JPH07288043A - Coated electric wire and manufacturing method thereof - Google Patents

Coated electric wire and manufacturing method thereof

Info

Publication number
JPH07288043A
JPH07288043A JP6078307A JP7830794A JPH07288043A JP H07288043 A JPH07288043 A JP H07288043A JP 6078307 A JP6078307 A JP 6078307A JP 7830794 A JP7830794 A JP 7830794A JP H07288043 A JPH07288043 A JP H07288043A
Authority
JP
Japan
Prior art keywords
electric wire
alkenylsilane
copolymer
silicone oil
wire
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP6078307A
Other languages
Japanese (ja)
Other versions
JP3521952B2 (en
Inventor
Tadashi Asanuma
浅沼  正
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsui Toatsu Chemicals Inc
Original Assignee
Mitsui Toatsu Chemicals Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsui Toatsu Chemicals Inc filed Critical Mitsui Toatsu Chemicals Inc
Priority to JP07830794A priority Critical patent/JP3521952B2/en
Publication of JPH07288043A publication Critical patent/JPH07288043A/en
Application granted granted Critical
Publication of JP3521952B2 publication Critical patent/JP3521952B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

(57)【要約】 【構成】金属線にアルケニルシランとオレフィンの共重
合体とシリコーンオイルを含有する組成物を加熱溶融し
て被覆してなる被覆電線、およびアルケニルシランとオ
レフィンの共重合体とシリコーンオイルを含有する組成
物を加熱溶融し、金属線を被覆するように成形して被覆
電線とし、ついで塩化ロジウムのトリフェニルフォスフ
ィン錯体等の触媒の溶液に浸漬し処理することにより、
あるいは放射線を照射することにより架橋被覆電線を製
造する方法。 【効果】金属線から被覆を容易に剥がすことのできる被
覆電線を提供できる。
(57) [Summary] [Structure] A coated wire obtained by heating and melting a composition containing a metal wire containing a copolymer of alkenylsilane and olefin and silicone oil, and a copolymer of alkenylsilane and olefin. By heating and melting a composition containing silicone oil to form a covered electric wire by molding so as to cover a metal wire, and then by immersing the composition in a solution of a catalyst such as a triphenylphosphine complex of rhodium chloride and treating the metal wire,
Alternatively, a method for producing a crosslinked coated electric wire by irradiating with radiation. [Effect] It is possible to provide a covered electric wire in which the covering can be easily peeled off from the metal wire.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は被覆電線に関する。詳し
くは、特定のポリマーを含有する組成物で被覆してなる
被覆電線および架橋被覆電線の製造方法に関する。
FIELD OF THE INVENTION The present invention relates to a coated electric wire. Specifically, it relates to a method for producing a covered electric wire and a crosslinked electric wire covered with a composition containing a specific polymer.

【0002】[0002]

【従来の技術】金属線を溶融樹脂で被覆した被覆電線は
種々の電気用の用途に利用されておりなかでもポリエチ
レンを用い放射線(通常は電子線である。)を照射して
架橋した架橋被覆電線は耐熱性に優れており多く利用さ
れている。
2. Description of the Related Art A covered electric wire in which a metal wire is covered with a molten resin is used for various electric purposes. Among them, polyethylene is used and crosslinked by irradiation with radiation (usually an electron beam). Electric wires have excellent heat resistance and are widely used.

【0003】[0003]

【発明が解決しようとする課題】従来の架橋被覆電線は
電子線を比較的多量に照射する必要があり、高価な照射
設備を必要とするし、またポリエチレン以外のポリオレ
フィンでは架橋がほとんど進行せず良好な架橋被覆電線
とすることができないという問題があり、特に難燃剤と
して最近のハロゲン化物を使用しない傾向から無機酸化
物あるいは水酸化物を使用する場合には、電子線のエネ
ルギーを大幅に高めないと架橋できないという問題があ
った。一方ポリオレフィンにアルコキシシラン類をグラ
フトしたポリオレフィンを用いて被覆電線とし次いで水
で架橋したものは、電子線の照射設備などの高価な設備
を必要としないものの得られる架橋被覆電線の耐水性、
耐熱性に難があるという問題がある。
The conventional cross-linked coated electric wire needs to be irradiated with a relatively large amount of electron beams, requires expensive irradiation equipment, and cross-linking hardly progresses with polyolefins other than polyethylene. There is a problem that it is not possible to make a good cross-linked coated electric wire, and especially when using an inorganic oxide or hydroxide as a flame retardant because of the tendency not to use a recent halide, the electron beam energy is significantly increased. There was a problem that it could not be cross-linked without it. On the other hand, what was crosslinked with water using a polyolefin grafted with alkoxysilanes on the polyolefin and then crosslinked with water, the water resistance of the crosslinked coated electric wire, which does not require expensive equipment such as electron beam irradiation equipment,
There is a problem that heat resistance is poor.

【0004】これに対しては、本発明者は先にアルケニ
ルシランとオレフィンの共重合体を用いる方法を提案し
たがこの場合には、アルケニルシランとオレフィンの共
重合体は、金属と極めて接着性に富むため被覆を剥がす
必要のない用途には、電線は縒れ難いと言う利点を有す
るが、通常の被覆電線の用途には、被覆が剥がれ難いた
め接点と接続して用いるため被覆を剥がすのが困難であ
るという問題があり、被覆するに先立って金属線を弗素
系の樹脂で処理することを提案したがこれでは操作が煩
雑であるという問題がある。
In response to this, the present inventor has previously proposed a method using a copolymer of alkenylsilane and olefin. In this case, the copolymer of alkenylsilane and olefin is extremely adhesive to a metal. It has the advantage that the wire is difficult to twist in applications where the coating does not need to be peeled off because it is rich in the However, it has been proposed to treat the metal wire with a fluorine-based resin prior to coating, but this has a problem that the operation is complicated.

