JPH0730435B2 - Immersion member for molten metal plating bath - Google Patents

Immersion member for molten metal plating bath

Info

Publication number
JPH0730435B2
JPH0730435B2 JP3262898A JP26289891A JPH0730435B2 JP H0730435 B2 JPH0730435 B2 JP H0730435B2 JP 3262898 A JP3262898 A JP 3262898A JP 26289891 A JP26289891 A JP 26289891A JP H0730435 B2 JPH0730435 B2 JP H0730435B2
Authority
JP
Japan
Prior art keywords
coating
tio
metal
hot
plating bath
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP3262898A
Other languages
Japanese (ja)
Other versions
JPH05106011A (en
Inventor
富男 近藤
公志 大石
晃 丸山
生欣 宮島
和美 谷
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tocalo Co Ltd
Nippon Steel Corp
Original Assignee
Tocalo Co Ltd
Sumitomo Metal Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tocalo Co Ltd, Sumitomo Metal Industries Ltd filed Critical Tocalo Co Ltd
Priority to JP3262898A priority Critical patent/JPH0730435B2/en
Publication of JPH05106011A publication Critical patent/JPH05106011A/en
Publication of JPH0730435B2 publication Critical patent/JPH0730435B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】この発明は、溶融金属めっき浴浸
漬部材に関するもので、特に溶融亜鉛、溶融アルミニウ
ム、溶融錫、溶融亜鉛アルミニウム合金に対して優れた
耐侵食性を有する溶融金属めっき浴浸漬部材に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a molten metal plating bath dipping member, and particularly to a molten metal plating bath dipping having excellent corrosion resistance to molten zinc, molten aluminum, molten tin and molten zinc aluminum alloy. Regarding members.

【0002】[0002]

【従来の技術】近年、耐食性、溶接性および塗装性に優
れた溶融金属めっき鋼板等の表面処理鋼板は、自動車
用、土木、建築用あるいは家電用等の用途の需要が急速
に拡大している。この表面処理鋼板の製造法としては、
主として連続溶融亜鉛めっき法、連続溶融アルミニウム
めっき法等の連続溶融金属めっき法が採用されている。
連続溶融金属めっき法は、図1に示すとおり、連続炉に
おいて機械的性質の調整ならびに表面を清浄、活性化さ
れた鋼帯1は、スナウト2を介して溶融金属槽3中に浸
漬され、浴中のシンクロール4によって進行方向が転換
され、サポートロール5、6を経由して溶融金属槽3か
ら引上げられたのち、ワイピングノズル7から気体を噴
射して過剰のめっき液を絞取ってめっき付着量を調整さ
れためっき鋼帯1は、トップロール8を経由してその後
常温まで冷却される。
2. Description of the Related Art In recent years, surface-treated steel sheets such as hot-dip galvanized steel sheets which are excellent in corrosion resistance, weldability and paintability have been rapidly expanding in applications such as automobiles, civil engineering, construction and home appliances. . As a method of manufacturing this surface-treated steel sheet,
Continuously hot dip galvanizing methods, continuous hot dip aluminum plating methods and the like are mainly used.
In the continuous hot metal plating method, as shown in FIG. 1, the steel strip 1 whose mechanical properties have been adjusted and whose surface has been cleaned and activated in a continuous furnace is immersed in a hot metal bath 3 through a snout 2 and bathed. The direction of travel is changed by the sink roll 4 inside, and the molten metal tank 3 is pulled up via the support rolls 5 and 6, and then a gas is jetted from the wiping nozzle 7 to squeeze the excess plating solution and deposit the plating. The plated steel strip 1 whose amount has been adjusted is cooled to room temperature after passing through the top roll 8.

【0003】上記連続金属めっき法の溶融金属槽中に浸
漬され、あるいは溶融金属の飛散し易い場所で使用され
るシンクロール4、サポートロール5、6等の溶融金属
めっき浴浸漬部材は、溶融金属との直接接触あるいは溶
融金属が付着した高温のめっき鋼帯1と接触する。この
ため、溶融金属めっき浴浸漬部材としては、溶融金属に
よる侵食が発生し難く、めっき鋼帯との接触による摩耗
が少なく、部材表面に浴中に浮遊するFe−Zn合金で
あるドロス成分などの合金層が付着、生成し難く、付着
した溶融金属の剥離ならびに保守点検が容易で、部材と
しての寿命が長く低コストで、しかも高温の溶融金属中
に浸漬した際の熱衝撃によく耐えることなどの性能が要
求される。
The molten metal plating bath dipping members such as the sink rolls 4, the support rolls 5 and 6 which are immersed in the molten metal bath of the above-mentioned continuous metal plating method or used in a place where the molten metal is easily scattered are the molten metal. Direct contact with or contact with the high temperature plated steel strip 1 to which the molten metal adheres. Therefore, as the member for dipping in the molten metal plating bath, erosion by the molten metal is unlikely to occur, wear due to contact with the plated steel strip is small, and dross components such as Fe-Zn alloy floating in the bath on the member surface. The alloy layer is difficult to adhere and generate, the adhered molten metal can be easily peeled off and maintained and inspected, it has a long life as a member, low cost, and it can withstand thermal shock when immersed in high temperature molten metal. Performance is required.

