JPH0836736A - Magnetic recording media - Google Patents

Magnetic recording media

Info

Publication number
JPH0836736A
JPH0836736A JP6192757A JP19275794A JPH0836736A JP H0836736 A JPH0836736 A JP H0836736A JP 6192757 A JP6192757 A JP 6192757A JP 19275794 A JP19275794 A JP 19275794A JP H0836736 A JPH0836736 A JP H0836736A
Authority
JP
Japan
Prior art keywords
particles
average particle
layer
magnetic
caco
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
JP6192757A
Other languages
Japanese (ja)
Inventor
Hitoshi Hirayama
均 平山
Yukichi Morita
祐吉 森田
Shigeji Watase
茂治 渡瀬
Yoshio Kawakami
義雄 川上
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
TDK Corp
Original Assignee
TDK Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by TDK Corp filed Critical TDK Corp
Priority to JP6192757A priority Critical patent/JPH0836736A/en
Publication of JPH0836736A publication Critical patent/JPH0836736A/en
Withdrawn legal-status Critical Current

Abstract

(57)【要約】 (修正有) 【目的】 高出力が得られ、走行特性に優れ、捲き特
性、耐スクラッチ性、塗膜強度に優れる磁気記録媒体を
提供する。 【構成】 熱可塑性ポリマーを主成分とするフィルム層
の磁性層形成面と反対側に設けた外層は、大小2種の平
均粒径を備えるCaCO3 粒子を含有し外層の厚さをt
(μm)、CaCO3 粒子の大なる平均粒径をd1(μ
m)、CaCO3 粒子の小なる平均粒径をd2(μm)
とした場合、下記の条件を満たし、大なる平均粒径のC
aCO3 粒子は100〜1200ppm、小なる平均粒
径のCaCO3 粒子は3000〜10000ppmの範
囲で、外層内に含有される。 0.2≦d2≦0.8 d1−d2≧0.2であり 0.5≦t≦1.0の場合 0.6≦d1≦0.8t+0.4 1.0<t≦1.5の場合 0.6≦d1≦1.2
(57) [Summary] (Modified) [Purpose] To provide a magnetic recording medium having high output, excellent running characteristics, winding characteristics, scratch resistance, and coating film strength. The outer layer provided on the side opposite to the magnetic layer forming surface of the film layer containing a thermoplastic polymer as a main component contains CaCO 3 particles having an average particle size of two kinds, large and small, and has a thickness of t.
(Μm), the larger average particle size of CaCO 3 particles is d1 (μm
m), the smaller average particle size of CaCO 3 particles is d2 (μm)
When the above is satisfied, the following conditions are satisfied, and C having a large average particle size is used.
The aCO 3 particles are contained in the outer layer in the range of 100 to 1200 ppm, and the CaCO 3 particles having a smaller average particle size are contained in the range of 3000 to 10000 ppm. 0.2 ≦ d2 ≦ 0.8 d1-d2 ≧ 0.2 and 0.5 ≦ t ≦ 1.0 0.6 ≦ d1 ≦ 0.8t + 0.4 1.0 <t ≦ 1.5 Case 0.6 ≦ d1 ≦ 1.2

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は磁気記録媒体に係り、特
に高出力が得られるとともに、走行特性にも優れ、さら
には捲き特性、耐スクラッチ性、および塗膜強度にも優
れる磁気記録媒体に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a magnetic recording medium, and more particularly to a magnetic recording medium which can obtain a high output and is excellent in running characteristics, winding characteristics, scratch resistance and coating strength. .

【0002】[0002]

【従来の技術】従来、磁気記録媒体に用いられる支持体
の構成を多層構造とし、多層構造の最外層である表面層
の中に2種類以上の平均粒径をもつ微粒子を含有させ、
耐スクラッチ性、耐ダビング性を向上させたもの(特開
平3−150127号,特開平4−138251号)
や、耐削れ性、耐ダビング性を兼ね備えさせたもの(特
開平4−138251号)が報告されている。このよう
に磁気記録媒体に用いられる支持体の構成をいわゆる多
層の構造とし、多層構造の最外層である表面層の中に2
種類の平均粒径をもつ微粒子を含有させることはすでに
行われている。
2. Description of the Related Art Conventionally, a support used in a magnetic recording medium has a multi-layer structure, and the outermost surface layer of the multi-layer structure contains fine particles having an average particle size of two or more.
With improved scratch resistance and dubbing resistance (Japanese Patent Laid-Open Nos. 3-150127 and 4-138251)
Also, a material having both abrasion resistance and dubbing resistance (JP-A-4-138251) has been reported. As described above, the support used in the magnetic recording medium has a so-called multi-layered structure, and two layers are formed in the outermost surface layer of the multi-layered structure.
It has already been done to incorporate fine particles with different average particle sizes.

【0003】ところで、磁気記録媒体の高密度化、高出
力化は現在もなお要望されている事項であり、このよう
な要求に適した磁気記録媒体として飽和磁化が大きいこ
とが要求されている。このため8ミリビデオやデジタル
オーディオテープ(DAT)、また放送局用の業務用ビ
デオ等では、鉄を主成分とする針状の磁性金属粒子が使
用されている。また、さらには金属薄膜を利用した高記
録密度用磁気記録媒体も開発され実用化に至っている。
By the way, there is still a demand for higher density and higher output of magnetic recording media, and a magnetic recording medium suitable for such requirements is required to have a large saturation magnetization. For this reason, needle-shaped magnetic metal particles containing iron as a main component are used in 8 mm video, digital audio tape (DAT), commercial video for broadcasting stations and the like. Furthermore, a magnetic recording medium for high recording density using a metal thin film has been developed and put into practical use.

【0004】磁気記録媒体の高出力化へのアプローチの
一手法として、媒体表面の平滑化が検討されている。す
なわち、記録媒体の表面を平滑にして、スペーシングロ
スを低減させることにより、高い出力を得る努力がなさ
れている。しかしながら非磁性支持体の表面を平滑にす
ればするほど、平滑化に伴う高出力化の実現は達成しや
すくなるもののこれと相反して、摩擦係数の増大、それ
に伴う走行の不安定性、テープ削れ等の発生という問題
が生じる。この相反する特性を両立させるために、上記
の公知となっている多層構造の支持体を用いて両者のバ
ランスを考慮した設計をしたり、あるいは、例えば磁性
層中に含まれる脂肪酸等の潤滑剤を増加させ、表面平滑
性に重点を置きつつも走行性を確保する等の手法が採択
され得る。
Smoothing of the surface of a medium is being studied as one approach to increasing the output of a magnetic recording medium. That is, efforts are being made to obtain high output by smoothing the surface of the recording medium and reducing spacing loss. However, the smoother the surface of the non-magnetic support, the easier it will be to achieve higher output due to smoothing, but in contrast to this, the friction coefficient increases, the instability of running and tape scraping increase. The problem of occurrence of the above occurs. In order to achieve both of these contradictory properties, a support having a well-known multi-layer structure as described above is used in consideration of the balance between the two, or a lubricant such as a fatty acid contained in the magnetic layer is used. Can be adopted to secure the running property while increasing the surface area and focusing on the surface smoothness.

