JPH08248564A - Photographic substrate - Google Patents
Photographic substrateInfo
- Publication number
- JPH08248564A JPH08248564A JP4847695A JP4847695A JPH08248564A JP H08248564 A JPH08248564 A JP H08248564A JP 4847695 A JP4847695 A JP 4847695A JP 4847695 A JP4847695 A JP 4847695A JP H08248564 A JPH08248564 A JP H08248564A
- Authority
- JP
- Japan
- Prior art keywords
- film
- layer
- polyester
- acid
- weight
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【0001】[0001]
【産業上の利用分野】本発明はハロゲン化銀写真感光材
料の写真用支持体に関し、特に物理的性質の優れたポリ
エステルを主構成成分とするハロゲン化銀カラー写真感
光材料の小型化に有用な写真用支持体に関する。BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a photographic support for a silver halide photographic light-sensitive material, and is particularly useful for miniaturization of a silver halide color photographic light-sensitive material mainly composed of polyester having excellent physical properties. It relates to a photographic support.
【0002】[0002]
【従来の技術】近年、ハロゲン化銀写真感光材料(以下
写真フィルムと略すこともある)の用途は多様化してお
り、撮影時のフィルム巻き出しの高速化、撮影倍率の高
倍率化、撮影装置の小型化が著しく進んでいる。このた
め写真フィルム用の支持体には、優れた機械的強度、寸
法安定性等の優れた物理的性質が要求されている。更
に、ロールフィルム状の写真フィルムでは、そのロール
径の小径化が要求されている。2. Description of the Related Art In recent years, the use of silver halide photographic light-sensitive materials (hereinafter sometimes abbreviated as photographic film) has been diversified, and the speed of film unwinding at the time of shooting, the increase in shooting magnification, the shooting apparatus Has been significantly miniaturized. Therefore, the support for photographic film is required to have excellent physical properties such as excellent mechanical strength and dimensional stability. Further, in a roll film-shaped photographic film, it is required to reduce the roll diameter.
【0003】一般のカラーネガフィルムの様なロールフ
ィルム状の写真フィルムは、従来から写真用支持体とし
て、セルローストリアセテートフィルム(以下TACフ
ィルムと略す)が使われてきたが、ロール径を小径化す
る要求に対して、TACフィルムは機械的強度が小さい
ため、フィルムの厚さを薄くすることができず、また巻
癖がつき易く、小型化という新たなニーズにTACフィ
ルムでは応えられなかった。つまり、多数のフィルムを
現像処理前にプレスプライスして接続しリールに巻き付
ける工程で、巻芯の小型化により巻癖が強く付いてしま
うことにより、取り扱いにくく、搬送不良が起こるとい
う問題がある。For a roll film type photographic film such as a general color negative film, a cellulose triacetate film (hereinafter abbreviated as TAC film) has been conventionally used as a photographic support, but it is required to reduce the roll diameter. On the other hand, since the TAC film has a low mechanical strength, the thickness of the film cannot be made thin, and the TAC film is apt to have a winding tendency. Therefore, the TAC film cannot meet the new need for miniaturization. That is, in the process of press-placing and connecting a large number of films before the developing process and winding them around a reel, there is a problem in that the winding habit is strongly attached due to the downsizing of the winding core, which makes it difficult to handle and causes conveyance failure.
【0004】この課題に対して、機械的強度が強く、優
れた透明性、寸法安定性を有しているポリエチレンテレ
フタレート(以下PETと略す)フィルムを使用する試
みがなされている。PETフィルムは、確かに厚さを薄
くしてロール径の小径化には対応できるものの、ロール
フィルム状の写真フィルムにPETフィルムを写真用支
持体として用いる場合、PETフィルムにはTACフィ
ルムにみられるような現像処理後の巻癖回復性がなく、
大きな巻癖が残るため、その後の作業性に問題があるこ
とが分かった。例えば仕分け作業がやりにくかったり、
写真印画紙に画像を焼き付ける工程等で、擦り傷の発
生、焦点のぼけ、搬送時のジャミング等が生じてしまう
等の問題が多発した。To solve this problem, attempts have been made to use a polyethylene terephthalate (hereinafter abbreviated as PET) film having high mechanical strength, excellent transparency and dimensional stability. Although the PET film can certainly be made thinner so that the roll diameter can be reduced, when the PET film is used as a roll film-shaped photographic film as a photographic support, the PET film is found in the TAC film. There is no curl recovery after development like this,
It was found that there was a problem in workability after that, because a large curl remained. For example, sorting work is difficult,
In the process of printing an image on photographic printing paper, there have been many problems such as scratches, defocusing, and jamming during transportation.
【0005】[0005]
【発明が解決しようとする課題】そこで、膜厚を薄くし
ても、PETフィルムより機械的強度が強く、巻癖がよ
り付きにくい写真用支持体として使用出来るプラスチッ
クフィルムが求められていた。少しでもこれらの要求を
満足出来る可能性のあるプラスチックフィルムとしてポ
リエステルの中ではPETと同様な構造のポリエチレン
ナフタレートフィルム(以下PENと略すこともあ
る)、詳しくはポリエチレン-2,6-ナフタレートがあ
る。ポリエチレン-2,6-ナフタレートフィルムはPET
フィルムより機械的強度が大きく薄手化が出来、巻癖も
若干付きにくいことがわかったが、逆に感光層との接着
性がより劣ること、PENフィルム自体が蛍光性を持
ち、しかも若干のヘーズがあること等このままでは写真
用支持体として実用化することは出来なかった。Therefore, there has been a demand for a plastic film which has a higher mechanical strength than a PET film and is less prone to curling even when the film thickness is reduced, and which can be used as a photographic support. Among the polyesters, there is a polyethylene naphthalate film having the same structure as PET (hereinafter sometimes abbreviated as PEN), more specifically polyethylene-2,6-naphthalate, as a plastic film capable of satisfying these requirements even a little. . Polyethylene-2,6-naphthalate film is PET
It was found that the film has higher mechanical strength than the film and can be made thinner, and it is less likely to have a curl, but on the contrary, the adhesiveness to the photosensitive layer is poorer, and the PEN film itself has fluorescence and some haze. However, it could not be put to practical use as a photographic support.
【0006】ガラス転移温度が90〜200℃のポリエステ
ルフィルムと感光層との接着性を改良する方法が特開平
6-266050号明細書に記載されている。すなわち、この方
法はフィルム支持体温度を70〜230℃に加熱した状態で
紫外線照射処理をすることにより、これらのポリエステ
ルフィルム表面から15μmまでのポリエステル分子の固
有粘度を1〜5%低下させるべく分解し、その面にこれ
らのポリエステルに対する膨潤溶剤を含む下引液を塗設
することにより感光層との接着性を向上させるいうもの
である。しかしながら、この方法では加熱状態で紫外線
を照射し、膨潤溶剤で処理するという条件はフィルムに
とっては苛酷なものであり、フィルム表面を脆くし場合
によっては逆に接着性を劣化させたり、しかも着色が強
くなったり、ポリエステルの膨潤溶剤がフィルムに残留
し、不必要な臭みが半永久的に残ったり写真フィルムと
して好ましくない状態になってしまう。また下引作業的
にも、下引塗布設備的にも膨潤溶剤の毒性に対しても考
慮する必要性から作業の安全性確保のための高価な設備
が必要になったり、作業者に対しても毒物の取り扱いや
臭気等についての特別な配慮が必要になる。A method for improving the adhesion between a polyester film having a glass transition temperature of 90 to 200 ° C. and a photosensitive layer is disclosed in Japanese Patent Laid-Open No.
6-266050. That is, in this method, UV irradiation treatment is performed with the film support temperature being heated to 70 to 230 ° C. to decompose the intrinsic viscosity of polyester molecules up to 15 μm from the surface of these polyester films by 1 to 5%. Then, by coating an undercoat liquid containing a swelling solvent for these polyesters on the surface, the adhesiveness to the photosensitive layer is improved. However, in this method, the condition that the film is irradiated with ultraviolet rays in a heated state and treated with a swelling solvent is severe for the film, and the film surface is made brittle, which may adversely deteriorate the adhesiveness, or cause coloring. The swelling solvent of polyester becomes strong, and the swelling solvent of polyester remains in the film, and unnecessary odor remains semipermanently, which is not preferable as a photographic film. In addition, since it is necessary to consider the toxicity of the swelling solvent in terms of undercoating work, undercoating equipment, and expensive work equipment to ensure work safety, Also requires special consideration regarding the handling of toxic substances and odors.
【0007】本発明の第1の目的は、カメラの小型化に
対応出来る写真フィルムのための写真用支持体を提供す
ることにある。第2の目的は、機械的強度が優れている
ため薄手化が出来、感光層との接着性に優れ、取り扱い
が容易で、巻癖が付きにくく、透明性に優れ、かつ寸法
安定性に優れた写真用支持体を提供することにある。A first object of the present invention is to provide a photographic support for a photographic film which can cope with miniaturization of a camera. The second purpose is that it has excellent mechanical strength, can be thinned, has excellent adhesiveness with the photosensitive layer, is easy to handle, has less curl, has excellent transparency, and has excellent dimensional stability. To provide a photographic support.
【0008】[0008]
【課題を解決するための手段】本発明者らは、ジカルボ
ン酸成分がナフタレンジカルボン酸であるポリエステル
を主構成成分とするポリエステルフィルム表面に紫外線
を照射し、照射後の赤外線吸収強度が下記式(1)及び
式(2)で示される関係を満たした該ポリエステルフィ
ルム表面に官能性基を有する水性ポリマー化合物を下引
層として塗設することによって上記課題を達成した。The inventors of the present invention irradiate the surface of a polyester film whose main constituent is a polyester whose dicarboxylic acid component is naphthalene dicarboxylic acid with ultraviolet rays, and the infrared absorption intensity after irradiation is represented by the following formula ( The above object was achieved by coating an aqueous polymer compound having a functional group as an undercoat layer on the surface of the polyester film satisfying the relationships represented by 1) and the formula (2).
【0009】式(1) 0.90≦I1133/I1142≦1.05 式(2) 0.90≦I1330/I1340≦1.10 ここで、I1133は波数が1133cm-1に対する赤外線吸収強
度 I1142は波数が1142cm-1に対する赤外線吸収強度 I1330は波数が1330cm-1に対する赤外線吸収強度 I1340は波数が1340cm-1に対する赤外線吸収強度 を表す。[0009] Equation (1) 0.90 ≦ I1133 / I1142 ≦ 1.05 Equation (2) 0.90 ≦ I1330 / I1340 ≦ 1.10 where the infrared absorption intensity for infrared absorption intensity I1142 is wavenumber 1142cm -1 against wavenumber 1133cm -1 I1133 I1330 is wave number infrared absorption intensity I1340 is the wave number for the 1330 cm -1 representative of the infrared absorption strength for 1340 cm -1.
【0010】また、水性ポリマー化合物をビニルコポリ
マーラテックス又は水性コポリエステルにすることによ
って、接着性に優れた写真用支持体を得ることが出来
た。更にポリエステルフィルムを、ポリエチレン-2,6-
ナフタレートを主構成成分とするポリマーとすることに
よって、薄膜化が出来、寸法安定性に優れ、かつ巻癖の
付きにくい写真用支持体を得ることが出来た。Further, by using a vinyl copolymer latex or an aqueous copolyester as the aqueous polymer compound, a photographic support having excellent adhesiveness could be obtained. Polyester film, polyethylene-2,6-
By using naphthalate as a main component, a photographic support having a thin film, excellent dimensional stability, and less curl can be obtained.
【0011】以下、本発明を詳細に説明する。The present invention will be described in detail below.
【0012】本発明のポリエステルの主構成成分として
の酸成分としては、ナフタレンジカルボン酸であり、詳
しくは1,4-ナフタレンジカルボン酸、2,6-ナフタレンジ
カルボン酸、1,5-ナフタレンジカルボン酸、2,7-ナフタ
レンジカルボン酸等であり、中でも2,6-ナフタレンジカ
ルボン酸が合成のやり易さ、フィルムの物理的性質等か
ら好ましい。The acid component as the main constituent of the polyester of the present invention is naphthalenedicarboxylic acid, specifically 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 1,5-naphthalenedicarboxylic acid, Among them are 2,7-naphthalenedicarboxylic acid and the like, of which 2,6-naphthalenedicarboxylic acid is preferred from the viewpoint of easiness of synthesis and physical properties of the film.
【0013】主構成成分以外のポリエステルを構成する
ジカルボン酸成分として、テレフタル酸、イソフタル
酸、フタル酸、5-アルカリ金属スルホイソフタル酸、2,
6-ナフタレンジカルボン酸、2,7-ナフタレンジカルボン
酸、1,4-ナフタレンジカルボン酸、1,5-ナフタレンジカ
ルボン酸、ジフェニレンジカルボン酸、ジフェニレンス
ルホンジカルボン酸、ジフェニルエーテルジカルボン
酸、ジフェニルエタンジカルボン酸、シクロヘキサンジ
カルボン酸、ジフェニルジカルボン酸、ジフェニルチオ
エーテルジカルボン酸、ジフェニルケトンジカルボン
酸、フェニルインダンジカルボン酸等を挙げることが出
来る。As the dicarboxylic acid component constituting the polyester other than the main component, terephthalic acid, isophthalic acid, phthalic acid, 5-alkali metal sulfoisophthalic acid, 2,
6-naphthalene dicarboxylic acid, 2,7-naphthalene dicarboxylic acid, 1,4-naphthalene dicarboxylic acid, 1,5-naphthalene dicarboxylic acid, diphenylene dicarboxylic acid, diphenylene sulfone dicarboxylic acid, diphenyl ether dicarboxylic acid, diphenylethane dicarboxylic acid, Examples thereof include cyclohexanedicarboxylic acid, diphenyldicarboxylic acid, diphenylthioetherdicarboxylic acid, diphenylketone dicarboxylic acid, phenylindanedicarboxylic acid and the like.
【0014】主構成成分としてのグリコール成分として
は、エチレングリコール、1,4−シクロヘキサンジメ
タノール、2′,2′−ビス(4−ヒドロキシフェニ
ル)プロパン、1,4−シクロヘキサンジオール等を挙
げることが出来るが、エチレングリコールが好ましい。Examples of the glycol component as a main constituent include ethylene glycol, 1,4-cyclohexanedimethanol, 2 ', 2'-bis (4-hydroxyphenyl) propane, 1,4-cyclohexanediol and the like. Yes, but ethylene glycol is preferred.
【0015】主構成成分以外のポリエステルを構成する
グリコールとしては、エチレングリコール、プロピレン
グリコール、テトラメチレングリコール、1,4−シク
ロヘキサンジメタノール、2′,2′-ビス(4-ヒドロキシ
フェニル)プロパン、2′,2′-ビス(4-ヒドロキシエト
キシフェニル)プロパン、ビス(4-ヒドロキシフェニ
ル)スルホン、ビスフェノール、フルオレンジヒドロキ
シエチルエーテル、ジエチレングリコール、ネオペンチ
ルグリコール、ハイドロキノン、1,4−シクロヘキサ
ンジオール、ポリエチレングリコール等を挙げることが
できる。As the glycol constituting the polyester other than the main constituents, ethylene glycol, propylene glycol, tetramethylene glycol, 1,4-cyclohexanedimethanol, 2 ', 2'-bis (4-hydroxyphenyl) propane, 2 ′, 2′-Bis (4-hydroxyethoxyphenyl) propane, bis (4-hydroxyphenyl) sulfone, bisphenol, full orange hydroxyethyl ether, diethylene glycol, neopentyl glycol, hydroquinone, 1,4-cyclohexanediol, polyethylene glycol, etc. Can be mentioned.
【0016】本発明に用いることの出来るポリエステル
の好ましい具体例を下記に示すが、本発明がこれに限定
されるものではない。Preferred specific examples of the polyester that can be used in the present invention are shown below, but the present invention is not limited thereto.
【0017】ポリエチレン-2,6-ナフタレート〔2,6-ナ
フタレンジカルボン酸/エチレングリコール(100/10
0)〕 (略号PEN) コポリエステル: 〔2,6-ナフタレンジカルボン酸/エチレングリコール/
1,4-シクロヘキサンジメタノール(100/70/30)〕
(略号NGC) 〔2,6-ナフタレンジカルボン酸/エチレングリコール/
ビスフェノールA(100/60/40)〕 (略号NEB
A) 〔2,6-ナフタレンジカルボン酸/テレフタル酸/エチレ
ングリコール(70/30/100)〕 (略号NTE) 〔2,6-ナフタレンジカルボン酸/テレフタル酸/エチレ
ングリコール/1,4-シクロヘキサンジメタノール(60/
40/50/50)〕 (略号NTEC) 〔2,6-ナフタレンジカルボン酸/シクロヘキサンジカル
ボン酸/エチレングリコール/ネオペンチルグリコール
(70/30/70/30)〕 (略号NCDENP) 本発明のジカルボン酸成分がナフタレンジカルボン酸で
あるポリエステルを主構成成分とするという範囲内には
ナフタレンジカルボン酸を主構成成分とするポリエステ
ルを主の配合成分とする他のポリエステルとの混合物も
含まれる。例えば:(混合比は重量%) PEN/PET=60〜95/40〜5 PEN/コポリエステル〔テレフタル酸/シクロヘキサ
ンジメタノール(100/100)〕=60〜95/30〜5 PEN/コポリエステル〔テレフタル酸/ビスフェノー
ルA(100/100)〕=60〜95/40〜5 NGC/PET=70〜90/30〜10 NTEC/PET=70〜90/30〜10 等が挙げられる。Polyethylene-2,6-naphthalate [2,6-naphthalenedicarboxylic acid / ethylene glycol (100/10
0)] (abbreviation PEN) copolyester: [2,6-naphthalenedicarboxylic acid / ethylene glycol /
1,4-Cyclohexanedimethanol (100/70/30)]
(Abbreviation NGC) [2,6-naphthalenedicarboxylic acid / ethylene glycol /
Bisphenol A (100/60/40)] (Abbreviation NEB
A) [2,6-naphthalenedicarboxylic acid / terephthalic acid / ethylene glycol (70/30/100)] (abbreviation NTE) [2,6-naphthalenedicarboxylic acid / terephthalic acid / ethylene glycol / 1,4-cyclohexanedimethanol (60 /
40/50/50)] (abbreviation NTEC) [2,6-naphthalenedicarboxylic acid / cyclohexanedicarboxylic acid / ethylene glycol / neopentyl glycol (70/30/70/30)] (abbreviation NCDENP) Dicarboxylic acid component of the present invention Within the range in which the main component is a polyester which is naphthalene dicarboxylic acid, a mixture with another polyester whose main compounding component is a polyester containing naphthalene dicarboxylic acid as a main component is also included. For example: (mixing ratio is% by weight) PEN / PET = 60 to 95/40 to 5 PEN / copolyester [terephthalic acid / cyclohexanedimethanol (100/100)] = 60 to 95/30 to 5 PEN / copolyester [ Terephthalic acid / bisphenol A (100/100)] = 60 to 95/40 to 5 NGC / PET = 70 to 90/30 to 10 NTEC / PET = 70 to 90/30 to 10 and the like.
【0018】本発明におけるポリエステルの主構成成分
とは、全エステル結合中のナフタレンジカルボン酸の占
める割合が50モル%以上であり、高度の物理的性質を望
むには75モル%以上が好ましく、特に好ましくは90重量
%以上である。100%であるポリエチレンナフタレー
ト、その中でもポリエチレン-2,6-ナフタレートが本発
明には最も好ましいものの一つである。 一般にポリエステルフィルムの性質の中であまり望まし
くないものの一つとしてデラミネーションがある。デラ
ミネーションは配向結晶化によってフィルム自身が平面
方向に層状に剥離し易くなる現象で、写真用支持体上の
感光層と共に剥離し、接着性が見かけ上悪いと判断され
ることがあり、実用的にも好ましくない。また前記高温
下紫外線照射処理を行ってフィルム表面の分子を劣化さ
せる方法は脆さからフィルムがデラミネーションを起こ
し易く、その結果一つの原因として接着性が悪くなる。The main constituent component of the polyester in the present invention is that the proportion of naphthalenedicarboxylic acid in all the ester bonds is 50 mol% or more, and 75 mol% or more is preferable in order to obtain high physical properties. It is preferably 90% by weight or more. 100% polyethylene naphthalate, of which polyethylene-2,6-naphthalate is one of the most preferred for the present invention. Generally, one of the less desirable properties of polyester film is delamination. Delamination is a phenomenon in which the film itself easily peels into layers in the plane direction due to oriented crystallization, and it may be peeled together with the photosensitive layer on the photographic support, and it may be judged that the adhesiveness is apparently poor. Is also not preferable. In addition, the method of degrading the molecules on the film surface by performing ultraviolet irradiation treatment at a high temperature tends to cause delamination of the film due to its brittleness, resulting in poor adhesiveness as one of the causes.
【0019】この性質に対して、酸成分としてを金属塩
スルホネート基を有する芳香族ジカルボン酸やポリアル
キレングリコール等を共重合構成単位としてポリエステ
ルに含ませることによって本発明者らは改善出来ること
を見いだした。金属塩スルホネート基を有する芳香族ジ
カルボン酸としては、5-ナトリウムスルホイソフタル
酸、2-ナトリウムスルホイソフタル酸、4-ナトリウムス
ルホイソフタル酸、4-ナトリウムスルホ-2,6-ナフタレ
ンジカルボン酸、2-ナトリウムスルホテレフタル酸等が
好ましい。金属塩はナトリウム以外にリチウム、カリウ
ム、セシウム等であっても良いが、製造上重合させ易い
か、また安定なものとしては5-ナトリウムスルホイソフ
タル酸が好ましい。またグリコール成分としてポリエチ
レングリコール、ポリプロピレングリコール、ポリテト
ラメチレングリコール、ポリ(コ-エチレングリコール
−コ-プロピレングリコール)等が好ましい。中でも透
明性を低下させないためにはポリエチレングリコールが
特に好ましい。これらの成分は全ポリエステルの構成単
位として2〜8重量%含有すると好ましく、特に3〜6
重量%が好ましい。The present inventors have found that, with respect to this property, the present invention can be improved by incorporating an aromatic dicarboxylic acid having a metal salt sulfonate group, a polyalkylene glycol or the like as an acid component into a polyester as a copolymerization structural unit. It was As the aromatic dicarboxylic acid having a metal salt sulfonate group, 5-sodium sulfoisophthalic acid, 2-sodium sulfoisophthalic acid, 4-sodium sulfoisophthalic acid, 4-sodium sulfo-2,6-naphthalenedicarboxylic acid, 2-sodium Sulfoterephthalic acid and the like are preferable. The metal salt may be lithium, potassium, cesium or the like in addition to sodium, but 5-sodium sulfoisophthalic acid is preferable because it is easily polymerized in production and is stable. As the glycol component, polyethylene glycol, polypropylene glycol, polytetramethylene glycol, poly (co-ethylene glycol-co-propylene glycol) and the like are preferable. Among them, polyethylene glycol is particularly preferable because it does not reduce the transparency. It is preferable that these components are contained in an amount of 2 to 8% by weight as a constituent unit of all polyesters, and particularly 3 to 6% by weight.
Weight percent is preferred.
【0020】フィルムの耐熱性を向上する目的で2′,
2′-ビス(ヒドロキシフェニル)プロパン(通称ビスフ
ェノールAといわれている)、の如きアルキレンビスフ
ェノール化合物を加えるとよい。ポリエステルの全エス
テル結合に対してビスフェノールAを1〜10重量%含有
するのが好ましい。2 ', for the purpose of improving the heat resistance of the film,
It is advisable to add an alkylenebisphenol compound such as 2'-bis (hydroxyphenyl) propane (commonly called bisphenol A). It is preferable to contain 1 to 10% by weight of bisphenol A based on the total ester bonds of the polyester.
【0021】本発明の写真用支持体に有用なフィルムは
カルボン酸成分がナフタレンジカルボン酸を主構成成分
としてなっている一枚のポリエステルフィルムであって
も、また最外層に該ポリエステルを有する積層されたフ
ィルムであっても良い。The film useful for the photographic support of the present invention is a single polyester film whose carboxylic acid component is mainly naphthalene dicarboxylic acid, or is laminated with the polyester as the outermost layer. It may be a film.
【0022】本発明出願人の下では、かつて、巻癖の付
きにくいフィルムの探索がなされていた。その研究の中
で、金属スルホネート基を有する芳香族ジカルボン酸を
構成成分として有する変性ポリエステルフィルムには経
時収縮性があることに注目し、他のポリエステルフィル
ムと変性ポリエステルとを積層することによって、いろ
いろな巻癖傾向のフィルムを得ることが出来た。例え
ば、2層に積層した場合には、変性ポリエステル側にカ
ールし易いため、ポリエステル層側を内巻きにすること
によって巻癖の付きにくいフィルムになったが、時間が
経時するに従い変性ポリエステル層側にカールが戻って
しまうので巻癖の改善は出来なかった。3層積層の場合
には、変性ポリエステルを内層にするか、外層にするか
によって、巻癖の性質は異なり、前者の積層構造の方が
好結果が得られることが本発明出願人の下で既に発見し
ていた。Under the applicant of the present invention, there has been a search for a film which is hard to have a curl. In that research, it was noted that a modified polyester film having an aromatic dicarboxylic acid having a metal sulfonate group as a constituent has shrinkage property over time, and various polyester films were laminated with a modified polyester to obtain various I was able to obtain a film with a tendency to curl. For example, when two layers are laminated, curling tends to occur on the modified polyester side. Therefore, by winding the polyester layer inward, a film with less curl is formed, but with time, the modified polyester layer side I couldn't improve the curling habit because the curls would return. In the case of a three-layer lamination, the nature of the curl is different depending on whether the modified polyester is the inner layer or the outer layer, and the former laminated structure gives better results. Had already discovered.