【0004】上記要求に応えられるめっき浴浸漬部材と
しては、表面にJIS H8303(1976)に制定
のCo基自溶合金を溶射したロール、10%以上のWC
あるいはCrC、TiCの一種または二種以上で残部が
熱間耐食性金属、その酸化物あるいはこれらの二種以
上、または不可避的不純物からなる0.1〜2.4mm
の厚さの表面被覆層を有する有する部材(特公昭58−
37386号公報)、表面にZrO2:20〜60重量
%(以下単に%という)と残部Al2O3からなるセラミ
ック被覆層を施した部材(特公平2−43819号公
報)、表面にサーメットの被覆層を有する部材におい
て、上記被覆層を、Co5〜28%を含むWC−Co系
サーメット材料による気孔率が1.8%以下の溶射被覆
層とした部材(特公平2−55502号公報)、あるい
は酸化物または炭化物を主成分とするセラミック溶射皮
膜を形成した鋼鉄性ロールのその表面に、化学的緻密化
処理皮膜を形成したロール(実開平3−63565号公
報)等多くの提案が行われている。
As a plating bath dipping member that can meet the above requirements, a roll having a surface coated with a Co-based self-fluxing alloy established in JIS H8303 (1976), 10% or more WC
Or 0.1 to 2.4 mm consisting of one or more of CrC and TiC, with the balance being a hot-corrosion resistant metal, its oxide or two or more of these, or inevitable impurities.
Having a surface coating layer having a thickness of
37386 JP), ZrO the surface 2: 20-60 wt% (hereinafter simply% hereinafter) and subjected to ceramic coating layers and the balance Al 2 O 3 member (KOKOKU 2-43819 JP), the surface of the cermet In the member having a coating layer, the coating layer is a thermal spray coating layer having a porosity of 1.8% or less by a WC-Co cermet material containing Co5 to 28% (Japanese Patent Publication No. 2-55502). Alternatively, many proposals have been made, such as a roll having a chemically densified film formed on the surface of a steel roll having a ceramic sprayed film containing oxide or carbide as a main component (Japanese Utility Model Publication No. 3-63565). ing.

【0005】[0005]

【発明が解決しようとする課題】上記従来技術のCo基
自溶合金を溶射したロールおよび特公平2−43819
号公報に開示の部材は、それ以前の表面無処理ロールに
比較すると、めっき浴浸漬部材として長寿命を有してい
るものの、2週間程度使用すると溶射皮膜中の皮膜成分
の一部が溶融金属と反応して部材表面に合金層を生じた
り、あるいは皮膜内に存在する微細間隙や気孔に溶融金
属が浸入することによって部材表面の皮膜が局部的に剥
離し、部材基材が露呈して溶融金属と反応して合金層を
形成する。また、健全皮膜部であってもめっき浴中に浮
遊するFe−Zn合金であるドロス成分が表面に局部的
に付着する結果、周囲健全部とめっき鋼帯に対するめっ
き特性が異なり、めっき鋼帯に不均一模様を生じたり、
付着生成物による押込み疵を生じるため、めっき鋼板の
表面品質を著しく低下させる。
Rolls sprayed with the Co-based self-fluxing alloy of the prior art and Japanese Patent Publication No. 2-43819.
The member disclosed in Japanese Patent Publication has a long life as a member for immersion in a plating bath, as compared with the surface-untreated rolls before that, but when used for about 2 weeks, a part of the film components in the sprayed film is molten metal. React to form an alloy layer on the surface of the member, or the molten metal penetrates into the fine gaps and pores that exist in the film, causing the film on the member surface to peel off locally, exposing the member base material and melting. It reacts with the metal to form an alloy layer. Further, even in the sound film portion, the dross component, which is an Fe-Zn alloy floating in the plating bath, locally adheres to the surface, and as a result, the plating characteristics for the surrounding sound portion and the plated steel strip are different, It may cause uneven patterns,
Since indentation flaws are caused by the adhered products, the surface quality of the plated steel sheet is significantly reduced.

【0006】また、特公昭58−37386号公報に開
示の部材は、WC、Cr3C2、TiCなどの炭化物を使
用するため、めっき金属に対する耐食性に優れている
が、この炭化物のみでは部材基材に対する密着性などの
機械的強度に乏しく、共存する金属成分の添加が不可欠
となる。しかし、添加金属の種類によっては、めっき金
属と冶金、拡散反応をおこして侵食されることがある。
金属酸化物や金属炭化物は、物性として溶融めっき金属
に対し耐食性を有するが、部材表面保護を目的として溶
射皮膜ののような被覆層を形成して実用に供すると、被
覆層そのものが耐溶融亜鉛性を持つと同時に、溶融めっ
き金属に対する環境遮断性を有し、部材を溶融めっき金
属から保護するよう機能する必要がある。しかし従来技
術における溶融金属浴浸漬部材保護皮膜は、皮膜成分に
金属を含有するか、あるいは皮膜内に溶融めっき金属が
侵入するに十分な気孔が存在するため、皮膜構成化学成
分の特性で耐溶融めっき金属性に優れているとしても、
その機能を十分に発揮できる状態にないのが実情であ
る。さらに、耐溶融めっき金属性に優れている特公平2
−55502号公報の部材においても、微小なドロス成
分の局部的な付着があってこれがめっき鋼帯に転写さ
れ、高度な表面均一性を要求されるめっき鋼板製造用途
に対しては十分でない。
Further, since the member disclosed in Japanese Patent Publication No. 58-37386 uses carbides such as WC, Cr 3 C 2 and TiC, it is excellent in corrosion resistance against plated metal. Poor mechanical strength, such as adhesion to materials, requires the addition of coexisting metal components. However, depending on the type of the added metal, it may erode due to metallurgical and diffusion reactions with the plated metal.
Metal oxides and metal carbides have corrosion resistance to hot-dip galvanized metal as a physical property, but if a coating layer such as a thermal spray coating is formed for practical use for the purpose of protecting the surface of a member, the coating layer itself will not have a resistance to hot dip zinc. At the same time, it must have an environmental barrier property to the hot dip plated metal and function to protect the member from the hot dip plated metal. However, the protective coating for molten metal bath immersion member in the prior art contains a metal in the coating component or has sufficient pores for the hot-dip galvanized metal to penetrate into the coating. Even if it has excellent plating metal properties,
The reality is that it is not in a state where it can fully exercise its functions. Furthermore, Japanese Patent Publication No. 2 which has excellent hot dip galvanizing resistance
Even in the member of Japanese Patent No. 55502, minute dross components are locally adhered and transferred to the plated steel strip, which is not sufficient for use in the production of plated steel sheets requiring high surface uniformity.