【0005】[0005]

【発明が解決しようとする課題】しかしながら、単に、
すでに開示されている上記多層構造の支持体を転用する
のみでは、高出力が得られるとともに、走行特性にも優
れ、さらには捲き特性、耐スクラッチ性、および塗膜強
度にも優れる磁気記録媒体の実現の可能性は極めて乏し
いと言える。また、高出力化の品質要求に応じるべく表
面の平滑性に重点を置き、このぶん走行性をカバーする
ために例えば磁性層中に含まれる脂肪酸等の潤滑剤を増
加させ、両者のバランスを両立させる手法では、増量さ
れて添加された潤滑剤が他の特性への弊害をもたらすこ
とがある。例えば、塗膜の物理特性の低下、余剰の潤滑
剤が引き起こす塗膜表面の析出等である。特に、使用磁
性材の比表面積が大きい場合、脂肪酸の添加量の増量
は、塗膜物性の低下を招いてしまう。
However, simply,
By simply diverting the already-disclosed support of the above-mentioned multilayer structure, high output can be obtained, and excellent running characteristics can be obtained, and further, winding characteristics, scratch resistance, and coating film strength It is extremely unlikely to be realized. Also, in order to meet the demand for high output quality, the surface smoothness is emphasized, and in order to cover this running property, for example, the amount of lubricant such as fatty acid contained in the magnetic layer is increased to achieve a balance between the two. In such a method, the lubricant added in an increased amount may have a bad influence on other properties. For example, deterioration of physical properties of the coating film, precipitation of the coating film surface caused by excess lubricant, and the like. In particular, when the specific surface area of the magnetic material used is large, increasing the amount of fatty acid added leads to a decrease in the physical properties of the coating film.

【0006】このような実情のもとに本発明は創案され
たものであり、その目的は、従来の非磁性支持体を平滑
化して高出力を得、かつ走行特性をも向上させるという
本来相反する特性の両立を達成するとともに、さらには
捲き特性、耐スクラッチ性、および塗膜強度にも優れる
磁気記録媒体を提供することにある。
The present invention was devised under such circumstances, and its purpose is to provide a conventional non-magnetic support member with a smooth surface to obtain a high output and also to improve running characteristics. It is an object of the present invention to provide a magnetic recording medium that achieves both of the properties described above, and that is also excellent in winding properties, scratch resistance, and coating film strength.

【0007】[0007]

【課題を解決するための手段】このような目的を達成す
るために、本発明は、可撓性支持体上に磁性層を設けて
なる磁気記録媒体において、前記可撓性支持体は熱可塑
性ポリマーを主成分とするフィルム層と、該フィルム層
の少なくとも磁性層形成面の反対側に設けられた外層と
を有し、前記外層は、少なくとも大小2種の平均粒径を
備えるCaCO3 粒子を含有しており、外層の厚さをt
(μm)、CaCO3 粒子の大なる平均粒径をd1(μ
m)、CaCO3 粒子の小なる平均粒径をd2(μm)
とした場合、含有されるべく大小2種のCaCO3 平均
粒径d1およびd2は、それぞれ外層の厚さtとの関係
で、下記の条件を満たし、かつ前記大なる平均粒径のC
aCO3 粒子は100〜1200ppmの範囲で、前記
小なる平均粒径のCaCO3 粒子は3000〜1000
0ppmの範囲で、それぞれ前記外層内に含有されるよ
うに構成される。
In order to achieve such an object, the present invention provides a magnetic recording medium having a magnetic layer provided on a flexible support, wherein the flexible support is thermoplastic. It has a film layer containing a polymer as a main component, and an outer layer provided at least on the opposite side of the magnetic layer forming surface of the film layer, and the outer layer comprises CaCO 3 particles having at least two kinds of average particle diameters. And the thickness of the outer layer is t
(Μm), the larger average particle size of CaCO 3 particles is d1 (μm
m), the smaller average particle size of CaCO 3 particles is d2 (μm)
In this case, the CaCO 3 average particle diameters d1 and d2 of two kinds, large and small, to be contained satisfy the following conditions in relation to the thickness t of the outer layer, respectively, and C of the large average particle diameter is
The aCO 3 particles are in the range of 100 to 1200 ppm, and the CaCO 3 particles having a smaller average particle diameter are 3000 to 1000.
In the range of 0 ppm, each is contained in the outer layer.

【0008】(1)0.5≦t≦1.0の場合 0.6≦d1≦0.8t+0.4 0.2≦d2≦0.8 d1−d2≧0.2 (2)1.0<t≦1.5の場合 0.6≦d1≦1.2 0.2≦d2≦0.8 d1−d2≧0.2 以下、本発明の好適な具体例について詳細に説明する。(1) 0.5 ≦ t ≦ 1.0 0.6 ≦ d1 ≦ 0.8t + 0.4 0.2 ≦ d2 ≦ 0.8 d1-d2 ≧ 0.2 (2) 1.0 <When t ≦ 1.5 0.6 ≦ d1 ≦ 1.2 0.2 ≦ d2 ≦ 0.8 d1-d2 ≧ 0.2 Hereinafter, preferred examples of the present invention will be described in detail.

【0009】図1は、本発明の磁気記録媒体の好適な構
成例を示す概略断面図である。図1に示されるように、
磁気記録媒体1は可撓性支持体2上に磁性層5を設けて
構成される。そして、可撓性支持体2は、熱可塑性ポリ
マーを主成分とするフィルム層3と、該フィルム層3の
磁性層形成面と反対側に設けられた外層4とを有する2
層構造のフィルムから構成されている。そして、外層4
は熱可塑性ポリマーを主成分とし、この外層4の中には
後述するような少なくとも大小2種の平均粒径を備える
CaCO3 粒子が含有されている。
FIG. 1 is a schematic sectional view showing a preferred example of the structure of the magnetic recording medium of the present invention. As shown in FIG.
The magnetic recording medium 1 is constructed by providing a magnetic layer 5 on a flexible support 2. The flexible support 2 has a film layer 3 containing a thermoplastic polymer as a main component, and an outer layer 4 provided on the side of the film layer 3 opposite to the magnetic layer forming surface 2
It is composed of a layered film. And the outer layer 4
Is mainly composed of a thermoplastic polymer, and the outer layer 4 contains CaCO 3 particles having at least two kinds of average particle diameters as described later.

【0010】本発明において、フィルム層3および外層
4に使用される熱可塑性ポリマーは、テレフタル酸、ナ
フタレン−2,6−ジカルボン酸等の芳香族カルボン酸
と、エチレングリコール、ジエチレングリコール、プロ
ピレングリコール、ブチレングリコール等とを重縮合さ
せて得られる芳香族ポリエステルとすることが好まし
い。このような熱可塑性ポリマーの代表的なものとし
て、ポリエチレンテレフタレート(PET)、ポリエチ
レン−2,6−ナフタレート(PEN)等が挙げられ
る。また、フィルム層3に使用する熱可塑性ポリマーと
外層4に使用する熱可塑性ポリマーの組み合わせは任意
に設定することができ、例えば、外層4にPETを使用
しフィルム層3にPENを使用する組み合わせ、外層4
にPENを使用しフィルム層3にPETを使用する組み
合わせ等とすることができる。また、フィルム層3ある
いは外層4に、2種以上の熱可塑性ポリマーを使用して
もよい。
In the present invention, the thermoplastic polymer used in the film layer 3 and the outer layer 4 is an aromatic carboxylic acid such as terephthalic acid or naphthalene-2,6-dicarboxylic acid, and ethylene glycol, diethylene glycol, propylene glycol or butylene. An aromatic polyester obtained by polycondensation with glycol or the like is preferable. Typical examples of such a thermoplastic polymer include polyethylene terephthalate (PET) and polyethylene-2,6-naphthalate (PEN). Further, the combination of the thermoplastic polymer used for the film layer 3 and the thermoplastic polymer used for the outer layer 4 can be set arbitrarily, for example, a combination using PET for the outer layer 4 and PEN for the film layer 3, Outer layer 4
It is possible to use a combination of using PEN for the film and PET for the film layer 3. Moreover, you may use 2 or more types of thermoplastic polymers for the film layer 3 or the outer layer 4.

【0011】尚、本発明においてフィルム層3に使用さ
れる熱可塑性ポリマーは、バージンポリマーに限定され
ず、再生ポリマーであってもよい。
The thermoplastic polymer used in the film layer 3 in the present invention is not limited to a virgin polymer and may be a recycled polymer.

