries Co Ltd, Jujo Paper Co Ltd filed Critical Nippon Paper Industries Co Ltd
Priority to JP27498893A priority Critical patent/JP3724820B2/en
Publication of JPH07101143A publication Critical patent/JPH07101143A/en
Application granted granted Critical
Publication of JP3724820B2 publication Critical patent/JP3724820B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To provide an ink jet recording method for recording a printing image of high printing quality on uncoated type recording paper. CONSTITUTION:In an ink jet recording method applying an ink droplet to uncoated paper, the surface tension gamma1 of the ink droplet is about 24<=gamma1<=70dyn/cm and the critical surface tension gammac of the uncoated paper is about 22<=gammac<=1.6(gamma1--24)<1/2>+22dyn/cm.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、インクジェット記録方
法に関し、特にプレーンペーパー等の非塗工紙に高印字
品質の記録をするためのインクジェット記録方法に関す
る。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to an ink jet recording method, and more particularly to an ink jet recording method for recording a high print quality on uncoated paper such as plain paper.

【0002】[0002]

【従来技術】インクジェット記録方式は、種々の機構に
よりインクの小滴を吐出し、記録用紙上に付着させるこ
とによりドットを形成し記録を行うものであり、ドット
インパクトタイプの記録方式に比べて騒音がない上、フ
ルカラー化が容易であり、高速印字が可能であるなどの
利点がある。
2. Description of the Related Art The ink jet recording method is one in which small droplets of ink are ejected by various mechanisms and adhered onto a recording sheet to form dots for recording, which is more noise-free than the dot impact type recording method. In addition, there are advantages that it is easy to make full color and high-speed printing is possible.

【0003】しかしながら、インクジェット記録におい
ては、使用するインクと紙のマッチングが重要であり、
このマッチングが不適切であると、インクがにじんだり
インク濃度が低下して高品位の画像を得ることがず、ま
た、インクの吸収速度が遅くなって高速記録に適さなく
なったり、フルカラー化が困難となる。そこで、従来、
インクジェット記録用紙としては、原紙の表面にインク
の吸収を促進することのできる顔料を含有した記録層を
設ける、いわゆる塗工紙が専用紙として使用されてい
る。
However, in ink jet recording, it is important to match the ink used and the paper,
If this matching is inadequate, the ink will bleed or the ink density will drop, and a high-quality image will not be obtained, and the ink absorption speed will be slow, making it unsuitable for high-speed recording, and making full-color difficult. Becomes So, conventionally,
As the ink jet recording paper, so-called coated paper is used as a special paper in which a recording layer containing a pigment capable of promoting ink absorption is provided on the surface of the base paper.

【0004】しかしながら、この塗工紙は専用紙である
ために高価であるため、安価な非塗工紙を使用して、高
品質のインクジェット記録を得ることが望まれていた。
そこで、非塗工紙タイプのインクジェット記録用紙とし
て、表面サイズ剤(澱粉、ポリビニルアルコール、スチ
レン−アクリル系樹脂)等を添加したり、原紙に使用す
るパルプの叩解度を高くした記録紙が開発されている。
However, since this coated paper is expensive because it is a special paper, it has been desired to obtain high quality ink jet recording by using inexpensive uncoated paper.
Therefore, as an uncoated paper type inkjet recording paper, a recording paper was developed in which a surface sizing agent (starch, polyvinyl alcohol, styrene-acrylic resin) was added, or the pulp used as the base paper had a high beating degree. ing.