【0007】さらに実開平3−63565公報に開示の
部材は、部材表面の溶射皮膜上に化学的緻密化処理皮膜
を形成させることによって、特公昭58−37386号
公報、特公平2−55502号公報の部材よりも合金層
付着性を改善したものであるが、低アルミニウム含有%
のZnめっき浴においては、軽微な合金層巻付きを生
じ、問題の完全解決に至らないのが実態である。
Further, the member disclosed in Japanese Utility Model Laid-Open No. 3-63565 has a chemical densification treatment film formed on the thermal spray coating on the surface of the member, and thus, Japanese Patent Publication No. 58-37386 and Japanese Patent Publication No. 2-55502. The alloy layer adhesion is improved over that of the above-mentioned member, but the low aluminum content%
In the Zn plating bath described above, the fact that a slight alloy layer winding occurs and the problem cannot be completely solved.

【0008】この発明の目的は、溶融金属めっき浴中に
浸漬した場合においても、部材表面への合金層巻付きや
異物付着を抑制でき、しかも皮膜剥離等の熱衝撃性に優
れた溶融金属めっき浴浸漬部材を提供することにある。
An object of the present invention is to prevent molten alloy plating from winding the alloy layer and adhering foreign matter onto the surface of the member even when immersed in a molten metal plating bath, and having excellent thermal shock resistance such as film peeling. To provide a bath dipping member.

【0009】[0009]

【課題を解決するための手段】本発明者らは、上記目的
を達成すべく次のとおり鋭意試験研究を行った。その結
果、部材表面に形成するセラミックス材料皮膜としてA
l2O3−TiO2擬2元系金属酸化物皮膜は、溶融めっ
き金属に対する濡れ性が小さく、したがって反応速度が
著しく小さいこと、また、溶射皮膜として一般的に用い
られているAl2O3単体、Cr2O3、安定化ZrO2な
どに比較し、状態図における固相線温度が2000〜1
700℃と比較的低く、プラズマあるいは酸素−炭化水
素燃焼炎溶射熱源中で軟化・溶融し易いため、気孔率の
小さい緻密な皮膜を形成させることができること、さら
に、Al2O3−TiO2擬2元系金属酸化物皮膜の表面
上および皮膜上層部に、酸化クロムセラミックスコーテ
ィング層からなる化学的緻密化処理皮膜を形成すること
によって、溶融めっき金属に対する濡れ性が大幅に改善
でき、皮膜と溶融めっき金属との反応が防止できること
を究明し、この発明に到達した。
[Means for Solving the Problems] The inventors of the present invention conducted the following earnest test research in order to achieve the above object. As a result, as a ceramic material film formed on the surface of the member, A
The l 2 O 3 -TiO 2 pseudo binary metal oxide coating has a low wettability with respect to the hot-dip metal and therefore has a remarkably low reaction rate, and the Al 2 O 3 which is generally used as a thermal spray coating. Compared with simple substance, Cr 2 O 3 , stabilized ZrO 2, etc., the solidus temperature in the phase diagram is 2000-1.
700 ° C. and comparatively low, plasma or oxygen - for easily softened and melted in a hydrocarbon combustion flame spraying heat source, that can form a small dense coating porosity, further, Al 2 O 3 -TiO 2 pseudo By forming a chemical densification treatment film consisting of a chromium oxide ceramics coating layer on the surface of the binary metal oxide film and the upper layer of the film, the wettability to hot-dip galvanized metal can be greatly improved and The inventors have reached the present invention by investigating that a reaction with a plated metal can be prevented.

【0010】すなわちこの発明は、表面にAl2O3−T
iO2擬2元系金属酸化物を溶射被覆して保護層を形成
してなる溶融金属めっき浴浸漬部材である。
That is, according to the present invention, Al 2 O 3 -T is formed on the surface.
It is a member for dipping in a molten metal plating bath, which is formed by spray-coating an iO 2 pseudo binary metal oxide to form a protective layer.

【0011】また、表面にAl2O3−TiO2擬2元系
金属酸化物を溶射被覆して保護層を形成し、該保護層表
面層に酸化クロムセラミックスコーティング層からなる
化学的緻密化処理皮膜を形成してなる溶融金属めっき浴
浸漬部材である。
Further, the surface is chemically coated with Al 2 O 3 --TiO 2 pseudo binary metal oxide to form a protective layer, and the surface layer of the protective layer is chemically densified by a chromium oxide ceramics coating layer. It is a molten metal plating bath immersion member formed with a film.

【0012】上記Al2O3−TiO2擬2元系金属酸化
物が両者の固溶体複合物であって、TiO2を0.5〜
50%含有し、不純物としてCr2O3、CaO、SiO
2、ZrO2、MgO、FeO、Fe2O3、Fe3O4のう
ちの1種または2種以上を5%未満含有している溶融金
属めっき浴浸漬部材である。
The Al 2 O 3 -TiO 2 pseudo-binary metal oxide is a solid solution composite of the two , and the TiO 2 content is 0.5-0.5.
50% content, Cr 2 O 3 , CaO, SiO as impurities
The molten metal plating bath dipping member contains less than 5% of one or two or more of 2 , ZrO 2 , MgO, FeO, Fe 2 O 3 and Fe 3 O 4 .

【0013】[0013]

【作用】一般に金属酸化物材料は、溶融亜鉛、溶融アル
ミニウムなどの溶融めっき金属に接触したときの接触角
が大きいことが知られている。文献によれば代表的な金
属酸化物材料に対する値は、表1のとおりであり、溶融
めっき金属濡れ性についてのみで見れば、耐溶融めっき
金属皮膜として機能する。
It is generally known that metal oxide materials have a large contact angle when they come into contact with hot-dip galvanized metals such as hot-dip zinc and hot-dip aluminum. According to the literature, the values for representative metal oxide materials are as shown in Table 1, and the function as a hot-dip galvanizing metal film is observed only by the hot-dip galvanizing metal wettability.