【0023】そこで本発明者らは、3層以上の構成の最
外層にカルボン酸成分としてナフタレンジカルボン酸を
主構成成分とするポリエステルを用いることによって更
に巻癖の付きにくいフィルムを得ることを見いだし、本
発明の紫外線照射後、官能性基を有する水性ポリマー化
合物を主とした下引層を有する写真用支持体に3層以上
の積層フィルムを適用した。Therefore, the present inventors have found that by using a polyester having naphthalene dicarboxylic acid as a main constituent as a carboxylic acid component in the outermost layer having three or more layers, a film with less curl can be obtained. After the ultraviolet irradiation of the present invention, a laminated film having three or more layers was applied to a photographic support having an undercoat layer mainly containing an aqueous polymer compound having a functional group.
【0024】ここで本発明に用いられる積層ポリエステ
ルフィルムの構成について述べる。上述の如く、本発明
に用いられる積層フィルムの内層には変性ポリエステル
層、最外層にはカルボン酸成分としてナフタレンジカル
ボン酸を主構成成分とするポリエステル層が配置された
3層以上の積層フィルムであり、積層フィルムのその厚
さを二等分した場合、その分割した両側の層構成が非対
称的であることが特徴である。積層フィルムの厚み方向
を二等分する位置を中心として、その両側の積層構造が
互いに非対称になっているものであるということは、樹
脂の構成成分、樹脂の性質、層構成、製膜条件等をそれ
ぞれ変化させ、かつ適宜選択し組み合わせることによっ
て設計される。ここでいう非対称とは物理的、機械的あ
るいは化学的に相違することを意味し、異なった素材か
らなる層(全く異質の層)、層の構成順序、厚さ、構成
成分(共重合の構成単位の種類)、構成成分量(共重合
の構成単位の量比)、固有粘度等物性が異なっているこ
と等である。Here, the constitution of the laminated polyester film used in the present invention will be described. As described above, the laminated film used in the present invention is a laminated film of three or more layers in which a modified polyester layer is arranged in the inner layer and a polyester layer containing naphthalene dicarboxylic acid as a main constituent as a carboxylic acid component is arranged in the outermost layer. When the thickness of the laminated film is divided into two parts, it is characterized in that the divided layer structure on both sides is asymmetric. The fact that the laminated structure on both sides of the laminated film is asymmetric with respect to the position where the laminated film is divided into two equal parts in the thickness direction means that the constituent components of the resin, the properties of the resin, the layer constitution, film forming conditions, etc. Are changed, and are appropriately selected and combined. Asymmetrical here means that they are physically, mechanically, or chemically different, and are composed of layers of different materials (layers of completely different nature), the order in which the layers are formed, the thickness, and the constituents (copolymerization composition). The types of units), the amounts of constituent components (amount ratio of constituent units of copolymerization), and the physical properties such as intrinsic viscosity are different.
【0025】これらの積層フィルムの非対称性を測定す
る方法としては、各種分析機器を用いて行うことがで
き、とくに限定されないが、層構成についてはフィルム
の断面を顕微鏡観察、顕微鏡写真を撮影することにより
確認ができる。また、該フィルムを顕微鏡観察を行いな
がら、各層を削り取るか、フィルムを半分に分割する面
まで、それぞれ上下から削り取り上下の層それぞれの分
析対象物を得て、加水分解を行い液体クロマトグラフィ
ー、NMR等の各種測定装置で測定してもよいし、分析対
象物を溶媒に溶解後にNMR、GPC(ゲルパーミエーション
クロマトグラフィー)、固有粘度等の測定を行ってもよ
いし、分析対象物をそのまま粉末でX線分光機器、もし
くはKBr等に混ぜてIR(赤外分光機器)等の測定をする
ことができ、結果として絶対量、もしくはそれに相当す
る測定結果のピークの位置、強度の違い等でも非対称性
を測定することができる。A method for measuring the asymmetry of these laminated films can be carried out by using various analytical instruments and is not particularly limited, but regarding the layer constitution, the cross section of the film is observed under a microscope and a micrograph is taken. Can be confirmed by. Also, while observing the film under a microscope, scrape each layer, or scrape the film up to half to obtain the analytes of each of the upper and lower layers, and perform hydrolysis to perform liquid chromatography, NMR. It may be measured with various measuring devices such as, etc., or the analyte may be dissolved in a solvent and then NMR, GPC (gel permeation chromatography), intrinsic viscosity, etc. may be measured, or the analyte may be directly powdered. It is possible to measure IR (infrared spectroscopic instrument) etc. by mixing with X-ray spectroscopic instrument or KBr, etc., and as a result, it is asymmetrical in terms of absolute amount or peak position of the measurement result corresponding to it, intensity difference, etc. Sex can be measured.
【0026】次に、本発明に係わるポリエステル樹脂の
合成について述べる。Next, the synthesis of the polyester resin according to the present invention will be described.
【0027】本発明のカルボン酸成分がナフタレンジカ
ルボンを主構成成分としてなるポリエステルの合成は、
従来公知のポリエステルの製造法に従って行うことがで
きる。例えば、エステル化反応では酸成分をグリコール
成分との直接エステル化、酸成分をジメチルエステルと
してグリコールとエステル交換法、あるいは酸成分をあ
らかじめエチレングリコールのジハーフエステルとして
脱エチレングリコール化法よるエステル化のいずれも使
用できる。このエステル交換時に用いる触媒としては、
マンガン、カルシウム、亜鉛、コバルト等の金属の酢酸
塩、脂肪酸塩、炭酸塩等を挙げることができる。これら
の中でも、酢酸マンガン、酢酸カルシウムの水和物が好
ましく、さらにはこれらを混合したものが好ましい。前
記エステル交換時及び/又は重合時に反応を阻害したり
樹脂を着色したりしない範囲で水酸化物や脂肪族カルボ
ン酸の金属塩、第四級アンモニウム塩等を添加すること
も有効であり、中でも水酸化ナトリウム、酢酸ナトリウ
ム、テトラエチルアンモニウムハイドレート等が好まし
く、特に酢酸ナトリウム及びテトラエチルアンモニウム
ハイドレートが好ましい。The synthesis of the polyester in which the carboxylic acid component of the present invention is mainly composed of naphthalene dicarboxylic acid,
It can be performed according to a conventionally known method for producing polyester. For example, in the esterification reaction, a direct esterification of an acid component with a glycol component, a transesterification method with a glycol as an acid component as a dimethyl ester, or an esterification by a deethylene glycolization method as a dihalf ester of ethylene glycol as an acid component in advance Either can be used. As the catalyst used in this transesterification,
Examples thereof include acetates, fatty acid salts and carbonates of metals such as manganese, calcium, zinc and cobalt. Among these, hydrates of manganese acetate and calcium acetate are preferable, and a mixture of these is preferable. It is also effective to add a metal salt of a hydroxide or an aliphatic carboxylic acid, a quaternary ammonium salt, or the like within a range that does not inhibit the reaction or color the resin during the transesterification and / or the polymerization, and among others, Sodium hydroxide, sodium acetate, tetraethylammonium hydrate and the like are preferable, and sodium acetate and tetraethylammonium hydrate are particularly preferable.
【0028】ポリエステルを得るには、酸成分とグリコ
ール成分とを直接溶融重合法、エステル交換した後に溶
融重合を行う方法、または溶融重合で得られた樹脂を更
に分子量を高めるために固相重合する方法等公知の重合
合成方法を採用することができる。To obtain the polyester, the acid component and the glycol component are directly melt-polymerized, a method of carrying out melt-polymerization after transesterification, or a resin obtained by the melt-polymerization is solid-phase polymerized to further increase the molecular weight. A known polymerization synthesis method such as a method can be adopted.
【0029】ポリエステルの重合に用いる触媒としては
三酸化アンチモン、酸化亜鉛、二酸化マンガン、二酸化
チタン等が挙げられるが、中でも三酸化アンチモンが好
ましい。Examples of the catalyst used for the polymerization of polyester include antimony trioxide, zinc oxide, manganese dioxide, titanium dioxide, etc. Among them, antimony trioxide is preferable.
【0030】ポリエステルは共に重合段階でリン酸、亜
リン酸およびそれらのエステルならびに無機粒子(シリ
カ、カオリン、炭酸カルシウム、リン酸カルシウム、二
酸化チタン等)が含まれていてもよいし、重合後ポリマ
ーに無機粒子等がブレンドされていてもよい。さらに重
合段階、重合後のいずれかの段階で適宜に顔料、紫外線
吸収剤、酸化防止剤、マット剤、滑り剤、安定剤、界面
活性剤、分散剤、粘着防止剤、軟化剤、流動性付与剤等
を添加してもかまわない。Both of the polyesters may contain phosphoric acid, phosphorous acid and their esters and inorganic particles (silica, kaolin, calcium carbonate, calcium phosphate, titanium dioxide, etc.) at the polymerization stage, or the polymer after polymerization may be inorganic. Particles and the like may be blended. Further, at any stage after the polymerization and after the polymerization, pigments, ultraviolet absorbers, antioxidants, matting agents, slip agents, stabilizers, surfactants, dispersants, anti-tacking agents, softening agents, and imparting fluidity. You may add agent etc.
【0031】以上述べたポリエステル構成成分及び合成
法については、例えば高分子実験学第5巻「重縮合と重
付加」(共立出版、1980年)第103〜136頁、あるいは
「合成高分子V」(朝倉書店、1971年)第187〜286頁の
記載を参考に行うことができる。Regarding the polyester constituent components and the synthetic method described above, for example, Polymer Experimental Science Vol. 5, "Polycondensation and Polyaddition" (Kyoritsu Shuppan, 1980), pages 103 to 136, or "Synthetic Polymer V" (Asakura Shoten, 1971) It can be performed with reference to the description on pages 187 to 286.
【0032】次に、本発明のポリエステルフィルムの製
造方法について説明する。未延伸シートを得る方法およ
び縦方向に一軸延伸する方法は、従来公知の方法で行う
ことができる。例えば、原料のポリエステルをペレット
状に成型し、熱風乾燥または真空乾燥した後、溶融押出
し、Tダイよりシート状に押出して、静電印加法等によ
り冷却ドラムに密着させ、冷却固化させ、未延伸シート
を得る。次いで、得られた未延伸シートを複数のロール
群及び/又は赤外線ヒーター等の加熱装置を介してポリ
エステルのガラス転移温度(Tg)からTg+100℃の範
囲内に加熱し、一段または多段縦延伸する方法である。
延伸倍率は、通常2.5倍〜6倍の範囲で、続く横延伸が
可能な範囲とする必要がある。シートが多層構成の場合
の延伸温度の設定は各構成層のポリエステルのTgの中
で最も高いTgを基準にすることが好ましい。Next, the method for producing the polyester film of the present invention will be described. The method for obtaining an unstretched sheet and the method for uniaxially stretching in the machine direction can be performed by conventionally known methods. For example, the raw material polyester is molded into pellets, dried with hot air or vacuum dried, melt-extruded, extruded into a sheet from a T-die, adhered to a cooling drum by an electrostatic application method, cooled and solidified, and unstretched. Get the sheet. Then, the obtained unstretched sheet is heated within a range of Tg + 100 ° C. from the glass transition temperature (Tg) of polyester through a plurality of roll groups and / or a heating device such as an infrared heater, and a single-stage or multi-stage longitudinal stretching is performed. Is.
The draw ratio is usually in the range of 2.5 to 6 times, and it is necessary to set it in a range in which subsequent transverse stretching is possible. When the sheet has a multi-layered structure, the stretching temperature is preferably set based on the highest Tg of the polyesters of the respective constituent layers.
【0033】次に、上記の様にして得られた縦方向に一
軸延伸されたポリエステルフィルムを、Tg〜Tm−20℃
(Tm:融点)の温度範囲内で、横延伸し、次いで熱固
定する。横延伸倍率は通常3〜6倍であり、また、縦、
横延伸倍率の比は、得られた二軸延伸フィルムの物性を
測定し、好ましい特性を有するように適宜調整する。こ
の時、2つ以上に分割された延伸領域で温度差を1〜50
℃の範囲で順次昇温しながら横延伸すると巾方向の物性
の分布が低減でき好ましい。さらに横延伸後、フィルム
を、その最終横延伸温度以下でTg−40℃以上の範囲に
0.01〜5分間保持すると巾方向の物性の分布がさらに低
減でき好ましい。Next, the polyester film uniaxially stretched in the machine direction obtained as described above is subjected to Tg-Tm-20 ° C.
Within the temperature range of (Tm: melting point), transverse stretching is performed, and then heat setting is performed. The transverse stretching ratio is usually 3 to 6 times, and the longitudinal and
The ratio of the transverse stretching ratio is appropriately adjusted so that the obtained biaxially stretched film has its physical properties measured and has desirable characteristics. At this time, the temperature difference is 1 to 50 in the stretching region divided into two or more.
Lateral stretching while sequentially raising the temperature in the range of 0 ° C. is preferable because the distribution of physical properties in the width direction can be reduced. After the transverse stretching, the film is kept in the range of Tg-40 ° C or higher at the final transverse stretching temperature or lower.
Holding for 0.01 to 5 minutes is preferable because the distribution of physical properties in the width direction can be further reduced.
【0034】熱固定は、その最終横延伸温度より高温
で、Tm−20℃以下の温度範囲内で通常0.5〜300秒間熱
固定する。この際、2つ以上に分割された領域で温度差
を1〜100℃の範囲で順次昇温しながら熱固定すること
が好ましい。The heat setting is carried out at a temperature higher than the final transverse stretching temperature and usually within a temperature range of Tm-20 ° C. or lower for 0.5 to 300 seconds. At this time, it is preferable to heat-set while sequentially increasing the temperature difference in the range of 1 to 100 ° C. in the region divided into two or more.
【0035】熱固定されたフィルムは通常Tg以下まで
冷却され、フィルム両端のクリップ把持部分をカットし
ロール状に巻き取られる。この際、最終熱固定温度以
下、Tg以上の温度範囲内で、巾方向及び/または長手
方向に0.1〜10%弛緩処理することが好ましい。また、
冷却は、最終熱固定温度からTgまでを、毎秒100℃以下
の冷却速度で徐冷することが好ましい。冷却、弛緩処理
する手段は特に限定はなく、従来公知の手段で行える
が、特に複数の温度領域で順次冷却しながら、これらの
処理を行うことが、フィルムの寸法安定性向上の点で好
ましい。なお、冷却速度は、最終熱固定温度をT1、フ
ィルムが最終熱固定温度からTgに達するまでの時間を
tとしたとき、(T1−Tg)/tで求めた値である。
これら熱固定条件、冷却、弛緩処理条件のより最適な条
件は、フィルムを構成するポリエステルにより異なるの
で、得られた二軸延伸フィルムの物性を測定し、好まし
い特性を有するように適宜調整することにより決定すれ
ばよい。The heat-fixed film is usually cooled to Tg or less, cut at the clip holding portions at both ends of the film, and wound into a roll. At this time, it is preferable to perform a relaxation treatment in the width direction and / or the longitudinal direction by 0.1 to 10% within a temperature range of not higher than the final heat setting temperature and not lower than Tg. Also,
For cooling, it is preferable to gradually cool from the final heat setting temperature to Tg at a cooling rate of 100 ° C. or less per second. The means for cooling and relaxing treatment is not particularly limited and can be carried out by conventionally known means, but it is particularly preferable to perform these treatments while sequentially cooling in a plurality of temperature regions from the viewpoint of improving the dimensional stability of the film. The cooling rate is a value obtained by (T 1 −Tg) / t, where T 1 is the final heat setting temperature and t is the time required for the film to reach Tg from the final heat setting temperature.
More optimal conditions of these heat setting conditions, cooling, and relaxation treatment conditions differ depending on the polyester constituting the film, so by measuring the physical properties of the obtained biaxially stretched film and adjusting appropriately so as to have preferable properties. Just decide.
【0036】該ポリエステル樹脂の固有粘度は0.50〜0.
85が好ましく、0.55〜0.70の範囲が製膜し易さ、出来上
がったフィルムの機械的物性からいって特に好ましい。The intrinsic viscosity of the polyester resin is 0.50-0.
85 is preferable, and a range of 0.55 to 0.70 is particularly preferable in terms of easiness of film formation and mechanical properties of the finished film.
【0037】ここで固有粘度の測定法について触れる。
フィルムあるいはペレットを、フェノールと1,1,2,2-テ
トラクロロエタンの混合溶媒(重量比60/40)に溶か
し、濃度0.2g/dl、0.6g/dl、1.0g/dlの溶液を作製
し、ウベローデ型粘度計により、20℃で、それぞれの濃
度(C)における比粘度(ηsp)を求める。次いで、η
sp/CをCに対してプロットし、得られた直線を濃度ゼ
ロに補外して 固有粘度[η]=lim(ηsp/C) C→0 を求める。単位は、dl/gで示される。A method of measuring the intrinsic viscosity will be touched on here.
A film or pellet is dissolved in a mixed solvent of phenol and 1,1,2,2-tetrachloroethane (weight ratio 60/40) to prepare solutions with concentrations of 0.2g / dl, 0.6g / dl, 1.0g / dl. Using an Ubbelohde viscometer, the specific viscosity (ηsp) at each concentration (C) is determined at 20 ° C. Then η
Plot sp / C against C and extrapolate the obtained straight line to zero concentration to obtain the intrinsic viscosity [η] = lim (ηsp / C) C → 0. The unit is indicated by dl / g.
【0038】次に積層フィルムに用いられる変性ポリエ
ステルの合成について述べる。Next, the synthesis of the modified polyester used for the laminated film will be described.
【0039】変性ポリエステルの主構成成分としての酸
成分はテレフタル酸及びナフタレンジカルボン酸であ
り、またグリコール成分としてはエチレングリコールで
ある。ナフタレンジカルボン酸としてはナフタレン-2,6
-ジカルボン酸が好ましい。ここで変性ポリエステルの
主構成成分の全変性ポリエステルに占める割合は50モル
%以上が好ましく、好ましくは70モル%以上である。The acid component as the main constituent component of the modified polyester is terephthalic acid and naphthalene dicarboxylic acid, and the glycol component is ethylene glycol. Naphthalene-2,6 as naphthalene dicarboxylic acid
-Dicarboxylic acids are preferred. The proportion of the main constituent component of the modified polyester in the total modified polyester is preferably 50 mol% or more, and more preferably 70 mol% or more.
【0040】残りの変性部分は、テレフタル酸、ナフタ
レンジカルボン酸、金属スルホネート基を含有する芳香
族ジカルボン酸、イソフタル酸等の芳香族ジカルボン
酸、あるいはこれら芳香族ジカルボン酸とC1〜C4のア
ルコールとのジエステルあるいはC2〜C10のグリコー
ルとのジハーフエステル;アジピン酸、セバチン酸等の
脂肪族ジカルボン酸あるいはこれら脂肪族ジカルボン酸
とC1〜C4のアルコールとのジエステルあるいはC2〜
C10のグリコールとのジハーフエステル;ポリエチレン
オキシドジカルボン酸、ポリプロピレンオキシドジカル
ボン酸等のポリエーテルジカルボン酸あるいはC1〜C8
のアルコールとのジエステルあるいはC2〜C10のグリ
コールとのジハーフエステル等の酸成分と、エチレング
リコール、プロピレングリコール、ブタンジオール、ネ
オペンチルグリコール、p−キシリデングリコール、1,
4-シクロヘキサンジメタノール等のグリコール類;ジエ
チレングリコール、トリエチレングリコール、ポリエチ
レングリコール、ポリプロピレングリコール、ポリエチ
レンオキシド−ポリプロピレンオキシド共重合グリコー
ル等のポリオレフィンオキシドグリコール類等のグリコ
ール成分とのエステルあるいはポリエステル成分からな
っている。The remaining modified portion is terephthalic acid, naphthalenedicarboxylic acid, aromatic dicarboxylic acid containing a metal sulfonate group, aromatic dicarboxylic acid such as isophthalic acid, or these aromatic dicarboxylic acid and C 1 -C 4 alcohol. Or a dihalf ester with a C 2 to C 10 glycol; an aliphatic dicarboxylic acid such as adipic acid or sebacic acid, or a diester of these aliphatic dicarboxylic acids with a C 1 to C 4 alcohol or C 2
C 10 -glycol dihalf ester; polyether dicarboxylic acid such as polyethylene oxide dicarboxylic acid, polypropylene oxide dicarboxylic acid or C 1 -C 8
Acid component such as diester with alcohol or dihalf ester with C 2 to C 10 glycol, ethylene glycol, propylene glycol, butanediol, neopentyl glycol, p-xylidene glycol, 1,
Glycols such as 4-cyclohexanedimethanol; composed of ester or polyester components with glycol components such as diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, polyolefin oxide glycols such as polyethylene oxide-polypropylene oxide copolymer glycol .
【0041】変性ポリエステルの変性成分としての金属
スルホネート基を含有する芳香族ジカルボン酸類は、本
発明に使用される積層フィルムの内層の変性ポリエステ
ルの構成成分として重要である。つまり積層内層の経時
収縮性を付与するための一つの重要な要素である。金属
スルホネート基を含む芳香族ジカルボン酸としては、金
属スルホネート基を含むイソフタル酸が好ましく、また
金属イオンはナトリウム、カリウム、リチウム、セシウ
ム等のいずれかのアルカリ金属で、その中でもナトリウ
ムが好ましく、具体的には5-ナトリウムスルホイソフタ
ル酸、2-ナトリウムスルホイソフタル酸、4-ナトリウム
スルホイソフタル酸、4-ナトリウムスルホ−2,6-ナフタ
レンジカルボン酸あるいはこれらのジメチルエステル、
エチレングリコールジハーフエステルが好ましく、更に
好ましくは5-ナトリウムスルホイソフタル酸あるいはそ
のジメチルエステルまたはエチレングリコールジハーフ
エステルである。またその他下記化1で示されるグリコ
ールジハーフエステル等も挙げられる。金属スルホネー
ト基を有する芳香族ジカルボン酸の変性ポリエステルの
全エステル結合に対する割合は2〜10モル%の範囲がよ
く、好ましくは2〜7モル%で、特に好ましくは3〜6
モル%である。Aromatic dicarboxylic acids containing a metal sulfonate group as a modifying component of the modified polyester are important as a constituent component of the modified polyester of the inner layer of the laminated film used in the present invention. That is, it is one of the important factors for imparting the time-lapse shrinkability of the inner layer of the laminate. As the aromatic dicarboxylic acid containing a metal sulfonate group, isophthalic acid containing a metal sulfonate group is preferable, and the metal ion is any alkali metal such as sodium, potassium, lithium or cesium, and among them, sodium is preferable, and 5-sodium sulfoisophthalic acid, 2-sodium sulfoisophthalic acid, 4-sodium sulfoisophthalic acid, 4-sodium sulfo-2,6-naphthalenedicarboxylic acid or their dimethyl esters,
Ethylene glycol dihalf ester is preferable, and 5-sodium sulfoisophthalic acid or its dimethyl ester or ethylene glycol dihalf ester is more preferable. In addition, glycol dihalf ester represented by the following chemical formula 1 and the like are also included. The ratio of the aromatic dicarboxylic acid having a metal sulfonate group to the total ester bond of the modified polyester is preferably in the range of 2 to 10 mol%, preferably 2 to 7 mol%, particularly preferably 3 to 6 mol%.
Mol%.
【0042】[0042]
【化1】 Embedded image
【0043】変性ポリエステルの有用な変性成分として
のポリアルキレングリコール類が挙げられる。ポリアル
キレングリコールとしては、ポリエチレングリコールが
好ましく、変性ポリエステルの重要な変性成分である。
その数平均分子量は特に限定されないが、好ましくは30
0〜100,000でより好ましくは600〜10,000、特に好まし
くは1,000〜5,000である。ポリアルキレングリコールの
変性ポリエステルのポリエステル全重量に対して3〜10
重量%がよく、好ましく含有量は4〜8重量%である。Polyalkylene glycols are mentioned as useful modifying components of the modified polyester. Polyethylene glycol is preferable as the polyalkylene glycol, and is an important modifying component of the modified polyester.
The number average molecular weight is not particularly limited, but preferably 30
It is 0 to 100,000, more preferably 600 to 10,000, and particularly preferably 1,000 to 5,000. 3-10 based on the total weight of polyester of modified polyester of polyalkylene glycol
The weight% is good, and the content is preferably 4 to 8% by weight.