【0005】[0005]

【課題を解決するための手段】本発明者らは上記問題を
解決して被覆を簡単に剥がすことのできる被覆電線およ
び架橋被覆電線の製造方法について鋭意検討し本発明を
完成した。
Means for Solving the Problems The present inventors have completed the present invention by intensively studying a method for producing a covered electric wire and a crosslinked electric wire in which the coating can be easily peeled off by solving the above problems.

【0006】即ち本発明は、金属線にアルケニルシラン
とオレフィンの共重合体とシリコンーンオイルを含有す
る組成物を加熱溶融して被覆してなる被覆電線である。
[0006] That is, the present invention is a covered electric wire obtained by heating and melting a composition containing a metal wire containing a copolymer of alkenylsilane and olefin and silicone oil.

【0007】以下に本発明の被覆電線についてその製造
方法を示すことでさらに説明する。
The coated electric wire of the present invention will be further described below by showing its manufacturing method.

【0008】本発明においてアルケニルシランとしては
少なくとも一つのSi−H結合を有するものが好ましく
用いられ、例えば下記一般式(化1)で表される化合
物、
In the present invention, an alkenylsilane having at least one Si--H bond is preferably used, and for example, a compound represented by the following general formula (Formula 1),

【0009】[0009]

【化1】H2C=CH-(CH2)n -SiHp R3-p (式中nは0〜12、pは1〜3、Rは炭素数1 〜12の炭
化水素残基。)が例示でき、具体的にはビニルシラン、
アリルシラン、ブテニルシラン、ペンテニルシラン、あ
るいはこれらのモノマーの一部のSi−H結合のHがク
ロルで置換された化合物などが例示できる。
Embedded image H 2 C═CH— (CH 2 ) n —SiH p R 3-p (wherein n is 0 to 12, p is 1 to 3 and R is a hydrocarbon residue having 1 to 12 carbon atoms). ) Can be exemplified, and specifically, vinyl silane,
Examples thereof include allylsilane, butenylsilane, pentenylsilane, and compounds in which H of some Si—H bonds of these monomers is replaced with chlorine.

【0010】またオレフィンとしては下記一般式(化
2)で示される化合物、
As the olefin, a compound represented by the following general formula (Formula 2),

【0011】[0011]

【化2】H2C=CH-R (式中Rは水素または炭素数1 〜12の炭化水素残基。)
が例示でき、具体的にはエチレン、プロピレン、ブテン
-1、ペンテン-1、ヘキセン-1、2-メチルペンテン、ヘプ
テン-1、オクテン-1などのα−オレフィンの他にスチレ
ンまたはその誘導体も例示される。
Embedded image H 2 C═CH—R (wherein R is hydrogen or a hydrocarbon residue having 1 to 12 carbon atoms.)
Can be exemplified, and specifically, ethylene, propylene, butene
In addition to α-olefins such as -1, pentene-1, hexene-1, 2-methylpentene, heptene-1, and octene-1, styrene and its derivatives are also exemplified.

【0012】本発明においてオレフィンとアルケニルシ
ランの共重合体は、不活性溶媒を使用する溶媒法の他に
塊状重合法、気相重合法で製造することができる。製造
に用いる触媒としては、遷移金属化合物と有機金属化合
物からなる触媒を用いるのが一般的であり、遷移金属化
合物としてはハロゲン化チタンが、有機金属化合物とし
ては有機アルミニウム化合物が好ましく用いられる。
In the present invention, the copolymer of olefin and alkenylsilane can be produced by a bulk polymerization method or a gas phase polymerization method in addition to the solvent method using an inert solvent. As a catalyst used for production, a catalyst composed of a transition metal compound and an organometallic compound is generally used, and a titanium halide is preferably used as the transition metal compound and an organoaluminum compound is preferably used as the organometallic compound.

【0013】具体的には四塩化チタンを金属アルミニウ
ム、水素或いは有機アルミニウムで還元して得た三塩化
チタンを電子供与性化合物で変性処理したものと有機ア
ルミニウム化合物、さらに必要に応じ含酸素有機化合物
などの電子供与性化合物からなる触媒系、或いはハロゲ
ン化マグネシウム等の担体或いはそれらを電子供与性化
合物で処理したものにハロゲン化チタンを担持して得た
遷移金属化合物触媒と有機アルミニウム化合物、必要に
応じ含酸素有機化合物などの電子供与性化合物からなる
触媒系、あるいは塩化マグネシウムとアルコールの反応
物を炭化水素溶媒中に溶解し、ついで四塩化チタンなど
の沈澱剤で処理することで炭化水素溶媒に不溶化し、必
要に応じエステル、エーテルなどの電子供与性の化合物
で処理し、ついでハロゲン化チタンで処理する方法など
によって得られる遷移金属化合物触媒と有機アルミニウ
ム化合物、必要に応じ含酸素有機化合物などの電子供与
性化合物からなる触媒系等が例示される(例えば、以下
の文献に種々の例が記載されている。Ziegler-Natta Ca
talysts and Polymerization by John Boor Jr(Academi
c Press),Journal of Macromorecular Science Reviews
in MacromolecularChemistry and Physics,C24(3) 355
-385(1984)、同C25(1) 578-597(1985)) 。
Specifically, titanium trichloride obtained by reducing titanium tetrachloride with metallic aluminum, hydrogen or organoaluminum, modified with an electron donating compound, an organoaluminum compound, and optionally an oxygen-containing organic compound. Such as a catalyst system composed of an electron-donating compound, a carrier such as magnesium halide, or a transition metal compound catalyst obtained by supporting titanium halide on the carrier treated with an electron-donating compound and an organoaluminum compound, if necessary. A catalyst system consisting of an electron-donating compound such as an oxygen-containing organic compound or a reaction product of magnesium chloride and alcohol is dissolved in a hydrocarbon solvent, and then treated with a precipitating agent such as titanium tetrachloride to form a hydrocarbon solvent. Insolubilize, treat with electron donating compounds such as ester and ether if necessary, then Examples thereof include a catalyst system comprising a transition metal compound catalyst obtained by a method of treating with titanium rogenide and an organoaluminum compound, and optionally an electron-donating compound such as an oxygen-containing organic compound (for example, various references in the following documents). An example is given of: Ziegler-Natta Ca
talysts and Polymerization by John Boor Jr (Academi
c Press), Journal of Macromorecular Science Reviews
in Macromolecular Chemistry and Physics, C24 (3) 355
-385 (1984), C25 (1) 578-597 (1985)).