【0014】[0014]

【表1】 [Table 1]

【0015】そこで本発明者らは、プラズマ溶射手段を
用い、各種金属酸化物溶射皮膜の溶融亜鉛に対するぬれ
性を調査した。金属酸化物セラミックスとしては、純A
l2O3、Al2O3−5%TiO2混合物、Al2O3−5
%TiO2固溶体、Al2O3−13%TiO2混合物、A
l2O3−13%TiO2固溶体、Al2O3−40%Ti
O2混合物、Al2O3−40%TiO2固溶体、Cr
2O3、ZrO2−8%Y2O 3の9種とした。試験は、直
径30mm、長さ300mmの軟鋼製の円柱試験片を準
備し、その外周に上記9種の材料をプラズマ溶射法で溶
射して200μmの厚さで溶射皮膜を被成させた。これ
を480℃の溶融亜鉛中に10日間侵漬したのち取出
し、溶射皮膜と溶融亜鉛とのぬれ状態を観察した。その
結果を表2に示す。
Therefore, the present inventors have established a plasma spraying means.
Wetting of various metal oxide sprayed coatings against molten zinc
The sex was investigated. As metal oxide ceramics, pure A
l2O3, Al2O3-5% TiO2Mixture, Al2O3-5
% TiO2Solid solution, Al2O3-13% TiO2Mixture, A
l2O3-13% TiO2Solid solution, Al2O3-40% Ti
O2Mixture, Al2O3-40% TiO2Solid solution, Cr
2O3, ZrO2-8% Y2O 39 kinds of. The test is straightforward
A cylinder test piece made of mild steel with a diameter of 30 mm and a length of 300 mm is prepared.
The above 9 kinds of materials are sprayed on the outer periphery by plasma spraying method.
Then, a thermal spray coating was formed to a thickness of 200 μm. this
Soaked in molten zinc at 480 ℃ for 10 days and then removed
Then, the wet state of the sprayed coating and the molten zinc was observed. That
The results are shown in Table 2.

【0016】[0016]

【表2】 [Table 2]

【0017】表2から明らかなとおり、溶融亜鉛にぬれ
難いとされているいずれの材料も溶融亜鉛の侵食を受
け、溶融亜鉛が溶射皮膜内に侵入していた。すなわち、
溶射皮膜が破壊され溶融亜鉛と鋼基材が反応し、溶射皮
膜は基材保護機能を果たしていないことが判明した。こ
れは溶融めっき金属と反応し難い皮膜材料であっても、
溶融めっき金属の侵入を防止するのに十分な低気孔率で
ないと、保護皮膜にはなり得ないことを示すものであ
る。本発明者らは溶融亜鉛が保護皮膜内に侵入する要因
の一つである皮膜の微細構造、すなわち気孔率に着目
し、気孔率を溶融亜鉛の侵入を防止するのに十分小さく
するための方法について検討した。溶射皮膜は、その原
理上ある伝播速度を持った火炎流中に材料を投入し、材
料粒子が飛行動作を与えられ、その間に軟化、溶融、基
材に衝突、偏平、積層することによって形成される。し
たがって、皮膜は、本質的に気孔を有することになる。
R>しかし火炎流速を増大させると、粒子の運動エネルギ
ーが大きくなり、その結果基材に対する大きな衝突エネ
ルギーが付与され、衝突粒子の偏平、密着が進行し、生
成皮膜内の気孔率を著しく小さくすることができる。し
かし火炎流速を増大させると、材料粒子の火炎中での滞
留時間が短くなり、その結果粒子の軟化、溶融効率が低
下することになる。したがって溶融温度などの物性から
適用できる材料は限定されることになる。そこで、高速
ガス炎溶射法を用い、前記9種の材料について成膜性を
試験した。その結果を表3に示す。なお、表3中の○は
正常に成膜、×は成膜せずを示す。
As is clear from Table 2, all materials which are considered to be difficult to wet with molten zinc were eroded by the molten zinc, and the molten zinc penetrated into the thermal spray coating. That is,
It was found that the sprayed coating was destroyed and the molten zinc reacted with the steel base material, and the sprayed coating did not fulfill the function of protecting the base material. Even if this is a coating material that does not easily react with hot-dip metal,
This indicates that a protective film cannot be obtained unless the porosity is low enough to prevent the hot-dip metal from entering. The inventors of the present invention focused on the microstructure of the coating, that is, the porosity, which is one of the factors by which molten zinc penetrates into the protective coating, and a method for making the porosity small enough to prevent the penetration of molten zinc. Was examined. A thermal spray coating is formed by introducing a material into a flame flow that has a certain propagation velocity in principle, and the material particles are given a flying motion, during which they soften, melt, collide with the base material, flatten, and stack. It Therefore, the coating will essentially have porosity.
R> However, when the flame velocity is increased, the kinetic energy of the particles increases, and as a result, a large collision energy is applied to the substrate, the flattening and adhesion of the collision particles progress, and the porosity in the formed film is significantly reduced. be able to. However, when the flame velocity is increased, the residence time of the material particles in the flame becomes shorter, and as a result, the softening and melting efficiency of the particles decrease. Therefore, applicable materials are limited due to physical properties such as melting temperature. Then, the high-speed gas flame spraying method was used to test the film forming properties of the above nine kinds of materials. The results are shown in Table 3. It should be noted that in Table 3, ∘ indicates normal film formation, and x indicates no film formation.

【0018】[0018]

【表3】 [Table 3]

【0019】表3に示すとおり、9種の材料のうち、A
l2O3−5%TiO2固溶体、Al2O3−13%TiO2
固溶体、Al2O3−40%TiO2固溶体の3種が溶射
皮膜を形成したが、他の6種は溶射皮膜を形成しなかっ
た。このことは、高速ガス炎溶射法では、ガス炎温度が
2800℃程度であり、材料粒子の火炎内滞留時間にお
ける受熱条件から、成膜性に及ぼす材料軟化、溶融温度
条件の合致が必要であり、この3種のみがこの条件を満
たしたものと考えられる。そこで、画像解析装置を用い
てこれら3種の溶射皮膜の微細構造(主として気孔率)
をプラズマ溶射皮膜との比較で観察した。その結果を表
4に示す。
As shown in Table 3, among 9 kinds of materials, A
l 2 O 3 -5% TiO 2 solid solution, Al 2 O 3 -13% TiO 2
Three kinds of solid solution and Al 2 O 3 -40% TiO 2 solid solution formed a sprayed coating, but the other 6 kinds did not form a sprayed coating. This means that in the high-speed gas flame spraying method, the gas flame temperature is about 2800 ° C., and it is necessary to match the material softening and melting temperature conditions that affect the film forming property from the heat receiving conditions during the residence time of the material particles in the flame. , It is considered that only these three species satisfy this condition. Therefore, the fine structure (mainly porosity) of these three types of thermal spray coatings was analyzed using an image analysis device.
Was observed in comparison with the plasma spray coating. The results are shown in Table 4.