【0005】しかしながら、例えば表面サイズ剤を過剰
に添加することによってインクのにじみを抑えた非塗工
紙の場合には、インクの吸収速度が低下し、叩解度を高
くすることによってにじみを減少させた非塗工紙の場合
には、不透明性が低下したり、地合が悪化する等の欠点
があり、多色のインクジェット記録に適応することが困
難であるのみならず、単色のインクジェット記録に対し
ても、十分に満足することのできる品質の記録を得るこ
とはできなかった。
However, in the case of uncoated paper in which ink bleeding is suppressed by adding an excessive surface sizing agent, for example, the ink absorption speed decreases, and the beating degree is increased to reduce bleeding. In the case of uncoated paper, there are drawbacks such as reduced opacity and deterioration of formation, which makes it difficult to adapt to multi-color inkjet recording and also to single-color inkjet recording. Again, we were not able to obtain a satisfactory quality record.

【0006】そこで、本発明者らは、表面サイズ剤の種
類やその添加量を変更することにより、更に改善したイ
ンクジェット記録用紙を提案をした(特願平4−286
874号、特願平4−356137号)。しかしなが
ら、インクジェットプリンター用のインクはメーカーや
機種によって異なるため、その物性値も様々である。従
って、ある機種、あるインクに対して良好な記録用紙で
あっても、他の機種やインクに対しては良好でないとい
う場合が多々存在する。
Therefore, the present inventors have proposed an improved inkjet recording paper by changing the type of surface sizing agent and the amount thereof added (Japanese Patent Application No. 4-286).
874, Japanese Patent Application No. 4-356137). However, since inks for inkjet printers differ depending on manufacturers and models, their physical property values are also various. Therefore, there are many cases where a recording paper that is good for a certain model and a certain ink is not good for another model and a certain ink.

【0007】また、普通紙(非塗工紙)対応のカラーイ
ンクジェットプリンターに対するニーズが高まるに伴っ
てインクの吸収性がより重要となるので、インクの吸収
性を良好なものとするために、記録インクの表面張力を
低下させる傾向にある。しかしながら、記録インクの表
面張力が低い領域では、記録紙にサイズ剤を添加する等
の従来の方法だけでは、インクのにじみ(ドット形状の
悪化)を防止することができず、新たな対応が模索され
ていた。
In addition, as the need for a color ink jet printer compatible with plain paper (non-coated paper) increases, the ink absorbency becomes more important. Therefore, in order to improve the ink absorbability, recording is performed. It tends to lower the surface tension of the ink. However, in the area where the surface tension of the recording ink is low, ink bleeding (deterioration of dot shape) cannot be prevented only by the conventional method such as adding a sizing agent to the recording paper, and new measures are sought. It had been.

【0008】[0008]

【発明が解決しようとする課題】そこで、本発明者ら
は、非塗工紙を用いて、インクジェット記録によって良
好な多色記録を得るために鋭意検討した結果、インクジ
ェット記録用紙の臨界表面張力と記録インクの表面張力
との間に一定の関係を持たせた場合には、高い品質の多
色記録が得られることを見出し、本発明に到達した。
Therefore, as a result of intensive investigations by the present inventors to obtain good multicolor recording by ink jet recording using uncoated paper, it was found that the critical surface tension of the ink jet recording paper was The present invention has been completed by finding that high quality multicolor recording can be obtained when a certain relationship is provided between the surface tension of the recording ink and the surface tension of the recording ink.

【0009】従って、本発明の第1の目的は、非塗工タ
イプの記録紙を用いて、インク(ドット)のにじみが少
なく、高い品質の記録を得ることができるインクジェッ
ト記録方法を提供することにある。本発明の第2の目的
は、非塗工タイプの記録紙に、良好な多色記録を迅速に
行うためのインクジェット記録方法を提供することにあ
る。
Therefore, a first object of the present invention is to provide an ink jet recording method using a non-coated type recording paper, in which ink (dot) bleeding is small and high quality recording can be obtained. It is in. A second object of the present invention is to provide an ink jet recording method for rapidly performing good multicolor recording on a non-coated type recording paper.