【0014】あるいは炭化水素溶剤に可溶な遷移金属触
媒とアルミノキサンからなる触媒を用いて重合すること
もできる。
Alternatively, the polymerization can be carried out by using a transition metal catalyst soluble in a hydrocarbon solvent and a catalyst comprising aluminoxane.

【0015】ここで電子供与性化合物としては通常エー
テル、エステル、オルソエステル、アルコキシ硅素化合
物などの含酸素化合物が好ましく例示でき、さらにアル
コール、アルデヒド、水なども使用可能である。
As the electron-donating compound, oxygen-containing compounds such as ethers, esters, orthoesters and alkoxysilicon compounds can be preferably exemplified, and alcohols, aldehydes, water and the like can also be used.

【0016】有機アルミニウム化合物としては、トリア
ルキルアルミニウム、ジアルキルアルミニウムハライ
ド、アルキルアルミニウムセスキハライド、アルキルア
ルミニウムジハライドが使用でき、アルキル基としては
メチル基、エチル基、プロピル基、ブチル基、ヘキシル
基などが例示され、ハライドとしては塩素、臭素、沃素
が例示される。また上記有機アルミニウムと水または結
晶水とを反応することで得られるオリゴマー〜ポリマー
であるアルミノキサンも利用できる。
As the organoaluminum compound, trialkylaluminum, dialkylaluminum halide, alkylaluminum sesquihalide and alkylaluminum dihalide can be used, and examples of the alkyl group include methyl group, ethyl group, propyl group, butyl group and hexyl group. Examples of the halide include chlorine, bromine and iodine. Further, an aluminoxane which is an oligomer or a polymer obtained by reacting the above organoaluminum with water or water of crystallization can also be used.

【0017】ここでアルケニルシランとオレフィンの重
合割合としては特に制限は無いが、ポリオレフィンと混
合して用いる場合には、通常アルケニルシランが 0.001
〜30モル%程度、好ましくは0.1 〜10モル%である。ま
た単独で用いる場合には0.0001〜 1モル%程度である。
Here, the polymerization ratio of alkenylsilane and olefin is not particularly limited, but when it is used as a mixture with polyolefin, alkenylsilane is usually 0.001.
It is about 30 to 30 mol%, preferably 0.1 to 10 mol%. When used alone, it is about 0.0001 to 1 mol%.

【0018】重合体の分子量としては特に制限はない
が、ポリオレフィンと混合して用いる場合にはポリオレ
フィンの分子量と同程度あるいはそれ以下とするのが好
ましい。好ましい分子量としては 135℃のテトラリン溶
液で測定した極限粘度数が0.1〜10程度である。
The molecular weight of the polymer is not particularly limited, but when it is mixed with a polyolefin, the molecular weight is preferably the same as or lower than the molecular weight of the polyolefin. As a preferable molecular weight, the intrinsic viscosity number measured with a tetralin solution at 135 ° C. is about 0.1 to 10.

【0019】ポリオレフィン(例えば、下記のような混
合して用いるポリオレフィンが使用できる。)にアルケ
ニルシランをグラフト重合して得たグラフト共重合体も
本発明の目的に使用可能であり、その場合、ポリオレフ
ィンにアルケニルシランをグラフトする方法としては特
に制限はなく、通常のグラフト共重合に用いる方法及び
条件が利用でき、通常は用いるポリオレフィンとアルケ
ニルシランをパーオキサイドなどのラジカル開始剤の存
在下にラジカル開始剤の分解温度以上に加熱することで
簡単にグラフト共重合することができる。
A graft copolymer obtained by graft-polymerizing an alkenylsilane onto a polyolefin (for example, the following mixed polyolefin can be used) can be used for the purpose of the present invention. There is no particular limitation as to the method for grafting alkenylsilane to, and the method and conditions used for ordinary graft copolymerization can be used. Normally, the polyolefin and alkenylsilane used are radical initiator in the presence of a radical initiator such as peroxide. Graft copolymerization can be easily carried out by heating above the decomposition temperature of.

【0020】本発明において必要に応じ上記共重合体と
混合して用いるポリオレフィンとしては上記一般式(化
2)で示されるオレフィン、具体的にはエチレン、プロ
ピレン、ブテン-1、ペンテン-1、ヘキセン-1、2-メチル
ペンテン、ヘプテン-1、オクテン-1などのα−オレフィ
ンあるいは、スチレンまたはその誘導体の単独重合体、
相互のランダム共重合体、或いは、始めにオレフィン単
独、或いは少量の他のオレフィンと共重合し、ついで2
種以上のオレフィンを共重合することによって製造され
る所謂ブロック共重合体などが例示される。
In the present invention, the polyolefin used as a mixture with the above-mentioned copolymer, if necessary, is an olefin represented by the general formula (Formula 2), specifically ethylene, propylene, butene-1, pentene-1, hexene. 1, α-olefins such as 2-methylpentene, heptene-1, and octene-1, or a homopolymer of styrene or a derivative thereof,
Random copolymers with each other, or first with olefins alone or with small amounts of other olefins, then 2
Examples thereof include so-called block copolymers produced by copolymerizing at least one olefin.