【0020】[0020]

【表4】 [Table 4]

【0021】表4に示すとおり、高速ガス炎溶射法によ
って形成されたAl2O3−TiO2固溶体系3種の溶射
皮膜は、いずれも気孔率0.5%以下を示し、緻密な微
細構造を有する皮膜であることが判明した。そこでぬれ
性調査のときと同様、これら3種のAl2O3−TiO2
固溶体系溶射皮膜を、直径30mm、長さ300mmの
軟鋼製の円柱試験片外周に高速ガス炎溶射法により20
0μmの厚さで形成させた。これを480℃の溶融亜鉛
浴中に10日間浸漬したのち取出し、溶射皮膜と溶融亜
鉛との反応状態を観察した。その結果、溶射皮膜はいず
れも溶融亜鉛にぬれておらず、かつ溶融亜鉛の皮膜内へ
の侵入も認められなかった。
As shown in Table 4, the sprayed coatings of Al 2 O 3 -TiO 2 solid solution type 3 formed by the high-velocity gas flame spraying method all have a porosity of 0.5% or less and a fine microstructure. It was found to be a film having Therefore, as with the wettability investigation, these three types of Al 2 O 3 —TiO 2
A solid solution sprayed coating was applied on the outer circumference of a mild steel cylindrical test piece with a diameter of 30 mm and a length of 300 mm by a high-speed gas flame spraying method.
It was formed to a thickness of 0 μm. This was immersed in a molten zinc bath at 480 ° C. for 10 days and then taken out, and the reaction state of the sprayed coating and molten zinc was observed. As a result, none of the thermal spray coatings was wet with molten zinc, and no infiltration of molten zinc into the coating was observed.

【0022】上記皮膜の形成は、高速ガス炎溶射法に限
定され、プラズマ溶射法等の低流速の溶射法では得られ
ないという問題を有している。そこでいずれの溶射法に
おいても、前記Al2O3−TiO2固溶体系材料の有用
性を発揮させる方法について検討を重ねた。その結果、
Al2O3−TiO2固溶体系材料の溶射皮膜表面上およ
び皮膜上層部に後述する化学的緻密化処理皮膜を形成す
ることによって、飛躍的に対溶融亜鉛性が向上すること
を見い出した。ここで化学的緻密化処理の方法は、予め
Al2O3−TiO2固溶体系材料の溶射皮膜を部材表面
に形成し、ついでこの部材をクロム酸を含む水溶液中に
浸漬するか、あるいはこの部材表面にクロム酸を含む水
溶液を噴霧する。この処理によって溶射皮膜表面は、ク
ロム酸で被覆されると共に、その溶射皮膜中にピンホー
ルが存在すれば、クロム酸水溶液がその中に浸透するこ
ととなる。その後、ロール表面を被覆したクロム酸皮膜
を、200〜500℃に加熱する。この処理によって前
記クロム酸中の水分が蒸発揮散すると共に、Cr2O3が
残渣物として溶射皮膜上やピンホール中に残存し、ロー
ルの溶射皮膜表面部に薄い酸化クロムのセラミックコー
ティング層が形成される。このクロム酸水溶液中への浸
漬と加熱を数回繰返すと、Cr2O3のコーティング層は
次第に厚くなり、対溶融亜鉛性が向上する。
The formation of the above-mentioned coating is limited to the high-speed gas flame spraying method and has a problem that it cannot be obtained by a low-flow rate spraying method such as a plasma spraying method. Therefore, in any of the thermal spraying methods, a method for exerting the usefulness of the Al 2 O 3 —TiO 2 solid solution material was examined. as a result,
It has been found that by forming a chemical densification treatment film described later on the surface of the sprayed coating of Al 2 O 3 -TiO 2 solid solution material and on the coating upper layer portion, the resistance to molten zinc is dramatically improved. Here, the chemical densification method is carried out by forming a sprayed coating of Al 2 O 3 —TiO 2 solid solution type material on the surface of the member in advance and then immersing this member in an aqueous solution containing chromic acid, or The surface is sprayed with an aqueous solution containing chromic acid. By this treatment, the surface of the sprayed coating is coated with chromic acid, and if pinholes are present in the sprayed coating, the chromic acid aqueous solution will penetrate into the surface. Then, the chromic acid film which coat | covered the roll surface is heated at 200-500 degreeC. By this treatment, water in the chromic acid is evaporated and Cr 2 O 3 remains as a residue on the spray coating or in the pinholes, forming a thin chromium oxide ceramic coating layer on the surface of the spray coating of the roll. To be done. When the immersion in the chromic acid aqueous solution and the heating are repeated several times, the Cr 2 O 3 coating layer becomes thicker and the resistance to molten zinc is improved.