【0044】変性ポリエステルの変性成分としての脂肪
族ジカルボン酸としては、アジピン酸、ピメリン酸、ス
ベリン酸、アゼライン酸、セバチン酸等が挙げられる
が、アジピン酸、スベリン酸、アゼライン酸が好まし
く、特にアジピン酸が好ましく用いられる。脂肪族ジカ
ルボン酸のポリエステル全重量に対して3〜10重量%が
よく、好ましくは4〜8重量%であるが、ポリアルキレ
ングリコールとこの脂肪族ジカルボン酸とを共に用いる
場合には、合わせて3〜10重量%が好ましく、特に4〜
8重量%が好ましい。Examples of the aliphatic dicarboxylic acid as the modifying component of the modified polyester include adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, and the like. Adipic acid, suberic acid, azelaic acid are preferred, and adipic acid is particularly preferred. Acids are preferably used. It is preferably 3 to 10% by weight, and preferably 4 to 8% by weight, based on the total weight of the polyester of the aliphatic dicarboxylic acid, but when the polyalkylene glycol and this aliphatic dicarboxylic acid are used together, the total amount is 3 ~ 10 wt% is preferred, especially 4 ~
8% by weight is preferred.
【0045】その他、変性ポリエステルのポリエーテル
ジカルボン酸としては、ポリエチレンオキシジカルボン
酸、ポリプロピレンオキシジカルボン酸、ポリ(エチレ
ン/プロピレン)オキシジカルボン酸、ポリテトラメチ
レンオキシジカルボン酸及びその共重合体等が好ましい
が、ポリエステルの重合反応性やフィルムの平面安定性
の点で特に、下記式で示されるポリエチレンオキシジカ
ルボン酸エステルを用いるのがより好ましい。In addition, as the polyether dicarboxylic acid of the modified polyester, polyethyleneoxydicarboxylic acid, polypropyleneoxydicarboxylic acid, poly (ethylene / propylene) oxydicarboxylic acid, polytetramethyleneoxydicarboxylic acid and copolymers thereof are preferable. From the viewpoints of polymerization reactivity of polyester and plane stability of the film, it is more preferable to use polyethyleneoxydicarboxylic acid ester represented by the following formula.
【0046】 R1OOCCH2-(OCH2CH2)n-OCH2COOR2 ここで、R1,R2は水素または炭素数1〜8のアルキル
基、nは正の整数である。また、ポリエーテルジカルボ
ン酸成分の変性割合としては、全ポリエステル重量の2
〜30重量%、好ましくは5〜15重量%、特に好ましくは
7〜12重量%である。R 1 OOCCH 2 — (OCH 2 CH 2 ) n —OCH 2 COOR 2 Here, R 1 and R 2 are hydrogen or an alkyl group having 1 to 8 carbon atoms, and n is a positive integer. The modification ratio of the polyether dicarboxylic acid component is 2% of the total polyester weight.
-30% by weight, preferably 5-15% by weight, particularly preferably 7-12% by weight.
【0047】変性ポリエステル樹脂の合成は、前記の従
来公知のポリエステルの製造法に従って行うことができ
る。変性ポリエステル樹脂の具体的な合成方法は米国特
許第4,217,441号、特開平5-210199号に記載されてお
り、これらの方法によって本発明に有用な変性ポリエス
テル樹脂は合成され得る。The modified polyester resin can be synthesized according to the above-mentioned conventionally known polyester production method. Specific methods for synthesizing the modified polyester resin are described in US Pat. No. 4,217,441 and JP-A-5-210199, and the modified polyester resin useful in the present invention can be synthesized by these methods.
【0048】本発明に有用な変性ポリエステル樹脂の固
有粘度は0.35〜0.85が好ましく、特に0.40〜0.70が好ま
しい。The modified polyester resin useful in the present invention preferably has an intrinsic viscosity of 0.35 to 0.85, particularly 0.40 to 0.70.
【0049】変性ポリエステル樹脂の変性割合は、使用
出来る範囲で、更に他の成分と共重合されていても良い
し、他の樹脂がブレンドされていてもかまわない。ブレ
ンドされる樹脂としては、ポリエステル系の樹脂が好ま
しい。The modification ratio of the modified polyester resin may be such that it can be copolymerized with other components or blended with other resins, as long as it can be used. The resin to be blended is preferably a polyester resin.
【0050】次に、積層フィルムの製膜法について述べ
る。Next, a method for forming a laminated film will be described.
【0051】本発明に有用な積層フィルムは本質的には
積層する工程を除いた他の製膜工程は、前記1枚のフィ
ルムのそれと変わりはない。例えば、最外層1種と内層
1種の2種の樹脂を用いた3層構成の積層フィルムは次
ぎのように作られる。まず、二つ乃至三つの別々の真空
乾燥機でそれぞれの樹脂を前記ポリエステルと同様に減
圧乾燥し、三つの別々の押出機にそれぞれの樹脂を投入
し、溶融押出した後、一つの導管にそれぞれの溶融樹脂
が上下になるように導き、導管内で3層の溶融樹脂が層
流をなして一つのスリットを持つ押出口金から冷却ドラ
ム上に押し出されて一つの未延伸シートを形成させる
か、またダイスの三つの導入口にそれぞれの押出機で溶
融されたポリマーを導入し、ダイの三つのスリットか
ら、あるいはダイ内で三つのポリマーが一つのスリット
に結合されるようになっている押出口金から、層流状に
なった熔融ポリマーの3層を冷却ドラム上に押出して、
一つのシートを形成させて冷却ドラム上で冷却固化し
て、3層積層の未延伸フィルムを得た後、縦延伸、横延
伸、熱固定等常法の二軸延伸フィルムを得る前記ポリエ
ステルの製膜工程を通して積層フィルムを作る方法で本
発明に有用な方法である。また別の方法は3種の溶融ポ
リマーを別々のスリットから段々にシートを冷却ドラム
上に押出し冷却固化させる別位置製膜法もあり、これも
本発明に有用である。これらを共押出法とも呼ぶ。The laminated film useful in the present invention is essentially the same as that of the above-mentioned one film except for the step of laminating. For example, a three-layer laminated film using two kinds of resins, one outermost layer and one inner layer, is produced as follows. First, each resin is dried under reduced pressure in the same manner as the polyester with two or three separate vacuum dryers, each resin is charged into three separate extruders, melt-extruded, and then each into one conduit. The molten resin of the above is guided up and down, and three layers of molten resin form a laminar flow in the conduit and are extruded from the extrusion die having one slit onto the cooling drum to form one unstretched sheet. In addition, the polymer melted by each extruder is introduced into the three inlets of the die, and the three polymers are bonded to one slit through the three slits of the die or within the die. From the outlet gold, extruded three layers of laminar molten polymer onto a cooling drum,
A single sheet is formed and solidified by cooling on a cooling drum to obtain a three-layer laminated unstretched film, and then a biaxially stretched film obtained by a conventional method such as longitudinal stretching, transverse stretching and heat setting. It is a method useful in the present invention as a method of making a laminated film through a membrane process. Another method is another position film forming method in which three types of molten polymers are extruded from different slits in stages and then cooled and solidified on a cooling drum, which is also useful in the present invention. These are also called coextrusion methods.
【0052】この他に別々に製膜したフィルムをラミネ
ーションして積層する方法がある。すなわち、3種の樹
脂を別々に未延伸フィルムを、あるいは一軸延伸フィル
ムを作り、それらにアンカー剤、接着剤等をコーティン
グした後、この3種のフィルムをラミネートして積層
し、次いでこれを二軸延伸し、熱固定する方法である。
しかしこの方法は工程が複雑で設備費がかかり過ぎるの
と品質の面から実用的ではなく、簡易性から共押出法が
好ましい。In addition to this, there is a method of laminating and laminating separately formed films. That is, three kinds of resins are separately formed into unstretched films or uniaxially stretched films, which are coated with an anchor agent, an adhesive, etc., and these three kinds of films are laminated and laminated, and then the two films are laminated. It is a method of axially stretching and heat setting.
However, this method is not practical in terms of quality because the process is complicated and the equipment cost is too high, and the coextrusion method is preferable because of its simplicity.
【0053】変性ポリエステル樹脂を押出機で溶融する
温度は前述の単層の場合の条件と同様であり、260〜320
℃の範囲が適しており、好ましくは280〜310℃である。
共押出する場合、変性ポリエステル樹脂の溶融温度は最
外層に用いられる本発明のポリエステル樹脂と同じ温度
で溶融することが好ましい。また三つの樹脂の内、Tm
が最も高い樹脂の溶融温度に合わせるのがよい。The temperature at which the modified polyester resin is melted in the extruder is the same as the conditions for the above-mentioned single layer, and is 260 to 320.
A range of ℃ is suitable, preferably 280 ~ 310 ℃.
In the case of coextrusion, the modified polyester resin preferably melts at the same temperature as the polyester resin of the present invention used in the outermost layer. Also, of the three resins, Tm
It is better to match the highest melting temperature of the resin.
【0054】なお、ここで樹脂層、最外層、内部層等の
層とは、支持体となる樹脂の、ある厚さを持っているフ
ィルムをいい、下引層、帯電防止層、乳剤層等の層とは
区別される。The resin layer, the outermost layer, the inner layer and the like are films having a certain thickness of the resin serving as a support, such as an undercoat layer, an antistatic layer and an emulsion layer. Is distinct from the layers of.
【0055】本発明において好ましく採用出来る積層構
造は、両最外層がナフタレンジカルボン酸を主構成成分
とするポリエステルであり、内部層が少なくとも1層が
変性ポリエステルである。該ポリエステルはナフタレン
ジカルボン酸を主構成成分の前記例示のポリエステルを
この積層フィルムに適用できることはいうまでもない。
その中でも、最外層の該ポリエステルがポリエチレンナ
フタレート、特にポリエチレン-2,6-ナフタレート(P
EN)であり、内部層の変性ポリエステルが5-ナトリウ
ムスルホイソフタル酸、ポリエチレングリコールをを構
成成分として含有する変性ポリエステル(以下Mと略す
ことがある)であって、最外層と内部層との厚さの比率
がPEN(上外):M:PEN(下外)=2〜4:10:8
〜6の範囲にあるのが特に好ましい。なおこの場合、積
層フィルムに感光層を塗設する面は上記比率で述べた下
外の最外層に行うのが好ましく、巻癖が非常に付きにく
い写真用支持体を得ることができる。In the laminated structure preferably used in the present invention, both outermost layers are polyesters containing naphthalenedicarboxylic acid as a main constituent, and at least one inner layer is a modified polyester. Needless to say, the above-mentioned polyester having naphthalene dicarboxylic acid as a main constituent can be applied to this laminated film.
Among them, the outermost polyester is polyethylene naphthalate, especially polyethylene-2,6-naphthalate (P
EN) and the modified polyester of the inner layer is a modified polyester containing 5-sodium sulfoisophthalic acid and polyethylene glycol as constituent components (hereinafter sometimes abbreviated as M), and the thickness of the outermost layer and the inner layer is Ratio of PEN (top outside): M: PEN (bottom outside) = 2 to 4: 10: 8
It is particularly preferable that it is in the range of -6. In this case, it is preferable that the laminated film is coated with the photosensitive layer on the outermost lower layer described in the above ratio, so that a photographic support having extremely little curl can be obtained.
【0056】本発明に係わる積層構造フィルムの厚みの
総和は特に限定されず、用途に応じて任意に定めること
ができるが、通常40〜180μmであるが、特に薄手の場合
には65〜100μmが好ましい。The total thickness of the laminated structure film according to the present invention is not particularly limited and can be arbitrarily determined according to the application, but it is usually 40 to 180 μm, but especially when it is thin, it is 65 to 100 μm. preferable.
【0057】変性ポリエステルはPET等通常のポリエ
ステルより酸化を受け易く、変性ポリエステルには酸化
防止剤を混合することが望ましく、具体的には、ヒンダ
ードフェノール系化合物、アリルアミノ系化合物、ホス
ファイト系化合物、チオエステル系化合物等が挙げら
れ、市販のものが使用できる。これらの中でも、ヒンダ
ードフェノール系が好ましいが、その種類に限定される
ものではない。酸化防止剤の添加は合成及び製膜工程に
おいていずれで行ってもよいが、酸化防止を効果的にす
るには押出し工程の前に添加するのが最も好ましい。そ
の含有量は通常、変性ポリエステルによる積層フィルム
の濁度を増大させずに、かつ優れた写真性能を得るため
には、変性ポリエステルに対して、0.01〜2重量%の添
加でよく、好ましくは0.1〜0.5重量%である。なお酸化
防止剤は1種単独で使用してもよいし、2種以上組み合
わせて使用してもよい。Modified polyesters are more susceptible to oxidation than ordinary polyesters such as PET, and it is desirable to add an antioxidant to the modified polyesters. Specifically, hindered phenol compounds, allylamino compounds, phosphite compounds are preferred. , Thioester compounds and the like, and commercially available products can be used. Among these, hindered phenols are preferable, but the kind is not limited. The antioxidant may be added in any of the synthesis and film forming steps, but it is most preferable to add it before the extrusion step in order to effectively prevent the antioxidant. In order to obtain excellent photographic performance without increasing the turbidity of the laminated film made of the modified polyester, the content thereof may be 0.01 to 2% by weight based on the modified polyester, preferably 0.1% by weight. ~ 0.5% by weight. The antioxidants may be used alone or in combination of two or more.
【0058】本発明のポリエステルは単層フィルムにし
ろ、積層フィルムにしろ、ライトパイピング現象を防止
するために、染料を含有させることが出来る。このよう
な目的で配合される染料としては、その種類に特に限定
があるわけではないが、フィルムの製造上、耐熱性に優
れていることが必要であり、アンスラキノン系やペリノ
ン系の染料が挙げられる。また、色調としては、一般の
写真感光材料に見られるようにグレーあるいはブルー着
色の染料が用いられる。これらの染料としては、バイエ
ル社製のマクロレックス・シリーズ、住友化学(株)社
製のスミプラスト・シリーズ、三菱化学(株)社製のダ
イアレジン・シリーズ、日本火薬(株)社製カヤセット
・シリーズ等ポリエステル用として市販されているもの
の中から一種単独で、もしくは二種以上の染料を必要な
色調となるように混合して用いることができる。この
際、フィルムの分光透過率を400〜700nmの波長範囲で60
%以上85%以下とし、感光材料の一般的な性質上グレー
のいろにするのが好ましく、ライトパイピング現象を防
止し、かつ良好な写真プリントを得る上で好ましい。本
発明に用いられる積層フィルムのライトパイピング防止
には、最外層に染料を含有させるだけでその目的は達成
される。The polyester of the present invention may be a single layer film or a laminated film, and may contain a dye in order to prevent the light piping phenomenon. The dye to be blended for such a purpose is not particularly limited in its type, but in the production of the film, it is necessary that it has excellent heat resistance, and anthraquinone-based or perinone-based dyes may be used. Can be mentioned. As the color tone, a gray or blue dye is used, as seen in general photographic light-sensitive materials. Examples of these dyes include the Macrolex series manufactured by Bayer, the Sumiplast series manufactured by Sumitomo Chemical Co., Ltd., the dialesin series manufactured by Mitsubishi Chemical Co., Ltd., and the Kayaset series manufactured by Nippon Kayaku Co., Ltd. From the commercially available products for polyester, one kind may be used alone, or two or more kinds of dyes may be mixed and used so as to obtain a necessary color tone. At this time, the spectral transmittance of the film is 60 in the wavelength range of 400 to 700 nm.
% Or more and 85% or less, it is preferable to use a gray color because of the general property of the light-sensitive material, and it is preferable in order to prevent the light piping phenomenon and to obtain a good photographic print. In order to prevent light piping of the laminated film used in the present invention, the purpose can be achieved only by adding a dye to the outermost layer.
【0059】本発明のポリエステルフィルムには、必要
に応じて易滑性を付与することもできる。易滑性付与手
段としては、特に限定はないが、ポリエステルに不活性
無機粒子を添加する外部粒子添加方法、ポリエステルの
合成時に添加する触媒を析出させる内部粒子析出方法、
あるいは界面活性剤等をフィルム表面に塗布する方法等
が一般的である。これらの中でも、析出する粒子を比較
的小さくコントロールできる内部粒子析出方法が、フィ
ルムの透明性を損なうことなく易滑性を付与できるので
好ましい。この場合の触媒としては、公知の各種触媒が
使用できるが、特にCa、Mnを使用すると高い透明性が得
られるので好ましい。これらの触媒は一種でも良いし、
二種以上を併用しても良い。If necessary, the polyester film of the present invention may be provided with slipperiness. The slipperiness imparting means is not particularly limited, but an external particle addition method of adding inert inorganic particles to polyester, an internal particle precipitation method of precipitating a catalyst to be added during the synthesis of polyester,
Alternatively, a method of applying a surfactant or the like on the film surface is generally used. Among these, the internal particle deposition method in which the deposited particles can be controlled to be relatively small is preferable because slipperiness can be imparted without impairing the transparency of the film. As the catalyst in this case, various known catalysts can be used, but Ca and Mn are particularly preferable because high transparency can be obtained. These catalysts may be one kind,
You may use 2 or more types together.
【0060】本発明の写真用支持体はポリエステルフィ
ルム(積層の場合には最外層のポリエステル)の少なく
とも1面に紫外線照射処理を施し、官能基を有する水性
ポリマーをその面に塗設して下引層を設けたものであ
る。ここで紫外線照射について記述する。The photographic support of the present invention is prepared by subjecting at least one side of a polyester film (the outermost layer of polyester in the case of lamination) to ultraviolet irradiation, and coating an aqueous polymer having a functional group on that side. It is provided with a pulling layer. Here, the ultraviolet irradiation will be described.
【0061】本発明のポリエステルフィルムへの紫外線
照射は、一軸延伸前、一軸延伸後、二軸延伸後、熱固定
後のいずれでもよく、複数の工程で2段階以上に分けて
行っても良い。照射方法は特に限定はなく、光源の種
類、光源とフィルムとの距離、フィルムの温度、処理中
の雰囲気の種類、照射時間等の組合わせを適宜調整する
ことができる。例えば光源としては、低圧、中圧、高圧
何れの紫外線ランプを使用することが出来、本発明に有
効な発光波長は180〜320nmで、石英製の殺菌灯(低圧水
銀灯)、中圧水銀灯、高圧水銀灯、ブラックライト等各
種の紫外線ランプが適している。中でも253.7nmの発光
ピークを持つ低圧水銀灯が照射効率が良く、好ましく用
いられる。紫外線照射中の雰囲気は空気中、酸素中やオ
ゾンを含む媒体中等で行うことが好ましい。処理中のフ
ィルム温度は従来技術のように高温である必要はなく、
10〜30℃の常温で処理しても良好な接着強度が得られ
る。紫外線照射時間は例えば照射強度が100mW/cm2 の
とき0.5分からその効果が顕著に現れ、5時間以上でそ
の効果はほぼ飽和するのでそれ以上処理しても意味がな
い。あまり長すぎるとフィルムの脆化が著しくなる。従
って、0.5分以上5時間以内が好ましい。更に好ましく
は5分以上2時間以内である。紫外線照射処理された本
発明のポリエステルフィルム面は、下記二つの特定の波
数の赤外吸収強度(以下IR吸収強度と略す)比が下記
式(1)及び式(2)式を満たすように処理されていれ
ば優れた接着性を得ることが出来ることを本発明者らは
見いだした。The irradiation of the polyester film of the present invention with ultraviolet rays may be performed before uniaxial stretching, after uniaxial stretching, after biaxial stretching, or after heat setting, and may be performed in a plurality of steps in two or more steps. The irradiation method is not particularly limited, and the combination of the type of light source, the distance between the light source and the film, the temperature of the film, the type of atmosphere during processing, the irradiation time and the like can be appropriately adjusted. For example, as the light source, any of low-pressure, medium-pressure, and high-pressure ultraviolet lamps can be used, and the emission wavelength effective in the present invention is 180 to 320 nm. The germicidal lamp made of quartz (low-pressure mercury lamp), medium-pressure mercury lamp, high-pressure lamp Various ultraviolet lamps such as mercury lamps and black lights are suitable. Among them, a low pressure mercury lamp having an emission peak of 253.7 nm has good irradiation efficiency and is preferably used. It is preferable that the atmosphere during the ultraviolet irradiation is in the air, oxygen, a medium containing ozone, or the like. The film temperature during processing does not have to be as high as in the prior art,
Good adhesion strength can be obtained even when treated at room temperature of 10 to 30 ° C. With respect to the ultraviolet irradiation time, for example, when the irradiation intensity is 100 mW / cm 2 , the effect becomes remarkable from 0.5 minutes, and the effect is almost saturated after 5 hours or more, so there is no point in further processing. If it is too long, the film becomes extremely brittle. Therefore, it is preferably 0.5 minutes or more and 5 hours or less. More preferably, it is 5 minutes or more and 2 hours or less. The surface of the polyester film of the present invention that has been subjected to the ultraviolet irradiation treatment is treated so that the ratio of the infrared absorption intensities (hereinafter abbreviated as IR absorption intensities) of the following two specific wave numbers satisfies the following formulas (1) and (2). The present inventors have found that excellent adhesion can be obtained if this is done.
【0062】式(1) 0.90≦I1133/I1142≦1.05 式(2) 0.90≦I1330/I1340≦1.10 ここで、I1133は波数が1133cm-1に対するIR吸収強度 I1142は波数が1142cm-1に対するIR吸収強度 I1330は波数が1330cm-1に対するIR吸収強度 I1340は波数が1340cm-1に対するIR吸収強度 を表す。[0062] Equation (1) 0.90 ≦ I1133 / I1142 ≦ 1.05 Equation (2) 0.90 ≦ I1330 / I1340 ≦ 1.10 where, IR absorption intensity IR absorption intensity I1142 is wavenumber for 1142Cm -1 wave number is for 1133cm -1 I1133 I1330 is IR absorption intensity I1340 is wave number for wave numbers 1330 cm -1 represent the IR absorption intensity against 1340 cm -1.
【0063】なお、IR吸収強度は以下の方法で求めた
値である。すなわち、45mm×20mmの寸法の写真用支持体
又はフィルム試料を、ゲルマニウム結晶板(θ=60°)
の両面に1枚ずつ密着させて、日本電子社製ATR−I
R測定装置(JIR-40型)を用いて測定した。なお、これ
らのIR吸収強度の低下する理由は定かではないが、ポ
リエステル分子において何らかの変化が起こっているも
のと考えられる。The IR absorption intensity is a value obtained by the following method. That is, a photographic support or film sample having a size of 45 mm × 20 mm is put into a germanium crystal plate (θ = 60 °).
ATR-I made by JEOL Ltd.
It measured using the R measuring device (JIR-40 type). The reason why the IR absorption intensity decreases is not clear, but it is considered that some change occurs in the polyester molecule.
【0064】本発明のカルボン酸がナフタレンジカルボ
ン酸であるポリエステルは太陽光あるいは紫外線を当て
ると蛍光を発光する性質がある。この蛍光の発光は今の
所、ハロゲン化銀写真感光材料にどのような影響を与え
るか定かではないが、ハロゲン化銀写真感光材料にとっ
て好ましいものではない。ところが、本発明の紫外線照
射を行うと、この蛍光の発光がほとんどなくなることを
見いだした。また蛍光の発光の度合いが紫外線照射量に
よっても変化し、本発明の紫外線照射量程度の光量を与
えると蛍光が消失する。The polyester of which the carboxylic acid of the present invention is naphthalene dicarboxylic acid has a property of emitting fluorescence when exposed to sunlight or ultraviolet rays. It is unclear at present how this fluorescent emission will affect the silver halide photographic light-sensitive material, but it is not preferable for the silver halide photographic light-sensitive material. However, it was found that when the UV irradiation of the present invention was carried out, the emission of this fluorescence was almost eliminated. Further, the degree of fluorescence emission also changes depending on the ultraviolet irradiation amount, and the fluorescence disappears when a light amount equivalent to the ultraviolet irradiation amount of the present invention is applied.
【0065】次に、本発明の紫外線照射処理後のポリエ
ステルフィルム表面への下引について述べる。Next, the undercoating on the surface of the polyester film after the ultraviolet irradiation treatment of the present invention will be described.
【0066】本発明者らはほぼ室温にて紫外線照射した
ポリエステル面に、官能基を有する水性ポリマー化合物
を下引層として塗設することによって、優れた接着性が
得られることを見いだした。The present inventors have found that excellent adhesion can be obtained by coating an aqueous polymer compound having a functional group as an undercoat layer on a polyester surface which has been irradiated with ultraviolet rays at about room temperature.
【0067】本発明の官能性基を有する水性ポリマー化
合物はビニルコポリマーラテックス及び/又は水性コポ
リエステルである。The aqueous polymeric compound having functional groups of the present invention is a vinyl copolymer latex and / or an aqueous copolyester.