【0012】フィルム層3は上記のような熱可塑性ポリ
マーの他に、防錆剤、帯電防止剤等の無機および有機添
加剤や、カーボンブラック等の粒子を添加してもよい。
また、再生ポリマーに含有される滑剤は、0.001〜
10重量%の範囲で用いることができる。そして、フィ
ルム層3の厚みは、磁気記録媒体の用途に応じて3〜7
5μm程度とすることができる。
In addition to the above-mentioned thermoplastic polymers, the film layer 3 may contain inorganic and organic additives such as rust preventives and antistatic agents, and particles such as carbon black.
The lubricant contained in the recycled polymer is 0.001 to
It can be used in the range of 10% by weight. The thickness of the film layer 3 is 3 to 7 depending on the application of the magnetic recording medium.
It can be about 5 μm.

【0013】外層4には少なくとも大小2種の平均粒径
を備えるCaCO3 粒子が含有されており、外層4の厚
さをt(μm)、CaCO3 粒子の大なる平均粒径をd
1(μm)、CaCO3 粒子の小なる平均粒径をd2
(μm)とした場合、含有されるべく大小2種のCaC
O3 平均粒径d1およびd2は、それぞれ外層の厚さt
との関係で下記の条件を満たすように設定される。
The outer layer 4 contains CaCO 3 particles having at least two kinds of average particle sizes, the thickness of the outer layer 4 is t (μm), and the large average particle size of CaCO 3 particles is d.
1 (μm), the smaller average particle size of CaCO 3 particles is d2
(Μm), two types of CaC, large and small, to be included
The O 3 average particle diameters d1 and d2 are respectively the outer layer thickness t
It is set to satisfy the following conditions in relation to.

【0014】(1)0.5≦t≦1.0の場合 0.6≦d1≦0.8t+0.4 0.2≦d2≦0.8 d1−d2≧0.2 (2)1.0<t≦1.5の場合 0.6≦d1≦1.2 0.2≦d2≦0.8 d1−d2≧0.2 すなわち、(1)外層4の厚さtが、0.5μm以上
1.0μm以下の場合では、含有されるCaCO3 粒子
の大なる平均粒径d1の範囲は、下限が0.6μm以上
であって、上限が厚さtの関数で表わされて(0.8t
+0.4)μm以下とされ、さらに好ましい範囲は、
0.4t+0.4≦d1≦0.4t+0.6とされる。
また、CaCO3 粒子の小なる平均粒径d2の範囲は、
0.2μm以上0.8μm以下、より好ましくは、0.
4〜0.6μmとされる。しかも、大なる平均粒径d1
と小なる平均粒径d2との差(d1−d2)は、0.2
μm以上、好ましくは、0.3〜0.6μmとされる。
前記大なる平均粒径d1が下限値未満となると、走行性
の悪化、捲き性の不良という不都合が生じ、これとは反
対に大なる平均粒径d1が上限値を超えると、耐スクラ
ッチ性の悪化という不都合が生じる。前記小なる平均粒
径d2が下限値の0.2μm未満となると、摩擦が増加
してしまうという不都合が生じ、これとは反対に小なる
平均粒径d2が0.8μmの上限値を超えると、電磁変
換特性の低下という不都合が生じる。前記平均粒径d1
と小なる平均粒径d2との差(d1−d2)が、0.2
μm未満となると大粒子に基づく効果が低下するという
不都合が生じる。
(1) In the case of 0.5 ≦ t ≦ 1.0 0.6 ≦ d1 ≦ 0.8t + 0.4 0.2 ≦ d2 ≦ 0.8 d1-d2 ≧ 0.2 (2) 1.0 <T ≦ 1.5 0.6 ≦ d1 ≦ 1.2 0.2 ≦ d2 ≦ 0.8 d1-d2 ≧ 0.2 That is, (1) the thickness t of the outer layer 4 is 0.5 μm or more. In the case of 1.0 μm or less, the range of the large average particle diameter d1 of the CaCO 3 particles contained is such that the lower limit is 0.6 μm or more and the upper limit is expressed by a function of the thickness t (0. 8t
+0.4) μm or less, and a more preferable range is
0.4t + 0.4 ≦ d1 ≦ 0.4t + 0.6.
Further, the range of the smaller average particle diameter d2 of CaCO 3 particles is
0.2 μm or more and 0.8 μm or less, more preferably 0.
It is set to 4 to 0.6 μm. Moreover, the large average particle diameter d1
And the difference (d1-d2) from the average particle diameter d2 is 0.2
The thickness is not less than μm, preferably 0.3 to 0.6 μm.
If the large average particle diameter d1 is less than the lower limit value, the running property deteriorates and the winding property is inferior. On the contrary, if the large average particle diameter d1 exceeds the upper limit value, the scratch resistance is deteriorated. The inconvenience of deterioration occurs. If the small average particle diameter d2 is less than the lower limit value of 0.2 μm, friction will increase, and on the contrary, if the small average particle diameter d2 exceeds the upper limit value of 0.8 μm. However, there is a problem that the electromagnetic conversion characteristics are deteriorated. The average particle size d1
And the difference (d1-d2) from the average particle size d2 that is smaller is 0.2
If it is less than μm, there is a disadvantage that the effect due to large particles decreases.

【0015】一方、(2)外層4の厚さtが、1.0μ
mを超え1.5μm以下の場合では、含有されるCaC
O3 粒子の大なる平均粒径d1の範囲は、0.6μm以
上1.2μm以下、さらに好ましくは、0.8〜1.0
μmとされる。また、CaCO3 粒子の小なる平均粒径
d2の範囲は、0.2μm以上0.8μm以下、より好
ましくは、0.4〜0.6μmとされる。しかも、大な
る平均粒径d1と小なる平均粒径d2との差(d1−d
2)は、0.2μm以上、好ましくは、0.3〜0.6
μmとされる。これらの数値範囲が個々にそれぞれ外れ
た場合、上記(1)の場合に対応した不都合がそれぞれ
生じる。
On the other hand, (2) the thickness t of the outer layer 4 is 1.0 μm.
If more than 1.5 m and less than 1.5 μm, CaC contained
The range of the large average particle diameter d1 of the O 3 particles is 0.6 μm or more and 1.2 μm or less, and more preferably 0.8 to 1.0.
μm. Further, the range of the smaller average particle diameter d2 of the CaCO 3 particles is 0.2 μm or more and 0.8 μm or less, and more preferably 0.4 to 0.6 μm. Moreover, the difference between the large average particle diameter d1 and the small average particle diameter d2 (d1-d
2) is 0.2 μm or more, preferably 0.3 to 0.6
μm. If these numerical ranges are out of the individual range, inconveniences corresponding to the above case (1) occur.

【0016】前記大なる平均粒径のCaCO3 粒子は、
100〜1200ppm、より好ましくは、200〜8
00ppmの範囲で、小なる平均粒径のCaCO3 粒子
は3000〜10000ppm、より好ましくは、40
00〜8000ppmの範囲で、それぞれ外層4の中に
含有される。大なる平均粒径のCaCO3 粒子の含有率
が100ppm未満となると、大粒子添加による効果、
すなわち走行性、捲き性の向上が図れないという不都合
が生じ、また、1200ppmを超えると表面悪化によ
る電磁変換特性の低下や粗大突起により耐スクラッチ性
が悪くなるという不都合が生じる。小なる平均粒径のC
aCO3 粒子の含有率が3000ppm未満となると、
摩擦が増加してしまうという不都合が生じ、また、10
000ppmを超えると電磁変換特性が低下してしまう
という不都合が生じる。なお、CaCO3 粒子の含有率
は、外層4の乾燥後の固形分中の重量含有率である。
The CaCO 3 particles having a large average particle size are
100 to 1200 ppm, more preferably 200 to 8
In the range of 00 ppm, CaCO 3 particles having a smaller average particle size are 3000 to 10000 ppm, and more preferably 40
It is contained in the outer layer 4 in the range of 0.00 to 8000 ppm. When the content of CaCO 3 particles having a large average particle diameter is less than 100 ppm, the effect of adding large particles,
That is, the running property and the winding property cannot be improved, and when the content exceeds 1200 ppm, the electromagnetic conversion characteristics are deteriorated due to surface deterioration and the scratch resistance is deteriorated due to coarse projections. C with smaller average particle size
When the content of aCO 3 particles is less than 3000 ppm,
The inconvenience of increased friction occurs, and 10
If it exceeds 000 ppm, the electromagnetic conversion characteristics will be deteriorated. The content of CaCO 3 particles is the weight content in the solid content of the outer layer 4 after drying.