【0021】これらのポリオレフィンの製造法について
は既に公知であり種々の銘柄のものが市場で入手可能で
ある。またアルケニルシランを用いない他は上記オレフ
ィンとアルケニルシランの共重合体の製造法と同様に行
うことでも製造可能である。
Methods for producing these polyolefins are already known and various brands are available on the market. It can also be produced by the same method as the method for producing a copolymer of olefin and alkenylsilane except that alkenylsilane is not used.

【0022】本発明においてはアルケニルシランとオレ
フィンの共重合体およびシリコーンオイルと混合して用
いる添加剤として、ポリオレフィンの他に安定剤、フィ
ラーなど公知の種々の添加剤が利用でき、特に以下に示
す、無機酸化物あるいは無機水酸化物を用いると難燃性
に優れたものとなる。
In the present invention, various known additives such as stabilizers and fillers can be used in addition to polyolefin as the additive to be used by mixing with the copolymer of alkenylsilane and olefin and silicone oil. If an inorganic oxide or an inorganic hydroxide is used, the flame retardancy becomes excellent.

【0023】本発明において無機酸化物あるいは無機水
酸化物とは、周期律表 I、II、III族の金属の酸化物あ
るいは水酸化物あるいはこれらの混合物または他の無機
化合物との混合物などが例示される。特にII、III 族の
金属の酸化物、水酸化物が好ましく利用できる。具体的
には、水酸化マグネシウム、酸化マグネシウム、水酸化
アルミニウム、酸化アルミニウム、水酸化バリウム、酸
化バリウムあるいはこれらの混合物、複合体が好ましく
利用される。ここで無機酸化物あるいは無機水酸化物を
使用する場合の使用割合としては、前述の必要に応じて
併用するポリオレフィン、添加剤も含めて全組成物中の
1〜80wt%、好ましくは5〜50wt%とするのが一般的で
ある。難燃のため上記無機酸化物あるいは無機水酸化物
を利用する場合には、架橋は触媒と接触するのが好まし
く、放射線を用いると透過力の大きい放射線を利用する
必要がある。
In the present invention, examples of the inorganic oxide or inorganic hydroxide include oxides or hydroxides of metals of Group I, II, and III of the Periodic Table, or mixtures thereof or mixtures with other inorganic compounds. To be done. Particularly, oxides and hydroxides of Group II and III metals can be preferably used. Specifically, magnesium hydroxide, magnesium oxide, aluminum hydroxide, aluminum oxide, barium hydroxide, barium oxide, or a mixture or complex thereof is preferably used. Here, the use ratio of the inorganic oxide or the inorganic hydroxide is 1 to 80% by weight, preferably 5 to 50% by weight of the total composition including the above-mentioned polyolefin which is optionally used in combination and additives. Generally, it is set to%. When the above-mentioned inorganic oxide or inorganic hydroxide is used for flame retardancy, it is preferable that the crosslinking is brought into contact with the catalyst, and it is necessary to use radiation having a large penetrating power when radiation is used.

【0024】本発明においてシリコーンオイルとして
は、下記一般式(化3)で表される化合物が例示でき
る。
In the present invention, examples of the silicone oil include compounds represented by the following general formula (Formula 3).

【0025】[0025]

【化3】 (式中Rは同じでも異なっていても良く、水素または炭
素数1〜20の炭化水素残基、nは1以上の整数。)。
[Chemical 3] (In the formula, R may be the same or different and is hydrogen or a hydrocarbon residue having 1 to 20 carbon atoms, and n is an integer of 1 or more.).

【0026】特に好ましくは一方のRが水素であるSi
−H基を有するシリコーンオイルである。
Particularly preferably, Si in which one R is hydrogen
It is a silicone oil having a -H group.

【0027】このような化合物は対応する下記一般式
(化4)で表されるアルキルジクロロシラン、あるいは
アリルジクロロシランなどを水で加水分解することで製
造することができる。
Such a compound can be produced by hydrolyzing a corresponding alkyldichlorosilane represented by the following general formula (Formula 4) or allyldichlorosilane with water.

【0028】[0028]

【化4】R2SiCl2 (式中Rは同じでも異なっていても良く、水素または炭
素数1〜20の炭化水素残基。)。
Embedded image R 2 SiCl 2 (wherein R may be the same or different and is hydrogen or a hydrocarbon residue having 1 to 20 carbon atoms).

【0029】このシリコーンオイルのアルケニルシラン
とオレフィンの共重合体に対する使用割合としては、通
常アルケニルシランとオレフィンの共重合体 100重量部
に対し0.1 〜60重量部、好ましくは1.0 〜40重量部であ
る。これより少ないと改良効果が小さい。
The ratio of the silicone oil to the alkenylsilane / olefin copolymer is usually 0.1 to 60 parts by weight, preferably 1.0 to 40 parts by weight, per 100 parts by weight of the alkenylsilane / olefin copolymer. . If it is less than this, the improvement effect is small.

【0030】本発明においては、アルケニルシランとオ
レフィンの共重合体はシリコーンオイルと、必要に応じ
ポリオレフィンあるいは他の添加剤などと混合して組成
物とし、加熱溶融して金属線を被覆するように成形され
る。ここで金属線に被覆する成形方法としては、通常の
方法がそのまま適用でき、クロスヘッド型ダイあるいは
アンギュラオフセット型ダイを設けた押出し機を用いる
のが一般的である。押出し条件としては特に制限はない
が、通常 150〜 300℃で押出すのが一般的である。
In the present invention, the copolymer of alkenylsilane and olefin is mixed with silicone oil and, if necessary, polyolefin or other additives to prepare a composition, which is heated and melted to coat the metal wire. Molded. As a molding method for coating the metal wire, a usual method can be applied as it is, and an extruder equipped with a crosshead die or an angular offset die is generally used. There are no particular restrictions on the extrusion conditions, but it is common to extrude at 150 to 300 ° C.