【0068】本発明に係わる水性ポリマー化合物の官能
基としては、カルボン酸基、スルホン酸基、水酸基、ア
ミド基、グリシジル基であり、カルボン酸又はスルホン
酸はフリーの酸であっても、アルカリ金属塩であっても
よい。アルカリ金属としてはリチウム、ナトリウム、カ
リウム、セシウムであって、ナトリウムが好ましい。The functional group of the aqueous polymer compound according to the present invention is a carboxylic acid group, a sulfonic acid group, a hydroxyl group, an amide group or a glycidyl group. Even if the carboxylic acid or sulfonic acid is a free acid, it may be an alkali metal. It may be salt. The alkali metal is lithium, sodium, potassium or cesium, with sodium being preferred.
【0069】本発明に用いられるビニルコポリマーラテ
ックスの官能基を有するビニルモノマー以外のビニルモ
ノマーとしては、ブタジエン、イソプレン等の共役ジエ
ンモノマー、1,4-ペンタジエン、1,4-ヘキサジエン等の
非共役ジエンモノマー、スチレン、メチルスチレン、ジ
ビニルスチレン等のスチレン及びその誘導体モノマー、
メチルメタクリレート、エチルメタクリレート、プロピ
ルメタクリレート(n-、i-),ブチルメタクリレート
(n、s、t)、シクロヘキシルメタクリレート、エチル
ヘキシルメタクリレート、フェニルメタクリレート、ベ
ンジルメタクリレート、フェネチルメタクリレート、エ
チレングリコール-ジメタクリレート等のメタクリル酸
エステルモノマー、メチルアクリレート、エチルアクリ
レート、プロピルアクリレート(n-、i-),ブチルアク
リレート(n、s、t)、シクロヘキシルアクリレート、
エチルヘキシルアクリレート、フェニルアクリレート、
ベンジルアクリレート、フェネチルアクリレート、エチ
レングリコール-ジアクリレート等のアクリル酸エステ
ルモノマー、塩化ビニル、塩化ビニリデン、酢酸ビニ
ル、が挙げられる。Vinyl monomers other than the vinyl monomer having a functional group of the vinyl copolymer latex used in the present invention include conjugated diene monomers such as butadiene and isoprene, and non-conjugated dienes such as 1,4-pentadiene and 1,4-hexadiene. Monomers, styrene such as styrene, methyl styrene and divinyl styrene, and their derivative monomers,
Methacrylic acid such as methyl methacrylate, ethyl methacrylate, propyl methacrylate (n-, i-), butyl methacrylate (n, s, t), cyclohexyl methacrylate, ethylhexyl methacrylate, phenyl methacrylate, benzyl methacrylate, phenethyl methacrylate, ethylene glycol-dimethacrylate Ester monomer, methyl acrylate, ethyl acrylate, propyl acrylate (n-, i-), butyl acrylate (n, s, t), cyclohexyl acrylate,
Ethylhexyl acrylate, phenyl acrylate,
Examples thereof include acrylic acid ester monomers such as benzyl acrylate, phenethyl acrylate and ethylene glycol-diacrylate, vinyl chloride, vinylidene chloride and vinyl acetate.
【0070】本発明のビニルコポリマーラテックスの官
能性基を有する含カルボン酸モノマーとしてはアクリル
酸、メタクリル酸、イタコン酸、マレイン酸等及びこれ
らの塩等が挙げられ、含スルホン酸モノマーとしてはス
チレンスルホン酸、ビニルベンジルスルホン酸、ビニル
スルホネート、3-スルホプロピル-メチルアクリルアミ
ド、N-(2−スルホ−1,1−ジメチルエチル)アクリ
ルアミド及びこれらの塩等が挙げられ、含水酸基モノマ
ーとしては2-ヒドロキシエチルアクリレート、2-ヒドロ
キシエチルメタクリレート、ヒドロキシメチルスチレ
ン、ポリエチレングリコール-モノアクリレート、ポリ
エチレングリコール-モノメタクリレート、ポリプロピ
レングリコール-アクリレート、ポリプロピレングリコ
ール-メタクリレート、ポリ(コ-エチレン-コ-プロピレ
ングリコール)-モノアクリレート、ポリ(コ-エチレン
-コ-プロピレングリコール)-モノメタクリレート等が
挙げられ、含アミド基モノマーとしては、アクリルアミ
ド、メチルアクリルアミド、ジメチルアクリルアミド、
エチルアクリルアミド、ブチルアクリルアミド、フェニ
ルアクリルアミド、ベンジルアクリルアミド、シクロヘ
キシルアクリルアミド、ジアセトンアクリルアミド等が
挙げられ、含グリシジル基モノマーとして、グリシジル
アクリレート、グリシジルメタクリレート等が挙げられ
る。上記挙げられたモノマーに限定されるものではな
い。Examples of the carboxylic acid-containing monomer having a functional group of the vinyl copolymer latex of the present invention include acrylic acid, methacrylic acid, itaconic acid, maleic acid and the like and salts thereof, and the sulfonic acid-containing monomer is styrene sulfone. Acid, vinylbenzyl sulfonic acid, vinyl sulfonate, 3-sulfopropyl-methylacrylamide, N- (2-sulfo-1,1-dimethylethyl) acrylamide and salts thereof, and the like, and the hydroxyl group-containing monomer is 2-hydroxy. Ethyl acrylate, 2-hydroxyethyl methacrylate, hydroxymethyl styrene, polyethylene glycol-monoacrylate, polyethylene glycol-monomethacrylate, polypropylene glycol-acrylate, polypropylene glycol-methacrylate, poly ( Co-ethylene-co-propylene glycol) -monoacrylate, poly (co-ethylene
-Co-propylene glycol) -monomethacrylate and the like. Examples of the amide-containing group monomer include acrylamide, methyl acrylamide, dimethyl acrylamide,
Examples thereof include ethyl acrylamide, butyl acrylamide, phenyl acrylamide, benzyl acrylamide, cyclohexyl acrylamide, and diacetone acrylamide. Examples of the glycidyl group-containing monomer include glycidyl acrylate and glycidyl methacrylate. It is not limited to the monomers listed above.
【0071】本発明に係わる官能性基を有するビニルコ
ポリマーラテックスは、官能基を有するモノマーのビニ
ルコポリマー中の重量比は、1〜60%であり、官能基に
よりその割合は変わってもかまわない。例えばカルボン
酸基を有するモノマーは3〜40%、スルホン酸基を有す
るモノマーは3〜40%、アミド基を有するモノマーは3
〜50%、またグリシジル基を有するモノマーは10〜60%
が好ましい。In the vinyl copolymer latex having a functional group according to the present invention, the weight ratio of the monomer having a functional group in the vinyl copolymer is 1 to 60%, and the ratio may be changed depending on the functional group. For example, a monomer having a carboxylic acid group is 3 to 40%, a monomer having a sulfonic acid group is 3 to 40%, and a monomer having an amide group is 3%.
~ 50%, 10-60% for monomers with glycidyl groups
Is preferred.
【0072】本発明に有用なビニルコポリマーラテック
スを合成する場合には上記モノマーの重合開始剤、分散
剤等が用いられる。When synthesizing the vinyl copolymer latex useful in the present invention, a polymerization initiator, a dispersant or the like of the above monomers is used.
【0073】重合開始剤としては過酸化水素、過硫酸カ
リ、過硫酸アンモン、キュメンパーオキシド、過酸化ベ
ンゾイル、α,α′-アゾビスイソブチロニトリル、α,
α′-アゾビスブチルカルボン酸ナトリウム等が挙げら
れ、これら過酸化物と硫酸第1鉄あるいは硫酸第1鉄ア
ンモニウム等と組み合わせてレドックス重合を行うこと
も出来る。As the polymerization initiator, hydrogen peroxide, potassium persulfate, ammonium persulfate, cumene peroxide, benzoyl peroxide, α, α′-azobisisobutyronitrile, α,
Examples thereof include sodium α'-azobisbutylcarboxylate, and the redox polymerization can be carried out by combining these peroxides with ferrous sulfate or ferrous ammonium sulfate.
【0074】また分散剤として界面活性剤が用いられ
る。界面活性剤としてはアニオン活性剤、カチオン活性
剤、ノニオン活性剤、親水性コロイドバインダー等を使
用することが出来る。A surfactant is used as a dispersant. As the surfactant, an anion activator, a cation activator, a nonion activator, a hydrophilic colloid binder and the like can be used.
【0075】アニオン活性剤としてはAs the anion activator,
【0076】[0076]
【化2】 Embedded image
【0077】等を挙げることが出来る。And the like.
【0078】カチオン活性剤としてはAs the cationic activator,
【0079】[0079]
【化3】 Embedded image
【0080】等を挙げることが出来る。And the like.
【0081】ノニオン活性剤としてはAs the nonionic activator,
【0082】[0082]
【化4】 [Chemical 4]
【0083】等を挙げることが出来る。And the like.
【0084】両性イオン活性剤としてはAs the zwitterionic activator,
【0085】[0085]
【化5】 Embedded image
【0086】等を挙げることが出来る。And the like.
【0087】親水性コロイドにはアニオンポリマー、カ
チオンポリマー、ノニオンポリマー、両性イオンポリマ
ーがあり、いずれもバインダーとして用いることが出来
る。アニオンポリマーとしてはカルボキシメチルセルロ
ース、スチレンスルホン酸ナトリウムコポリマー、アク
リル酸ナトリウムコポリマー、本発明に用いられる水性
コポリエステル(後述)の他Hydrophilic colloids include anionic polymers, cationic polymers, nonionic polymers and zwitterionic polymers, all of which can be used as a binder. Examples of anionic polymers include carboxymethyl cellulose, sodium styrenesulfonate copolymer, sodium acrylate copolymer, and other aqueous copolyesters (described later) used in the present invention.
【0088】[0088]
【化6】 [Chemical 6]
【0089】等を挙げることが出来る。And the like.
【0090】カチオンポリマーとしてはAs the cationic polymer
【0091】[0091]
【化7】 [Chemical 7]
【0092】等を挙げることが出来る。And the like.
【0093】ノニオンポリマーとしてはポリビニルアル
コール、ポリエチレンオキサイド、ポリプロピレンオキ
サイド、ヒドロキシエチルセルロース、メチルセルロー
ス、デキストリン、ポリビニルピロリドン、ポリアクリ
ルアミド等を挙げることが出来る。Examples of nonionic polymers include polyvinyl alcohol, polyethylene oxide, polypropylene oxide, hydroxyethyl cellulose, methyl cellulose, dextrin, polyvinyl pyrrolidone and polyacrylamide.
【0094】両性イオンポリマーとしてはゼラチン、カ
ゼイン、等を挙げることが出来る。ラテックス中に添加
される界面活性剤の量は0.1〜5.0重量%でよい。また、
ラテックス中に添加されるバインダーの量はラテックス
固形分に対して、0.5〜50重量%であり、好ましくは1
〜20重量%である。これら本発明のビニルコポリマーラ
テックスは通常のラテックス重合法によって容易に作る
ことが出来る。Examples of zwitterionic polymers include gelatin and casein. The amount of surfactant added to the latex may be 0.1-5.0% by weight. Also,
The amount of the binder added to the latex is 0.5 to 50% by weight based on the latex solid content, preferably 1
~ 20% by weight. These vinyl copolymer latexes of the present invention can be easily prepared by a usual latex polymerization method.
【0095】(合成例) P−1の合成 1リットルの4つ口フラスコに撹拌器、温度計、滴下ロ
ート、窒素導入管、還流冷却器を施し、窒素ガスを導入
し、脱酸素を行いつつ、蒸留水350mlを加えて内温が80
℃となるまで加熱した。下記化7の分散剤を4.5g添加
し、更に重合開始剤として過硫酸アンモニウム0.45gを
添加し、次いでブチルアクリレート120g、スチレン60
g、グリシジルメタクリレート120gの混合モノマーを
1時間かけてゆっくりと滴下し、 8時間撹拌を続けてた
後、反応させ乳白色のラテックスコポリマーを得た。こ
れを水蒸気蒸留で未反応のモノマーを除去する。その後
冷却しアンモニア水でpH6に調整しビニルコポリマーラ
テックスP−1を得た。(Synthesis Example) Synthesis of P-1 A 1-liter four-necked flask was equipped with a stirrer, a thermometer, a dropping funnel, a nitrogen introducing tube, and a reflux condenser, and nitrogen gas was introduced to perform deoxidation. , Add 350 ml of distilled water and the internal temperature is 80
Heated to 0 ° C. 4.5 g of the dispersant of the following chemical formula 7 was added, and further 0.45 g of ammonium persulfate was added as a polymerization initiator, then 120 g of butyl acrylate and 60 g of styrene.
g, a mixed monomer of 120 g of glycidyl methacrylate was slowly added dropwise over 1 hour, and the mixture was stirred for 8 hours and then reacted to obtain a milky white latex copolymer. This is steam-distilled to remove unreacted monomers. Then, the mixture was cooled and adjusted to pH 6 with aqueous ammonia to obtain vinyl copolymer latex P-1.
【0096】本発明に有用なビニルコポリマーの例を下
記に示したが、これらに限定されるものではない。これ
らP−2〜P−12のコポリマーラテックスはP−1と同
様に合成し得たものである。Examples of vinyl copolymers useful in the present invention are shown below, but are not limited thereto. The copolymer latex of P-2 to P-12 can be synthesized in the same manner as P-1.
【0097】[0097]
【化8】 Embedded image
【0098】[0098]
【化9】 [Chemical 9]
【0099】[0099]
【化10】 [Chemical 10]
【0100】官能基のない比較としてのビニルコポリマ
ーラテックスの例HP−1〜3を下記に示す。なお合成
については上記ラテックスの合成法と同様に行える。Examples of comparative vinyl copolymer latices HP-1 to HP3 without functional groups are shown below. The synthesis can be performed in the same manner as the above-mentioned latex synthesis method.
【0101】[0101]
【化11】 [Chemical 11]
【0102】本発明の下引液に用いられる水性コポリエ
ステルは主構成成分、親水性構成成分とその他の変性成
分とからなっている。The aqueous copolyester used in the subbing solution of the present invention comprises a main constituent, a hydrophilic constituent and other modifying components.
【0103】該水性コポリエステルの主構成成分として
はテレフタル酸又はナフタレンジカルボン酸とエチレン
グリコールとからなるポリエステル部分であり、全コポ
リエステルに対して40モル%以上は必要で、好ましくは
50〜85モル%である。The main constituent component of the aqueous copolyester is a polyester portion composed of terephthalic acid or naphthalenedicarboxylic acid and ethylene glycol, and 40 mol% or more is necessary with respect to the total copolyester, and preferably
It is 50 to 85 mol%.
【0104】該水性コポリエステルの親水性構成成分と
してはカルボン酸又はスルホン酸等の官能基を側鎖に有
する芳香族ジカルボン酸とグリコールとからなる親水性
コポリエステル部分であり、全コポリエステルに対して
5〜35モル%含まれるのが好ましく、更に7〜30モル
%、特に10〜25モル%あるのが好ましい。官能基を有す
る芳香族ジカルボン酸としては、5-ナトリウムスルホイ
ソフタル酸、2-ナトリウムスルホイソフタル酸、4-ナト
リウムスルホイソフタル酸、4-ナトリウムスルホ−2,6-
ナフタレンジカルボン酸等を挙げることが出来る。中で
も金属塩スルホイソフタル酸が好ましく、金属イオンは
ナトリウム、カリウム、リチウム、セシウム等のアルカ
リ金属で、ナトリウムが好ましい。The hydrophilic constituent component of the aqueous copolyester is a hydrophilic copolyester portion composed of an aromatic dicarboxylic acid having a functional group such as a carboxylic acid or a sulfonic acid in the side chain and a glycol. 5 to 35 mol%, more preferably 7 to 30 mol%, especially 10 to 25 mol%. As the aromatic dicarboxylic acid having a functional group, 5-sodium sulfoisophthalic acid, 2-sodium sulfoisophthalic acid, 4-sodium sulfoisophthalic acid, 4-sodium sulfo-2,6-
Examples thereof include naphthalenedicarboxylic acid. Among them, the metal salt sulfoisophthalic acid is preferable, and the metal ion is an alkali metal such as sodium, potassium, lithium or cesium, and sodium is preferable.
【0105】該水性コポリエステルの親水性構成成分と
しては官能基が主鎖に有するポリアルキレングリコール
とジカルボン酸とからなる親水性コポリエステル部分で
あり、全コポリエステルに対して3〜20重量%含まれる
ことが好ましく、特に4〜15重量%あれば好ましい。ポ
リアルキレングリコールとしては、ポリエチレングリコ
ール、ポリプロピレングリコール、ポリ-コ-エチレング
リコール-コ-プロピレングリコールが挙げられるが、ポ
リエチレングリコールが好ましい。ポリエチレングリコ
ールの数平均分子量は特に限定されないが、好ましくは
10〜10,000で、より好ましくは20〜8,000、特に好まし
くは30〜3,000である。The hydrophilic constituent component of the aqueous copolyester is a hydrophilic copolyester portion composed of a polyalkylene glycol having a functional group in the main chain and a dicarboxylic acid, and is contained in an amount of 3 to 20% by weight based on the whole copolyester. It is preferable that the amount is 4 to 15% by weight. Polyalkylene glycols include polyethylene glycol, polypropylene glycol, poly-co-ethylene glycol-co-propylene glycol, with polyethylene glycol being preferred. The number average molecular weight of polyethylene glycol is not particularly limited, but preferably
It is 10 to 10,000, more preferably 20 to 8,000, and particularly preferably 30 to 3,000.
【0106】該水性コポリエステルのその他の変性構成
成分としての酸成分とグリコール成分を、下記に示す
が、これらに限定されるものではない。The acid component and glycol component as other modified constituents of the aqueous copolyester are shown below, but the invention is not limited thereto.
【0107】ジカルボン酸としては、テレフタル酸、2,
6-ナフタレンジカルボン酸、他のナフタレンジカルボン
酸、イソフタル酸等の芳香族ジカルボン酸、アジピン
酸、ピメリン酸、スベリン酸、アゼライン酸、セバチン
酸等の脂肪族ジカルボン酸、ポリエチレンオキシドジカ
ルボン酸、ポリプロピレンオキシドジカルボン酸等のポ
リエーテルジカルボン酸等が挙げられるが、アジピン
酸、スベリン酸、アゼライン酸が好ましく、特にアジピ
ン酸が好ましく用いられる。脂肪族ジカルボン酸のポリ
エステル全重量に対して3〜10重量%がよく、好ましく
は4〜8重量%であるが、ポリアルキレングリコールと
この脂肪族ジカルボン酸とを共に用いる場合には、合わ
せて3〜20重量%が好ましく、特に4〜15重量%が好ま
しい。これらのジカルボン酸はカルボン酸のまま、ある
いはジメチルエステル、炭素数1〜8のジハーフエステ
ルの形でエステル化反応あるいは重合反応に用いること
が出来るが、エステルの場合、ジメチルエステル、ジエ
チレングリコールハーフエステルが好ましい。As the dicarboxylic acid, terephthalic acid, 2,
6-Naphthalenedicarboxylic acid, other naphthalenedicarboxylic acid, aromatic dicarboxylic acid such as isophthalic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid and other aliphatic dicarboxylic acid, polyethylene oxide dicarboxylic acid, polypropylene oxide dicarboxylic acid Examples thereof include polyether dicarboxylic acids such as acids, but adipic acid, suberic acid, and azelaic acid are preferable, and adipic acid is particularly preferable. It is preferably 3 to 10% by weight, and preferably 4 to 8% by weight, based on the total weight of the polyester of the aliphatic dicarboxylic acid, but when the polyalkylene glycol and this aliphatic dicarboxylic acid are used together, the total amount is 3 -20% by weight is preferable, and 4-15% by weight is particularly preferable. These dicarboxylic acids can be used in the esterification reaction or polymerization reaction in the form of carboxylic acid as they are, or in the form of dimethyl ester or dihalf ester having 1 to 8 carbon atoms. In the case of ester, dimethyl ester or diethylene glycol half ester is used. preferable.
【0108】グリコールとしては、エチレングリコー
ル、プロピレングリコール、ブタンジオール、ネオペン
チルグリコール、p−キシリデングリコール、1,4-シク
ロヘキサンジメタノール、ジエチレングリコール、トリ
エチレングリコール等を挙げることが出来る。Examples of glycols include ethylene glycol, propylene glycol, butanediol, neopentyl glycol, p-xylidene glycol, 1,4-cyclohexanedimethanol, diethylene glycol and triethylene glycol.
【0109】本発明に係わる水性コポリエステル樹脂の
固有粘度は0.30〜0.85が好ましく、下引性能から特に0.
40〜0.60が好ましい。The intrinsic viscosity of the water-based copolyester resin according to the present invention is preferably 0.30 to 0.85, and is particularly 0.
40 to 0.60 is preferable.
【0110】水性コポリエステル樹脂の合成は、従来公
知のポリエステルの製造法に従って行うことが出来、ま
た、前記変性ポリエステルの項で述べたエステル化及び
重合法をそのまま応用出来、触媒、添加剤等についても
同様であり、ここでは省略する。水性コポリエステル樹
脂の具体的な合成方法は米国特許第4,217,441号、特開
平5-210199号に記載されており、これらの方法によって
本発明に有用なコポリエステル樹脂は合成され得る。The aqueous copolyester resin can be synthesized according to a conventionally known method for producing a polyester, and the esterification and polymerization methods described in the section of the modified polyester can be directly applied to the catalyst, additives, etc. Is also the same, and is omitted here. Specific methods for synthesizing the aqueous copolyester resin are described in US Pat. No. 4,217,441 and JP-A-5-210199, and the copolyester resin useful in the present invention can be synthesized by these methods.
【0111】水性コポリエステルの合成例を以下に示
す。A synthetic example of the aqueous copolyester is shown below.
【0112】(CP−1の合成)テレフタル酸ジメチル
エステル38.74重量部、イソフタル酸ジメチルエステル3
1.95重量部、ナトリウム-5-スルホイソフタル酸ジメチ
ルエステル10.34重量部、エチレングリコール54.48重量
部を混合し、酢酸カルシウム一水塩0.073重量部及び酢
酸マンガン0.024重量部を添加し、窒素気流下において1
70〜220℃でメタノールを留去しながらエステル交換反
応を行った後、リン酸トリメチル0.05重量部、重合触媒
として三酸化アンチモン0.04重量部及び1,4-シクロヘキ
シルジカルボン酸17.17重量部を加え220〜235℃の反応
温度でほぼ理論量の水を留去してエステル化を行った。
その後更に反応系内を減圧、昇温し、最終的に280℃、
0.2mmHgで2時間重縮合を行った。得られたコポリエス
テル樹脂CP−1の固有粘度(前記同様)は0.45であっ
た。得られた水性コポリエステルは帯電防止組成物に使
用するため95℃の熱水中で3時間撹拌し30%の水溶液と
した。(Synthesis of CP-1) 38.74 parts by weight of terephthalic acid dimethyl ester, 3 parts of isophthalic acid dimethyl ester
1.95 parts by weight, sodium-5-sulfoisophthalic acid dimethyl ester 10.34 parts by weight, ethylene glycol 54.48 parts by weight are mixed, calcium acetate monohydrate 0.073 parts by weight and manganese acetate 0.024 parts by weight are added, and the mixture is mixed under nitrogen flow to 1
After carrying out the transesterification reaction while distilling off methanol at 70 to 220 ° C, 0.05 parts by weight of trimethyl phosphate, 0.04 parts by weight of antimony trioxide as a polymerization catalyst and 17.17 parts by weight of 1,4-cyclohexyldicarboxylic acid were added to 220 to 220 ° C. The esterification was carried out at a reaction temperature of 235 ° C. by distilling off almost the theoretical amount of water.
After that, the pressure inside the reaction system was further reduced and the temperature was raised to 280 ° C,
Polycondensation was carried out at 0.2 mmHg for 2 hours. The obtained copolyester resin CP-1 had an intrinsic viscosity (as described above) of 0.45. The aqueous copolyester obtained was stirred in hot water at 95 ° C. for 3 hours to prepare a 30% aqueous solution for use in the antistatic composition.
【0113】(CP−2の合成)テレフタル酸83重量
部、イソフタル酸41.5重量部、エチレングリコール77重
量部に酢酸カルシウム一水和物0.1重量部を添加し、常
法によりエステル化反応を行った。得られた生成物に5-
ナトリウムスルホジ(β-ヒドロキシエチル)イソフタ
ル酸55重量部をエチレングリコール溶液(濃度35重量
%)として加え、ポリエチレングリコール(平均重合度
2,000)13重量部、三酸化アンチモン0.05重量部、テト
ラメチルアンモニウムハイドロオキサイド0.15重量部,
リン酸トリメチルエステル0.13重量部を添加した。次い
で徐々に255℃に昇温、減圧して行き、280℃、0.2mmHg
で1.5時間重合を行い、冷却して、固有粘度0.52を有す
るコポリエステル樹脂CP−2を得た。得られた水性コ
ポリエステルを帯電防止組成物に使用するため95℃の熱
水中で3時間撹拌し30重量%の水溶液とした。(Synthesis of CP-2) 0.1 part by weight of calcium acetate monohydrate was added to 83 parts by weight of terephthalic acid, 41.5 parts by weight of isophthalic acid and 77 parts by weight of ethylene glycol, and esterification reaction was carried out by a conventional method. . 5-in the product obtained
55 parts by weight of sodium sulfodi (β-hydroxyethyl) isophthalic acid was added as an ethylene glycol solution (concentration: 35% by weight) to give polyethylene glycol (average degree of polymerization).