【0017】上述のCaCO3 粒子の平均粒径d1およ
びd2は以下のように測定される。すなわち、磁気記録
媒体を熱硬化性エポキシ樹脂で包埋し、ダイアモンドカ
ッターにて薄く切断したサンプルを透過型電子顕微鏡
(TEM)(日本電子(株)製JEM100CX)にて
観察し、観察場所を変えて粒子数500個以上から平均
値を求める。また、外層の平均厚みの測定方法は、磁気
記録媒体を熱硬化性エポキシ樹脂で包埋し、ダイアモン
ドカッターにて薄く切断したサンプルを上記のTEMに
て観察し、観察場所を変えて外層の10箇所の厚さから
平均値を求める。
The average particle diameters d1 and d2 of the above CaCO 3 particles are measured as follows. That is, a magnetic recording medium was embedded with a thermosetting epoxy resin, and a sample thinly cut with a diamond cutter was observed with a transmission electron microscope (TEM) (JEM100CX manufactured by JEOL Ltd.), and the observation location was changed. The average value is calculated from the number of particles of 500 or more. The method for measuring the average thickness of the outer layer is as follows. A magnetic recording medium is embedded in a thermosetting epoxy resin, and a sample thinly cut with a diamond cutter is observed with the above-mentioned TEM. Calculate the average value from the thickness of the spot.

【0018】ところで、外層4の中に含有される粒子と
してCaCO3 粒子を選定したのは、主に、PETとの
親和性が良く、フィルムからの脱落が少ないという理由
に基づく。
By the way, the reason why the CaCO 3 particles are selected as the particles contained in the outer layer 4 is mainly because the particles have good affinity with PET and are less likely to fall off from the film.

【0019】また、前記外層4には、上記のような大小
2種の平均粒径を備えるCaCO3粒子および熱可塑性
ポリマーの他に、必要に応じて1次粒径0.1μm以下
のα−Al2 O3 、γ−Al2 O3 、θ−Al2 O3 δ
−Al2 O3 等を500〜10000ppmの範囲で含
有させることができる。
Further, in the outer layer 4, in addition to the CaCO 3 particles and the thermoplastic polymer having the above-mentioned two kinds of average particle diameters of large and small, an α-particle having a primary particle diameter of 0.1 μm or less is used, if necessary. Al 2 O 3 , γ-Al 2 O 3 , θ-Al 2 O 3 δ
The -al 2 O 3 or the like can be contained in a range of 500~10000Ppm.

【0020】上述のようなフィルム層3と外層4の2層
構造を備え、かつ二軸配向されたポリエステルフィルム
は、例えば、以下のように製造することができる。ま
ず、粒子を実質的に含有しないフィルム層用の熱可塑性
ポリマーと、所定の粒子を含有した外層用の熱可塑性ポ
リマーとを準備し、これらを公知の共押出し機(2層用
の矩形の合流ブロックを有する共押出し機等)により2
層共押出しを行い、静電印加キャスト法を用いて表面温
度30℃のキャスティングドラムに巻きつけて冷却固化
することにより、フィルム層3の片面に外層4を備えた
2層構造の未延伸フィルムを作成する。この共押出しに
おける吐出量を調節することにより、未延伸フィルムの
総厚さ、外層の厚さを制御する。次に、この未延伸フィ
ルムを長手方向(MD方向)に2.5〜5.0倍延伸し
て一軸延伸フィルムとし、さらに、この一軸延伸フィル
ムを100℃に加熱しながら延伸速度2000%/分程
度で幅方向に2.5〜4.0倍延伸した後、定長下で熱
処理することにより、二軸配向ポリエステルフィルムを
得ることができる。
The biaxially oriented polyester film having the two-layer structure of the film layer 3 and the outer layer 4 as described above can be manufactured, for example, as follows. First, a thermoplastic polymer for a film layer that does not substantially contain particles and a thermoplastic polymer for an outer layer that contains predetermined particles are prepared, and a known co-extruder (rectangular confluence for two layers is used). 2) by co-extruder with block)
The layer is coextruded, and is wound around a casting drum having a surface temperature of 30 ° C. using an electrostatically applied casting method to be cooled and solidified to obtain an unstretched film having a two-layer structure having an outer layer 4 on one surface of the film layer 3. create. By adjusting the discharge amount in this co-extrusion, the total thickness of the unstretched film and the thickness of the outer layer are controlled. Next, this unstretched film is stretched 2.5 to 5.0 times in the longitudinal direction (MD direction) to give a uniaxially stretched film, and the uniaxially stretched film is further heated at 100 ° C. while stretching at a rate of 2000% / min. A biaxially oriented polyester film can be obtained by stretching the film in the width direction by 2.5 to 4.0 times and then heat-treating it under a fixed length.

【0021】本発明の磁気記録媒体を構成する磁性層5
に用いられる磁性粉末は特に限定はされない。磁性粉末
としては、例えば、γ−Fe2 O3 、Co含有γ−Fe
2 O3 、Fe3 O4 、Co含有Fe3 O4 、CrO2 、
バリウムフェライト、ストロンチウムフェライト等の酸
化物微粉末、Fe、Co、Ni、Co−Fe、Co−F
e−Ni、Co−Ni、Co−Mn、Co−Si、Co
−Au、Co−Pt等の金属あるいは合金微粉末、炭化
鉄等がいずれも使用可能である。これらの磁性粉末を用
いた磁性層の形成は、磁性粉末および脂肪酸等をバイン
ダ中に分散した磁性塗料を可撓性支持体上に塗布、乾燥
することにより行うことができる。本発明においては、
このような塗布型の磁性層を設ける場合に、用いる磁性
粉末の比表面積が30〜60m2 /gの比較的大きい範
囲であっても、磁性層中に含有される脂肪酸量は塗膜と
の重量比において、0.5〜1.5wt%含有されるこ
とで走行性は十分に担保される。用いるバインダとして
は、公知の各種樹脂バインダはいずれも使用可能であ
る。さらに、溶媒は特に制限はなく、例えば、シクロヘ
キサノン、メチルエチルケトン、メチルイソブチルケト
ン等のケトン系、トルエン等の芳香族系等の各種溶媒を
目的に応じて適宜選択することができる。磁性塗料に
は、必要に応じて無機微粒子、潤滑剤等の各種添加剤を
含有させてもよい。また、磁性層として、真空蒸着法、
スパッタリング法等により上記の磁性金属を可撓性支持
体上に直接成膜することにより、金属薄膜型の磁性層を
形成してもよい。
Magnetic layer 5 constituting the magnetic recording medium of the present invention
The magnetic powder used for is not particularly limited. Examples of the magnetic powder include γ-Fe 2 O 3 and Co-containing γ-Fe.
2 O 3 , Fe 3 O 4 , Co-containing Fe 3 O 4 , CrO 2 ,
Fine oxide powder of barium ferrite, strontium ferrite, etc., Fe, Co, Ni, Co-Fe, Co-F
e-Ni, Co-Ni, Co-Mn, Co-Si, Co
A fine metal or alloy powder such as —Au or Co—Pt, iron carbide or the like can be used. The formation of a magnetic layer using these magnetic powders can be carried out by applying a magnetic coating in which a magnetic powder, a fatty acid, and the like are dispersed in a binder, onto a flexible support and then drying. In the present invention,
When such a coating type magnetic layer is provided, even if the specific surface area of the magnetic powder used is in a relatively large range of 30 to 60 m 2 / g, the amount of fatty acid contained in the magnetic layer is different from that of the coating film. In terms of the weight ratio, the content of 0.5 to 1.5 wt% ensures sufficient runnability. As the binder to be used, any of various known resin binders can be used. Further, the solvent is not particularly limited and, for example, various solvents such as a ketone system such as cyclohexanone, methyl ethyl ketone and methyl isobutyl ketone and an aromatic system such as toluene can be appropriately selected according to the purpose. The magnetic paint may contain various additives such as inorganic fine particles and a lubricant, if necessary. Further, as the magnetic layer, a vacuum deposition method,
A metal thin film type magnetic layer may be formed by directly forming the above-mentioned magnetic metal on a flexible support by a sputtering method or the like.