【0031】金属線としては特に制限はないが、金、
銀、銅、アルミニウム、鉄またはそれらの合金を用いる
のが一般的である。
The metal wire is not particularly limited, but gold,
It is common to use silver, copper, aluminum, iron or alloys thereof.

【0032】こうして得られた被覆電線は架橋する場合
には、ついで放射線が照射されるか触媒と接触される。
When the coated electric wire thus obtained is cross-linked, it is then irradiated with radiation or brought into contact with a catalyst.

【0033】放射線としては、電子線、γ線、X線、紫
外線などが例示される。透過性の点からγ線、X線が好
ましく、照射線量としては、通常0.1 〜100Mrad 程度、
好ましくは1 〜50Mrad程度である。照射温度としては50
℃以下で行われ、特に低温で行う必要はなく室温で行え
ば良い。照射を高温で行うと成形物が変形するとか、架
橋が効率的でないなどの問題がある。従って照射は比較
的低温で行って、照射後に加熱してラジカルを完全に消
去するのが好ましい。
Examples of the radiation include electron beams, γ rays, X rays and ultraviolet rays. From the viewpoint of transparency, γ-rays and X-rays are preferable, and the irradiation dose is usually about 0.1 to 100 Mrad,
It is preferably about 1 to 50 Mrad. 50 as the irradiation temperature
It is carried out at a temperature of not higher than 0 ° C., and it is not necessary to carry out at a particularly low temperature and it may be carried out at room temperature. When irradiation is performed at a high temperature, there are problems such as deformation of the molded product and inefficient crosslinking. Therefore, it is preferable that the irradiation is performed at a relatively low temperature and the radicals are completely erased by heating after the irradiation.

【0034】好ましく用いられる触媒としては、塩化ロ
ジウムのトリフェニルフォスフィン錯体などのロジウム
の塩、あるいはチタン酸エステルなどの下記一般式(化
5)で示す周期律表IVB 族金属のアルコキシ化合物が例
示される。
Examples of catalysts preferably used include rhodium salts such as triphenylphosphine complex of rhodium chloride, and alkoxy compounds of Group IVB metal of the periodic table represented by the following general formula (Formula 5) such as titanate. To be done.

【0035】[0035]

【化5】R1 n M(O-R2)4-n (式中R1 、R2 は、同じか異なる炭素数1 〜12の炭化
水素残基、nは0〜3の整数、Mはチタン、ジルコニウ
ム、ハフニウムから選ばれた金属。) 。
Embedded image R 1 n M (OR 2 ) 4-n (wherein R 1 and R 2 are the same or different hydrocarbon residues having 1 to 12 carbon atoms, n is an integer of 0 to 3 and M is titanium). , A metal selected from zirconium and hafnium.).

【0036】接触は上記触媒を後述の溶媒に溶解して、
その溶液に被覆電線を連続的にあるいは回分的に浸漬す
ることで行われる。利用される溶媒としては、具体的に
は炭素数1 〜20の炭化水素化合物、ハロゲン化炭化水素
化合物が利用でき、特にハロゲン化炭化水素化合物、芳
香族炭化水素化合物が好ましく利用される。具体的にベ
ンゼン、トルエン、キシレン、エチルベンゼン、ジクロ
ロメタン、クロロホルム、ジクロロエタン、トリクロロ
エタン、パークロロエタンなどが例示される。
For contacting, the above catalyst is dissolved in a solvent described below,
It is performed by immersing the coated electric wire in the solution continuously or batchwise. As the solvent to be used, specifically, a hydrocarbon compound having 1 to 20 carbon atoms and a halogenated hydrocarbon compound can be used, and particularly, a halogenated hydrocarbon compound and an aromatic hydrocarbon compound are preferably used. Specific examples include benzene, toluene, xylene, ethylbenzene, dichloromethane, chloroform, dichloroethane, trichloroethane, perchloroethane and the like.

【0037】触媒の濃度としては0.000001〜1000g /リ
ットル程度、通常0.00001 〜10g /リットル程度で行わ
れる。接触時間としては、触媒の濃度、触媒溶液の温
度、共重合体の形状、共重合体中のアルケニルシランの
濃度などによって好ましい時間は異なるが通常数分〜数
十時間である。浸漬の際の温度としては、成形物が変形
しない範囲で、高温であるのが架橋反応の速度の点で好
ましいが、通常常温〜200 ℃、好ましくは常温〜150 ℃
程度である。この際、触媒の分散を助けるため攪拌する
ことも勿論可能である。
The catalyst concentration is about 0.000001 to 1000 g / liter, usually about 0.00001 to 10 g / liter. The contact time varies depending on the concentration of the catalyst, the temperature of the catalyst solution, the shape of the copolymer, the concentration of alkenylsilane in the copolymer, and the like, but is usually several minutes to several tens hours. The temperature at the time of immersion is preferably a high temperature in the range where the molded product is not deformed, from the viewpoint of the rate of the crosslinking reaction, but is usually room temperature to 200 ° C, preferably room temperature to 150 ° C.
It is a degree. At this time, it is of course possible to stir to assist the dispersion of the catalyst.

【0038】成形物中のアルケニルシラン含量としては
共重合体中のアルケニルシラン含量にもよるが、通常成
形物中の共重合体の割合は 0.1wt%以上であり、成形物
中のアルケニルシランが0.0001wt%以上存在するように
するのが好ましい。好ましくは成形物中のアルケニルシ
ランとしては0.0001〜 1.0wt%程度である。
Although the alkenylsilane content in the molded product depends on the alkenylsilane content in the copolymer, the proportion of the copolymer in the molded product is usually 0.1 wt% or more, and the alkenylsilane content in the molded product is It is preferable that 0.0001 wt% or more is present. The alkenylsilane content in the molded product is preferably about 0.0001 to 1.0 wt%.

【0039】[0039]

【実施例】以下に実施例を示しさらに本発明を説明す
る。
EXAMPLES The present invention will be further described with reference to the following examples.