2,000) 13 parts by weight, antimony trioxide 0.05 parts by weight, tetramethylammonium hydroxide 0.15 parts by weight,
0.13 parts by weight of phosphoric acid trimethyl ester was added. Next, gradually raise the temperature to 255 ° C and reduce the pressure to 280 ° C and 0.2 mmHg.
Polymerization was carried out for 1.5 hours and then cooled to obtain a copolyester resin CP-2 having an intrinsic viscosity of 0.52. In order to use the obtained aqueous copolyester in an antistatic composition, it was stirred in hot water at 95 ° C. for 3 hours to give a 30% by weight aqueous solution.
【0114】(CP−3の合成)テレフタル酸95重量
部、イソフタル酸20重量部、エチレングリコール90重量
部に酢酸亜鉛二水塩0.1重量部を添加し、定法によりエ
ステル化反応を行った。得られた生成物に5-ナトリウム
スルホジ(β-ヒドロキシエチル)イソフタル酸45重量
部とアジピン酸8重量部をエチレングリコール溶液を濃
度35重量%として加え、三酸化アンチモン0.07重量部、
リン酸トリメチルエステル0.13重量部を添加した。次い
で窒素気流下徐々に255℃に昇温、減圧して行き、エチ
レングリコールを流出させ、285℃、0.7mmHgで重合を行
い、固有粘度0.50を有するコポリエステル樹脂CP−3
を得た。得られた水性コポリエステルを帯電防止組成物
に使用するため95℃の熱水中で3.5時間撹拌し30重量%
の水分散液とした。(Synthesis of CP-3) 0.1 part by weight of zinc acetate dihydrate was added to 95 parts by weight of terephthalic acid, 20 parts by weight of isophthalic acid and 90 parts by weight of ethylene glycol, and an esterification reaction was carried out by a conventional method. To the obtained product, 45 parts by weight of 5-sodium sulfodi (β-hydroxyethyl) isophthalic acid and 8 parts by weight of adipic acid were added in an ethylene glycol solution at a concentration of 35% by weight, and 0.07 part by weight of antimony trioxide,
0.13 parts by weight of phosphoric acid trimethyl ester was added. Then, the temperature was gradually raised to 255 ° C under a nitrogen stream, the pressure was reduced, ethylene glycol was allowed to flow out, polymerization was carried out at 285 ° C and 0.7 mmHg, and a copolyester resin CP-3 having an intrinsic viscosity of 0.50 was obtained.
I got To use the obtained aqueous copolyester in an antistatic composition, stir in hot water at 95 ° C for 3.5 hours to obtain 30% by weight.
Of water dispersion.
【0115】上記水性ポリマーを下引液に調製し、紫外
線を照射処理したフィルム面に塗設する。下引液には他
の界面活性剤、帯電防止剤、アンチハレーション剤、ク
ロスオーバーカット剤、着色染料、顔料、増粘剤、塗布
助剤、カブリ防止剤、酸化防止剤、紫外線吸収剤、紫外
線安定剤、エッチング処理剤、磁性粉、マット剤等の各
種添加剤を一種または二種以上含有していてもよい。The above-mentioned aqueous polymer is prepared as a subbing solution and applied on the surface of a film which has been irradiated with ultraviolet rays. Other surfactants, antistatic agents, antihalation agents, crossover cut agents, coloring dyes, pigments, thickeners, coating aids, antifoggants, antioxidants, UV absorbers, UV rays One kind or two or more kinds of various additives such as a stabilizer, an etching treatment agent, a magnetic powder and a matting agent may be contained.
【0116】下引液を塗布する方法は特に限定はない
が、従来から知られている各種の方法を用いることがで
きる。例えば、上記の素材を水分散液とし、エアーナイ
フコーター、ディップコーター、カーテンコーター、ワ
イヤーバーコーター、グラビアコーター、エクストルー
ジョンコーター等各種塗布機を用いることが出来る。The method of applying the subbing liquid is not particularly limited, but various conventionally known methods can be used. For example, various coating machines such as an air knife coater, a dip coater, a curtain coater, a wire bar coater, a gravure coater and an extrusion coater can be used by using the above material as an aqueous dispersion.
【0117】塗布に際して、本発明では特に必要ではな
いが、コロナ放電処理、グロー放電処理、プラズマ処
理、火炎処理等の表面活性化処理を前もって行ってもよ
い。Although not particularly required in the present invention, a surface activation treatment such as corona discharge treatment, glow discharge treatment, plasma treatment, flame treatment or the like may be carried out before coating.
【0118】本発明の下引層の上に一層または二層以上
の下引層上層を設けてもよい。On the undercoat layer of the present invention, one or two or more upper layers of the undercoat layer may be provided.
【0119】本発明の下引された写真用支持体を感光層
等を塗布する前あるいは後使用するまでの間、公知の過
熱処理方法を施すことによって、巻癖を付きにくくする
ことが出来る。公知の方法とは特開昭51-16358号明細書
(米国特許第4,141,735号と同じ)に記載されている方
法で、ポリエステルフィルムの巻癖を低減する方法とし
て、ポリエステルのTgを30℃ないし5℃下廻る温度範
囲で0.1〜1,500時間にわたって加熱処理するというもの
である。本発明の写真用支持体にこの方法を応用する場
合にはガラス転移温度以下ガラス転移温度−30℃以上の
温度で加熱処理するのが好ましい。処理時間は上記同様
に0.1〜1,500時間の範囲で行える。同様な巻癖を付きに
くくする他の方法も本発明の写真用支持体に応用出来
る。例えば、特開平6-51437号、同6-82959号、同6-8296
0号及び同6-82961号各明細書に記載されている方法であ
る。A curling habit can be less likely to occur by subjecting the undercoated photographic support of the present invention to a known overheat treatment method before or after the application of the photosensitive layer or the like to the use thereof. The known method is the method described in JP-A-51-16358 (the same as U.S. Pat. No. 4,141,735), and as a method for reducing the curl of the polyester film, the Tg of the polyester is 30 ° C to 5 ° C. The heat treatment is carried out at a temperature range below ℃ for 0.1 to 1,500 hours. When this method is applied to the photographic support of the present invention, it is preferable to perform heat treatment at a temperature not higher than the glass transition temperature and not lower than the glass transition temperature −30 ° C. The treatment time can be in the range of 0.1 to 1,500 hours as described above. Other methods for reducing the tendency to have a similar curl can be applied to the photographic support of the present invention. For example, JP-A-6-51437, JP-A-6-82959 and JP-A-6-8296.
No. 0 and No. 6-82961 are the methods described in each specification.
【0120】TgおよびTmの測定は下記の方法によって
行った。フィルムあるいはペレット10mgを、毎分300cm3
の窒素気流中、300℃で溶融し、直ちに液体窒素中で急
冷する。この急冷サンプルを示差走査型熱量計(理学電
器社製、DSC8230型)にセットし、毎分100ccの窒素気流
中、毎分10℃の昇温速度で昇温し、TgおよびTmを検出
する。Tgはベースラインが偏奇し始める温度と、新た
にベースラインに戻る温度との平均値、Tmはその吸熱
ピークのピーク温度とした。なお、測定開始温度は、測
定されるTgより50℃以上低い温度とする。The Tg and Tm were measured by the following method. 10 mg film or pellet, 300 cm 3 per minute
Melt at 300 ° C in nitrogen stream and immediately quench in liquid nitrogen. This quenched sample is set in a differential scanning calorimeter (DSC8230, manufactured by Rigaku Denki Co., Ltd.), and the temperature is raised at a rate of 10 ° C./min in a nitrogen stream of 100 cc / min to detect Tg and Tm. Tg is the average value of the temperature at which the baseline starts to become eccentric and the temperature at which the baseline newly returns, and Tm is the peak temperature of the endothermic peak. The measurement start temperature is a temperature lower than the measured Tg by 50 ° C. or more.
【0121】本発明のポリエステルフィルムの厚みは特
に限定がある訳ではないが、その使用目的に応じて必要
な強度を有する様に設定すればよい。特にハロゲン化銀
写真ネガ用カラー感光材料に用いられる場合は、20〜12
5μm、特に40〜90μmであることが好ましい。また、医
用や印刷用写真感光材料に用いられる場合は、50〜200
μm、特に60〜180μmであることが好ましい。The thickness of the polyester film of the present invention is not particularly limited, but may be set so as to have a necessary strength depending on the purpose of use. Especially when used in a color light-sensitive material for a silver halide photographic negative,
It is preferably 5 μm, particularly 40 to 90 μm. When used in medical and printing photographic light-sensitive materials, 50 to 200
It is preferably μm, particularly 60 to 180 μm.
【0122】本発明のポリエステルフィルムは、写真感
度を見かけ上低下させるへーズはネガからの焼き付け時
間が長くなることが懸念されるため、また焼き付けた画
像がぼけてしまい不鮮明になる場合もあるため、写真用
支持体のヘーズが3%以下であることが好ましい。更に
好ましくは1%以下である。上記ヘーズは、ASTM-D1003
-52に従って測定したものである。In the polyester film of the present invention, the haze that apparently lowers the photographic sensitivity may increase the baking time from the negative, and the baked image may be blurred and unclear. The haze of the photographic support is preferably 3% or less. More preferably, it is 1% or less. The haze is based on ASTM-D1003
Measured according to -52.
【0123】次に、ハロゲン化銀写真感光材料の感光層
を写真用支持体の上に形成させる方法について説明す
る。Next, a method for forming a light-sensitive layer of a silver halide photographic light-sensitive material on a photographic support will be described.
【0124】本発明に係わるハロゲン化銀感光材料に用
いられるハロゲン化銀乳剤のハロゲン化銀粒子その他の
添加剤、例えば化学増感剤、分光増感色素、硬膜剤、界
面活性剤、カラーカプラー等に関しては特に制限はな
く、例えばリサーチ・ディスクロージャー(Research D
isclosure)No.308119(以下、RD308119と略す)に記載
されているものを用いることができる。記載箇所を以下
に示す。Silver halide grains and other additives of the silver halide emulsion used in the silver halide light-sensitive material according to the present invention, for example, chemical sensitizers, spectral sensitizing dyes, hardeners, surfactants, color couplers. There are no particular restrictions on the items such as Research Disclosure (Research D
isclosure) No. 308119 (hereinafter abbreviated as RD308119) can be used. The description location is shown below.
【0125】 〔項目〕 〔RD308119の頁〕 ヨード組成 993 I−A 項 製造方法 〃 〃 及び994 E項 晶癖 正常晶 〃 〃 双晶 〃 〃 エピタキシャル 〃 〃 ハロゲン組成 一様 993 I−B項 一様でない 〃 〃 ハロゲンコンバージョン 993 I−C項 ハロゲン置換 〃 〃 金属含有 993 I−D項 単分散 995 I−F項 溶剤添加 〃 〃 潜像形成位置 表面 995 I−G項 内面 〃 〃 適用感光材料 ネガ 995 I−H項 ポジ(内部カブリ粒子含) 〃 〃 乳剤を混合している 995 I−J項 脱塩 995 II−A項 ハロゲン化銀乳剤には、物理熟成、化学熟成及び分光増
感を行ったものを使用する。このような工程で使用され
る添加剤は、リサーチ・ディスクロージャーNo.17643、
同No.l8716及び同No.308119(それぞれ、以下RDl7643、
RDl8716及びRD308119と略す)に記載されている。記載
箇所を以下に示す。[Item] [Page of RD308119] Iodine composition 993 IA Item Manufacturing method 〃 and 994 E Item Crystal habit Normal crystal 〃 Twin crystal 〃 〃 Epitaxial 〃 〃 Halogen composition Uniform 993 IB Item uniform Not 〃 Halogen conversion 993 I-C item Halogen substitution 〃 Metal-containing 993 I-D item Monodisperse 995 I-F item Solvent addition 〃 Latent image forming surface 995 I-G inner surface 〃 Applied photosensitive material Negative 995 Item IH Positive (including internal fog grains) 〃 〃 Mixed emulsion 995 IJ Item Desalting 995 II-A Item The silver halide emulsion was subjected to physical ripening, chemical ripening and spectral sensitization. Use one. Additives used in such processes, Research Disclosure No. 17643,
Same No. l8716 and same No. 308119 (hereinafter referred to as RDl7643,
(Abbreviated as RDl 8716 and RD308119). The description location is shown below.
【0126】 〔項目〕 〔RD308119の頁〕 〔RD17643〕 〔RD18716〕 化学増感剤 996 III−A項 23 648 分光増感剤 996 IV−A,B,C,D, 23〜24 648〜9 E〜J項 強色増感剤 996 IV−A〜E,J項 23〜24 648〜9 かぶり防止剤 998 VI 24〜25 649 安定剤 998 VI 24〜25 649 使用できる写真用添加剤も上記RDに記載されている。
記載箇所を以下に示す 〔項目〕 〔RD308119の頁〕 〔RD17643〕 〔RD18716〕 色濁り防止剤 1002 VII−I項 25 650 色素画像安定剤 1001 VII−J項 25 増白剤 998 V 24 紫外線吸収剤 1003 VIII−C項 25〜26 XIII−C項 光吸収剤 1003 VIII 25〜26 光散乱剤 1003 VIII フィルタ染料 1003 VIII 25〜26 バインダー 1003 IX 26 651 帯電防止剤 1006 XIII 27 650 硬膜剤 1004 X 26 651 可塑剤 1006 XII 27 650 潤滑剤 1006 XII 27 650 活性剤・塗布助剤 1005 XI 26〜27 650 マット剤 1007 XVI 現像剤 1011 XX-B項 (感材中に含有) また、種々のカプラーを使用することができ、その具体
例も上記RDに記載されている。関連ある記載箇所を下記
に示す。[Item] [Page of RD308119] [RD17643] [RD18716] Chemical sensitizer 996 III-A 23 648 Spectral sensitizer 996 IV-A, B, C, D, 23-24 648-9 E ~ J Item Supersensitizer 996 IV-A ~ E, J item 23 ~ 24 648 ~ 9 Antifoggant 998 VI 24 ~ 25 649 Stabilizer 998 VI 24 ~ 25 649 The photographic additives that can be used are also in the above RD. Has been described.
Descriptions are shown below [Item] [Page of RD308119] [RD17643] [RD18716] Color turbidity inhibitor 1002 VII-I 25 650 Dye image stabilizer 1001 VII-J 25 Whitening agent 998 V 24 UV absorber 1003 VIII-C 25-26 XIII-C Light absorber 1003 VIII 25-26 Light scattering agent 1003 VIII Filter dye 1003 VIII 25-26 Binder 1003 IX 26 651 Antistatic agent 1006 XIII 27 650 Hardener 1004 X 26 651 Plasticizer 1006 XII 27 650 Lubricant 1006 XII 27 650 Activator / Coating aid 1005 XI 26 to 27 650 Matting agent 1007 XVI Developer 1011 XX-B (included in the photosensitive material) Also use various couplers And specific examples thereof are also described in the above RD. The relevant description is shown below.
【0127】 〔項目〕 〔RD308119の頁〕 〔RD17643〕 イエローカプラー 1001 VII−D項 25 VII−C〜G項 マゼンタカプラー 1001 VII−D項 25 VII−C〜G項 シアンカプラー 1001 VII−D項 25 VII−C〜G項 カラードカプラー 1002 VII−G項 25 VII−G項 DIRカプラー 1001 VII−F項 25 VII−F項 BARカプラー 1002 VII−F項 その他の 1001 VII−F項 有用残基放出 カプラー アルカリ可溶性 1001 VII−E項 カプラー 使用する添加剤はRD308119XIVに記載されている分散法
などにより添加することができる。[Items] [Page of RD308119] [RD17643] Yellow coupler 1001 VII-D item 25 VII-C to G magenta coupler 1001 VII-D item 25 VII-C to G cyan coupler 1001 VII-D item 25 VII-C to G Colored coupler 1002 VII-G 25 VII-G DIR coupler 1001 VII-F 25 VII-F BAR coupler 1002 VII-F Other 1001 VII-F useful residue releasing coupler Alkali Soluble 1001 VII-E coupler The additives used can be added by the dispersion method described in RD308119XIV.
【0128】カラー感光材料には前述のRD308119 VII-
K項に記載されているフィルター層や中間層などの補助
層を設けることができる。また前述のRD308119 VII-K
項に記載されている順層、逆層、ユニット構成などの様
々な層構成をとることができる。For the color light-sensitive material, the above-mentioned RD308119 VII-
An auxiliary layer such as a filter layer or an intermediate layer described in the section K can be provided. Also, the aforementioned RD308119 VII-K
Various layer configurations such as the forward layer, the reverse layer, and the unit configuration described in the section can be adopted.
【0129】この発明の写真フィルムを現像処理するに
は、例えばT.H.ジェームズ著、セオリイ・オブ・ザ
・ホトグラフィック・プロセス第4版(The Theory of
ThePhotographic Process Forth Edition)第291頁〜第
334頁、およびジャーナル・オブ・ザ・アメリカン・ケ
ミカル・ソサエティ(JournaI of the American Chemic
al Society)第73巻、第3,100頁(1951)に記載されて
いる公知の現像剤を使用することができる。また、カラ
ー写真感光材料は前述のRD17643の28〜29頁、RDl8716の
615頁及びRD308119のXIXに記載されている通常の方法に
よって、現像処理することができる。To process the photographic film of the present invention, for example, T.I. H. James, The Theory of The Photographic Process 4th Edition
ThePhotographic Process Forth Edition) Page 291 ~
Page 334, and the Journal of the American Chemic
Al Society), Vol. 73, page 3,100 (1951), known developers can be used. Color photographic light-sensitive materials are described in RD17643, pages 28-29, RDl8716.
The development can be carried out by a usual method described on page 615 and XIX of RD308119.
【0130】ハロゲン化銀写真感光材料はカラーフィル
ム、カラー用印画紙、印刷用フィルム等のようにほとん
どが感光層が片面にあるものであるが、医療用フィルム
のように両面に感光層があるものもある。片面感光層の
フィルムには一般にバック層がその裏側に設けられてい
る。バック層としては、帯電防止層、ハレーション防止
層、イラジエーション防止層、磁気記録層等がある。ハ
レーション防止層やイラジエーション防止層には一般に
染料を含むゼラチン層からなっている。帯電防止層には
帯電防止剤を含みゼラチン層あるいは帯電防止剤自身が
層を形成するものもある。Most silver halide photographic light-sensitive materials have a light-sensitive layer on one side like color films, color photographic papers, printing films, etc., but have a light-sensitive layer on both sides like a medical film. There are also things. A backside layer is generally provided on the back side of a film having a single-sided photosensitive layer. Examples of the back layer include an antistatic layer, an antihalation layer, an irradiation prevention layer, a magnetic recording layer and the like. The antihalation layer and the irradiation prevention layer are generally gelatin layers containing a dye. In some antistatic layers, an antistatic agent is included and a gelatin layer or the antistatic agent itself forms a layer.
【0131】〈バック層〉支持体の片面に感光層がある
感光材料の感光層のない反対側に設けられる層をバック
層という。ハロゲン化銀感光材料の種類によってバック
層が設けられる。バック層には親水性ポリマーバインダ
ーが用いられる場合が多いが、感光層のバインダーと同
様なゼラチンが最も好ましく使用され、アルカリ処理オ
セインゼラチン、酸処理オセインゼラチン、酸処理ピッ
グスキンゼラチン、フタル化ゼラチン等のゼラチン誘導
体等のいろいろなゼラチンが使用される。必要に応じて
このゼラチンバック層に他の親水性ポリマー、マット
剤、滑り剤、界面活性剤、硬膜剤、染料、増粘剤、ポリ
マーラテックス、前記帯電防止剤等を添加することがで
きる。<Back Layer> A layer provided on the opposite side of a photosensitive material having a photosensitive layer on one side of a support without the photosensitive layer is called a back layer. A back layer is provided depending on the type of silver halide light-sensitive material. A hydrophilic polymer binder is often used for the back layer, but gelatin similar to the binder for the photosensitive layer is most preferably used. Alkali-treated ossein gelatin, acid-treated ossein gelatin, acid-treated pigskin gelatin, phthalated Various gelatins such as gelatin derivatives such as gelatin are used. If necessary, other hydrophilic polymers, matting agents, slip agents, surfactants, hardeners, dyes, thickeners, polymer latices, the above antistatic agents and the like can be added to the gelatin back layer.
【0132】《帯電防止層》本発明の写真用支持体を用
いたハロゲン化銀写真感光材料に有用な帯電防止層に
は、一般にハロゲン化銀写真感光材料に用いられている
帯電防止剤、帯電防止組成物のほとんどを用いることが
できる。そのうち、特に、特公昭48-23451号記載のスチ
レンスルホン酸ナトリウムの共重合体、 特開昭53-82876
号記載のビニルベンジルスルホン酸ナトリウムの共重合
物等のアルカリ金属スルホン酸型アニオン高分子帯電防
止剤、特開昭54-159222号、その他に記載のトリエチレ
ンジアミンとキシリデンジクロライド等のジハライドよ
りなる重合体を代表とするアイオネン重合体、トリエチ
レンジアミン等のジアミンとキシリデンジクロライド等
のジハライドよりなる縮合物あるいはアイオネン重合体
がビニル共重合体の架橋剤の役目をしているアイオネン
架橋型共重合体粒子、同記載のトリエチレンジアミン等
のジアミンとキシリデンジクロライド等のジハライドよ
りなる縮合物あるいは重合体が架橋型ビニル共重合体の
側鎖に結合しているアイオネン側鎖ペンダント型架橋共
重合体粒子等の第4級トリエチレンジアミンを構成要素
とするカチオン型アイオネン高分子帯電防止剤、特公昭
60-51693号記載のベンジルトリアルキルアンモニウムク
ロライド基を側鎖に持つ架橋型共重合体粒子等の第4級
ベンジルアミンカチオン型高分子帯電防止剤、特開昭57
-104931号記載のSnO2、TiO2、ZnO、In2O3、SiO2、Mo
O3、WO3の金属酸化物及び/又はこれらの金属複合酸化物
を主体とする結晶性金属酸化物微粉末帯電防止剤、特公
昭57-12979号記載のアルミナゾル組成物、特開平2-2527
26号、同2-255770号、同2-308246号、同2-304554号、欧
州特許0602713A1号、その他等に記載のπ電子系導電性
ポリマー帯電防止剤、例えばポリイソチアナフテン及び
その誘導体、ポリチオフェン及びその誘導体、ポリピロ
ール及びその誘導体、ポリアニリン及びその誘導体、ポ
リチオフェン、ポリピロール又はポリアニリンを側鎖に
持つ分岐状ポリマー、ポリフェニレンビニレン及びその
誘導体、ポリチオフェンビニレン及びその誘導体等が有
用である。<Antistatic Layer> An antistatic layer useful in a silver halide photographic light-sensitive material using the photographic support of the present invention includes an antistatic agent generally used in a silver halide photographic light-sensitive material, an electrostatic charge. Most of the prevention compositions can be used. Among them, particularly, a copolymer of sodium styrenesulfonate described in JP-B-48-23451, JP-A-53-82876.
Alkali metal sulfonic acid type anionic polymer antistatic agents such as copolymers of sodium vinylbenzyl sulfonate described in JP-A No. 54-159222, and diethylene compounds such as triethylenediamine and dihalide such as xylidene dichloride described in JP-A-54-159222. Ionene polymer represented by coalescence, ionene cross-linked copolymer particles in which a condensate composed of diamine such as triethylenediamine and dihalide such as xylidene dichloride or the ionene polymer serves as a cross-linking agent for vinyl copolymer. The ionene side chain pendant type crosslinked copolymer particles in which a condensate or a polymer consisting of a diamine such as triethylenediamine and a dihalide such as xylidene dichloride is bonded to a side chain of the crosslinked vinyl copolymer. Cationic eye containing quaternary triethylenediamine as a constituent element Nene polymer antistatic agent, JP-B
Quaternary benzylamine cationic polymer antistatic agents such as cross-linked copolymer particles having a benzyltrialkylammonium chloride group as a side chain described in JP-A-60-51693;
-104931 No. SnO 2 , TiO 2 , ZnO, In 2 O 3 , SiO 2 , Mo
O 3 , a crystalline metal oxide fine powder antistatic agent mainly composed of WO 3 metal oxide and / or a metal composite oxide thereof, an alumina sol composition described in JP-B-57-12979, JP-A-2-2527
No. 26, No. 2-255770, No. 2-308246, No. 2-304554, European Patent 0602713A1, and other π-electron conductive polymer antistatic agents described in, for example, polyisothianaphthene and its derivatives, Polythiophene and its derivatives, polypyrrole and its derivatives, polyaniline and its derivatives, polythiophene, branched polymers having polypyrrole or polyaniline in the side chain, polyphenylene vinylene and its derivatives, polythiophene vinylene and its derivatives, etc. are useful.