【0022】磁性層の厚みは、塗布型磁性層の場合は
0.1〜6μm程度であり、この磁性層の30〜92重
量%を磁性粉末が占めるような構成が好ましい。また、
近年行われているように磁性塗料を湿潤状態で多層塗布
して多層構造の磁性層を設けてもよい。この場合、非磁
性液、樹脂の溶解液等も使用可能であり、磁性層の層構
成も適宜選択することができる。また、金属薄膜型の磁
性層の場合、磁性層の厚みは0.1〜0.4μm、特に
0.15〜0.25μm程度が好ましい。
The thickness of the magnetic layer is about 0.1 to 6 μm in the case of the coating type magnetic layer, and it is preferable that the magnetic powder occupies 30 to 92% by weight of this magnetic layer. Also,
As in recent years, magnetic coating may be applied in multiple layers in a wet state to provide a magnetic layer having a multilayer structure. In this case, a non-magnetic liquid, a resin solution, or the like can be used, and the layer structure of the magnetic layer can be appropriately selected. In the case of a metal thin film type magnetic layer, the thickness of the magnetic layer is preferably 0.1 to 0.4 μm, and more preferably 0.15 to 0.25 μm.

【0023】図2には本発明のさらに好適な具体例が示
される。
FIG. 2 shows a further preferred embodiment of the present invention.

【0024】図2に示される構成例が前記図1に示され
る構成例と異なるのは、フィルム層3の磁性層5形成面
側にもさらに外層4が同じように形成されている点にあ
る。磁性層5形成面側の外層4も前記磁性層形成面と反
対側に設けられた外層4の所定の条件を満たす様に形成
される。すなわち磁性層5形成面側の外層4にも少なく
とも大小2種の平均粒径を備えるCaCO3 粒子が含有
させられており、それらの平均粒径d1およびd2は、
それぞれ外層の厚さtとの関係で上記の条件を満たすよ
うに設定されているのである。このように可撓性支持体
2を所定の外層4,4を備える3層構造のフィルムとす
ることにより、特に、電磁変換特性と走行性の両方に極
めて優れた効果が発現され、さらには中間層のフィラー
ををなくしたり、中間層に再生材を使用したりすること
によるコストダウンが可能となるというメリット(効
果)が生じる。
The constitutional example shown in FIG. 2 differs from the constitutional example shown in FIG. 1 in that the outer layer 4 is also formed on the side of the film layer 3 on which the magnetic layer 5 is formed. . The outer layer 4 on the side where the magnetic layer 5 is formed is also formed so as to satisfy the predetermined condition of the outer layer 4 provided on the side opposite to the side where the magnetic layer is formed. That is, the outer layer 4 on the side where the magnetic layer 5 is formed also contains CaCO 3 particles having at least two types of average particle sizes, and the average particle sizes d1 and d2 are:
Each of them is set so as to satisfy the above conditions in relation to the thickness t of the outer layer. By thus forming the flexible support 2 as a film having a three-layer structure including the predetermined outer layers 4 and 4, particularly, an extremely excellent effect is exhibited in both electromagnetic conversion characteristics and running property, and further, it is intermediate. There is an advantage (effect) that the cost can be reduced by eliminating the filler in the layer and using the recycled material in the intermediate layer.

【0025】上述のようなフィルム層3と外層4,4の
3層構造の二軸配向されたポリエステルフィルムは、例
えば、以下のように製造することができる。まず、粒子
を実質的に含有しないフィルム層用の熱可塑性ポリマー
と、所定の粒子を含有した外層用の熱可塑性ポリマーと
を準備し、これらを公知の共押出し機(3層用の矩形の
合流ブロックを有する共押出し機等)により3層共押出
しを行い、静電印加キャスト法を用いて表面温度30℃
のキャスティングドラムに巻きつけて冷却固化すること
により、フィルム層の両面に外層を備えた3層構造の未
延伸フィルムを作成する。この共押出しにおける吐出量
を調節することにより、未延伸フィルムの総厚さ、外層
の厚さを制御する。次に、この未延伸フィルムを長手方
向(MD方向)に2.5〜5.0倍延伸して一軸延伸フ
ィルムとし、さらに、この一軸延伸フィルムを100℃
に加熱しながら延伸速度2000%/分程度で幅方向に
2.5〜4.0倍延伸した後、定長下で熱処理すること
により、二軸配向ポリエステルフィルムを得ることがで
きる。
The biaxially oriented polyester film having the three-layer structure of the film layer 3 and the outer layers 4 and 4 as described above can be manufactured, for example, as follows. First, a thermoplastic polymer for a film layer that does not substantially contain particles and a thermoplastic polymer for an outer layer that contains predetermined particles are prepared, and these are mixed with a known co-extruder (rectangular confluence for three layers). 3 layer co-extrusion by a co-extrusion machine having a block, etc., and a surface temperature of 30 ° C. using an electrostatically applied casting method.
The film is wound around a casting drum of 1 and cooled and solidified to prepare an unstretched film having a three-layer structure having outer layers on both sides of the film layer. By adjusting the discharge amount in this co-extrusion, the total thickness of the unstretched film and the thickness of the outer layer are controlled. Next, this unstretched film is stretched 2.5 to 5.0 times in the longitudinal direction (MD direction) to give a uniaxially stretched film, and the uniaxially stretched film is further cooled to 100 ° C.
A biaxially oriented polyester film can be obtained by drawing 2.5 to 4.0 times in the width direction at a drawing rate of about 2000% / min while heating to 1, and then heat-treating under a fixed length.

【0026】なお、上述してきた図1および図2に示さ
れる磁気記録媒体の支持体の磁性層形成面や支持体の裏
面側には、さらにそれぞれ公知の種々のアンダコート層
やバックコート層を設けてもよい。
Incidentally, various known undercoat layers and backcoat layers are further formed on the magnetic layer forming surface of the support of the magnetic recording medium shown in FIGS. 1 and 2 and on the back surface side of the support, respectively. It may be provided.

