JPH0851115A - Method for manufacturing semiconductor device - Google Patents

Method for manufacturing semiconductor device

Info

Publication number
JPH0851115A
JPH0851115A JP7218891A JP21889195A JPH0851115A JP H0851115 A JPH0851115 A JP H0851115A JP 7218891 A JP7218891 A JP 7218891A JP 21889195 A JP21889195 A JP 21889195A JP H0851115 A JPH0851115 A JP H0851115A
Authority
JP
Japan
Prior art keywords
pad
substrate
semiconductor substrate
semiconductor
particles
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP7218891A
Other languages
Japanese (ja)
Other versions
JP2755927B2 (en
JPH0851115A5 (en
Inventor
Katsuya Okumura
勝弥 奥村
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toshiba Corp
Original Assignee
Toshiba Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toshiba Corp filed Critical Toshiba Corp
Priority to JP7218891A priority Critical patent/JP2755927B2/en
Publication of JPH0851115A publication Critical patent/JPH0851115A/en
Application granted granted Critical
Publication of JP2755927B2 publication Critical patent/JP2755927B2/en
Publication of JPH0851115A5 publication Critical patent/JPH0851115A5/ja
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

(57)【要約】 【課題】 本発明は、半導体基板の素子への熱影響を軽
減でき、拡散層の再拡散等を抑制することが可能な半導
体装置の製造方法を提供する。 【解決手段】 球状のAuからなる導電性連結粒を形成
する工程と、支持基板上の所望位置に前記連結粒を複数
個配列、固定する工程と、半導体素子が少なくとも形成
され、かつ表面にパッドが形成された半導体基板を前記
支持基板上にその連結粒と該半導体基板のパッドとが合
致するように配置する工程と、前記連結粒を前記半導体
基板のパッドに前記連結粒および前記パッドを溶融させ
ることなく圧接させ、パッド側に移行させる工程とを具
備したことを特徴とする。
The present invention provides a method for manufacturing a semiconductor device, which can reduce the thermal influence on elements of a semiconductor substrate and can suppress re-diffusion of a diffusion layer. SOLUTION: A step of forming conductive connecting particles of spherical Au, a step of arranging and fixing a plurality of the connecting particles at a desired position on a supporting substrate, at least a semiconductor element is formed, and a pad is formed on the surface. Arranging the semiconductor substrate on which the connecting particles are formed on the supporting substrate so that the connecting particles and the pads of the semiconductor substrate match, and melting the connecting particles and the connecting particles to the pads of the semiconductor substrate. And a step of transferring to the pad side without pressing.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【発明の属する技術分野】本発明は、半導体装置の製造
方法に関し、特に半導体基板上のパッドに導電性連結粒
を移行させる工程を改良した半導体装置の製造方法に係
わる。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method of manufacturing a semiconductor device, and more particularly to a method of manufacturing a semiconductor device with an improved process of transferring conductive connecting particles to pads on a semiconductor substrate.

【0002】[0002]

【従来の技術】従来、半導体装置においては信号の入出
力端子であるパッドを外部基板に接続するために、該パ
ッドにメッキ手段によりバンプを形成することが行われ
ている。しかしながら、かかる方法ではバンプを充分な
大きさに成長させられず、しかもメッキ法を採用するこ
とから複雑な工程を必要とし、更にバンプが硬く外部基
板との接合信頼性が低いという問題があった。
2. Description of the Related Art Conventionally, in a semiconductor device, in order to connect a pad, which is a signal input / output terminal, to an external substrate, a bump is formed on the pad by a plating means. However, with such a method, the bumps cannot be grown to a sufficient size, and since the plating method is used, complicated steps are required, and the bumps are hard and the bonding reliability with the external substrate is low. .

【0003】このようなことから、本出願人は金属、特
に柔らかいAuやAlからなる連結粒をパッドに固着
し、該連結粒を介して外部基板に固着、接続する方法を
提案した。以下、この連結粒のパッドへの固着方法を図
17に示す外部にヒ―タ1が配設された内径40μmの
銃筒2からなる連結粒固着機3を参照して詳細に説明す
る。
In view of the above, the present applicant has proposed a method in which connecting particles made of metal, particularly soft Au or Al, are fixed to the pad, and fixed and connected to the external substrate via the connecting particles. Hereinafter, the method of fixing the connected particles to the pad will be described in detail with reference to the connected particle fixing machine 3 shown in FIG. 17 which is composed of a barrel 2 having an inside diameter of 40 μm with a heater 1 disposed outside.