【0023】高速ガス炎溶射法およびプラズマ溶射法を
用いてTiO25%を含むAl2O3−TiO2系固溶体、
TiO213%を含むAl2O3−TiO2系固溶体、Ti
O240%を含むAl2O3−TiO2系固溶体の3種の溶
射皮膜を、直径30mm、長さ300mmの鋼製の円柱
試験片外周に200μmの厚さに被成したのち、前記化
学的緻密化処理皮膜を10μmの厚さ形成させ、ついで
480℃の溶融亜鉛浴中に10日間浸漬後取出し、皮膜
と溶融亜鉛との反応状態を観察した。その結果を表5に
示す。なお、表5中の対亜鉛ぬれ性欄の○は合金層付着
良好を示す。
Al 2 O 3 -TiO 2 based solid solution containing 5% of TiO 2 by using a high speed gas flame spraying method and a plasma spraying method,
Al 2 O 3 -TiO 2 based solid solution containing 13% of TiO 2 , Ti
Three kinds of thermal sprayed coatings of Al 2 O 3 —TiO 2 based solid solution containing 40% of O 2 were coated on the outer circumference of a steel cylinder test piece having a diameter of 30 mm and a length of 300 mm to a thickness of 200 μm, and then the above chemical An artificial densification treatment film was formed to a thickness of 10 μm, then immersed in a molten zinc bath at 480 ° C. for 10 days and then taken out, and the reaction state between the film and the molten zinc was observed. The results are shown in Table 5. In addition, in the column of wettability to zinc in Table 5, ◯ indicates that the adhesion of the alloy layer was good.

【0024】[0024]

【表5】 [Table 5]

【0025】表5に示すとおり、皮膜は、いずれの溶射
法の場合においても溶融亜鉛にぬれておらず、かつ皮膜
内への溶融亜鉛の侵入も全く認められなかった。これは
本質的に溶融亜鉛にぬれ難いAl2O3−TiO2系固溶
体を用い、しかも溶射皮膜表面上および上層部に化学的
緻密化処理皮膜を形成させることによって、溶射方法の
如何にかかわらず、溶融亜鉛浴中でその基材に対する保
護皮膜としての機能と、基材表面への溶融めっき浴成分
付着を防止できることを意味している。特に高速ガス炎
溶射法に対し、気孔率の高いプラズマ溶射法において
も、高速ガス炎溶射法と同等の効果を発揮していること
は、化学的緻密化処理によって気孔部への酸化クロムデ
ポジットの浸透が有効であることを証明するものであ
り、また、高速ガス炎溶射法と併用することによって、
さらに効果を発揮することは勿論である。
As shown in Table 5, the coating was not wet with molten zinc in any of the spraying methods, and no infiltration of molten zinc into the coating was observed. This is because an Al 2 O 3 —TiO 2 type solid solution which is essentially insoluble in molten zinc is used, and a chemical densification treatment film is formed on the surface and the upper layer of the spray coating, regardless of the spraying method. In other words, it means that it can function as a protective film for the substrate in the hot dip zinc bath and can prevent the components of the hot dipping bath from adhering to the surface of the substrate. Especially in the high-velocity gas flame spraying method, even in the plasma spraying method with high porosity, the same effect as in the high-speed gas flame spraying method is exhibited. It proves that the penetration is effective, and when used in combination with the high-speed gas flame spraying method,
Needless to say, it is even more effective.

【0026】この発明の溶融金属めっき浴浸漬部材は、
表面に形成したAl2O3−TiO2擬2元系金属酸化物
の溶射被覆保護層が溶融めっき金属に対するぬれ性が小
さく、溶融めっき金属との反応速度が著しく小さい。ま
た、溶射皮膜として一般的に用いられているAl2O3単
体、Cr2O3、安定化ZrO2などに比較し、状態図に
おける固相線温度が2000〜1700℃と比較的低
く、プラズマあるいは酸素−炭化水素燃焼炎溶射熱源中
で軟化・溶融し易いため、気孔率の小さい緻密な皮膜を
形成させることができ、溶融めっき金属中に浸漬された
とき、溶融めっき金属の皮膜内への侵入を防止すること
ができる。
The molten metal plating bath immersion member of the present invention is
The Al 2 O 3 —TiO 2 pseudo binary metal oxide sprayed coating protective layer formed on the surface has a low wettability with respect to the hot dip plated metal, and the reaction rate with the hot dip plated metal is extremely low. In addition, compared with Al 2 O 3 simple substance, Cr 2 O 3 and stabilized ZrO 2 which are generally used as a thermal spray coating, the solidus temperature in the phase diagram is relatively low at 2000 to 1700 ° C. Alternatively, since it easily softens and melts in an oxygen-hydrocarbon combustion flame spraying heat source, it is possible to form a dense film with a small porosity, and when immersed in the hot-dip galvanized metal, when it is immersed in the hot-dip galvanized metal, Intrusion can be prevented.

【0027】さらにこの発明の溶融金属めっき浴浸漬部
材は、表面に形成したAl2O3−TiO2擬2元系金属
酸化物の溶射被覆保護層表面層に、酸化クロムセラミッ
クスコーティング層からなる化学的緻密化処理皮膜を形
成したから、溶融めっき金属に対して極めてぬれ難く、
皮膜と溶融めっき金属との反応が防止され、溶融めっき
金属の皮膜内への侵入および部材表面の保護を図ること
ができる。
Further, the member for dipping in the molten metal plating bath according to the present invention comprises a chemical coating consisting of a chromium oxide ceramics coating layer on the surface layer of the Al 2 O 3 --TiO 2 pseudo binary metal oxide sprayed coating protective layer formed on the surface. Since a film for densification is formed, it is extremely difficult to wet the galvanized metal,
The reaction between the coating and the hot-dip metal can be prevented, and the hot-dip metal can penetrate into the coating and protect the surface of the member.

【0028】上記溶射材料成分としては、TiO2を
0.5〜50%含有するAl2O3−TiO2固溶体複合
物が好ましい。また、溶射皮膜厚さは、20μm未満で
は被覆の効果が認められず、600μmを超えると保護
層としての効果が増大せず、溶射に多くの時間と経費を
要し経済的でなく、かつ剥離損耗の発生確率が大きくな
るため、20〜600μmとするのが好ましい。さら
に、溶射皮膜保護層表面上および上層部に形成する化学
的緻密化処理皮膜の厚さは、0.5μm未満では化学的
緻密化処理が不十分で、溶射保護層中に存在するピンホ
ール中にクロム酸が十分に浸透せず、溶射保護層の表面
も完全に被覆できない。また、逆に30μmを超えると
効果が頭打ちとなり、コーティング処理に多くの時間と
経費を要するので得策でないため、0.5〜30μmと
するのが好ましい。
The thermal spray material component is preferably an Al 2 O 3 -TiO 2 solid solution composite containing 0.5 to 50% of TiO 2 . Further, if the thickness of the sprayed coating is less than 20 μm, the effect of coating is not recognized, and if it exceeds 600 μm, the effect as a protective layer does not increase, and it takes a lot of time and cost for spraying, and it is not economical and peels off. Since the probability of occurrence of wear increases, it is preferably 20 to 600 μm. Furthermore, if the thickness of the chemical densification treatment film formed on the surface of the thermal spray coating protection layer and on the upper layer is less than 0.5 μm, the chemical densification treatment is insufficient and pinholes existing in the thermal spray protection layer Chromic acid does not sufficiently penetrate into the surface, and the surface of the thermal spray protection layer cannot be completely covered. On the other hand, if the thickness exceeds 30 μm, the effect will reach the ceiling and the coating process requires a lot of time and cost, which is not a good idea. Therefore, the thickness is preferably 0.5 to 30 μm.