【0027】[0027]

【作用】本発明のごとく外層4には少なくとも大小2種
の平均粒径を備えるCaCO3粒子を含有させ、それら
の平均粒径d1およびd2を、それぞれ外層の厚さtと
の関係で上記の条件を満たすように設定する。すると、
理論的にはいまだ不明確ではあるが、小なる平均粒径を
備えるCaCO3 粒子が表面粗さを形成し、表面層の厚
みと近接した大なる平均粒径を備えるCaCO3 粒子
が、走行時常に接地する少数突起を形成するものと考え
られる。所定範囲の大小の異なる粒子の組み合わせによ
り、電磁変換特性の劣化は引き起こさず、走行性のみに
寄与する突起構造が形成される。また、2種の粒子によ
って形成された突起構造が少量の脂肪酸添加のみで良好
な走行性が得られるものと推測される。これにより、過
剰遊離脂肪酸が存在する弊害を解消し、高出力でかつ走
行性に優れた磁気記録媒体が得られる。
As in the present invention, the outer layer 4 contains CaCO 3 particles having at least two kinds of average particle sizes, the average particle size d1 and d2 of each of which is described above in relation to the thickness t of the outer layer. Set to meet the conditions. Then
Theoretically there is still unclear to form CaCO 3 particles surface roughness having an average particle size smaller becomes the average particle size CaCO 3 particles having a large becomes close to the thickness of the surface layer, during travel It is considered that the minority projections that are always grounded are formed. The combination of particles of different sizes within a predetermined range forms a protrusion structure that does not cause deterioration of electromagnetic conversion characteristics and contributes only to the traveling property. Further, it is speculated that the protrusion structure formed by the two kinds of particles can provide good runnability only by adding a small amount of fatty acid. As a result, the adverse effects of the presence of excess free fatty acids can be eliminated, and a magnetic recording medium with high output and excellent running performance can be obtained.

【0028】[0028]

【実施例】以下、本発明を実施例に基づいて更に詳細に
説明する。 (実施例1)ジメチルテレフタレート100重量部、エ
チレングリコール75重量部、酢酸カルシウム一水塩
0.07重量部を反応容器中で加熱し、エステル交換反
応を行わせしめた後、この反応化合物に、無機フィラー
としてCaCO3 、Al2 O3、リン酸0.06重量部
を含むエチレングリコールスラリーおよび酸化アンチモ
ン0.04重量部を加え、加熱し重合反応を行った。C
aCO3 、Al2 O3 量は最終的に得られるポリマーに
対して0.54wt%、0.3wt%になるように調整
した。重合終了後、ポリマーをペレット化した。これを
外層用の熱可塑性ポリマーAとした。また、常法によっ
て、実質的に粒子を含有しないPETを製造し、これを
フィルム層用の熱可塑性ポリマーBとした。
EXAMPLES The present invention will now be described in more detail based on examples. (Example 1) 100 parts by weight of dimethyl terephthalate, 75 parts by weight of ethylene glycol, and 0.07 parts by weight of calcium acetate monohydrate were heated in a reaction vessel to cause a transesterification reaction. As a filler, CaCO 3 , Al 2 O 3 , an ethylene glycol slurry containing 0.06 parts by weight of phosphoric acid, and 0.04 parts by weight of antimony oxide were added and heated to carry out a polymerization reaction. C
The amounts of aCO 3 and Al 2 O 3 were adjusted to 0.54 wt% and 0.3 wt% with respect to the finally obtained polymer. After the polymerization was completed, the polymer was pelletized. This was designated as a thermoplastic polymer A for the outer layer. In addition, a PET containing substantially no particles was produced by a conventional method, and this was used as a thermoplastic polymer B for a film layer.

【0029】次に、これらの熱可塑性ポリマーA、Bを
それぞれ180℃で3時間減圧乾燥し、それぞれを2台
の押し出し機に供給し、300℃で溶融しながら上記2
種の熱可塑性ポリマーを3層用の矩形の合流ブロックで
合流積層し、静電印加キャスト法を用いて表面温度30
℃のキャスティングドラムに巻きつけて冷却固化した。
これにより、熱可塑性ポリマーBからなるフィルム層の
両面に熱可塑性ポリマーAからなる外層を備えた3層構
造の未延伸フィルムを作成した。この共押出しにおい
て、吐出量を調節することにより、未延伸フィルムの総
厚さ、熱可塑性ポリマーAからなる外層の厚さを制御し
た。
Next, each of these thermoplastic polymers A and B was dried under reduced pressure at 180 ° C. for 3 hours, supplied to two extruders and melted at 300 ° C.
Thermoplastic polymers of the kind are combined and laminated in a rectangular confluent block for three layers, and a surface temperature of 30 is applied using an electrostatically applied casting method.
It was wound around a casting drum at ℃ and cooled and solidified.
In this way, an unstretched film having a three-layer structure was prepared in which the outer layer made of the thermoplastic polymer A was provided on both sides of the film layer made of the thermoplastic polymer B. In this co-extrusion, the total thickness of the unstretched film and the thickness of the outer layer made of the thermoplastic polymer A were controlled by adjusting the discharge amount.

【0030】次に、この未延伸フィルムを温度80℃に
てロールの周速差を利用して長手方向(MD方向)に
2.5〜5.0倍延伸して一軸延伸フィルムとした。さ
らに、ステンタを用いて上記の一軸延伸フィルムを10
0℃に加熱しながら延伸速度2000%/分で幅方向に
2.5〜4.0倍延伸した後、定長下で200℃にて5
秒間熱処理することにより、可撓性支持体としての3層
構造の二軸配向PET(厚さ14μm)を得た。
Next, this unstretched film was stretched at a temperature of 80 ° C. in the longitudinal direction (MD direction) by a factor of 2.5 to 5.0 using the peripheral speed difference of the rolls to obtain a uniaxially stretched film. Further, the above uniaxially stretched film 10
While heating at 0 ° C, the film was stretched at a stretching rate of 2000% / min in the width direction by 2.5 to 4.0 times, and then at a constant length at 200 ° C for 5 times.
By heat treatment for 2 seconds, biaxially oriented PET (thickness: 14 μm) having a three-layer structure as a flexible support was obtained.

【0031】このようにして作成した二軸配向PETの
外層の平均厚みt(μm)、CaCO3 粒子の大なる平
均粒径d1(μm)、CaCO3 粒子の小なる平均粒径
d2(μm)およびこれらの粒子の含有量をそれぞれ下
記表1に示した。なお、2つの外層は両方とも同じ組成
および厚さとした。
The average thickness t of the outer layer of the thus two was created by axially oriented PET (μm), an average particle diameter d1 becomes larger of CaCO 3 particles ([mu] m), an average particle diameter d2 becomes smaller of CaCO 3 particles ([mu] m) The contents of these particles are shown in Table 1 below. The two outer layers had the same composition and thickness.

【0032】次に、磁性層を形成するために下記の組成
の磁性塗料を用意した。
Next, a magnetic coating material having the following composition was prepared to form a magnetic layer.