【0004】まず、ヒ―タを内蔵した支持台(図示せ
ず)上に複数のパッド4が形成された半導体基板5を配
置する。つづいて、銃筒3を前記半導体基板5のパッド
4に位置合せした後、銃筒2をヒ―タ1によって約35
0℃に保持し、該銃筒2に内径40μmの球状をなすA
uからなる連結粒6を挿入し、圧縮窒素7により前記連
結粒6を加熱しながら加速度をもたせて放射して前記支
持台により約300℃に加熱されているパッド4上に熱
圧接して固着する。しかしながら、上記従来の連結粒の
固着方法では一度に複数個の連結粒を半導体基板のパッ
ドに固着できず、半導体装置の生産性が低いという問題
があった。
First, a semiconductor substrate 5 having a plurality of pads 4 formed thereon is arranged on a support table (not shown) containing a heater. Next, after aligning the barrel 3 with the pad 4 of the semiconductor substrate 5, the barrel 2 is moved by the heater 1 to about 35 mm.
Hold the temperature at 0 ° C., and make a spherical shape A with an inner diameter of 40 μm in the barrel 2.
The connecting grains 6 made of u are inserted, and the connecting grains 6 are heated by the compressed nitrogen 7 while being accelerating and radiated to be fixed by thermocompression bonding onto the pad 4 heated to about 300 ° C. by the supporting table. To do. However, the above-described conventional method of fixing the connecting particles has a problem that a plurality of connecting particles cannot be fixed to the pad of the semiconductor substrate at one time and the productivity of the semiconductor device is low.

【0005】[0005]

【発明が解決しようとする課題】本発明は、半導体基板
の素子への熱影響を軽減でき、拡散層の再拡散等を抑制
することが可能な半導体装置の製造方法を提供しようと
するものである。
SUMMARY OF THE INVENTION The present invention is intended to provide a method of manufacturing a semiconductor device which can reduce the thermal influence on the elements of the semiconductor substrate and can suppress the re-diffusion of the diffusion layer. is there.

【0006】[0006]

【課題を解決するための手段】本発明は、Auからなる
球状の導電性連結粒を形成する工程と、支持基板上の所
望位置に前記連結粒を複数個配列、固定する工程と、半
導体素子が少なくとも形成され、かつ表面にパッドが形
成された半導体基板を前記支持基板上にその連結粒と該
半導体基板のパッドとが合致するように配置する工程
と、前記連結粒を前記半導体基板のパッドに前記連結粒
および前記パッドを溶融させることなく圧接させ、パッ
ド側に移行させる工程とを具備したことを特徴とする半
導体装置の製造方法である。
According to the present invention, a step of forming spherical conductive connecting particles made of Au, a step of arranging and fixing a plurality of the connecting particles at a desired position on a supporting substrate, and a semiconductor device. And at least forming a semiconductor substrate on the surface of which a pad is formed on the supporting substrate so that the connecting grain and the pad of the semiconductor substrate are aligned with each other; And a step of bringing the connecting particles and the pad into pressure contact with each other without melting and transferring to the pad side.

【0007】本発明は、予め支持基板上に複数個のAu
からなる導電性連結粒を所望の配列状態で仮固定し、こ
の支持基板上にパッドが形成された半導体基板を該パッ
ドが前記連結粒に合致するように配置し、該連結粒をパ
ッドに前記連結粒および前記パッドを溶融させることな
く圧接させて同パッドに移行させることによって、半導
体基板の素子に多大な熱影響を与えることなく、複数個
の導電性連結粒を効率よく半導体基板のパッドに固着で
きる半導体装置の製造方法を提供できる。
According to the present invention, a plurality of Au are previously formed on the supporting substrate.
The conductive connecting particles consisting of are temporarily fixed in a desired arrangement state, a semiconductor substrate having pads formed on the supporting substrate is arranged so that the pads match the connecting particles, and the connecting particles are attached to the pads. By transferring the connecting particles and the pad to the pads by pressing them without melting them, the conductive connecting particles can be efficiently applied to the pads of the semiconductor substrate without significantly affecting the elements of the semiconductor substrate. A method of manufacturing a semiconductor device that can be fixed can be provided.