【0010】[0010]

【課題を解決するための手段】本発明の上記の諸目的
は、非塗工紙にインク滴を施すインクジェット記録方法
であって、前記インク滴の表面張力γ1 が約24≦γ1
≦70dyn/cmであると共に、前記非塗工紙の臨界
表面張力γc が約22≦γc ≦1.6(γ1 −24)
1/2 +22dyn/cmの範囲であることを特徴とする
インクジェット記録方法により達成された。
The above-mentioned various objects of the present invention are an ink jet recording method for applying ink drops to uncoated paper, wherein the surface tension γ 1 of the ink drops is about 24 ≦ γ 1
≦ 70 dyn / cm in conjunction with which, the critical surface tension gamma c of non-coated paper about 22 ≦ γ c ≦ 1.6 (γ 1 -24)
It was achieved by an ink jet recording method characterized by a range of 1/2 +22 dyn / cm.

【0011】本発明において、非塗工紙とは、原紙の表
面に顔料を3g/m2 以上含有する塗工層を有しない紙
を意味する。本発明のインクジェット記録方法に使用さ
れるインクは、水、又は水と水溶性有機溶剤の混合物を
溶媒とし、必要に応じて界面活性剤、粘度調整剤、表面
張力調整剤等が添加された公知のものの中から適宜選択
して使用することができるが、本発明においては、特に
その表面張力γ1 が、約24〜70dyn/cmの範囲
のものを使用する(図1参照)。
In the present invention, the non-coated paper means a paper which does not have a coating layer containing a pigment of 3 g / m 2 or more on the surface of the raw paper. The ink used in the inkjet recording method of the present invention uses water or a mixture of water and a water-soluble organic solvent as a solvent, and a surfactant, a viscosity adjusting agent, a surface tension adjusting agent, etc., are added as necessary. Among them, those having a surface tension γ 1 of about 24 to 70 dyn / cm are used in the present invention (see FIG. 1).

【0012】記録インクの表面張力が24dyn/cm
未満となると、インクのにじみを抑えることが困難とな
り、70dyn/cmを超えると、インクの乾燥性が不
十分となる。本発明で使用するインクジェット記録用紙
としては、その臨界表面張力が約22〜33dyn/c
mのものを使用する。臨界表面張力が33dyn/cm
を超えると、インクの吸収性は良いがインクがにじみ易
く、記録濃度も低下する。逆に22dyn/cm未満の
場合にはインクの吸収性が不十分となる。
The surface tension of the recording ink is 24 dyn / cm.
When it is less than 70%, it becomes difficult to suppress ink bleeding, and when it exceeds 70 dyn / cm, the drying property of the ink becomes insufficient. The inkjet recording paper used in the present invention has a critical surface tension of about 22 to 33 dyn / c.
Use m. Critical surface tension is 33 dyn / cm
When it exceeds, the ink absorbability is good, but the ink is likely to bleed and the recording density is lowered. On the contrary, if it is less than 22 dyn / cm, the ink absorbency becomes insufficient.

【0013】本発明においては、特に、表面張力が約2
4〜40dyn/cmのインクを用いる場合には、記録
面の臨界表面張力が、約22〜1.6(γ1 −24)
1/2 +22dyn/cmの記録紙に記録することが好ま
しく、表面張力が約40〜70dyn/cmのインクを
用いる場合には、臨界表面張力が約(γ1 −40)1/2
+22〜1.6(γ1 −24)1/2 +22の範囲にある
記録紙を使用することが、何れも、インクの吸収性(乾
燥性)の観点から好ましい。上記の好ましい範囲は、ジ
スマン(Zisman)プロットに基づいて作成した図
1における斜線部で表される。
In the present invention, in particular, the surface tension is about 2.
In the case of using the ink of 4~40dyn / cm, the critical surface tension of the recording surface, about 22~1.6 (γ 1 -24)
1/2 + is preferably recorded on a recording paper 22dyn / cm, if the surface tension is used ink about 40~70dyn / cm, the critical surface tension of about (gamma 1 -40) 1/2
+ 22~1.6 (γ 1 -24) is the use of paper in the range of 1/2 +22, both from the viewpoint of ink absorbing property (drying). The above-mentioned preferable range is represented by the shaded area in FIG. 1 created based on the Zisman plot.