【0033】 (磁性塗料の組成) Co−被着γ−Fe2 O3 (比表面積(BET値)35m2 /g) … 100重量部 塩化ビニル−酢酸ビニル共重合体 … 12重量部 ポリウレタン樹脂 … 8重量部 α−Al2 O3 … 3重量部 カーボンブラック … 3重量部 脂肪酸(ステアリン酸) … 2.6重量部 メチルエチルケトン … 80重量部 シクロヘキサノン … 80重量部 トルエン … 40重量部 上記の組成の磁性塗料をSGM(サンドグラインドミ
ル)中で4時間分散した後、ポリイソシアネート硬化剤
4部を添加して30分間攪拌混合した。得られた塗料を
フィルターで循環濾過し、しかる後この塗料を上述のよ
うに作成した各二軸配向PETフィルムの片面に磁場を
印加しながら磁性塗料を塗布し乾燥させた。次いで、表
面加工処理(カレンダリング)を施した後、12.7m
m幅にスリットしてビデオテープ(磁気記録媒体)サン
プルを作製した。 (実施例2〜25)可撓性支持体(二軸配向PET)の
外層の平均厚みt(μm)、CaCO3 粒子の大なる平
均粒径d1(μm)、CaCO3 粒子の小なる平均粒径
d2(μm)、CaCO3 粒子含有量、脂肪酸含有量等
を下記表1に示されるように種々変えた。それ以外は、
前記実施例1と同様にして実施例2〜25のビデオテー
プ(磁気記録媒体)サンプルを作製した。 (比較例1〜10)可撓性支持体(二軸配向PET)の
外層の平均厚みt(μm)、CaCO3 粒子の大なる平
均粒径d1(μm)、CaCO3 粒子の小なる平均粒径
d2(μm)、CaCO3 粒子含有量、脂肪酸含有量等
を下記表2に示されるように種々変えた。それ以外は、
前記実施例1と同様にして比較例1〜10のビデオテー
プ(磁気記録媒体)サンプルを作製した。
(Composition of magnetic paint) Co-adhered γ-Fe 2 O 3 (specific surface area (BET value) 35 m 2 / g) 100 parts by weight vinyl chloride-vinyl acetate copolymer 12 parts by weight Polyurethane resin 8 parts by weight α-Al 2 O 3 3 parts by weight carbon black 3 parts by weight fatty acid (stearic acid) 2.6 parts by weight methyl ethyl ketone 80 parts by weight cyclohexanone 80 parts by weight toluene 40 parts by weight Magnetic properties of the above composition The coating material was dispersed in SGM (sand grind mill) for 4 hours, 4 parts of a polyisocyanate curing agent was added, and the mixture was stirred and mixed for 30 minutes. The obtained coating material was circulated and filtered with a filter, and then the coating material was dried by applying a magnetic coating to one surface of each of the biaxially oriented PET films prepared as described above while applying a magnetic field. Then, after performing surface processing (calendering), 12.7m
A video tape (magnetic recording medium) sample was prepared by slitting the film into a width of m. (Example 2-25) flexible average of the outer layer of the support (biaxially oriented PET) Thickness t (μm), CaCO 3 mean particle size particle large consisting of d1 (μm), CaCO 3 becomes small particle mean particle The diameter d2 (μm), CaCO 3 particle content, fatty acid content, etc. were variously changed as shown in Table 1 below. Other than that,
The video tape (magnetic recording medium) samples of Examples 2 to 25 were prepared in the same manner as in Example 1. (Comparative Examples 1-10) a flexible average of the outer layer of the support (biaxially oriented PET) Thickness t (μm), CaCO 3 mean particle size particle large consisting of d1 (μm), CaCO 3 becomes small particle mean particle The diameter d2 (μm), CaCO 3 particle content, fatty acid content, etc. were variously changed as shown in Table 2 below. Other than that,
The video tape (magnetic recording medium) samples of Comparative Examples 1 to 10 were prepared in the same manner as in Example 1.

【0034】[0034]

【表1】 [Table 1]

【0035】[0035]

【表2】 表1および表2に示される実施例1〜25および比較例
1〜10の各サンプルについて、以下に示す項目を測定
評価した。
[Table 2] For each sample of Examples 1 to 25 and Comparative Examples 1 to 10 shown in Table 1 and Table 2, the following items were measured and evaluated.

【0036】中心線平均粗さ(Ra) (株)小坂研究所製表面形状測定装置サーフコーダーF
E−3F型を用い、針半径2μm、倍率5万倍、カット
オフ0.08mmの条件下にチャートを書かせ、JIS
B 0601(1982)に準拠して求めた。なお、
測定長0.8mm、n=10の平均値とし、単位はnm
に換算した。
Center Line Average Roughness (Ra) Surface Profile Measuring Device Surfcoder F, made by Kosaka Laboratory Ltd.
Using the E-3F type, let the chart be written under the conditions of a needle radius of 2 μm, a magnification of 50,000 times and a cutoff of 0.08 mm.
It was determined according to B 0601 (1982). In addition,
Measured length 0.8 mm, average value of n = 10, unit is nm
Converted to.

【0037】C/N特性 ヒューレットパッカード社製シンセサイザー3325A
にて得られる周波数4MHzの信号を、日本ビクター
(株)製ビデオカセットレコーダーBR7000Aを用
いて磁気記録媒体に記録した後、同ビデオカセットレコ
ーダーにて再生し、ヒューレットパッカード社製スペク
トラムアナライザー3585Aにて再生信号の4MHz
と3.9MHzの出力比を計測した。そして、標準テー
プ(TDK(株)製)の出力を0dBとして、その差を
示した。
C / N Characteristics Hewlett Packard Synthesizer 3325A
After recording the signal of frequency 4MHz obtained in 1. on a magnetic recording medium using a video cassette recorder BR7000A manufactured by Victor Company of Japan, Ltd., it is reproduced by the same video cassette recorder and reproduced by a spectrum analyzer 3585A manufactured by Hewlett-Packard Company. 4MHz of signal
And an output ratio of 3.9 MHz was measured. Then, the output of the standard tape (manufactured by TDK Corporation) was set to 0 dB, and the difference was shown.

【0038】走行摩擦 島多技研(株)製テープ摩擦試験機(model:RT
F−2000)を使用して摩擦係数を測定した。測定
は、テープの走行面側を3mm径のステンレス製のピン
に180°捲き付け、テープに一定のバックテンション
(20g)を負荷し、走行スピードを3.3cm/se
cとしてこの時の摩擦係数を測定した。
Running friction Shimata Giken Co., Ltd. tape friction tester (model: RT)
F-2000) was used to measure the coefficient of friction. For the measurement, the running surface side of the tape was wound around a stainless steel pin having a diameter of 3 mm by 180 °, a constant back tension (20 g) was applied to the tape, and the running speed was 3.3 cm / se.
The coefficient of friction at this time was measured as c.

【0039】走行性 VTRにて20秒間PLAYし、リワインドトルク25
0g/cmでREW(リワインド)する作業を50回繰
り返し、そのREW時間を計測し、走行安定性を5段階
にランク付けした。
[0039] and PLAY 20 seconds by the running of VTR, rewind torque 25
The work of REW (rewinding) at 0 g / cm was repeated 50 times, the REW time was measured, and the running stability was ranked in 5 stages.

【0040】判断基準は以下の通り。The judgment criteria are as follows.

【0041】◎…平均REW時間が6秒以内で、かつ5
0回のREW時間にばらつきがない ○〜◎…平均REW時間が7秒以内で、かつ50回のR
EW時間にばらつきがない ○…平均REW時間が7秒以内で、かつ50回のREW
時間にばらつきが少ない △…平均REW時間が7秒以上で、かつ50回のREW
時間にばらつきが非常に大きい ×…平均REW時間が9秒以上か、走行ストップしてし
まう捲き性 SONY社製HSP800にて、転写後の捲き姿(2次
捲き)を目視評価し、5段階にランク付けした。判断基
準は以下の通り。
A: Average REW time is within 6 seconds and 5
There is no variation in the REW time of 0 times ○ to ◎ ... The average REW time is within 7 seconds and R of 50 times
There is no variation in EW time ..... Average REW time is within 7 seconds and 50 times of REW.
There is little variation in time. △ ... Average REW time is 7 seconds or more and 50 times of REW.
Or time variation is very large × ... Average REW time 9 seconds or more, by the running stop to cause Maki of SONY Corporation HSP800, Maki appearance after the transfer (the secondary Maki) was visually evaluated, in 5 steps Ranked. The judgment criteria are as follows.

【0042】◎…捲き乱れが無い ○〜◎…ほとんど捲き乱れが無い ○…若干捲き乱れが確認できる △…捲き乱れが発生する ×…非常に捲き乱れが発生するか、脱線してしまう耐スクラッチ性 VTRにてPLAY、REWを50回繰り返し走行さ
せ、ベース走行面のスクラッチを5段階にランク付けし
た。
∘: No winding disorder ○ to ◎: Almost no winding disorder ○: Slight winding disorder can be confirmed Δ: Winding disorder occurs ×: Extremely winding disorder or derailing Scratch resistance PLAY, REW were repeatedly run 50 times on the sex VTR, and the scratches on the base running surface were ranked in 5 stages.

【0043】判断基準は以下の通り。The judgment criteria are as follows.