【0008】[0008]

【実施例】以下、本発明を三次元LSIの製造に適用し
た例について図面を参照して詳細に説明する。 (I)まず、二次元のLSI製造法により厚さ450μ
mのシリコンウェハ11に半導体素子、素子間の配線
(いずれも図示せず)及びAl膜からなる50μm×5
0μmのパッド12、13を形成した。なお、これらパ
ッドのうち、後述する連結孔に対応するパッド13の一
部は、層間絶縁膜に形成された開孔部内に埋込まれ、か
つ該開孔部底部の基板表面には薄い酸化膜が形成されて
いる。この酸化膜は、ダイソ―トテストの障害となるパ
ッドの基板表面への電気的な接続を防止するために用い
られる。但し、前記薄い酸化膜の代わりに開孔部の底部
を含む周辺の基板表面にpn接合を作るための不純物拡
散層を形成してもよい。つづいて、前記パッド13に対
応するシリコンウェハ11の裏面に等方性エッチングと
異方性エッチングの組合わせにより開口寸法が30μm
×30μm、深さが50μmのワインカップ状の孔14
を開孔した(図1図示)。なお、エッチングは、いずれ
もフッ素系又は塩素系ガスのプラズマを用いて行なっ
た。
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS An example in which the present invention is applied to the manufacture of a three-dimensional LSI will be described in detail below with reference to the drawings. (I) First, the thickness is 450 μm by the two-dimensional LSI manufacturing method.
50 μm × 5 consisting of a semiconductor element, wiring between elements (none of which are shown) and an Al film on a silicon wafer 11 of m.
The 0 μm pads 12 and 13 were formed. Of these pads, a part of a pad 13 corresponding to a connecting hole described later is embedded in an opening formed in the interlayer insulating film, and a thin oxide film is formed on the substrate surface at the bottom of the opening. Are formed. This oxide film is used to prevent electrical connection of the pad to the substrate surface, which hinders the die-sort test. However, instead of the thin oxide film, an impurity diffusion layer for forming a pn junction may be formed on the peripheral substrate surface including the bottom of the opening. Next, the opening size is 30 μm on the back surface of the silicon wafer 11 corresponding to the pad 13 by a combination of isotropic etching and anisotropic etching.
Wine cup-shaped hole 14 of × 30 μm and depth of 50 μm
Was opened (shown in FIG. 1). The etching was performed using plasma of fluorine-based gas or chlorine-based gas.

【0009】(II)次いで、図2に示すように前記シリ
コンウェハのダイソ―トテストを行なった後、ダイシン
グを施して個々のチップを作り、選別を行なって良品チ
ップ15を得た。つづいて、図3に示すように良品チッ
プ15の裏面全体を異方性エッチングを行なって厚さ4
5μmの薄板状の積層用半導体基板16を作製した。こ
の異方性エッチングの工程において、裏面に開口された
ワインカップ状の孔14は略その形状が保持されながら
エッチングされるため、テ―パ状の連結孔17が形成さ
れた。また、前記エッチングに際して前述した開孔部底
部の薄い酸化膜除去を行なって、該連結孔17の底部に
開孔部に対応してパッド13の一部を露出させた。
(II) Next, as shown in FIG. 2, the silicon wafer was subjected to a die-sort test, and then dicing was performed to make individual chips, which were selected to obtain non-defective chips 15. Subsequently, as shown in FIG. 3, the entire back surface of the good chip 15 is anisotropically etched to a thickness of 4
A 5 μm thin plate-shaped semiconductor substrate 16 for lamination was produced. In this anisotropic etching step, since the wine cup-shaped hole 14 opened on the back surface is etched while maintaining its shape, a taper-shaped connecting hole 17 is formed. Further, during the etching, the thin oxide film on the bottom of the opening is removed to expose a part of the pad 13 at the bottom of the connecting hole 17 corresponding to the opening.

【0010】(III) 次いで、図4に示すように前記積層
用半導体基板16の連結孔17に例えばAuからなる球
状の連結粒24を固着するが、この方法を図8〜図10
に示す工程により詳細に説明する。
(III) Next, as shown in FIG. 4, spherical connecting particles 24 made of, for example, Au are fixed in the connecting holes 17 of the semiconductor substrate 16 for lamination.
The process will be described in detail below.