【0014】本発明における記録インクの表面張力及び
インクジェット記録用紙の臨界表面張力は、いずれも公
知の測定手段によって適宜測定することができる。例え
ば、記録インクの表面張力は、協和界面化学株式会社製
の自動界面張力計(PD−Z型)で測定することがで
き、記録用紙の臨界表面張力は、同社の自動接触角計
(CD−Z型)で測定することができる。尚、ここでい
う接触角とは液体(液量4μl)滴下2秒後の値であ
る。
The surface tension of the recording ink and the critical surface tension of the ink jet recording paper in the present invention can be appropriately measured by known measuring means. For example, the surface tension of recording ink can be measured by an automatic interfacial tension meter (PD-Z type) manufactured by Kyowa Interface Science Co., Ltd., and the critical surface tension of recording paper can be measured by an automatic contact angle meter (CD- Z type). The contact angle referred to here is a value 2 seconds after dropping a liquid (liquid volume 4 μl).

【0015】インクジェット記録用紙の基紙は、少なく
とも98〜80重量%の木材パルプ及び2〜20重量%
の填料を含有するものが好ましい。填料としては、炭酸
カルシウム、シリカ、クレー、タルク、カオリナイト、
酸化チタン、プラスチックピグメント等を使用すること
ができる。上記材料の他に、更に、公知の内添サイズ
剤、歩留まり向上剤、紙力増強剤等を必要に応じて添加
することができる。
The base paper of the ink jet recording paper comprises at least 98-80% by weight of wood pulp and 2-20% by weight.
The one containing the filler is preferable. As the filler, calcium carbonate, silica, clay, talc, kaolinite,
Titanium oxide, plastic pigment, etc. can be used. In addition to the above materials, known internal sizing agents, retention aids, paper strength enhancers and the like can be added as required.

【0016】記録面の臨界表面張力を調整する手段とし
ては、例えば表面サイズ剤を用いる方法がある。この場
合の表面サイズ剤としては、高級脂肪酸系、スチレン−
アクリル系、スチレン−マレイン酸系、ポリアクリルア
ミド系の樹脂や、石油系樹脂等を目的に応じて使用する
ことができる。本発明においては、これらの中でも、イ
ンクにじみ抑制の観点から、高級脂肪酸系カチオンサイ
ズ剤を特に好ましく使用することができる。インクジェ
ット記録用紙を製造するために、原紙に塗工する塗工液
には、上記表面サイズ剤の他に、親水性樹脂(澱粉、ポ
リビニルアルコール等)、消泡剤、水溶性アルカリ性
塩、染料定着剤、流動変性剤、染料等も適宜添加され
る。
As a means for adjusting the critical surface tension of the recording surface, there is a method of using a surface sizing agent, for example. In this case, as the surface sizing agent, higher fatty acid type, styrene-
An acrylic resin, a styrene-maleic acid resin, a polyacrylamide resin, a petroleum resin, or the like can be used according to the purpose. In the present invention, among these, higher fatty acid cation sizing agents can be particularly preferably used from the viewpoint of suppressing ink bleeding. In addition to the above-mentioned surface sizing agent, hydrophilic resins (starch, polyvinyl alcohol, etc.), defoaming agents, water-soluble alkaline salts, dye fixing agents are used in the coating liquid applied to base paper for manufacturing inkjet recording paper. Agents, flow modifiers, dyes, etc. are also added as appropriate.

【0017】[0017]

【発明の効果】本発明のインクジェット記録方法によれ
ば、非塗工タイプの記録用紙を使用するにもかかわら
ず、インクの乾燥速度を遅くすることなく、インク(ド
ット)のにじみを最小限に抑えることができるため、高
い解像度で極めて高品質の画像を高速で記録することが
できるのみならず、フルカラー記録も容易である。
According to the ink jet recording method of the present invention, bleeding of ink (dots) can be minimized without slowing the drying speed of the ink, even though a non-coated type recording paper is used. Since this can be suppressed, not only high-quality images with high resolution can be recorded at high speed, but also full-color recording is easy.