【0029】[0029]

【実施例】【Example】

実施例1 図1に示す連続溶融亜鉛めっきラインのシンクロール4
およびサポートロール5、6について、高速ガス炎溶射
法を用い、13%のTiO2を含むAl2O3−TiO2固
溶体および40%のTiO2を含むAl2O3−TiO2固
溶体の2種類の溶射皮膜を、100μmの厚さで実機ロ
ールに被成させ、これを連続溶融亜鉛めっきラインの実
機溶融亜鉛めっき浴に浸漬し、各々2週間×2回の連続
使用を行った。そして1回目および2回目の各ロールの
めっき浴より引上げ後の合金層付着状況、溶射皮膜剥離
状況、溶射皮膜摩耗状況を目視観察した。その結果を表
6に示す。なお、表6中の○は良好、×は不具合ありを
示す。
Example 1 Sink roll 4 of the continuous hot-dip galvanizing line shown in FIG.
For the support rolls 5 and 6, two types of Al 2 O 3 —TiO 2 solid solution containing 13% TiO 2 and Al 2 O 3 —TiO 2 solid solution containing 40% TiO 2 were used by using a high speed gas flame spraying method. The thermal sprayed coating of No. 1 was applied to an actual machine roll with a thickness of 100 μm, and this was immersed in an actual machine hot-dip galvanizing bath of a continuous hot-dip galvanizing line, and continuously used for 2 weeks × 2 times. Then, the state of adhesion of the alloy layer, the state of peeling of the thermal spray coating, and the state of wear of the thermal spray coating after the pulling from the plating bath of each roll for the first time and the second time were visually observed. The results are shown in Table 6. In Table 6, ◯ means good, and X means trouble.

【0030】[0030]

【表6】 [Table 6]

【0031】この発明の溶射皮膜を表面に形成したロー
ルは、各々延べ約1ケ月の長期に亘り実機溶融亜鉛めっ
き浴での浸漬および実使用テストを行ったにもかかわら
ず、実使用時の合金層および異物付着等による押込み疵
等、めっき鋼板表面品質の不具合は一度も発生しなかっ
た。また、溶融亜鉛めっき浴から引上げ後のロール表面
には、表6に示すとおり合金層付着、異物付着は一切認
められなかった。また、ロール表面の付着亜鉛を除去し
たのち、皮膜観察を実施した結果、皮膜剥離や皮膜摩耗
等の現象は認められず、長期使用後においても健全な溶
射皮膜を保持していた。
The roll having the sprayed coating of the present invention formed on its surface was immersed in an actual hot-dip galvanizing bath for a total of about one month and was subjected to an actual use test, but the alloy was actually used. No defects in the surface quality of the plated steel sheet, such as indentation flaws due to adhesion of layers and foreign matter, occurred. Further, as shown in Table 6, no adhesion of the alloy layer and no adhesion of foreign matter were observed on the roll surface after being pulled up from the hot dip galvanizing bath. Further, as a result of observing the coating after removing the zinc deposited on the roll surface, no phenomenon such as coating peeling or coating abrasion was observed, and a sound thermal spray coating was retained even after long-term use.

【0032】実施例2 図1に示す連続溶融亜鉛めっきラインのシンクロール4
およびサポートロール5、6について、高速ガス炎溶射
法およびプラズマ溶射法を用い、13%のTiO2を含
むAl2O3−TiO2固溶体Aおよび40%のTiO2を
含むAl2O3−TiO2固溶体Bの2種類の溶射皮膜
を、100μmの厚さでロール表面に被成させ、さらに
酸化クロムのセラミックコーティング層の化学的緻密化
処理皮膜を前記溶射皮膜の上層に約10μmの厚さで形
成させた実機ロールを、連続溶融亜鉛めっきラインの実
機溶融亜鉛めっき浴に浸漬し、各々2週間×2回の連続
使用を行った。そして1回目および2回目の各ロールの
めっき浴より引上げ後の合金層付着状況、皮膜剥離状
況、皮膜摩耗状況を目視観察した。その結果を表7に示
す。なお、表7中の○は良好、×は不具合ありを示す。
Example 2 Sink roll 4 of the continuous hot-dip galvanizing line shown in FIG.
And the support rolls 5 and 6, high-speed gas flame spraying method and a plasma spraying method, 13% Al 2 O 3 containing Al 2 O 3 -TiO 2 solid solution A and 40% TiO 2 containing TiO 2 in -TiO 2 Two kinds of thermal spray coatings of solid solution B are coated on the roll surface with a thickness of 100 μm, and a chemical densification coating of a ceramic coating layer of chromium oxide is further formed on the thermal spray coating with a thickness of about 10 μm. The formed actual machine roll was immersed in the actual hot-dip galvanizing bath of the continuous hot-dip galvanizing line, and continuously used for 2 weeks × 2 times. Then, the state of adhesion of the alloy layer, the state of film peeling, and the state of film abrasion after pulling up from the plating bath of each roll for the first time and the second time were visually observed. The results are shown in Table 7. In Table 7, ◯ means good, and × means trouble.