【0011】まず、後述する連結粒が仮固定される部分
を含む周辺に凸部21が形成された厚さ1mmのガラス
支持基板22を用意し、この支持基板22の凸部21を
含む表面に回転塗布法により厚さ8〜10μmのポリイ
ミド膜23を形成し、150℃で30分間ベ―クして溶
剤を揮発させた。こうして形成されたポリイミド膜23
は、高温でのベ―クを行なわないため、柔らかく、若干
の粘着性を有していた。なお、該ポリイミド膜23には
後述する半導体基板との位置合せを行なうためのマ―ク
(図示せず)がエッチング等により形成されている。つ
づいて、ポリイミド膜23上に30μm径の球状をなす
Auからなる連結粒24を前述した図3で製造された半
導体基板6のパッド3と同様な配列位置で仮固定した
(図8図示)。
First, a glass support substrate 22 having a thickness of 1 mm is formed on the periphery of which a convex portion 21 is formed, including a portion where the connecting grains to be described later are temporarily fixed, and the surface of the supporting substrate 22 including the convex portion 21 is prepared. A polyimide film 23 having a thickness of 8 to 10 μm was formed by spin coating and baked at 150 ° C. for 30 minutes to volatilize the solvent. Polyimide film 23 thus formed
Since it was not baked at a high temperature, it was soft and had some tackiness. A mark (not shown) for aligning with a semiconductor substrate, which will be described later, is formed on the polyimide film 23 by etching or the like. Subsequently, 30 μm-diameter spherical connecting particles 24 made of Au having a diameter of 30 μm were temporarily fixed on the polyimide film 23 at the same arrangement position as the pad 3 of the semiconductor substrate 6 manufactured in FIG. 3 described above (see FIG. 8).

【0012】次いで、図9に示すようにガラス支持基板
22に前記半導体基板16を該基板16のパッド13を
有する連結孔17が支持基板22の連結粒24と合致す
るように配置させた。この位置合せは、支持基板22が
透明なガラスからなるため、該支持基板22の裏面側か
らポリイミド膜23に形成された図示しないマ―ク及び
半導体基板の裏面に付されたマ―ク(図示せず)とを合
致するように半導体基板16を移動させることにより行
なった。なお、図9中の18は基板16とパッド13と
を電気的に絶縁するための層間絶縁膜、19は該絶縁膜
18に形成され、パッド13の一部を前記連結孔17底
部に露出させるための開孔部である。つづいて、半導体
基板16のパッド13側より加熱機構を有する押え治具
25で300℃に加熱した状態で半導体基板16とガラ
ス支持基板22とを圧接することによって、Auからな
る連結粒24が基板16の連結孔17内上部のAlから
なるパッド13に接触しAu−Alの金属間化合物を形
成して固着した(図10図示)。この工程において、連
結粒24が仮固定されている支持基板22部分には凸部
21が形成されているため、連結粒24を基板16の連
結孔17内に挿入するに際して、支持基板22上のポリ
イミド膜21が基板16裏面側に接触することなく該連
結粒24を連結孔17内上部のパッド13に接触でき
る。なお、押え治具25に超音波を印加して連結粒の固
着を更に促進したり、低温での固着を行なうようにして
もよい。しかる後、ガラス支持基板22を下方に移動さ
せることにより、連結粒24はポリイミド膜23から剥
離した。こうした工程により図4に示すように連結孔1
7に対応するパッド13の露出部にAuの連結粒24が
固着された積層用半導体基板16を得た。
Next, as shown in FIG. 9, the semiconductor substrate 16 was placed on the glass supporting substrate 22 so that the connecting holes 17 having the pads 13 of the substrate 16 were aligned with the connecting grains 24 of the supporting substrate 22. In this alignment, since the support substrate 22 is made of transparent glass, a mark (not shown) formed on the polyimide film 23 from the back surface side of the support substrate 22 and a mark attached to the back surface of the semiconductor substrate (see FIG. (Not shown) is carried out by moving the semiconductor substrate 16 so as to agree with (not shown). In FIG. 9, 18 is an interlayer insulating film for electrically insulating the substrate 16 and the pad 13, 19 is formed on the insulating film 18, and a part of the pad 13 is exposed at the bottom of the connecting hole 17. It is an opening part for. Subsequently, the semiconductor substrate 16 and the glass supporting substrate 22 are pressed against each other from the pad 13 side of the semiconductor substrate 16 by the pressing jig 25 having a heating mechanism to press the semiconductor substrate 16 and the glass supporting substrate 22, so that the connecting particles 24 made of Au form the substrate. The pad 13 made of Al in the upper part of the connecting hole 17 of 16 was contacted to form an Au-Al intermetallic compound and fixed (FIG. 10). In this step, since the convex portion 21 is formed on the portion of the support substrate 22 to which the connecting particles 24 are temporarily fixed, when the connecting particles 24 are inserted into the connecting holes 17 of the substrate 16, the connecting substrate 24 on the supporting substrate 22 is inserted. The connecting grain 24 can be brought into contact with the pad 13 in the upper portion of the connecting hole 17 without the polyimide film 21 coming into contact with the back surface of the substrate 16. It should be noted that ultrasonic waves may be applied to the holding jig 25 to further promote the fixing of the connecting particles, or the fixing may be performed at a low temperature. Then, by moving the glass support substrate 22 downward, the connecting particles 24 were separated from the polyimide film 23. Through these steps, as shown in FIG.
Thus, the laminated semiconductor substrate 16 having the Au connecting particles 24 fixed to the exposed portion of the pad 13 corresponding to No. 7 was obtained.