【0133】《磁気記録層》必要に応じて、ハロゲン化
銀写真感光材料に下記の目的で、磁気記録材料を感光層
の上層面に、あるいはバック層の上層面に塗布してもよ
い。<Magnetic Recording Layer> If necessary, the silver halide photographic light-sensitive material may be coated with a magnetic recording material on the upper surface of the photosensitive layer or on the upper surface of the back layer for the following purposes.
【0134】例えば、画像部の横の乳剤面またはバック
面に、強磁性体の微粒子を分散したストライプ状の磁気
記録層を設け、音声や撮影時の条件などの情報を記録す
ることが、特開昭50-62627号公報、同49-4503号公報、
米国特許第3,243,376号明細書、同3,220,843号明細書な
どに記載され、また、写真感光材料のバック面に、磁性
体粒子の量、サイズなどを選択して必要な透明性を得た
透明磁気記録層を設けることが、米国特許第3,782,947
号明細書、同4,279,945号明細書、同4,302,523号明細書
などに記載されている。また、米国特許第4,947,196号
明細書、WO90/04254号には写真フィルムの裏面に磁
気記録を可能とする磁性体を含有した磁気記録層を有す
るロール状フィルムと共に磁気ヘッドを有する撮影用カ
メラが記載されている。For example, a stripe-shaped magnetic recording layer in which ferromagnetic fine particles are dispersed is provided on the emulsion surface or the back surface next to the image area to record information such as voice and shooting conditions. KAISHO 50-62627 publication, JP 49-4503 publication,
U.S. Pat. Nos. 3,243,376 and 3,220,843, etc., and a transparent magnetic recording on the back surface of a photographic light-sensitive material with the required transparency by selecting the amount and size of magnetic particles. Providing layers is described in U.S. Pat. No. 3,782,947.
No. 4,279,945, No. 4,302,523, and the like. Also, US Pat. No. 4,947,196 and WO90 / 04254 describe a photographing camera having a magnetic head together with a roll-shaped film having a magnetic recording layer containing a magnetic material that enables magnetic recording on the back surface of the photographic film. Has been done.
【0135】このように、ハロゲン化銀写真感光材料
に、例えば、写真感光材料の種類・製造番号、メーカー
名、乳剤 No.などの写真感光材料に関する各種の情
報、例えば、撮影日・時、絞り、露出時間、照明の条
件、使用フィルター、天候、撮影枠の大きさ、撮影機の
機種、アナモルフィックレンズの使用などのカメラ撮影
時の各種の情報、例えば、プリント枚数、フィルターの
選択、顧客の色の好み、トリミング枠の大きさなどのプ
リント時に必要な各種の情報、例えば、プリント枚数、
フィルターの選択、顧客の色の好み、トリミング枠の大
きさなどのプリント時に得られた各種の情報、その他顧
客情報などを入力しておくことは、管理の上からも、ま
た、プリント品質の向上、プリント作業の効率化の上か
ら上記の事柄が記録されると便利である。As described above, in the silver halide photographic light-sensitive material, various information on the photographic light-sensitive material such as the type / manufacturing number of the photographic light-sensitive material, the manufacturer name, the emulsion No. , Exposure time, lighting conditions, filter used, weather, size of shooting frame, camera model, use of anamorphic lens, and other various information at the time of camera shooting, for example, number of prints, selection of filter, customer Various information necessary for printing, such as the color preference and trimming frame size, for example, the number of prints,
Entering various information obtained at the time of printing such as filter selection, customer's color preference, trimming frame size, and other customer information is important for management and print quality improvement. It is convenient if the above-mentioned matters are recorded in order to improve the efficiency of printing work.
【0136】従来の写真感光材料においては、これら全
ての情報を入力することは不可能であって、わずかに、
撮影時に、撮影日・時、絞り、露出時間などの情報を光
学的に入力していたにすぎなかった。しかも、プリント
時においては、上記情報を写真感光材料へ入力すること
は、その手段がなく全く不可能であった。In the conventional photographic light-sensitive material, it is impossible to input all the information, and
At the time of shooting, I was only optically entering information such as the shooting date / time, aperture, and exposure time. Moreover, at the time of printing, it was completely impossible to input the above information into the photographic light-sensitive material because there was no means for that.
【0137】磁気記録方式は記録/再生が容易であると
ころから、写真感光材料へ上記各種の情報を入力するた
めに磁気記録方式を使用することが研究され、各種技術
が上記の如く提案されている。Since the magnetic recording system is easy to record / reproduce, the use of the magnetic recording system for inputting the above various information to the photographic light-sensitive material has been studied and various techniques have been proposed as described above. There is.
【0138】これらの磁気記録層を設けることによっ
て、従来困難であった上記各種の情報を写真感光材料中
に記録することが可能となり、さらに、音声や画像信号
をも記録できるという将来性を有している。By providing these magnetic recording layers, it becomes possible to record the above-mentioned various kinds of information in the photographic light-sensitive material, which has been difficult in the past, and further, it is possible to record voice and image signals. are doing.
【0139】磁気記録層に用いられる磁性体微粉末とし
ては、金属磁性体粉末、酸化鉄磁性体粉末、Co被着酸
化鉄磁性体粉末、二酸化クロム磁性体粉末、バリュウム
フェライト磁性体粉末などが使用できる。As the magnetic fine powder used in the magnetic recording layer, metal magnetic powder, iron oxide magnetic powder, Co-adhered iron oxide magnetic powder, chromium dioxide magnetic powder, barium ferrite magnetic powder, etc. are used. it can.
【0140】透明磁気記録層を感光層側に設ける場合に
は、磁気記録材料のバインダーとしては、ゼラチンの如
き親水性バインダーが用いられる。親水性バインダーの
場合にはゼラチンを用いるのが好ましい。感光層のない
バック側に磁気記録層を設ける場合には、セルロースナ
イトレートの如き疎水性の溶剤可溶バインダーが用いら
れる。When the transparent magnetic recording layer is provided on the photosensitive layer side, a hydrophilic binder such as gelatin is used as the binder of the magnetic recording material. In the case of a hydrophilic binder, gelatin is preferably used. When the magnetic recording layer is provided on the back side without the photosensitive layer, a hydrophobic solvent-soluble binder such as cellulose nitrate is used.
【0141】[0141]
【実施例】以下、実施例により本発明をさらに具体的に
詳述するが、下記実施例に限定されるものではない。The present invention will be described in more detail below with reference to examples, but the invention is not limited to the examples.
【0142】〔実施例1〕 〈写真用支持体の作製〉 《ポリエチレン-2,6-ナフタレート樹脂チップの作製》
2,6-ナフタレンジカルボン酸ジメチル100重量部、エチ
レングリコール60重量部にエステル交換触媒として酢酸
カルシウム水和物0.1重量部を添加し、常法に従ってエ
ステル交換反応を行った。得られた生成物に、三酸化ア
ンチモン0.05重量部、リン酸トリメチルエステル0.03重
量部を添加した。次いで、徐々に昇温、減圧にし、290
℃、0.5mmHgで重合を行い、固有粘度0.60のポリエチレ
ン-2-6-ナフタレート樹脂を得た。この樹脂の一部を着
色用のチップとするために、合成されたポリエチレン-
2,6-ナフタレート樹脂チップにバイエル社製染料マクロ
レックスグリーンG、マクロレックスレッド5Bを1:
1の割合で添加し、押出し機を用いて染料濃度が2000pp
mの着色マスター樹脂ペレットを作製した。Example 1 <Preparation of Photographic Support><< Preparation of Polyethylene-2,6-Naphthalate Resin Chip >>
To 100 parts by weight of dimethyl 2,6-naphthalenedicarboxylate and 60 parts by weight of ethylene glycol, 0.1 part by weight of calcium acetate hydrate as an ester exchange catalyst was added, and transesterification reaction was carried out according to a conventional method. Antimony trioxide (0.05 parts by weight) and phosphoric acid trimethyl ester (0.03 parts by weight) were added to the obtained product. Then, gradually raise the temperature and reduce the pressure to 290
Polymerization was carried out at 0.5 ° C. and 0.5 mmHg to obtain a polyethylene-2-6-naphthalate resin having an intrinsic viscosity of 0.60. Polyethylene synthesized to make a part of this resin into chips for coloring-
Bayer Dye Macrolex Green G, Macrolex Red 5B 1: 2,6-naphthalate resin chip 1:
It was added at a ratio of 1 and the dye concentration was 2000pp using an extruder.
m colored master resin pellets were prepared.
【0143】《ポリエチレン-2,6-ナフタレートフィル
ムの作製》上記ポリエチレン-2,6-ナフタレート樹脂と
着色マスター樹脂ペレットを重量比9:1の割合になる
ようにタンブラー型混合機でブレンドした。この後、15
0℃で8時間真空乾燥した後、300℃でTダイから層状に
溶融押出し、50℃の冷却ドラム上に静電印加しながら密
着させ、冷却固化させ,未延伸シートを得た。この未延
伸シートをロール式縦延伸機を用いて、135℃で縦方向
に3.3倍延伸した。得られた一軸延伸フィルムをテンタ
ー式横延伸機を用いて、第一延伸ゾーン145℃で総横延
伸倍率の50%延伸し、さらに第二延伸ゾーン155℃で総
横延伸倍率3.3倍となるように延伸した。次いで、100℃
で2秒間熱処理し、さらに第一熱固定ゾーン200℃で5
秒間熱固定し、第二熱固定ゾーン230℃で15秒間熱固定
した。次いで横方向に5%弛緩処理しながら室温まで60
秒かけて冷却し、フィルムをクリップから解放し、巻き
取り、厚さ90μmの二軸延伸フィルムを得た。これとは
別に着色マスターチップを混合しないで、ポリエチレン
-2,6-ナフタレート樹脂のみを同様に無色のフィルムを
製膜した。フィルムのヘーズをASTMD-1003-52に従い測
定した。<< Preparation of Polyethylene-2,6-Naphthalate Film >> The polyethylene-2,6-naphthalate resin and the colored master resin pellets were blended in a tumbler type mixer in a weight ratio of 9: 1. After this, 15
After vacuum-drying at 0 ° C. for 8 hours, the mixture was melt-extruded in layers from a T die at 300 ° C., adhered onto a cooling drum at 50 ° C. while electrostatically applied, and solidified by cooling to obtain an unstretched sheet. This unstretched sheet was stretched 3.3 times in the longitudinal direction at 135 ° C. using a roll type longitudinal stretching machine. Using a tenter type transverse stretching machine, the obtained uniaxially stretched film is stretched by 50% of the total transverse stretching ratio in the first stretching zone 145 ° C, and further in the second stretching zone 155 ° C so that the total transverse stretching ratio is 3.3 times. Was stretched. Then 100 ° C
Heat treatment for 2 seconds at 5 ℃ at the first heat setting zone at 200 ℃
Heat setting was performed for 2 seconds, and heat setting was performed for 15 seconds at the second heat setting zone of 230 ° C. Then, while performing a 5% relaxation treatment in the lateral direction, bring it to room temperature 60
After cooling for 2 seconds, the film was released from the clip and wound to obtain a biaxially stretched film having a thickness of 90 μm. Separately, do not mix the colored master chips
A colorless film was formed in the same manner using only -2,6-naphthalate resin. The haze of the film was measured according to ASTM D-1003-52.
【0144】〈紫外線照射〉別のラインに紫外線照射装
置を下記の如く設置した。千鳥状に配置されたロールを
複数持つフィルム搬送装置に全長25mにわたって、石英
管紫外線ランプをロールに平行にフィルムより15cmの距
離に所定の本数を配置した。フィルムの温度を25℃(比
較−1の場合には115℃)になるように予めフィルムを
加熱しておき、フィルムを上記装置に通し、フィルムの
搬送速度を調節することによって照射時間を変化させて
紫外線照射処理を行ったた。照射時間については表1に
示した。照射条件はポリエチレン-2,6-ナフタレートフ
ィルムの両面に照射強度100mW/cm2の石英管水銀ランプ
(主要ピーク253.7nm)を空気中で紫外線照射処理を行っ
た。紫外線照射処理済みフィルムのIR吸収強度比、ヘ
ーズを表2に示した。<Ultraviolet irradiation> An ultraviolet irradiation device was installed on another line as follows. A quartz tube ultraviolet lamp was placed in a predetermined number at a distance of 15 cm from the film in parallel with the roll over a length of 25 m in a film transport device having a plurality of rolls arranged in a staggered pattern. The film is heated in advance so that the temperature of the film becomes 25 ° C (115 ° C in the case of Comparative-1), the film is passed through the above-mentioned device, and the irradiation time is changed by adjusting the transport speed of the film. UV irradiation treatment was performed. The irradiation time is shown in Table 1. The irradiation conditions were such that both sides of the polyethylene-2,6-naphthalate film were subjected to ultraviolet irradiation treatment in the air with a quartz tube mercury lamp (main peak 253.7 nm) having an irradiation intensity of 100 mW / cm 2 . Table 2 shows the IR absorption intensity ratio and haze of the UV-irradiated film.
【0145】〈下引層塗布〉次いで、紫外線照射処理を
施したフィルム面に、下記の下引塗布液(a-1)を10m
l/m2の量塗布し、115℃で1分間乾燥し下引層(A-
1)を形成した。<Application of Undercoat Layer> Next, 10 m of the following undercoat coating solution (a-1) was applied to the surface of the film which had been subjected to the ultraviolet irradiation treatment.
l / m 2 applied and dried at 115 ° C for 1 minute, then the undercoat layer (A-
1) was formed.
【0146】 《感光層側の下引液(a-1)の調製》 P−2(固形分30%) 270g 化合物(UL−1) 0.8g ヘキサメチレン-1,6-ビスエチレンウレア 0.6g 水で1リットルに仕上げる。次いで、上記下引層面(A
-1)に8W/m2・minのコロナ放電処理を施し、下記の上
層塗布液(a-2)を乾燥後の厚みとして0.1μmになる
ように塗布し、110℃で乾燥し、上層(A-2)を形成し
た。<< Preparation of Undercoat Liquid (a-1) on Photosensitive Layer Side} P-2 (solid content 30%) 270 g Compound (UL-1) 0.8 g Hexamethylene-1,6-bisethyleneurea 0.6 g Water To 1 liter. Then, the undercoat layer surface (A
-1) was subjected to a corona discharge treatment of 8 W / m 2 · min, and the following upper layer coating solution (a-2) was applied to a dry thickness of 0.1 μm and dried at 110 ° C. A-2) was formed.
【0147】 《上層塗布液(a-2)》 ゼラチン 10g 化合物(UL−1) 0.2g 化合物(UL−2) 0.2g N,N′,N″-トリスアクリロイル-1,3,5-トリメチレントリアミン 0.1g シリカ粒子(平均粒径:3μm) 0.1g 水で1リットルに仕上げる。<< Upper Layer Coating Liquid (a-2) >> Gelatin 10 g Compound (UL-1) 0.2 g Compound (UL-2) 0.2 g N, N ′, N ″ -trisacryloyl-1,3,5-trimethylene Triamine 0.1 g Silica particles (average particle diameter: 3 μm) 0.1 g Water is made up to 1 liter.
【0148】 《バック層側の下引液(b-1)の調製》 P−1(固形分30%) 270g 化合物(UL−1) 0.8g ヘキサメチレン-1,6-ビスエチレンウレア 0.6g 水で1リットルに仕上げる。<< Preparation of Subbing Liquid (b-1) on Back Layer Side} P-1 (solid content 30%) 270 g Compound (UL-1) 0.8 g Hexamethylene-1,6-bisethyleneurea 0.6 g Water To 1 liter.
【0149】次いで、上記下引層面(B-1)に8W/m2・
minのコロナ放電処理を施し、塗布液(b-2)を乾燥後
の厚みとして0.1μmになるように塗布し、110℃で乾燥
し、上層(B-2)を形成した。Then, on the undercoat layer surface (B-1), 8 W / m 2 ·
The coating solution (b-2) was applied so that the thickness after drying was 0.1 μm, and dried at 110 ° C. to form the upper layer (B-2).
【0150】[0150]
【化12】 [Chemical 12]
【0151】《帯電防止層(B-2)の塗設》上記下引
層面(B-1)に8W/m2・minのコロナ放電処理を施し、
下記金属酸化物複合体帯電防止塗布液(b-2)を乾燥
後の厚みとして0.1μmになるように塗布し、110℃で乾
燥し、帯電防止層(B-2)を形成した。更にB-2の上
に上層液(b-3)を塗布し、110℃で乾燥し、上層(B
-3)を形成した。<< Coating of Antistatic Layer (B-2) >> The undercoat layer surface (B-1) was subjected to a corona discharge treatment of 8 W / m 2 · min,
The following metal oxide complex antistatic coating liquid (b-2) was applied so that the thickness after drying would be 0.1 μm, and dried at 110 ° C. to form an antistatic layer (B-2). Further, the upper layer liquid (b-3) is applied on B-2 and dried at 110 ° C. to form the upper layer (B
-3) was formed.
【0152】A−2及びB−3の上に下記感光層及び下
記磁気記録層を形成し、ハロゲン化銀カラー用写真感光
材料を作製した。The following photosensitive layer and magnetic recording layer were formed on A-2 and B-3 to prepare a photographic light-sensitive material for silver halide color.
【0153】《金属酸化物複合体微粒子導電性帯電防止
剤の作製》塩化第二錫230重量部、三酸化アンチモン23
重量部、をエタノール3,000重量部に溶解し均一溶液を
得た。この溶液に1Nの水酸化ナトリウム水溶液を上記
溶液のpHが3、になるまで滴下し、コロイド状態酸化第
二錫と酸化アンチモンの共沈殿を得た。得られた共沈殿
を50℃に24時間放置し、赤褐色のコロイド状沈殿を得
た。赤褐色コロイド状沈殿を遠心分離により分離した。
過剰なイオンを除くため沈殿に水を加え遠心分離によっ
て水洗した。この操作を3回繰り返し過剰イオンを除去
した。過剰イオンを除去したコロイド状沈殿200重量部
を1,500重量部に分散し、600℃に加熱した焼成炉に噴霧
し、青みがかった平均粒径0.2μmの酸化錫-酸化アンチ
モン複合体の微粒子粉末を得た。この微粒子粉末の比抵
抗は25Ω・cmであった。上記微粒子粉末40重量部と水60
重量部の混合液をpH7.0に調整し、撹拌機で粗分散の
後、横型サンドミル(商品名ダイノミル;WILLYA.BACHO
FENAG社製)で滞留時間が30分になるまで分散して調整
した。<< Preparation of Metal Oxide Complex Fine Particle Conductive Antistatic Agent >> 230 parts by weight of stannic chloride, antimony trioxide 23
Parts by weight were dissolved in 3,000 parts by weight of ethanol to obtain a uniform solution. A 1N sodium hydroxide aqueous solution was added dropwise to this solution until the pH of the above solution became 3, to obtain a coprecipitation of colloidal stannic oxide and antimony oxide. The resulting coprecipitate was left at 50 ° C. for 24 hours to obtain a reddish brown colloidal precipitate. The reddish brown colloidal precipitate was separated by centrifugation.
Water was added to the precipitate to remove excess ions, and the precipitate was washed with water by centrifugation. This operation was repeated 3 times to remove excess ions. 200 parts by weight of the colloidal precipitate from which excess ions have been removed is dispersed in 1,500 parts by weight and sprayed in a firing furnace heated to 600 ° C. to obtain a bluish tin oxide-antimony oxide composite fine particle powder with an average particle size of 0.2 μm. It was The specific resistance of this fine particle powder was 25 Ω · cm. 40 parts by weight of the fine particle powder and 60 parts of water
After adjusting the pH of the mixed solution of 7.0 parts by weight to roughly 7.0 with a stirrer, a horizontal sand mill (trade name: Dynomill; WILLYA.BACHO)
It was adjusted by dispersing with a FENAG) until the residence time reached 30 minutes.
【0154】 《帯電防止塗布液b-2》 上記金属酸化物複合体導電性粒子分散液 100重量部 ゼラチン 10重量部 水 100重量部 メタノール 600重量部 化合物(UL−1) 0.1重量部 《帯電防止上層塗布液b-3》 セルローストリアセテート 10重量部 アセトン 700重量部 メタノール 150重量部 ジクロルメタン 140重量部 《磁気記録層B-4の塗設》上記下引及び帯電防止加工
されたポリエチレン-2,6-ナフタレートのフィルムの反
感光層側のそれぞれB-3の面に下記磁気記録層塗布液
b-4を乾燥膜厚1.0μmになるように塗布し、それぞれ
磁気記録層をB-4とした。<< Antistatic Coating Liquid b-2 >> 100 parts by weight of the above-mentioned metal oxide complex conductive particle dispersion liquid 100 parts by weight gelatin 100 parts by weight water 600 parts by weight methanol 600 parts by weight 0.1 part by weight of compound (UL-1) << antistatic Upper layer coating liquid b-3 >> Cellulose triacetate 10 parts by weight Acetone 700 parts by weight Methanol 150 parts by weight Dichloromethane 140 parts by weight << Coating of magnetic recording layer B-4 >> Polyethylene coated with the above-mentioned undercoating and antistatic treatment-2,6- The following magnetic recording layer coating liquid b-4 was applied to the B-3 surface of the naphthalate film on the side opposite to the photosensitive layer so that the dry film thickness was 1.0 μm, and the magnetic recording layer was designated as B-4.
【0155】《磁気記録層塗布液b-4》カルナバワッ
クス 10重量部をトルエン150重量部で加熱溶解後冷却
し、これにシクロヘキサノン75重量部とメチルエチルケ
トン150重量部を混合した後、旭化成(株)製ニトロセル
ロースBTH-1/2 100重量部(固形分70重量%)及びCo被
着γ-Fe2O3(長軸0.8μm、Fe2+/Fe3+=0.2、Hc=600エ
ルステッド)5重量部を加え、ディゾルバーで1時間混
和し、その後サンドミルで分散し、分散液とした。<< Magnetic Recording Layer Coating Liquid b-4 >> Carnauba wax (10 parts by weight) was heated and dissolved in toluene (150 parts by weight), cooled, and then mixed with cyclohexanone (75 parts by weight) and methyl ethyl ketone (150 parts by weight). Made by Nitrocellulose BTH-1 / 2 100 parts by weight (solid content 70% by weight) and Co deposited γ-Fe 2 O 3 (major axis 0.8 μm, Fe 2+ / Fe 3+ = 0.2, Hc = 600 oersted) 5 Part by weight was added, and the mixture was mixed for 1 hour with a dissolver, and then dispersed with a sand mill to obtain a dispersion liquid.
【0156】《比較試料−1》下記比較−1下引液をフ
ィルム温度115℃で紫外線を照射した片面に下記比較−
1下引液を10cc/m2になるように塗布し、115℃で乾燥
し、A′−1とした。また紫外線照射した他の片面に下
記比較−1帯電防止層塗布液を乾燥0.3μmになるように
塗布し、115℃ で乾燥しB′−1とした。さらにこの上
に下記比較−1帯電防止上層塗布液を乾燥膜厚が0.1μm
になるように塗布し115℃で乾燥しB′−2とした。
B′−2の上に本発明と同様に上記磁気記録層b−4を
塗布し、またA′−1の上には本発明と同様に感光層を
塗設し比較用カラーフィルムとした。<Comparative Sample-1> Comparative Example 1 below-Comparative Example 1-Comparative Example 1-
1 subbing liquid was applied at 10 cc / m 2 and dried at 115 ° C. to obtain A′-1. Further, the following Comparative-1 antistatic layer coating liquid was applied to the other surface irradiated with ultraviolet rays so as to have a dryness of 0.3 μm, and dried at 115 ° C. to obtain B′-1. Furthermore, the following Comparative-1 antistatic upper layer coating solution was dried on it to give a dry film thickness of 0.1 μm.
To obtain B'-2.
The magnetic recording layer b-4 was coated on B'-2 as in the present invention, and the photosensitive layer was coated on A'-1 as in the present invention to give a comparative color film.
【0157】 《比較−1下引液》 ゼラチン 10g 水 10g 酢酸 10g メタノール 500g エチレンジクロライド 500g p-クロロフェノール 40g。Comparative-1 Subbing Solution Gelatin 10 g Water 10 g Acetic acid 10 g Methanol 500 g Ethylene dichloride 500 g p-Chlorophenol 40 g.
【0158】 《比較−1帯電防止層塗布液》 上記金属酸化物複合導電体微粒子分散液 100g ゼラチン 10g 水 100g メタノール 600g レゾルシン 20g ポリオキシエチレンノニルフェニルエーテル 0.1g。Comparative-1 Antistatic Layer Coating Liquid 100 g of the above-mentioned metal oxide composite conductor fine particle dispersion liquid 100 g gelatin 10 g water 100 g methanol 600 g resorcin 20 g polyoxyethylene nonylphenyl ether 0.1 g.
【0159】 《比較−1帯電防止層上層塗布液》 セルローストリアセテート 10g アセトン 700g メタノール 150g ジクロルメタン 100g p-クロロフェノール 40g。Comparative-1 Antistatic Layer Upper Layer Coating Liquid Cellulose triacetate 10 g Acetone 700 g Methanol 150 g Dichloromethane 100 g p-Chlorophenol 40 g.