【0018】[0018]

【実施例】以下、本発明を実施例によって更に詳述する
が、本発明はこれによって限定されるものではない。
EXAMPLES The present invention will be described in more detail below with reference to examples, but the present invention is not limited thereto.

【0019】実施例1〜8及び比較例1〜7 (1)記録用インク 下記の割合で混合した溶媒中に、色素(C.I.フード
ブルー2)が2mMとなるように加えて調製した、3種
類のインクを使用した。 記録インク(表面張力:69.5dyn/cm) 脱イオン水 100重量部 グリセリン 5重量部
Examples 1 to 8 and Comparative Examples 1 to 7 (1) Recording Ink A dye (CI Food Blue 2) was added to a solvent mixed in the following proportions so that the concentration was 2 mM. Three types of ink were used. Recording ink (surface tension: 69.5 dyn / cm) Deionized water 100 parts by weight Glycerin 5 parts by weight

【0020】 記録インク(表面張力:49.7dyn/cm) 脱イオン水 95重量部 イソプロピルアルコール 5重量部 グリセリン 5重量部 記録インク(表面張力:31.5dyn/cm) 脱イオン水 80重量部 イソプロピルアルコール 20重量部 グリセリン 5重量部Recording ink (surface tension: 49.7 dyn / cm) Deionized water 95 parts by weight Isopropyl alcohol 5 parts by weight Glycerin 5 parts by weight Recording ink (surface tension: 31.5 dyn / cm) Deionized water 80 parts by weight Isopropyl alcohol 20 parts by weight Glycerin 5 parts by weight

【0021】(2)記録用紙 記録用紙 LBKP(c.s.f.350ml)85重量部、カオ
リナイト15重量部、硫酸アルミニウム0.2重量部及
びアルケニルコハク酸無水物系サイズ剤(商品名:サイ
ズパインSA−850、荒川化学工業株式会社製)0.
02重量部を配合して、坪量64g/m2 の上質紙を抄
紙した。
(2) Recording Paper Recording Paper 85 parts by weight of LBKP (csf.350 ml), 15 parts by weight of kaolinite, 0.2 parts by weight of aluminum sulfate and an alkenylsuccinic anhydride sizing agent (trade name: Size Pine SA-850, manufactured by Arakawa Chemical Industries, Ltd.)
02 parts by weight was blended to produce a high-quality paper having a basis weight of 64 g / m 2 .

【0022】得られた上質紙表面に、サイズプレスを用
いてポリビニルアルコール(商品名:ゴーセノールN−
300、日本合成化学株式会社製)1.0重量%、サイ
ズ剤(商品名:ポリマロン360、荒川化学工業株式会
社製)0.1重量%及びリン酸二水素ナトリウム0.2
重量%を含有する水溶液を塗工してインクジェット記録
用紙を得た。
On the surface of the obtained high-quality paper, polyvinyl alcohol (trade name: Gohsenol N-
300, manufactured by Nippon Synthetic Chemical Industry Co., Ltd.) 1.0% by weight, sizing agent (trade name: Polymalon 360, manufactured by Arakawa Chemical Industry Co., Ltd.) 0.1% by weight, and sodium dihydrogen phosphate 0.2.
An ink jet recording paper was obtained by applying an aqueous solution containing 10% by weight.