【0033】[0033]

【表7】 [Table 7]

【0034】この発明の溶射皮膜を表面に形成したロー
ルは、各々延べ約1ケ月の長期に亘り実機亜鉛めっき浴
での浸漬および実使用テストを行ったにもかかわらず、
実使用時の合金層および異物付着等による押込み疵等、
めっき鋼板表面品質の不具合は一度も発生しなかった。
また、亜鉛めっき浴から引上げ後のロール表面には、表
7に示すとおり合金層付着、異物付着は一切認められな
かった。また、ロール表面の付着亜鉛を除去したのち、
皮膜観察を実施した結果、皮膜剥離や皮膜摩耗等の現象
は認められず、長期使用後においても健全な溶射皮膜を
保持していた。
The roll having the sprayed coating of the present invention formed on its surface was immersed in an actual galvanizing bath for a long period of about one month each and was subjected to an actual use test.
Indentation damage due to adhesion of alloy layer and foreign matter during actual use,
No defects in the surface quality of the plated steel sheet occurred.
Further, as shown in Table 7, no adhesion of the alloy layer or foreign matter was found on the surface of the roll after being pulled up from the galvanizing bath. Also, after removing the adhered zinc on the roll surface,
As a result of observing the film, no phenomenon such as film peeling and film abrasion was observed, and a sound thermal sprayed film was retained even after long-term use.

【0035】[0035]

【発明の効果】以上述べたとおり、この発明の溶射皮膜
を形成した溶融めっき金属浴浸漬部材は、溶融めっき金
属に対するぬれ性が大幅に改善され、浸漬部材表面への
合金層巻付きや異物付着が防止できるため、高品質のめ
っき鋼板の製造が可能となる。さらに、浸漬部材表面を
清浄な状態に保持でき、かつ皮膜剥離等の熱衝撃性に優
れるため、浸漬部材の長寿命化あるいは金属めっき浴よ
り引上げた後の部材整備性の向上および溶融めっきスケ
ジュールのチャンスフリー化を図ることができる。
As described above, the hot-dip galvanized metal bath-immersed member of the present invention, which has a significantly improved wettability with respect to the hot-dip galvanized metal, has an alloy layer winding and foreign matter adhered to the surface of the dipping member. Since it is possible to prevent this, it is possible to manufacture high-quality plated steel sheets. Furthermore, since the surface of the submerged member can be kept in a clean state and the thermal shock resistance such as film peeling is excellent, the life of the submerged member is extended or the maintainability of the member after being pulled up from the metal plating bath is improved and the hot dipping schedule is improved. Opportunity-free can be achieved.

【図面の簡単な説明】[Brief description of drawings]

【図1】連続溶融金属めっきラインの概要を示す模式図
である。
FIG. 1 is a schematic diagram showing an outline of a continuous hot-dip metal plating line.

【符号の説明】[Explanation of symbols]

1 鋼帯 2 スナウト 3 溶融金属槽 4 シンクロール 5、6 サポートロール 7 ワイピングノズル 8 トップロール 1 Steel strip 2 Snout 3 Molten metal tank 4 Sink roll 5, 6 Support roll 7 Wiping nozzle 8 Top roll

───────────────────────────────────────────────────── フロントページの続き (72)発明者 丸山 晃 和歌山県和歌山市湊1850番地 住友金属工 業株式会社 和歌山製鉄所内 (72)発明者 宮島 生欣 兵庫県神戸市東灘区深江北町4丁目13番4 号 トーカロ株式会社内 (72)発明者 谷 和美 兵庫県神戸市東灘区深江北町4丁目13番4 号 トーカロ株式会社内 ─────────────────────────────────────────────────── ─── Continuation of front page (72) Inventor Akira Maruyama 1850 Minato, Wakayama, Wakayama Sumitomo Metal Industries Co., Ltd. Wakayama Works (72) Inventor Ikino Miyajima 4-chome, Fukaekita-cho, Higashinada-ku, Kobe-shi, Hyogo 4 Tokaro Co., Ltd. (72) Inventor Kazumi Tani 4-13-4 Fukaekita-cho, Higashinada-ku, Kobe City, Hyogo Prefecture Tokaro Co., Ltd.

Claims (3)

【特許請求の範囲】[Claims] 【請求項1】 表面にAl2O3−TiO2擬2元系金属
酸化物を溶射被覆して保護層を形成したことを特徴とす
る溶融金属めっき浴浸漬部材。
1. A molten metal plating bath dipping member characterized in that a protective layer is formed by thermally spray-coating a surface of Al 2 O 3 —TiO 2 pseudo binary metal oxide.
【請求項2】 表面にAl2O3−TiO2擬2元系金属
酸化物を溶射被覆して保護層を形成し、該保護層表面層
に酸化クロムセラミックスコーティング層からなる化学
的緻密化処理皮膜を形成したことを特徴とする溶融金属
めっき浴浸漬部材。
2. A chemical densification treatment comprising a protective layer formed by spray-coating a surface of Al 2 O 3 —TiO 2 pseudo binary metal oxide to form a protective layer and a chromium oxide ceramic coating layer on the protective layer surface layer. A molten metal plating bath immersion member having a film formed thereon.
【請求項3】 Al2O3−TiO2擬2元系金属酸化物
が両者の固溶体複合物であって、TiO2を0.5〜5
0%含有し、不純物としてCr2O3、CaO、Si
O2、ZrO2、MgO、FeO、Fe2O3、Fe3O4の
うちの1種または2種以上を5%未満含有していること
を特徴とする請求項1および2記載の溶融金属めっき浴
浸漬部材。
3. An Al 2 O 3 —TiO 2 pseudo binary metal oxide is a solid solution composite of the two , and the TiO 2 content is 0.5 to 5.
0% content, Cr 2 O 3 , CaO, Si as impurities
The molten metal according to claim 1 or 2, which contains less than 5% of one or more of O 2 , ZrO 2 , MgO, FeO, Fe 2 O 3 , and Fe 3 O 4. Plating bath immersion member.
JP3262898A 1991-09-13 1991-09-13 Immersion member for molten metal plating bath Expired - Fee Related JPH0730435B2 (en)