【0040】実施例1 直径12mmの鋼球9kgの入った内容積4リットルの粉砕用
ポットを4個装備した振動ミルを用意する。各ポットに
窒素雰囲気下で塩化マグネシウム 300g、テトラエトキ
シシラン60mlおよびα, α, α−トリクロロトルエン45
mlを入れ、40時間粉砕した。こうして得た共粉砕物 300
gを5リットルのフラスコに入れ、四塩化チタン 1.5リ
ットルおよびトルエン 1.5リットルを加え、 100℃で30
分間撹拌処理し、次いで上澄液を除いた。再び四塩化チ
タン 1.5リットルおよびトルエン1.5 リットルを加え、
100℃で30分間撹拌処理し、次いで上澄液を除いた。そ
の後固形分をn-ヘキサンで繰り返し洗浄して遷移金属触
媒スラリーを得た。一部をサンプリングしてチタン分を
分析したところチタン分は 1.9wt%であった。
Example 1 A vibration mill equipped with four grinding pots having an inner volume of 4 liters and containing 9 kg of steel balls having a diameter of 12 mm was prepared. In each pot under a nitrogen atmosphere, 300 g of magnesium chloride, 60 ml of tetraethoxysilane and 45 of α, α, α-trichlorotoluene
ml was added and crushed for 40 hours. Co-ground product 300 thus obtained
In a 5 liter flask, add 1.5 liters of titanium tetrachloride and 1.5 liters of toluene, and add 30 liters at 100 ° C.
After stirring for a minute, the supernatant was removed. Add again 1.5 liters of titanium tetrachloride and 1.5 liters of toluene,
The mixture was stirred at 100 ° C for 30 minutes, and the supernatant was removed. Then, the solid content was repeatedly washed with n-hexane to obtain a transition metal catalyst slurry. When a part of the sample was sampled and the titanium content was analyzed, the titanium content was 1.9 wt%.

【0041】内容積5リットルのオートクレーブに窒素
雰囲気下トルエン40ml、上記遷移金属触媒 100mg、ジエ
チルアルミニウムクロライド 0.128ml、p-トルイル酸メ
チル0.06mlおよびトリエチルアルミニウム0.20mlを入
れ、プロピレン 1.5kg、ビニルシラン40gを加え、水素
1Nリットル圧入した後、75℃で2時間重合した。重合後
未反応のプロピレンをパージし、パウダーを取り出し、
濾過乾燥して 480gのパウダーを得た。
40 ml of toluene, 100 mg of the above transition metal catalyst, 0.128 ml of diethylaluminium chloride, 0.06 ml of methyl p-toluate and 0.20 ml of triethylaluminum were placed in an autoclave having an internal volume of 5 liters under a nitrogen atmosphere, and 1.5 kg of propylene and 40 g of vinylsilane were added. In addition, hydrogen
After 1N liter pressure injection, polymerization was carried out at 75 ° C for 2 hours. After polymerization, purge unreacted propylene, take out powder,
It was filtered and dried to obtain 480 g of powder.

【0042】135 ℃のテトラリン溶液で測定した極限粘
度数 (以下ηと略記する) 、示差熱分析装置を用い10℃
/min で昇温或いは降温することで融点及び結晶化温度
を最大ピーク温度として測定したところ、得られたパウ
ダーは、ηが1.72であり、融点153 ℃、結晶化温度 118
℃である結晶性のプロピレン共重合体であった。尚、元
素分析によればビニルシラン単位を 1.2wt%含有してい
た。
Intrinsic viscosity number (hereinafter abbreviated as η) measured with a tetralin solution at 135 ° C., using a differential thermal analyzer at 10 ° C.
When the melting point and the crystallization temperature were measured as the maximum peak temperature by raising or lowering the temperature at a rate of / min, the obtained powder had an η of 1.72, a melting point of 153 ° C and a crystallization temperature of 118 ° C.
It was a crystalline propylene copolymer having a temperature of ° C. According to elemental analysis, it contained 1.2 wt% of vinylsilane unit.

【0043】得られた共重合体50gに、プロピレンの単
独重合体( 上記方法でビニルシランを加えること無く重
合して製造、ηが2.25、6時間沸騰n-ヘキサンで抽出し
た時の抽出残分の割合が97.3%であるもの。)100g、シ
リコーンオイル(信越化学(株)製、KF−99)2
g、フェノール系の酸化防止剤 0.1gを加え良く混合し
たものを20mmφの押出機で 250℃で造粒した。次いでク
ロスヘッド型ダイを設けた同じく20mmφの押出機で 250
℃で直径1mmの銅線に0.1mm の厚さで樹脂が被覆される
ようにして被覆電線を成形した。
50 g of the obtained copolymer was produced by polymerizing a propylene homopolymer (without adding vinylsilane by the above-mentioned method, η was 2.25, and the extraction residue when extracted with boiling n-hexane for 6 hours. The ratio is 97.3%.) 100 g, silicone oil (KF-99, manufactured by Shin-Etsu Chemical Co., Ltd.) 2
g and 0.1 g of phenolic antioxidant were added and mixed well, and granulated at 250 ° C. with a 20 mmφ extruder. Next, using a 20 mmφ extruder equipped with a crosshead die, 250
A coated electric wire was formed by coating a copper wire having a diameter of 1 mm at 0.1 ° C. with a resin having a thickness of 0.1 mm.

【0044】ついでγ線を室温で10Mrad照射して架橋被
覆電線とした。架橋被覆電線を沸騰キシレンで12時間抽
出したところ不溶分は72.1wt%であり 250℃に加熱して
も被覆したポリプロピレンは垂れてこなかった。なお、
銅線から被覆は簡単に剥がれた。
Then, γ-rays were irradiated at room temperature for 10 Mrad to obtain a crosslinked electric wire. When the cross-linked coated wire was extracted with boiling xylene for 12 hours, the insoluble content was 72.1 wt% and the coated polypropylene did not drip even when heated to 250 ° C. In addition,
The coating was easily stripped from the copper wire.