【0160】〈ハロゲン化銀カラー写真感光材料の作
製〉 《多層カラー乳剤層等の塗設》上記加工済みのポリエチ
レン-2,6-ナフタレートフィルムのA−2、A′−1、
及びA″−2層面の上には25W/m2・minのコロナ放電
を施した後に、多層カラー写真構成層を第1層から順次
重層塗設した。<Preparation of silver halide color photographic light-sensitive material><< Coating of multi-layer color emulsion layer and the like >> A-2, A'-1, of the above-processed polyethylene-2,6-naphthalate film,
After the corona discharge of 25 W / m 2 · min was performed on the A ″ -2 layer surface, the multilayer color photographic constituent layers were sequentially applied in layers.
【0161】以下に示した写真構成層における塗布量は
ハロゲン化銀及びコロイド銀については、金属銀に換算
してg/m2単位で表した量を、又、カプラー、添加剤に
ついてはg/m2単位で表した量を、又増感色素について
は同一層内のハロゲン化銀1モル当たりのモル数で示し
た。The coating amount in the photographic constituent layers shown below is the amount expressed in g / m 2 unit in terms of metallic silver for silver halide and colloidal silver, and g / m for couplers and additives. Amounts expressed in m 2 units and, for sensitizing dyes, are expressed in moles per mole of silver halide in the same layer.
【0162】 《第1層:ハレーション防止層》 黒色コロイド銀 0.16 紫外線吸収剤(UV−1) 0.20 高沸点溶媒(OIL−1) 0.16 ゼラチン 1.60 《第2層:中間層》 化合物(SC−1) 0.14 高沸点溶媒(OIL−2) 0.17 ゼラチン 0.80 《第3層:低感度赤感性層》 沃臭化銀乳剤A 0.15 沃臭化銀乳剤B 0.35 増感色素(SD−1) 2.0×10
−4 増感色素(SD−2)
1.4×10-4 増感色素(SD−3) 1.4×10-5 増感色素(SD−4) 0.7×10-4 シアンカプラー(C−1) 0.53 カラードシアンカプラー(CC−1) 0.04 DIR化合物(Di−1) 0.025 高沸点溶媒(OIL−3) 0.48 ゼラチン 1.09 《第4層:中感度赤感性層》 沃臭化銀乳剤B 0.30 沃臭化銀乳剤C 0.34 増感色素(SD−1) 1.7×10-4 増感色素(SD−2) 0.86×10-4 増感色素(SD−3) 1.15×10-5 増感色素(SD−4) 0.86×10-4 シアンカプラー(C−1) 0.33 カラードシアンカプラー(CC−1) 0.013 DIR化合物(Di−1) 0.02 高沸点溶媒(OIL−1) 0.16 ゼラチン 0.79 《第5層:高感度赤感性層》 沃臭化銀乳剤D 0.95 増感色素(SD−1) 1.0×10-4 増感色素(SD−2) 1.0×10-4 増感色素(SD−3) 1.2×10-5 シアンカプラー(C−2) 0.14 カラードシアンカプラー(CC−1) 0.016 高沸点溶媒(OIL−1) 0.16 ゼラチン 0.79 《第6層:中間層》 化合物(SC−1)
0.09 高沸点溶媒(OIL−2) 0.11 ゼラチン 0.80 《第7層:低感度緑感性層》 沃臭化銀乳剤A 0.12 沃臭化銀乳剤B 0.38 増感色素(SD−4) 4.6×10-5 増感色素(SD−5) 4.1×10-4 マゼンタカプラー(M−1) 0.14 マゼンタカプラー(M−2) 0.14 カラードマゼンタカプラー(CM−1) 0.06 高沸点溶媒(OIL−4) 0.34 ゼラチン 0.70 《第8層:中間層》 ゼラチン 0.41 《第9層:中感度緑感性層》 沃臭化銀乳剤B 0.30 沃臭化銀乳剤C 0.34 増感色素(SD−6) 1.2×10-4 増感色素(SD−7) 1.2×10-4 増感色素(SD−8) 1.2×10-4 マゼンタカプラー(M−1) 0.04 マゼンタカプラー(M−2) 0.04 カラードマゼンタカプラー(CM−1) 0.017 DIR化合物(Di−2) 0.025 DIR化合物(Di−3) 0.002 高沸点溶媒(OIL−4) 0.12 ゼラチン 0.50 《第10層:高感度緑感性層》 沃臭化銀乳剤D 0.95 増感色素(SD−6) 7.1×10-5 増感色素(SD−7) 7.1×10-5 増感色素(SD−8) 7.1×10-5 マゼンタカプラー(M−1) 0.09 カラードマゼンタカプラー(CM−1) 0.011 高沸点溶媒(OIL−4) 0.11 ゼラチン 0.79 《第11層:イエローフィルター層》 黄色コロイド銀 0.08 化合物(SC−1) 0.15 高沸点溶媒(OIL−2) 0.19 ゼラチン 1.10 《第12層:低感度青感性層》 沃臭化銀乳剤A 0.12 沃臭化銀乳剤B 0.24 沃臭化銀乳剤C 0.12 増感色素(SD−9) 6.3×10-5 増感色素(SD−10) 1.0×10-5 イエローカプラー(Y−1) 0.50 イエローカプラー(Y−2) 0.50 DIR化合物(Di−4) 0.04 DIR化合物(Di−5) 0.02 高沸点溶媒(OIL−2) 0.42 ゼラチン 1.40 《第13層:高感度青感性層》 沃臭化銀乳剤C 0.15 増感色素(SD−9)
8.0×10-5 増感色素(SD−11) 3.1×10-5 イエローカプラー(Y−1) 0.12 高沸点溶媒(OIL−2) 0.05 ゼラチン 0.79 《第14層:第1保護層》 沃臭化銀乳剤(平均粒径0.08μm、沃化銀含有率1.0モル%) 0.40 紫外線吸収剤(UV−1) 0.065 高沸点溶媒(OIL−1) 0.07 高沸点溶媒(OIL−3) 0.07 ゼラチン 0.65 《第15層:第2保護層》 アルカリ可溶性マット剤(平均粒径2μm) 0.15 ポリメチルメタクリレート(平均粒径3μm) 0.04 滑り剤(WAX−1) 0.04 ゼラチン 0.55 尚上記組成物の他に、塗布助剤Su−1、分散助剤Su
−2、粘度調整剤、硬膜剤H−1、H−2、安定剤ST
−1、かぶり防止剤AF−1、平均分子量:10,000及び
平均分子量:1,100,000の2種のポリビニルピロリド
ン、及び防腐剤化合物(A)を添加した。<< First Layer: Antihalation Layer >> Black Colloidal Silver 0.16 Ultraviolet Absorber (UV-1) 0.20 High Boiling Solvent (OIL-1) 0.16 Gelatin 1.60 << Second Layer: Intermediate Layer >> Compound (SC-1) 0.14 High boiling point solvent (OIL-2) 0.17 Gelatin 0.80 << 3rd layer: low sensitivity red sensitive layer >> Silver iodobromide emulsion A 0.15 Silver iodobromide emulsion B 0.35 Sensitizing dye (SD-1) 2.0 × 10
-4 sensitizing dye (SD-2)
1.4 × 10 −4 Sensitizing dye (SD-3) 1.4 × 10 −5 Sensitizing dye (SD-4) 0.7 × 10 −4 Cyan coupler (C-1) 0.53 Colored cyan coupler (CC-1) 0.04 DIR compound (Di-1) 0.025 High boiling point solvent (OIL-3) 0.48 Gelatin 1.09 << Fourth layer: medium-sensitive red-sensitive layer >> Silver iodobromide emulsion B 0.30 Silver iodobromide emulsion C 0.34 Sensitizing dye (SD-1) 1.7 × 10 -4 sensitizing dye (SD-2) 0.86 × 10 -4 sensitizing dye (SD-3) 1.15 × 10 -5 sensitizing dye (SD-4) 0.86 × 10 -4 cyan coupler (C-1) ) 0.33 Colored cyan coupler (CC-1) 0.013 DIR compound (Di-1) 0.02 High boiling point solvent (OIL-1) 0.16 Gelatin 0.79 << Fifth layer: high-sensitivity red-sensitive layer >> Silver iodobromide emulsion D 0.95 Sensitized dye (SD-1) 1.0 × 10 -4 sensitizing dye (SD-2) 1.0 × 10 -4 sensitizing dye (SD-3) 1.2 × 10 -5 cyan coupler (C-2) 0.14 color Cyan coupler (CC-1) 0.016 High boiling solvent (OIL-1) 0.16 Gelatin 0.79 "Sixth Layer: Intermediate layer" Compound (SC-1)
0.09 High boiling point solvent (OIL-2) 0.11 Gelatin 0.80 << Seventh layer: low sensitivity green sensitive layer >> Silver iodobromide emulsion A 0.12 Silver iodobromide emulsion B 0.38 Sensitizing dye (SD-4) 4.6 × 10 -5 Sensitizing dye (SD-5) 4.1 × 10 -4 Magenta coupler (M-1) 0.14 Magenta coupler (M-2) 0.14 Colored magenta coupler (CM-1) 0.06 High boiling point solvent (OIL-4) 0.34 Gelatin 0.70 << Eighth layer: Intermediate layer Gelatin 0.41 <Ninth layer: Medium-sensitive green sensitive layer> Silver iodobromide emulsion B 0.30 Silver iodobromide emulsion C 0.34 Sensitizing dye (SD-6) 1.2 × 10 -4 Sensitizing dye (SD-7) 1.2 × 10 -4 Sensitizing dye (SD-8) 1.2 × 10 -4 Magenta coupler (M-1) 0.04 Magenta coupler (M-2) 0.04 Colored magenta coupler (CM-1) 0.017 DIR compound (Di-2) 0.025 DIR compound (Di-3) 0.002 High boiling point solvent (OIL-4) 0.12 Zera Emissions 0.50 "10th layer: high sensitivity green-sensitive layer" iodobromide emulsion D 0.95 Sensitizing dye (SD-6) 7.1 × 10 -5 Sensitizing dye (SD-7) 7.1 × 10 -5 sensitization Dye (SD-8) 7.1 × 10 -5 Magenta coupler (M-1) 0.09 Colored magenta coupler (CM-1) 0.011 High boiling point solvent (OIL-4) 0.11 Gelatin 0.79 << Eleventh layer: Yellow filter layer >> Yellow colloid Silver 0.08 Compound (SC-1) 0.15 High boiling point solvent (OIL-2) 0.19 Gelatin 1.10 << 12th layer: low sensitivity blue-sensitive layer >> Silver iodobromide emulsion A 0.12 Silver iodobromide emulsion B 0.24 Silver iodobromide emulsion C 0.12 Sensitizing dye (SD-9) 6.3 × 10 -5 Sensitizing dye (SD-10) 1.0 × 10 -5 Yellow coupler (Y-1) 0.50 Yellow coupler (Y-2) 0.50 DIR compound (Di-4 ) 0.04 DIR compound (Di-5) 0.02 High boiling point solvent (OIL-2) 0.42 Gelatin 1.40 << 13th layer: High Every time the blue-sensitive layer "silver iodobromide emulsion C 0.15 sensitizing dye (SD-9)
8.0 × 10 -5 Sensitizing dye (SD-11) 3.1 × 10 -5 Yellow coupler (Y-1) 0.12 High boiling point solvent (OIL-2) 0.05 Gelatin 0.79 << 14th layer: 1st protective layer >> Iodobromide Silver emulsion (average grain size 0.08 μm, silver iodide content 1.0 mol%) 0.40 UV absorber (UV-1) 0.065 High boiling point solvent (OIL-1) 0.07 High boiling point solvent (OIL-3) 0.07 Gelatin 0.65 << 15 layers: second protective layer >> Alkali-soluble matting agent (average particle size 2 μm) 0.15 Polymethylmethacrylate (average particle size 3 μm) 0.04 Sliding agent (WAX-1) 0.04 Gelatin 0.55 In addition to the above composition, coating aids Su-1, dispersion aid Su
-2, viscosity modifier, hardener H-1, H-2, stabilizer ST
-1, antifoggant AF-1, two kinds of polyvinylpyrrolidone having an average molecular weight of 10,000 and an average molecular weight of 1,100,000, and a preservative compound (A) were added.
【0163】上記試料に用いた乳剤は、下記のとおりで
ある。尚平均粒径は、立方体に換算した粒径で示した。
また、各乳剤は、金・硫黄増感を最適に施した。The emulsions used in the above samples are as follows. The average particle size is shown as a particle size converted into a cube.
Further, each emulsion was optimally subjected to gold / sulfur sensitization.
【0164】[0164]
【表1】 [Table 1]
【0165】試料はマルチスライドホッパー型コーター
にて、一回目は第1層から第8層までを、2回目はその
上に第9層から第15層までをそれぞれ同時に塗設した。
特定写真感度はISO420であった。尚試料の作成に用
いた各化合物の構造を以下に示す。The samples were simultaneously coated with a multi-slide hopper type coater at the first time from the first layer to the eighth layer, and at the second time onto the ninth layer to the fifteenth layer, respectively.
The specific photographic speed was ISO420. The structure of each compound used for the preparation of the sample is shown below.
【0166】[0166]
【化13】 [Chemical 13]
【0167】[0167]
【化14】 Embedded image
【0168】[0168]
【化15】 [Chemical 15]
【0169】[0169]
【化16】 Embedded image
【0170】[0170]
【化17】 [Chemical 17]
【0171】[0171]
【化18】 Embedded image
【0172】[0172]
【化19】 [Chemical 19]
【0173】[0173]
【化20】 Embedded image
【0174】[0174]
【化21】 [Chemical 21]
【0175】[0175]
【化22】 [Chemical formula 22]
【0176】〈現像処理〉上記カラー写真フィルム試料
の現像処理は下記の如き処方及び条件で行った。 《処理条件》 1. カラー現像 3分15秒 38.0±0.1℃ 2. 漂 白 6分30秒 38.0±3.0℃ 3. 水 洗 3分15秒 24〜41℃ 4. 定 着 6分30秒 38.0±3.0℃ 5. 水 洗 3分15秒 24〜41℃ 6. 安 定 3分15秒 38.0±3.0℃ 7. 乾 燥 50℃以下 各工程に用いる処理液組成を以下に示す。<Development Processing> The development processing of the above color photographic film sample was carried out under the following formulation and conditions. << Processing conditions >> 1. Color development 3 minutes 15 seconds 38.0 ± 0.1 ℃ 2. Bleach 6 minutes 30 seconds 38.0 ± 3.0 ℃ 3. Washing with water 3 minutes 15 seconds 24-41 ° C 4. Settling 6 minutes 30 seconds 38.0 ± 3.0 ° C 5. Washing with water 3 minutes 15 seconds 24-41 ° C 6. Stability 3 minutes 15 seconds 38.0 ± 3.0 ℃ 7. Drying 50 ° C or less The composition of the treatment liquid used in each step is shown below.
【0177】 《発色現像液処方》 4-アミノ-3-メチル-N-エチル-N-(β-ヒドロキシエチル) アニリン・硫酸塩 4.75g 無水亜硫酸ナトリウム 4.25g ヒドロキシルアミン・1/2硫酸塩 2.0g 無水炭酸カリウム 37.5g 臭化ナトリウム 1.3g ニトリロ三酢酸・ナトリウム塩(1水塩) 2.5g 水酸化カリウム 1.0g 水を加えて1リットルとする(pH=10.1)。<< Color Developer Formulation >> 4-Amino-3-methyl-N-ethyl-N- (β-hydroxyethyl) aniline / sulfate 4.75 g anhydrous sodium sulfite 4.25 g hydroxylamine / 1/2 sulfate 2.0 g Anhydrous potassium carbonate 37.5 g Sodium bromide 1.3 g Nitrilotriacetic acid sodium salt (monohydrate) 2.5 g Potassium hydroxide 1.0 g Water is added to make 1 liter (pH = 10.1).
【0178】 《漂白液処方》 エチレンジアミン四酢酸鉄(III)アンモニウム塩 100.0g エチレンジアミン四酢酸2アンモニウム塩 10.0g 臭化アンモニウム 150.0g 氷酢酸 10.0g 水を加えて1リットルとし、アンモニア水を用いてpH
6.0に調整する。<< Bleaching Solution Formulation >> Iron (III) ammonium diaminetetraacetate ammonium salt 100.0 g Ethylenediaminetetraacetic acid diammonium salt 10.0 g Ammonium bromide 150.0 g Glacial acetic acid 10.0 g Water was added to make 1 liter and pH was adjusted with ammonia water.
Adjust to 6.0.
【0179】 《定着液処方》 チオ硫酸アンモニウム 175.0g 無水亜硫酸ナトリウム 8.5g メタ亜硫酸ナトリウム 2.3g 水を加えて1リットルとし、酢酸を用いてpH6.0に調整
する。<< Fixing Solution Formulation >> Ammonium thiosulfate 175.0 g Anhydrous sodium sulfite 8.5 g Sodium metasulfite 2.3 g Water is added to make 1 liter, and pH is adjusted to 6.0 with acetic acid.
【0180】 《安定液処方》 ホルマリン(37%水溶液) 1.5ml コニダックス(コニカ(株)製) 7.5ml 水を加えて1リットルとする。<< Stabilizing Solution Formulation >> Formalin (37% aqueous solution) 1.5 ml Conidax (manufactured by Konica Corp.) 7.5 ml Water is added to make 1 liter.
【0181】〈評価方法〉 《IR吸収強度の測定》前出の方法を用いて測定し、各
波数の値を読み取り比を算出した。<Evaluation Method><< Measurement of IR Absorption Intensity >> Measurement was carried out by the method described above, and the value of each wave number was read to calculate the ratio.
【0182】《膜付き試験》作製したハロゲン化銀カラ
ーネガ用写真感光材料試料を23℃、55%RHの部屋で24
時間調湿し、試料をアルミニウム箔を黒色のポリエチレ
ンフィルムでラミネートしたバリヤ袋に入れ、40℃のオ
ーブンにて3週間加温した後、冷まし、開封して試料を
取り出し、未現像ドライ膜付き試験及び処理済みドライ
膜付き、またウエット膜付き試験を行った。なお、バリ
ヤ袋にて加温する方法は製品の有効期間中の性能を加速
的に予測するものである。<< Test with Film >> A sample of the photographic light-sensitive material for silver halide color negative thus prepared was used in a room at 23 ° C. and 55% RH for 24 hours.
After humidity conditioning, the sample was placed in a barrier bag laminated with aluminum foil with a black polyethylene film, heated in an oven at 40 ° C for 3 weeks, cooled, opened, and the sample was taken out. Undeveloped dry film test And, a test with a treated dry film and with a wet film was conducted. The method of heating with a barrier bag is for accelerating prediction of the performance of the product during its effective period.
【0183】《ドライ膜付き試験》20cm×20cmの大きさ
の未現像及び現像済みの試料の感光層面及びバック層を
水平面から45°の角度にしたカミソリで僅かにプラスチ
ックフィルム面にまで到達するように長さ30mmの傷をつ
けた。23℃、80%RHの雰囲気中に24時間調湿したのち
に傷を付けた部分を跨いで直角に、24mm幅のセロハンテ
ープ(ニチバン(株)製セロテープ、登録商標)を長さ
約50mm貼り付け角の丸いプラスチックで擦り密着させ
る。45°の傷の反対側に試料面に概ね平行にセロハンテ
ープの端を持ち急激に引っ張り引き剥がした。剥離され
た面積について膜面が剥がれた面積を調べ下記の如く評
価した。<< Test with dry film >> The photosensitive layer surface and the back layer of an undeveloped and developed sample of 20 cm × 20 cm are slightly reached to the plastic film surface with a razor having an angle of 45 ° from the horizontal plane. A 30 mm long scratch was made on. After conditioning the humidity in an atmosphere of 23 ° C and 80% RH for 24 hours, apply a cellophane tape with a width of 24 mm (cellophane tape manufactured by Nichiban Co., Ltd., a registered trademark) at a right angle across the scratched part and apply a length of about 50 mm. Rub it tightly with the rounded plastic. The end of the cellophane tape was held almost parallel to the sample surface on the side opposite to the 45 ° scratch, and was pulled and pulled off rapidly. Regarding the peeled area, the area where the film surface was peeled off was examined and evaluated as follows.
【0184】A :全く剥離されていない B :傷のところが若干剥離され、剥離面積が全面積の
10%未満が剥離された C :剥離面積が同10%以上50%未満が剥離された D :剥離面積が同50%以上80%未満が剥離された E :剥離面積が同80%以上若干残存しているぐらい剥
離された F :剥離の抵抗はほとんどなく完全に剥離された。A: Not peeled off at all B: Some scratches were peeled off, and the peeled area was the entire area.
Less than 10% peeled off C: Peeled area 10% or more and less than 50% peeled D: Peeled area 50% or more and less than 80% peeled E: Peeled area more than 80% slightly left Exfoliated as much as possible F: There was almost no resistance to exfoliation, and exfoliation was complete.
【0185】表2にドライ膜付きの結果を示した。Table 2 shows the results with a dry film.
【0186】《ウェット膜付き試験》20cm×20cmの大き
さの試料を現像処理液に前記条件でそれぞれを所定の時
間浸漬し、現像処理全時間経過後乾燥前に濡れたままの
試料をガラス台の上に乗せ、鋭利の針状のもので碁盤目
にきずを付けゴム手袋をした指先で力強く碁盤目の全面
積にわたって擦り、剥がれた面積を調べ下記の如く評価
した。<< Test with Wet Film >> Samples each having a size of 20 cm × 20 cm are immersed in a developing solution under the above-mentioned conditions for a predetermined time, and after the entire developing process has elapsed, the sample that remains wet before drying is placed on a glass table. It was rubbed over the entire area of the grid with a sharp needle-shaped object, scratched in the grid, and fingertips with rubber gloves, and the peeled area was examined and evaluated as follows.
【0187】A :全く剥離されていない B :傷の周りがごく僅か剥離された C :傷の周りが全面積の10%未満剥離された D :剥離面積が同10%以上50%未満剥離された E :剥離面積が同50%以上80%未満剥離された F :剥離面積が同80%以上若干残存しているぐらい剥
離された G :全面積が剥離されるかあるいはそれ以上剥離され
た 表2にウエット膜付きの結果を示した。A: Not peeled off at all B: Peeling around the scratch was very slight C: Peeling around the scratch was less than 10% of the total area D: Peeling area was peeled at 10% or more and less than 50% E: 50% or more and less than 80% of the peeled area was peeled F: 80% or more of the peeled area was peeled off to some extent G: The whole area was peeled off or more was peeled Table 2 shows the results with a wet film.
【0188】[0188]
【表2】 [Table 2]
【0189】〈評価と結果〉紫外線照射時間によりIR
吸収強度比が異なり、1分〜300分の範囲でヘーズ、膜
付き試験結果とも良好であった。600分では処理表面が
荒れヘーズ、膜付きとも劣化することがわかる。未処理
では膜付きが悪かった。比較−1の115℃という高温で
紫外線を処理され、下引にフィルムの溶媒を用いたもの
はヘーズが大きく、膜付きが悪くなることがわかった。<Evaluation and Results> IR was determined by UV irradiation time.
The absorption intensity ratio was different, and the haze and film-attached test results were good in the range of 1 minute to 300 minutes. It can be seen that at 600 minutes, the treated surface becomes rough and haze, and the film is deteriorated. When untreated, the film attachment was poor. It was found that the film treated with ultraviolet rays at a high temperature of 115 ° C. of Comparative-1 and using the solvent of the film as the subbing had a large haze, resulting in poor film formation.
【0190】〔実施例2〕 《写真用支持体2の作製》実施例1で合成したポリエチ
レン-2,6-ナフタレート(PEN)を用いて、PEN、
下記変性ポリエステル(M)及びPENの3層積層フィ
ルム(以下PEN/M/PENと略す)を下記の如く作
製した。Example 2 Preparation of Photographic Support 2 Using the polyethylene-2,6-naphthalate (PEN) synthesized in Example 1, PEN,
The following three-layer laminated film of modified polyester (M) and PEN (hereinafter abbreviated as PEN / M / PEN) was prepared as follows.
【0191】《変性ポリエステル(M)樹脂の合成》テ
レフタル酸100重量部、エチレングリコール64重量部に
酢酸カルシウム水和物0.1重量部を添加し、常法により
エステル化反応を行った。得られた生成物に5-ナトリウ
ムスルホジ(β-ヒドロキシエチル)イソフタル酸のエ
チレングリコール溶液(濃度35重量%)28重量部(5モ
ル%/全酸性分)、ポリエチレングリコール(数平均分
子量3000)8.1重量部(7重量%/ポリマー)、三酸化
アンチモン0.05重量部、リン酸トリメチルエステル0.13
重量部を添加した。次いで徐々に昇温、減圧し、280
℃、0.5mmHgで重合を行い固有粘度0.57を有する変性ポ
リエステル樹脂を得た。<< Synthesis of Modified Polyester (M) Resin >> 100 parts by weight of terephthalic acid and 64 parts by weight of ethylene glycol were added with 0.1 part by weight of calcium acetate hydrate, and esterification reaction was carried out by a conventional method. The obtained product was 28 parts by weight of ethylene glycol solution of 5-sodium sulfodi (β-hydroxyethyl) isophthalic acid (concentration 35% by weight) (5 mol% / total acid content), polyethylene glycol (number average molecular weight 3000). 8.1 parts by weight (7% by weight / polymer), antimony trioxide 0.05 parts by weight, phosphoric acid trimethyl ester 0.13
Parts by weight were added. Then gradually raise the temperature and reduce the pressure to 280
Polymerization was carried out at 0.5 ° C. and 0.5 mmHg to obtain a modified polyester resin having an intrinsic viscosity of 0.57.