【0044】◎…ベース走行面にキズがほとんど発生し
ていない ○〜◎…ベース走行面に浅いキズが若干発生している ○…ベース走行面に若干キズが発生している △…ベース走行面にかなりキズが発生している ×…ベース走行面に多数のキズが発生している塗膜強度 VTRにてスチル特性を評価し、5段階評価した。判断
基準は以下の通り。
⊚: Almost no scratch on the base running surface ○ to ◎: Slightly scratch on the base running surface ○: Slightly scratch on the base running surface Δ: Base running surface considerable scratches and rated the still characteristics in coating strength VTR many scratches occurred in the × ... base running surface that is occurring, and out to. The judgment criteria are as follows.

【0045】◎…スチル特性:120min以上 ○〜◎…スチル特性:60minを超え、120min
以下 ○…スチル特性:30minを超え、60min以下 △…スチル特性:10minを超え、30min以下 ×…スチル特性:10min以下 これらの測定評価結果を下記表3および表4に示す。
◎ ... Still characteristics: 120 min or more ○ to ◎ ... Still characteristics: over 60 min, 120 min
◯: Still characteristic: more than 30 min and 60 min or less Δ: Still characteristic: more than 10 min and 30 min or less × ... Still characteristic: 10 min or less The measurement evaluation results are shown in Tables 3 and 4 below.

【0046】[0046]

【表3】 [Table 3]

【0047】[0047]

【表4】 表3および表4に示される結果から明らかなように、本
発明の磁気記録媒体(実施例1〜25)は、特に高出力
が得られるとともに、走行特性にも優れ、さらには捲き
特性、耐スクラッチ性、および塗膜強度にも優れる。
[Table 4] As is clear from the results shown in Tables 3 and 4, the magnetic recording media of the present invention (Examples 1 to 25) were able to obtain particularly high output and were excellent in running characteristics as well as winding characteristics and durability. Excellent scratch resistance and coating strength.

【0048】[0048]

【発明の効果】以上詳述したように、本発明の磁気記録
媒体は、フィルム層の少なくとも磁性層形成面と反対側
に外層を備えており、この外層は、少なくとも大小2種
の平均粒径を備えるCaCO3 粒子を含有しており、そ
れらの平均粒径d1およびd2は、それぞれ外層の厚さ
tとの関係で所定の条件を満たすように設定されている
ので、特に高出力が得られるとともに、走行特性にも優
れ、さらには捲き特性、耐スクラッチ性、および塗膜強
度にも優れる磁気記録媒体が実現できる。
As described in detail above, the magnetic recording medium of the present invention is provided with an outer layer on at least the side opposite to the surface on which the magnetic layer is formed in the film layer, and the outer layer has at least two types of average particle diameters. In particular, a high output can be obtained, because the CaCO 3 particles containing are included and their average particle diameters d1 and d2 are set so as to satisfy a predetermined condition in relation to the thickness t of the outer layer. At the same time, it is possible to realize a magnetic recording medium which is excellent in running characteristics, winding characteristics, scratch resistance, and coating film strength.

【図面の簡単な説明】[Brief description of drawings]

【図1】本発明の磁気記録媒体の一例を示す概略断面図
である。
FIG. 1 is a schematic cross-sectional view showing an example of a magnetic recording medium of the present invention.

【図2】本発明の磁気記録媒体の一例を示す概略断面図
である。
FIG. 2 is a schematic sectional view showing an example of a magnetic recording medium of the present invention.

【符号の説明】[Explanation of symbols]

1…磁気記録媒体 2…可撓性支持体 3…フィルム層 4…外層 5…磁性層 1 ... Magnetic recording medium 2 ... Flexible support 3 ... Film layer 4 ... Outer layer 5 ... Magnetic layer

───────────────────────────────────────────────────── フロントページの続き (72)発明者 川上 義雄 東京都中央区日本橋一丁目13番1号 ティ ーディーケイ株式会社内 ─────────────────────────────────────────────────── ─── Continuation of the front page (72) Inventor Yoshio Kawakami 1-13-1 Nihonbashi, Chuo-ku, Tokyo Inside TDC Corporation

Claims (3)

【特許請求の範囲】[Claims] 【請求項1】 可撓性支持体上に磁性層を設けてなる磁
気記録媒体において、 前記可撓性支持体は熱可塑性ポリマーを主成分とするフ
ィルム層と、該フィルム層の少なくとも磁性層形成面と
反対側に設けられた外層とを有し、 前記外層は、少なくとも大小2種の平均粒径を備えるC
aCO3 粒子を含有しており、外層の厚さをt(μ
m)、CaCO3 粒子の大なる平均粒径をd1(μ
m)、CaCO3 粒子の小なる平均粒径をd2(μm)
とした場合、含有されるべく大小2種のCaCO3 平均
粒径d1およびd2は、それぞれ外層の厚さtとの関係
で下記の条件を満たし、かつ、前記大なる平均粒径のC
aCO3 粒子は100〜1200ppmの範囲で、前記
小なる平均粒径のCaCO3 粒子は3000〜1000
0ppmの範囲で、それぞれ前記外層内に含有されるこ
とを特徴とする磁気記録媒体。 (1)0.5≦t≦1.0の場合 0.6≦d1≦0.8t+0.4 0.2≦d2≦0.8 d1−d2≧0.2 (2)1.0<t≦1.5の場合 0.6≦d1≦1.2 0.2≦d2≦0.8 d1−d2≧0.2
1. A magnetic recording medium in which a magnetic layer is provided on a flexible support, wherein the flexible support is a film layer containing a thermoplastic polymer as a main component, and at least a magnetic layer of the film layer is formed. And an outer layer provided on the opposite side of the surface, wherein the outer layer has at least two kinds of average particle sizes, C and C.
It contains aCO 3 particles and has a thickness of t (μ
m), the larger average particle size of CaCO 3 particles is d1 (μ
m), the smaller average particle size of CaCO 3 particles is d2 (μm)
In this case, the CaCO 3 average particle sizes d1 and d2 of two kinds, large and small, to be contained satisfy the following conditions in relation to the thickness t of the outer layer, respectively, and C of the large average particle size is
The aCO 3 particles are in the range of 100 to 1200 ppm, and the CaCO 3 particles having a smaller average particle diameter are 3000 to 1000.
A magnetic recording medium, characterized in that each is contained in the outer layer within a range of 0 ppm. (1) In the case of 0.5 ≦ t ≦ 1.0 0.6 ≦ d1 ≦ 0.8t + 0.4 0.2 ≦ d2 ≦ 0.8 d1-d2 ≧ 0.2 (2) 1.0 <t ≦ In the case of 1.5 0.6 ≦ d1 ≦ 1.2 0.2 ≦ d2 ≦ 0.8 d1-d2 ≧ 0.2
【請求項2】 前記外層はさらに前記フィルム層の磁性
層形成面側にも形成される請求項1記載の磁気記録媒
体。
2. The magnetic recording medium according to claim 1, wherein the outer layer is further formed on the magnetic layer formation surface side of the film layer.
【請求項3】 前記磁性層中には磁性材料および脂肪酸
が含有されており、前記磁性材料は、30〜60m2 /
gの比表面積を備え、前記脂肪酸は塗膜との重量比にお
いて、0.5〜1.5wt%含有されることを特徴とす
る請求項1または請求項2に記載の磁気記録媒体。
3. A magnetic material and a fatty acid are contained in the magnetic layer, and the magnetic material is 30 to 60 m 2 /
3. The magnetic recording medium according to claim 1, wherein the magnetic recording medium has a specific surface area of g and contains 0.5 to 1.5 wt% of the fatty acid in a weight ratio with respect to the coating film.
JP6192757A 1994-07-26 1994-07-26 Magnetic recording media Withdrawn JPH0836736A (en)