【0045】比較例1 シリコーンオイルを用いなかった他は実施例1と同様に
したところ、銅線から被覆は簡単に剥がれなかった。
Comparative Example 1 The same procedure as in Example 1 was carried out except that silicone oil was not used, but the coating was not easily peeled off from the copper wire.

【0046】実施例2 ビニルシランに変えアリルシラン1gを用いた他は実施
例1と同様に重合してアリルシラン含量0.25wt%のプロ
ピレンの共重合体を製造した。共重合体のηは1.85であ
り、融点 158℃、結晶化温度 115℃、沸騰n-ヘプタンで
6時間抽出した時の抽出残分の割合が96.8%であった。
Example 2 Polymerization was carried out in the same manner as in Example 1 except that 1 g of allylsilane was used instead of vinylsilane to produce a propylene copolymer having an allylsilane content of 0.25 wt%. The η of the copolymer was 1.85, the melting point was 158 ° C., the crystallization temperature was 115 ° C., and the extraction residue ratio after extraction with boiling n-heptane for 6 hours was 96.8%.

【0047】この共重合体1000g、実施例1で用いたシ
リコーンオイル50g、フェノール系の酸化防止剤 1.0g
を混合し、実施例1と同様に造粒し、成形して被覆電線
とした。
1000 g of this copolymer, 50 g of the silicone oil used in Example 1, 1.0 g of a phenolic antioxidant
Were mixed, granulated and molded in the same manner as in Example 1 to obtain a covered electric wire.

【0048】ついで実施例1と同様にγ線を照射して架
橋被覆電線とした。架橋被覆電線を沸騰キシレンで12時
間抽出したところ不溶分は67.1wt%であった。なお、銅
線から被覆は簡単に剥がれた。
Then, in the same manner as in Example 1, γ-rays were irradiated to obtain a crosslinked electric wire. When the crosslinked electric wire was extracted with boiling xylene for 12 hours, the insoluble content was 67.1 wt%. The coating was easily peeled off from the copper wire.

【0049】実施例3 実施例1で得られた共重合体50gに、実施例1で用いた
プロピレンの単独重合体 100g、実施例1で用いたシリ
コーンオイル5g、フェノール系の酸化防止剤0.1 gを
加え良く混合したものを実施例1と同様に造粒し、成形
して被覆電線とした。
Example 3 50 g of the copolymer obtained in Example 1 was added with 100 g of the propylene homopolymer used in Example 1, 5 g of the silicone oil used in Example 1, and 0.1 g of a phenolic antioxidant. What was added and mixed well was granulated and molded in the same manner as in Example 1 to obtain a covered electric wire.

【0050】こうして得られた被覆電線をn-ブチルチタ
ネートを10g/リットルになる様に溶解したトルエン溶
液に浸漬し90℃で30分間処理した。処理した被覆電線を
沸騰キシレンで12時間抽出したところ不溶分は83.1wt%
であり 250℃に加熱しても被覆したポリプロピレンは垂
れてこなかった。なお、銅線から被覆は簡単に剥がれ
た。
The coated electric wire thus obtained was immersed in a toluene solution in which 10 g / l of n-butyl titanate was dissolved and treated at 90 ° C. for 30 minutes. When the treated covered electric wire was extracted with boiling xylene for 12 hours, the insoluble content was 83.1 wt%
The coated polypropylene did not sag even when heated to 250 ° C. The coating was easily peeled off from the copper wire.

【0051】また浸漬処理前の被覆電線をそのまま沸騰
キシレンで12時間抽出したところ、不溶分は 0.1wt%で
あり 250℃に加熱すると被覆が垂れてきた。なお、被覆
は簡単に剥がれた。
When the coated electric wire before the dipping treatment was extracted with boiling xylene for 12 hours as it was, the insoluble content was 0.1 wt% and the coating began to sag when heated to 250 ° C. The coating was easily peeled off.

【0052】実施例4 実施例2で得られた被覆電線を用い、触媒として塩化ロ
ジウムのトリフェニルフォスフィン錯体の 0.1g/リッ
トル溶液を用いた他は実施例3と同様に処理したとこ
ろ、処理した被覆電線の沸騰キシレンで12時間抽出した
時の不溶分は81.6wt%であり、 250℃に加熱しても垂れ
はなかった。なお、銅線から被覆は簡単に剥がれた。
Example 4 The procedure of Example 3 was repeated except that the coated electric wire obtained in Example 2 was used and a 0.1 g / l solution of a triphenylphosphine complex of rhodium chloride was used as a catalyst. The insoluble content of the coated electric wire extracted with boiling xylene for 12 hours was 81.6 wt%, and there was no sagging even when heated to 250 ° C. The coating was easily peeled off from the copper wire.

【0053】また浸漬処理前の被覆電線をそのまま沸騰
キシレンで12時間抽出したところ、不溶分は 0.2wt%で
あり 250℃に加熱すると垂れが生じた。なお、被覆は簡
単に剥がれた。
When the coated electric wire before the dipping treatment was directly extracted with boiling xylene for 12 hours, the insoluble content was 0.2% by weight, and when heated to 250 ° C., dripping occurred. The coating was easily peeled off.