【0023】記録用紙 記録用紙で抄紙した上質紙表面に、サイズプレスを用
いて、ポリビニルアルコール(商品名:PVA−11
7、クラレ株式会社製)1.0重量%、サイズ剤(商品
名:BLS−720、ミサワセラミック株式会社製)
0.5重量%及びリン酸二水素ナトリウム0.2重量%
を含有する水溶液を塗工してインクジェット記録用紙を
得た。
Recording paper Polyvinyl alcohol (trade name: PVA-11 was used on the surface of the high-quality paper made from the recording paper by using a size press.
7, Kuraray Co., Ltd.) 1.0% by weight, sizing agent (Brand name: BLS-720, Misawa Ceramics Co., Ltd.)
0.5 wt% and sodium dihydrogen phosphate 0.2 wt%
An aqueous solution containing a was coated to obtain an inkjet recording paper.

【0024】記録用紙 記録用紙で抄紙した上質紙表面に、サイズプレスを用
いて、酸化澱粉(商品名:エスサンサイザー700、味
の素株式会社製)1.0重量%、サイズ剤(商品名:バ
ソプラスト250D、バスフ株式会社製)0.01重量
%及びリン酸水素二ナトリウム0.2重量%を含有する
水溶液を塗工してインクジェット記録用紙を得た。
Recording paper Using a size press, 1.0% by weight of oxidized starch (trade name: Essan Sizer 700, manufactured by Ajinomoto Co., Inc.) and sizing agent (trade name: Vasoplast) were applied to the surface of the high-quality paper made from the recording paper. 250D, manufactured by Basuf Co., Ltd.) and an aqueous solution containing 0.01% by weight of disodium hydrogen phosphate and 0.2% by weight were applied to obtain an inkjet recording paper.

【0025】記録用紙 記録用紙で抄紙した上質紙表面に、サイズプレスを用
いてポリビニルアルコール(ゴーセノールN−300)
1.0重量%及びリン酸水素二ナトリウム0.2重量部
を含有する水溶液を塗工してインクジェット記録用紙を
得た。
Recording Paper Polyvinyl alcohol (Gosenol N-300) was applied to the surface of the high-quality paper made from the recording paper using a size press.
An aqueous solution containing 1.0% by weight and 0.2 part by weight of disodium hydrogen phosphate was applied to obtain an inkjet recording paper.

【0026】記録用紙 LBKP(c.s.f.350ml)94重量部、カオ
リナイト6重量部、硫酸アルミニウム0.2重量部及び
アルケニルコハク酸無水物系サイズ剤(商品名:サイズ
パインSA−850、荒川化学工業株式会社製)0.0
2重量部を配合して、坪量64g/m2 の上質紙を抄紙
した他は、記録用紙と全く同様にしてインクジェット
記録用紙を得た。
Recording paper LBKP (csf 350 ml) 94 parts by weight, kaolinite 6 parts by weight, aluminum sulfate 0.2 parts by weight and alkenylsuccinic anhydride sizing agent (trade name: Size Pine SA-850). Manufactured by Arakawa Chemical Industry Co., Ltd.) 0.0
An inkjet recording paper was obtained in exactly the same manner as the recording paper except that 2 parts by weight was blended and a high-quality paper having a basis weight of 64 g / m 2 was made.

【0027】(3)記録評価 カラーインクジェットプリンター(商品名:IO−72
5、シャープ株式会社製)及び前記3種類のインクを用
いて記録し、下記のようにしてその評価を行った。その
結果を表1に示す。尚、記録濃度はマクベス濃度計RD
−514を用いて反射濃度を測定した。
(3) Recording Evaluation Color Inkjet Printer (Product Name: IO-72
5, manufactured by Sharp Corporation) and the above three types of inks were used for recording, and the evaluation was performed as follows. The results are shown in Table 1. The recording density is Macbeth densitometer RD.
The reflection density was measured using -514.

【0028】ドット形状 ドットの形状を顕微鏡を用いて観察した。○印は形が良
好でにじみも少ないこと、△印は円形が崩れているこ
と、及び、×印は形が悪くにじみが多いことを、それぞ
れ示す。
Dot shape The shape of the dots was observed with a microscope. A circle indicates that the shape is good and there is little bleeding, a triangle indicates that the circle is broken, and a cross indicates that the shape is poor and there is much bleeding.