【0192】《3層積層フィルムの作成》上記M樹脂と
PEN樹脂と実施例1で作製した着色マスターチップと
ブレンドしたPEN樹脂を各々150℃で別々に真空乾燥
した後、3台の押出機を用いて(1台はM樹脂、2台は
PEN着色ブレンド樹脂)300℃で溶融押出し、3層の
両側の外層にPEN層、内部層にM層を、厚さの比が3
/10/7(PEN/M/PEN)になるように、また仕
上がりの総膜厚が90μmになるように、量を調節してT
ダイ内で層状に接合させて押出し、静電密着方法で冷却
ドラムに、密着させながら急冷固化させ、積層未延伸シ
ートを得た。次いで135℃で縦方向に3.5倍延伸した。続
いて150℃で横方向に3.5倍延伸した後230℃で熱固定し
て二軸延伸積層フィルムを得た。なお、着色していない
PEN樹脂を最外層にした二軸延伸した積層フィルムも
作製し、実施例1と同様にIR吸収強度測定のコントロ
ール試料とした。<< Preparation of Three-Layer Laminated Film >> The above M resin, PEN resin, and PEN resin blended with the colored master chip prepared in Example 1 were vacuum dried separately at 150 ° C., and then three extruders were used. (1 unit is M resin, 2 units are PEN colored blend resin), melt extruded at 300 ° C., PEN layer is on the outer layer on both sides of the 3 layers, M layer is on the inner layer, and the thickness ratio is 3
Adjust the amount so that it becomes / 10/7 (PEN / M / PEN) and the total film thickness of the finished product is 90 μm.
The layers were joined together in a die and extruded, and then rapidly cooled and solidified while being brought into close contact with a cooling drum by an electrostatic contact method to obtain a laminated unstretched sheet. Then, it was stretched 3.5 times in the longitudinal direction at 135 ° C. Subsequently, it was stretched 3.5 times in the transverse direction at 150 ° C. and then heat-set at 230 ° C. to obtain a biaxially stretched laminated film. A biaxially stretched laminated film having an uncolored PEN resin as the outermost layer was also prepared and used as a control sample for IR absorption intensity measurement in the same manner as in Example 1.
【0193】〈下引層形成〉積層フィルムの両面に8W
/m2・minのコロナ放電処理を施し、積層フィルムの膜
厚比7の面に下記下引塗布液a-10を乾燥膜厚0.8μmに
なるよう下引塗布し下引層A-10とした。また反対の膜
厚比3の側の面に下記下引塗布液b-10を乾燥膜厚0.8μ
mになるよう下引塗布し下引層B-10とした。<Formation of undercoat layer> 8 W on both sides of the laminated film
/ M 2 · min corona discharge treatment, undercoating the following undercoating solution a-10 on the surface of the laminated film with a film thickness ratio of 7 to a dry film thickness of 0.8 μm did. On the other side of the film having a film thickness ratio of 3, the undercoating coating solution b-10 described below was dried to a film thickness of 0.8 μm.
The undercoating was applied so as to have a thickness of m to obtain an undercoating layer B-10.
【0194】 《下引塗布液a-10》 P−2(固形分30%) 270g 化合物(UL−1) 0.6g ヘキサメチレン-1,6-ビスエチレンウレア 0.8g 水で1リットルに仕上げる。<< Undercoating liquid a-10 >> P-2 (solid content 30%) 270 g Compound (UL-1) 0.6 g Hexamethylene-1,6-bisethyleneurea 0.8 g Water is added to make 1 liter.
【0195】 《下引塗布液b-10》 P−1ラテックス液(固形分30%) 270g 化合物(UL−1) 0.6g ヘキサメチレン-1,6-ビスエチレンウレア 0.8g 水で1リットルに仕上げる。<< Undercoating liquid b-10 >> P-1 latex liquid (solid content 30%) 270 g Compound (UL-1) 0.6 g Hexamethylene-1,6-bisethyleneurea 0.8 g Finish with water to 1 liter .
【0196】なお、P−1,P−2以外の本発明のビニ
ルコポリマーラテックスについても表2に示したものを
用いて、上記a-10あるいはb-10を調製して実施例1と
同様に塗布乾燥し、下引層A−10、B−10を得た。As for the vinyl copolymer latex of the present invention other than P-1 and P-2, the a-10 or b-10 described above was prepared using the compounds shown in Table 2, and the same procedure as in Example 1 was conducted. After coating and drying, subbing layers A-10 and B-10 were obtained.
【0197】続いて、下引層B-10および下引層A-10の
上に8W/m2・minのコロナ放電を施し、それぞれの層
の上に下記帯電防止剤を含む帯電防止層塗布液b-11、
及び下記下引上層塗布液a-11をそれぞれ乾燥膜厚0.3μ
m及び0.1μmになるように塗設し、それぞれ帯電防止層
B-11層及び下引層A-11層とし、B-11の上に帯電防止
上層塗布液b-12を0.1μmになるように塗布し、帯電防
止及び下引された写真用支持体を得た。Subsequently, a corona discharge of 8 W / m 2 · min was applied on the undercoat layer B-10 and the undercoat layer A-10, and an antistatic layer containing the following antistatic agent was applied on each layer. Liquid b-11,
And the undercoating upper layer coating liquid a-11 described below each have a dry film thickness of 0.3 μm.
m and 0.1 μm so as to form an antistatic layer B-11 layer and an undercoat layer A-11 layer respectively, and an antistatic upper coating solution b-12 on B-11 to 0.1 μm. To obtain an antistatic and subbed photographic support.
【0198】 《帯電防止塗布液(b-11)》 ゼラチン 20g 下記π電子系導電性ポリマー(成分) 100mg/m2 になる重量 架橋剤A 5g 化合物(UL−1) 0.6g 化合物(UL−2) 0.2g 平均粒径3μmのシリカ粒子 0.1g 水で1リットルに仕上げた。<< Antistatic Coating Solution (b-11) >> Gelatin 20 g Weight of π-electron conductive polymer (component) 100 mg / m 2 below Crosslinking agent A 5 g Compound (UL-1) 0.6 g Compound (UL-2) ) 0.2 g Silica particles having an average particle size of 3 μm 0.1 g Water was made up to 1 liter.
【0199】 《帯電防止上層塗布液(b-12)》 化合物(UL−1) 0.2g 化合物(UL−2) 0.2g N,N′,N″-トリスアクリロイル-1,3,5-トリメチレントリアミン 0.1g ゼラチン 10g 平均粒径3μmのシリカ粒子 0.1g 水で1リットルに仕上げる。<< Antistatic Upper Layer Coating Liquid (b-12) >> Compound (UL-1) 0.2 g Compound (UL-2) 0.2 g N, N ′, N ″ -trisacryloyl-1,3,5-trimethylene Triamine 0.1 g Gelatin 10 g Silica particles with an average particle size of 3 μm 0.1 g Water to 1 liter.
【0200】 《下引上層塗布液a-11》 化合物(UL−1) 0.2g 化合物(UL−2) 0.2g N,N′,N″-トリスアクリロイル-1,3,5-トリメチレントリアミン 0.1g ゼラチン 10g 平均粒径3μmのシリカ粒子 0.1g 水で1リットルに仕上げる。<< Undercoating Upper Layer Coating Liquid a-11 >> Compound (UL-1) 0.2 g Compound (UL-2) 0.2 g N, N ′, N ″ -trisacryloyl-1,3,5-trimethylenetriamine 0.1 g Gelatin 10 g Silica particles having an average particle size of 3 μm 0.1 g Water is made up to 1 liter.
【0201】[0201]
【化23】 [Chemical formula 23]
【0202】なお、上記π電子系導電性ポリマーはポリ
(3,4-エチレンジオキシ-チオフェン)であり、下記の
ごとく合成される。The π-electron conductive polymer is poly (3,4-ethylenedioxy-thiophene), which is synthesized as follows.
【0203】《ポリ-3,4-ジエトキシチオフェンの合
成》ポリスチレンスルホン酸(数平均分子量3,700)30
gを1.5lの水に溶かし、窒素気流下、その中に72ミリ
モルのK2S2O8、0.375ミリモルのFe2(SO4)3、210ミリ
モルの3,4-ジエトキシチオフェンを加え、20℃で24時間
撹拌反応させた。これに更に750mlの水そ加え、強酸性
及び弱塩基性イオン交換樹脂(それぞれアンバーライト
(商品名)IR120とIRA400をその中に加えミックスベッ
ドとして室温で8時間撹拌して脱塩を行った。その後、
イオン交換樹脂を濾別し、ポリ-3,4-ジエトキシチオフ
ェンの分散液を得た。濃縮精製したポリマーを元素分析
とNMRによりこのものは平均重合度40であった。<< Synthesis of Poly-3,4-diethoxythiophene >> Polystyrenesulfonic acid (number average molecular weight 3,700) 30
g was dissolved in 1.5 l of water, and 72 mmol of K 2 S 2 O 8 , 0.375 mmol of Fe 2 (SO 4 ) 3 and 210 mmol of 3,4-diethoxythiophene were added thereto under a nitrogen stream. The reaction was allowed to stir at 20 ° C. for 24 hours. To this was further added 750 ml of water, and strongly acidic and weakly basic ion exchange resins (Amberlite (trade name) IR120 and IRA400, respectively, were added to the mixture, and the mixture was mixed at room temperature for 8 hours for desalting. afterwards,
The ion exchange resin was filtered off to obtain a poly-3,4-diethoxythiophene dispersion liquid. The polymer obtained by concentration and purification was found to have an average degree of polymerization of 40 by elemental analysis and NMR.
【0204】《比較試料》下記比較ビニルコポリマーラ
テックスHP−1〜3を用いて本発明の下引液と同様な
処方の下引液a″−10及びb″−10を紫外線照射処理さ
れたフィルムに本発明の下引と同様に塗布乾燥し、下引
層をA″−10及びB″−10とし、更に本発明の下引上層
塗布液a−11、帯電防止層塗布液b−11及び帯電防止上
層塗布液b−12を塗布してA″−11、B″−11、B″−
12とした。<< Comparative Samples >> Films obtained by subjecting the following comparative vinyl copolymer latexes HP-1 to HP-3 to UV-irradiated to the undercoat solutions a "-10 and b" -10 having the same formulation as the undercoat solution of the present invention. And coating and drying in the same manner as in the undercoating of the present invention to make the undercoating layers A ″ -10 and B ″ -10. Further, the undercoating upper layer coating solution a-11 of the present invention, the antistatic layer coating solution b-11 and Apply antistatic upper layer coating liquid b-12 to apply A ″ -11, B ″ -11, B ″ −
It was 12.
【0205】以下本発明とこれらのA−11及びA″−11
の上に実施例1と同様な感光層を、またB−12及びB″
−12の上に下記バック層を塗設してハロゲン化銀カラー
用写真感光材料を作製した。The present invention and these A-11 and A ″ -11 are as follows.
And a photosensitive layer similar to that used in Example 1, B-12 and B ″.
The following back layer was coated on -12 to prepare a silver halide color photographic light-sensitive material.
【0206】〈バック層〉 《バック層塗布液b−13の調製》ゼラチン36gを加温し
て溶解後、サポニン20%水溶液を11ml化合物(Lx−
1)を加え、増粘剤としてポリスチレンスルホン酸ナト
リウム塩800gを加えて粘度調整を行い、更にクエン酸
水溶液でpH5.4に調整し、ポリグリセロールとエピクロ
ルヒドリンとの反応生成物1.5gを加え更に架橋剤(硬
膜剤)A200mgを加え、水を加えて1リットルに仕上げ
てバック層塗布液b−13とした。<Back Layer><< Preparation of Back Layer Coating Liquid b-13 >> After dissolving 36 g of gelatin by heating, saponin 20% aqueous solution was added to 11 ml of compound (Lx-
1) was added, 800 g of polystyrene sulfonic acid sodium salt was added as a thickener to adjust the viscosity, pH was adjusted to 5.4 with an aqueous citric acid solution, and 1.5 g of a reaction product of polyglycerol and epichlorohydrin was added to further crosslink. Agent (hardener) A (200 mg) was added, and water was added to make 1 liter to prepare a back layer coating solution b-13.
【0207】《バック層保護膜層用塗布液b−14の調
製》ゼラチン50gを溶解後、2-スルホネートコハク酸ビ
ス(2-エチルヘキシル)エステルナトリウム塩を340m
g、塩化ナトリウムを3.4g、架橋剤B100mgを加えた。
さらにマット剤として平均粒径4μmのポリメチルメタ
クリレートを40mgとなるように添加し、水を加えて1リ
ットルに仕上げて保護層保護膜用塗布液b−14を調製し
た。<< Preparation of Back Layer Protective Layer Coating Solution b-14 >> After dissolving 50 g of gelatin, 2-sulfonate succinic acid bis (2-ethylhexyl) ester sodium salt was added to 340 m.
g, 3.4 g of sodium chloride and 100 mg of crosslinking agent B were added.
Further, as a matting agent, polymethyl methacrylate having an average particle diameter of 4 μm was added so as to have a concentration of 40 mg, and water was added to make 1 liter to prepare a coating liquid b-14 for a protective layer protective film.
【0208】《バック層の塗布は感光層の塗布》実施例
1の感光層塗布と同様にスライドホッパー型コーターで
B−13、B−14をそれぞれ塗布ゼラチン量を3.0g/m2
及び1.5g/m2になるように2層重層塗布してバック層B
−14とした。<< Back Layer Coating is a Photosensitive Layer Coating >> Similar to the photosensitive layer coating in Example 1, B-13 and B-14 were respectively coated with a slide hopper type coater to a gelatin amount of 3.0 g / m 2.
And back layer B by coating two layers to 1.5 g / m 2
It was set to -14.
【0209】[0209]
【化24】 [Chemical formula 24]
【0210】IR吸収強度比の測定及び膜付き試験を実
施例1と同様に行い、表3に結果を示した。The IR absorption intensity ratio measurement and the film attachment test were conducted in the same manner as in Example 1, and the results are shown in Table 3.
【0211】[0211]
【表3】 [Table 3]
【0212】〈評価と結果〉表3からわかるように、官
能基のないビニルコポリマーラテックスの下引は膜付き
が全く悪く、本発明の常温紫外線照射処理フィルムへの
官能基を有するビニルコポリマーラテックスによる下引
は良好な膜付き性を有することがわかった。<Evaluation and Results> As can be seen from Table 3, the undercoating of the vinyl copolymer latex having no functional group has a poor filming property, and the vinyl copolymer latex having a functional group was used for the room temperature ultraviolet irradiation-treated film of the present invention. It was found that the subbing has a good film attachment property.
【0213】〔実施例3〕実施例1と同様に着色マスタ
ーチップとPEN樹脂をブレンドした着色ブレンド樹脂
チップを一軸延伸までを実施例1と同様に行い、引き続
き下記インライン帯電防止下引塗布液a−20及びb−20
を両面に塗設し(二軸延伸後出来上がり膜厚が0.1μmに
なるように塗設)、更に続いてテンター式横延伸工程
で、145℃で横方向に3.5倍延伸した後、230℃で熱固定
して、冷却し、A-20及びB-20の帯電防止下引層を有す
る着色された厚さ90μmの二軸延伸フィルムを得た。次
に下引層A−20及びB−20の両面に8W/m2・minのコロ
ナ放電処理を施し、両面に下引液a−21及びb−21を乾
燥膜厚が0.8μmになるように塗布し、115℃で乾燥して
下引層A−21及びB−21を塗設した。Example 3 A colored blended resin chip obtained by blending a colored master chip and a PEN resin was uniaxially stretched in the same manner as in Example 1, and then the following in-line antistatic undercoat coating solution a was used. -20 and b-20
On both sides (applied so that the finished film thickness will be 0.1 μm after biaxial stretching), and then in a tenter-type transverse stretching process, after stretching 3.5 times in the transverse direction at 145 ° C, at 230 ° C After heat setting and cooling, a colored biaxially stretched film having a thickness of 90 μm and having an antistatic subbing layer of A-20 and B-20 was obtained. Then, both surfaces of the undercoat layers A-20 and B-20 were subjected to a corona discharge treatment of 8 W / m 2 · min, and the undercoat liquids a-21 and b-21 were applied to both surfaces so that the dry film thickness became 0.8 μm. And dried at 115 ° C. to form the undercoat layers A-21 and B-21.
【0214】 《インライン帯電防止下引液a−20及びb−20処方》 《下引液a-20及びb-20の調製》 前記CP−1 540g 化合物(UL−4) 60g 架橋剤C 12g 硫酸アンモニウム 0.5g ポリエチレングリコール 6g 水で1リットルに仕上げる。<< In-line Antistatic Subtraction Liquid a-20 and b-20 Formulation >> << Preparation of Subtraction Liquid a-20 and b-20 >> CP-1 540 g Compound (UL-4) 60 g Crosslinking agent C 12 g Ammonium sulfate 0.5g Polyethylene glycol 6g Make up to 1 liter with water.
【0215】 《下引上層液a−21の調製》 ゼラチン 10g 化合物(UL−1) 0.2g 化合物(UL−2) 0.2g N,N′,N″-トリスアクリロイル-1,3,5-トリメチレントリアミン 0.1g 平均粒径3μmのシリカ粒子 0.1g 水で1リットルに仕上げる。<< Preparation of Subbing Upper Layer Liquid a-21 >> Gelatin 10 g Compound (UL-1) 0.2 g Compound (UL-2) 0.2 g N, N ′, N ″ -trisacryloyl-1,3,5-tri Methylenetriamine 0.1 g Silica particles with an average particle size of 3 μm 0.1 g Water to 1 liter.
【0216】[0216]
【化25】 [Chemical 25]
【0217】なお、上記帯電防止下引塗布液のCP−1
の代わりにCP−2及びCP−3を用いて同様にB−20
を作製した。CP-1 of the above antistatic subbing coating liquid was used.
Similarly, using CP-2 and CP-3 instead of B-20
Was produced.
【0218】〈ハロゲン化銀カラー用写真感光材料の作
製〉A-21の上に実施例と同様に前記ハロゲン化銀カラ
ー写真感光層を塗布し、B-20の上に前記磁気記録層を
塗布し、カラーフィルムを作製した。<Preparation of silver halide color photographic light-sensitive material> The silver halide color photographic light-sensitive layer was coated on A-21, and the magnetic recording layer was coated on B-20. Then, a color film was produced.
【0219】《評価と結果》<< Evaluation and Results >>
【0220】[0220]
【表4】 [Table 4]
【0221】紫外線照射処理のPENフィルムに水性コ
ポリエステルを塗設し、実施例1と同様に試験した結
果、実施例1と同様な本発明の範囲内に良好な膜付きの
範囲があることが認められた。As a result of coating an aqueous copolyester on a UV-irradiated PEN film and conducting a test in the same manner as in Example 1, it was found that there was a range with good film formation within the range of the present invention similar to Example 1. Admitted.
【0222】〔実施例4〕実施例1のPENに替えて前
記NGC、NEBA、NTE、NTEC,NCDEN
P、それにPENとPETのブレンドのポリエステル樹
脂を実施例1と同様な合成法で合成し、これらのポリエ
ステル樹脂を用いて厚さ80μmのフィルムを実施例1と
同様に作製した。下引層、帯電防止層、磁気記録層、感
光層の組成と作製法は実施例1と同様にしてハロゲン化
銀カラー用写真フィルムを作製し、実施例1と同様な評
価を行った。[Embodiment 4] In place of the PEN of Embodiment 1, NGC, NEBA, NTE, NTEC, NCDEN are used.
A polyester resin of P and a blend of PEN and PET was synthesized by the same synthesis method as in Example 1, and a film having a thickness of 80 μm was produced in the same manner as in Example 1 using these polyester resins. A silver halide color photographic film was produced in the same manner as in Example 1 except that the composition and the production method of the undercoat layer, the antistatic layer, the magnetic recording layer and the photosensitive layer were the same as those of Example 1.
【0223】[0223]
【表5】 [Table 5]
【0224】〈評価と結果〉PENに代えてナフタレン
ジカルボン酸のポリエステルを主構成成分とするコポリ
エステルあるいはブレンドのフィルムの紫外線照射によ
るIR吸収強度比、ヘーズ、膜付きはPENフィルムの
それとほとんど同様な結果であることを認めた。<Evaluation and Results> The IR absorption intensity ratio by irradiation of ultraviolet rays of the film of a copolyester or a blend containing a naphthalene dicarboxylic acid polyester as a main constituent instead of PEN, haze, and film are almost the same as those of the PEN film. It was confirmed that it was the result.
【0225】[0225]
【発明の効果】ナフタレンジカルボン酸を主構成成分と
するポリエステル写真用支持体への感光層の接着性は難
しいとされて来たが、本発明によって接着性を改善し
た。その結果、写真用支持体の薄手化が出来、カメラの
小型化を可能とした。Although the adhesion of the photosensitive layer to the polyester photographic support containing naphthalenedicarboxylic acid as a main constituent has been considered to be difficult, the present invention improved the adhesion. As a result, the photographic support can be made thinner and the camera can be made smaller.
───────────────────────────────────────────────────── フロントページの続き (72)発明者 本田 誠 東京都日野市さくら町1番地コニカ株式会 社内 ─────────────────────────────────────────────────── ─── Continuation of front page (72) Inventor Makoto Honda Konica Stock Company, 1 Sakura-cho, Hino-shi, Tokyo In-house
Claims (6)
ン酸であるポリエステルを主構成成分とし、赤外線吸収
強度が下記式(1)及び式(2)で示される関係を満た
す様に紫外線照射されたフィルム表面上に、官能性基を
有する水性ポリマー化合物を主として含有した下引層を
有することを特徴とする写真用支持体。 式(1) 0.90≦I1133/I1142≦1.05 式(2) 0.90≦I1330/I1340≦1.10 ここで、I1133は波数が1133cm-1に対する赤外線吸収強
度 I1142は波数が1142cm-1に対する赤外線吸収強度 I1330は波数が1330cm-1に対する赤外線吸収強度 I1340は波数が1340cm-1に対する赤外線吸収強度 を表す。1. A film surface which is irradiated with ultraviolet rays such that a polyester whose dicarboxylic acid component is naphthalenedicarboxylic acid is a main constituent and whose infrared absorption intensity satisfies the relationships represented by the following formulas (1) and (2). And a subbing layer mainly containing an aqueous polymer compound having a functional group. Equation (1) 0.90 ≦ I1133 / I1142 ≦ 1.05 Equation (2) 0.90 ≦ I1330 / I1340 ≦ 1.10 where the infrared absorption intensity I1330 infrared absorption intensity I1142 I1133 is wavenumber for 1133Cm -1 wave number is for 1142Cm -1 wavenumber There wavenumber infrared absorption intensity I1340 for 1330 cm -1 represents an infrared absorption intensity against 1340 cm -1.
がビニルコポリマーラテックスであることを特徴とする
請求項1に記載の写真用支持体。2. The photographic support according to claim 1, wherein the aqueous polymer compound having a functional group is a vinyl copolymer latex.
が水性コポリエステルであることを特徴とする請求項1
に記載の写真用支持体。3. The aqueous polymer compound having the functional group is an aqueous copolyester.
The photographic support described in 1.
フタレートを主構成成分とすることを特徴とする請求項
1乃至請求項3の何れか1項に記載の写真用支持体。4. The photographic support according to claim 1, wherein the polyester mainly comprises polyethylene-2,6-naphthalate.
該積層の両最外層がジカルボン酸成分がナフタレンジカ
ルボン酸であるポリエステルを主構成成分とする層であ
り、該積層の内部層の少なくとも1層が変性ポリエステ
ルであることを特徴とする請求項1乃至請求項3の何れ
か1項に記載の写真用支持体。5. The polyester has a laminated structure,
2. Both outermost layers of the laminate are layers containing a polyester whose dicarboxylic acid component is naphthalenedicarboxylic acid as a main constituent, and at least one of the inner layers of the laminate is a modified polyester. The photographic support according to claim 3.
該積層の両最外層がポリエチレン-2,6-ナフタレートを
主構成成分とする層であり、該積層の内部層の該変性ポ
リエステルが金属スルホネート芳香族ジカルボン酸及び
/又はポリエチレングリコールを含有する変性ポリエス
テル層であることを特徴とする請求項1乃至請求項3又
は請求項5の何れか1項に記載の写真用支持体。6. The polyester has a laminated structure,
Both outermost layers of the laminate are layers containing polyethylene-2,6-naphthalate as a main constituent, and the modified polyester of the inner layer of the laminate is a modified polyester containing a metal sulfonate aromatic dicarboxylic acid and / or polyethylene glycol. A photographic support according to any one of claims 1 to 3 or 5, which is a layer.