【0054】実施例5 実施例1で得られた共重合体 50gに、実施例1で用いた
プロピレンの単独重合体 100g、実施例1で用いたシリ
コーンオイル2g、水酸化マグネシウム50g、フェノー
ル系の酸化防止剤 0.1gを加え良く混合したものを実施
例1と同様に造粒し、成形して被覆電線とした。この被
覆電線を実施例4と同様に触媒溶液で処理した。処理し
た被覆電線を沸騰キシレンで12時間抽出したところ不溶
分は94.1wt%であり 250℃に加熱しても被覆したポリプ
ロピレンは垂れてこなかった。また炎に接触させても燃
え上がらなかった。なお、銅線から被覆は簡単に剥がれ
た。
Example 5 To 50 g of the copolymer obtained in Example 1, 100 g of the propylene homopolymer used in Example 1, 2 g of the silicone oil used in Example 1, 50 g of magnesium hydroxide, What mixed 0.1 g of antioxidants and mixed well was granulated and shape | molded similarly to Example 1, and it was set as the coated electric wire. This coated electric wire was treated with the catalyst solution in the same manner as in Example 4. When the treated coated wire was extracted with boiling xylene for 12 hours, the insoluble content was 94.1 wt% and the coated polypropylene did not drip even when heated to 250 ° C. Moreover, it did not burn up even if it was brought into contact with the flame. The coating was easily peeled off from the copper wire.

【0055】また浸漬処理前の被覆電線をそのまま沸騰
キシレンで12時間抽出したところ、不溶分は 1.2wt%で
あり 250℃に加熱すると被覆が垂れてきた。なお、被覆
は簡単に剥がれた。
When the coated electric wire before the dipping treatment was extracted with boiling xylene for 12 hours as it was, the insoluble content was 1.2 wt%, and when heated to 250 ° C., the coating began to sag. The coating was easily peeled off.

【0056】実施例6 実施例2で得られた共重合体1000gと実施例1で用いた
シリコーンオイル50gと水酸化アルミニウム 200gとフ
ェノール系の酸化防止剤 1.0gを混合し、実施例1と同
様に造粒し、成形して被覆電線とした。この被覆電線を
実施例4と同様にして触媒溶液で処理したところ、処理
した被覆電線の沸騰キシレンで12時間抽出した時の不溶
分は87.0wt%であり、 250℃に加熱しても垂れはなく炎
に触れても燃え上がらなかった。なお、銅線から被覆は
簡単に剥がれた。
Example 6 As in Example 1, 1000 g of the copolymer obtained in Example 2, 50 g of the silicone oil used in Example 1, 200 g of aluminum hydroxide and 1.0 g of a phenolic antioxidant were mixed. Granulated and molded into a coated electric wire. When this coated electric wire was treated with the catalyst solution in the same manner as in Example 4, the insoluble content of the treated coated electric wire when extracted with boiling xylene for 12 hours was 87.0 wt%, and the sagging did not occur even when heated to 250 ° C. It didn't burn up even if I touched the flame. The coating was easily peeled off from the copper wire.

【0057】また浸漬処理前の被覆電線をそのまま沸騰
キシレンで12時間抽出したところ、不溶分は1.8 wt%で
あり 250℃に加熱すると垂れが生じた。なお、被覆は簡
単に剥がれた。
When the coated electric wire before the dipping treatment was extracted with boiling xylene for 12 hours as it was, the insoluble content was 1.8 wt%, and when it was heated to 250 ° C., dripping occurred. The coating was easily peeled off.

【0058】[0058]

【発明の効果】本発明の被覆電線は、被覆が金属線から
容易に剥がれ工業的に極めて価値がある。
INDUSTRIAL APPLICABILITY The coated electric wire of the present invention is industrially extremely valuable because the coating is easily peeled off from the metal wire.

フロントページの続き (51)Int.Cl.6 識別記号 庁内整理番号 FI 技術表示箇所 // C08L 23/02 LCQ 83/04 LRR Continuation of the front page (51) Int.Cl. 6 Identification number Office reference number FI technical display location // C08L 23/02 LCQ 83/04 LRR

Claims (6)

【特許請求の範囲】[Claims] 【請求項1】金属線にアルケニルシランとオレフィンの
共重合体とシリコーンオイルを含有する組成物を加熱溶
融して被覆してなる被覆電線。
1. A coated electric wire comprising a metal wire coated with a composition containing an alkenylsilane / olefin copolymer and silicone oil by heating and melting.
【請求項2】金属線にアルケニルシランとオレフィンの
共重合体とシリコーンオイルを含有する組成物を加熱溶
融して被覆した後、触媒と接触処理することを特徴とす
る架橋被覆電線の製造方法。
2. A method for producing a crosslinked electric wire, which comprises heating and melting a composition containing a copolymer of alkenylsilane and an olefin and silicone oil on a metal wire to coat the metal wire, and then contacting the composition with a catalyst.
【請求項3】金属線にアルケニルシランとオレフィンの
共重合体とシリコーンオイルを含有する組成物を加熱溶
融して被覆した後、放射線を照射することを特徴とする
架橋被覆電線の製造方法。
3. A method for producing a crosslinked electric wire, which comprises irradiating radiation after heating and melting a composition containing a copolymer of alkenylsilane and olefin and silicone oil on a metal wire and coating the composition.
【請求項4】金属線にアルケニルシランとオレフィンの
共重合体と、無機酸化物あるいは無機水酸化物と、シリ
コーンオイルを含有する組成物を加熱溶融して被覆した
後、触媒と接触処理することを特徴とする架橋被覆電線
の製造方法。
4. A composition comprising a metal wire containing an alkenylsilane / olefin copolymer, an inorganic oxide or an inorganic hydroxide, and a silicone oil is heated and melted to be coated, and then contact-treated with a catalyst. A method for producing a crosslinked electric wire, comprising:
【請求項5】シリコーンオイルがSi−H基を有するも
のである請求項1に記載の被覆電線。
5. The covered electric wire according to claim 1, wherein the silicone oil has a Si—H group.
【請求項6】シリコーンオイルがSi−H基を有するも
のである請求項2〜4に記載の方法。
6. The method according to claim 2, wherein the silicone oil has a Si—H group.
JP07830794A 1994-04-18 1994-04-18 Coated wire and method of manufacturing the same Expired - Fee Related JP3521952B2 (en)