【0029】インクの乾燥性 インクの乾燥性は、ベタ混色部(マゼンダ+イエロー)
を記録後に手で擦ってもインク汚れが生じなくなる迄の
時間(乾燥時間)によって評価した。○印はインク乾燥
時間が2秒未満であること、△印はインク乾燥時間が2
秒以上5秒未満であること、及び、×印はインク乾燥時
間が5秒以上であることを、それぞれ示す。
Dryability of ink The dryness of ink is determined by the solid color mixture portion (magenta + yellow).
Was evaluated by the time (drying time) until ink stains did not occur even after being rubbed by hand after recording. A circle indicates that the ink drying time is less than 2 seconds, and a triangle indicates that the ink drying time is 2 seconds.
2 seconds or more and less than 5 seconds, and x indicates that the ink drying time is 5 seconds or more.

【0030】[0030]

【表1】 [Table 1]

【図面の簡単な説明】[Brief description of drawings]

【図1】記録紙の臨界表面張力(γc )と記録インクの
表面張力(γ1 )との関係における、本発明のインクジ
ェット記録方法の範囲を示すグラフである。
FIG. 1 is a graph showing the range of the inkjet recording method of the present invention in the relationship between the critical surface tension (γ c ) of recording paper and the surface tension (γ 1 ) of recording ink.

───────────────────────────────────────────────────── フロントページの続き (72)発明者 飯森 良文 東京都新宿区上落合1−30−6 日本製紙 株式会社商品開発研究所内 ─────────────────────────────────────────────────── ─── Continued Front Page (72) Inventor Yoshifumi Iimori 1-30-6 Kamiochiai, Shinjuku-ku, Tokyo Inside Nippon Paper Industries Co., Ltd. Product Development Laboratory

Claims (2)

【特許請求の範囲】[Claims] 【請求項1】非塗工紙にインク滴を施すインクジェット
記録方法であって、前記インク滴の表面張力γ1 が約2
4≦γ1 ≦70dyn/cmであると共に、前記非塗工
紙の臨界表面張力γc が約22≦γc ≦1.6(γ1
24)1/2 +22dyn/cmの範囲であることを特徴
とするインクジェット記録方法。
1. An ink jet recording method in which ink drops are applied to uncoated paper, wherein the surface tension γ 1 of the ink drops is about 2.
4 ≦ γ 1 ≦ 70 dyn / cm, and the critical surface tension γ c of the uncoated paper is about 22 ≦ γ c ≦ 1.6 (γ 1
24) An ink jet recording method, characterized in that it is in the range of 1/2 +22 dyn / cm.
【請求項2】表面張力γ1 が約24〜40dyn/cm
の範囲にあるインクに対しては、臨界表面張力γc が約
22〜1.6(γ1 −24)1/2 +22dyn/cmの
範囲にある非塗工紙に印字し、表面張力γ1 が約40〜
70dyn/cmの範囲にあるインクに対しては、臨界
表面張力γc が約(γ1 −40)1/2+22〜 1.6
(γ1 −24)1/2 +22dyn/cmの範囲にある請
求項1に記載のインクジェット記録方法。
2. A surface tension γ 1 of about 24 to 40 dyn / cm.
For inks in the range of, printed on non-coated paper critical surface tension gamma c is in the range of about 22~1.6 (γ 1 -24) 1/2 + 22dyn / cm, a surface tension gamma 1 Is about 40 ~
For ink in the range of 70 dyn / cm, the critical surface tension γ c is about (γ 1 -40) 1/2 +22 to 1.6.
The ink jet recording method according to claim 1, wherein the amount is in the range of (γ 1 -24) 1/2 +22 dyn / cm.
JP27498893A 1993-10-06 1993-10-06 Inkjet recording method Expired - Lifetime JP3724820B2 (en)