【0013】(IV)次いで、二次元のLSI製造法によ
り厚さ450μmのシリコンウェハに半導体素子、素子
間の配線及びAl膜からなる50μm×50μmのパッ
ドを形成した。つづいて、ダイソ―トテストの後、前記
シリコンウェハをダイシングし、前記積層用半導体基板
16と電気的に接続される良品チップを選別し、図5に
示すようにこの良品チップ34表面のパッド35上に例
えばAuからなる球状の連結粒33を固着するが、この
方法を図11〜図13に工程により説明する。
(IV) Next, a 50 μm × 50 μm pad made of a semiconductor element, wiring between elements and an Al film was formed on a 450 μm thick silicon wafer by a two-dimensional LSI manufacturing method. Subsequently, after the die-sort test, the silicon wafer is diced to select non-defective chips electrically connected to the laminating semiconductor substrate 16, and as shown in FIG. The spherical connecting particles 33 made of, for example, Au are fixed to the above. This method will be described with reference to steps in FIGS. 11 to 13.

【0014】まず、厚さ1mmのガラス支持基板31表
面に回転塗布法により厚さ8〜10μmのポリイミド膜
32を形成し、150℃で30分間ベ―クして溶剤を揮
散させた。こうして形成されたポリイミド膜32は、高
温でのベ―クを行なわないため、柔らかく、若干の粘着
性を有していた。なお、該ポリイミド膜23には後述す
る半導体基板との位置合せを行なうためのマ―ク(図示
せず)がエッチング等により形成されている。つづい
て、ポリイミド膜32上に40μm径の球状をなすAu
からなる連結粒33を前記良品チップのパッドと同様な
配列位置で仮固定した(図11図示)。
First, a polyimide film 32 having a thickness of 8 to 10 μm was formed on the surface of a glass supporting substrate 31 having a thickness of 1 mm by a spin coating method, and baked at 150 ° C. for 30 minutes to volatilize the solvent. The polyimide film 32 thus formed was soft and had a slight adhesiveness because it was not baked at a high temperature. A mark (not shown) for aligning with a semiconductor substrate, which will be described later, is formed on the polyimide film 23 by etching or the like. Then, a spherical Au film having a diameter of 40 μm is formed on the polyimide film 32.
The connecting grains 33 consisting of were temporarily fixed at the same arrangement position as the pads of the non-defective chip (see FIG. 11).

【0015】次いで、図12に示すようにガラス支持基
板31に前述した方法により作製した良品チップ34を
その表面のパッド35が支持基板31の連結粒33と合
致するように配置させた。この位置合せは、支持基板3
1が透明なガラスからなるため、該支持基板31の裏面
側からポリイミド膜32に形成された図示しないマ―ク
及び良品チップ34の裏面に付されたマ―ク(図示せ
ず)とを合致するように良品チップ34を移動させるこ
とにより行なった。なお、図12中の36はチップ34
とパッド35とを電気的に絶縁するための層間絶縁膜で
ある。つづいて、良品チップ34側より加熱機構を有す
る押え治具37で300℃に加熱した状態で良品チップ
34とガラス支持基板31とを圧接することによって、
Auからなる連結粒33が良品チップ34表面のAlか
らなるパッド35に接触しAu−Alの金属間化合物を
形成して固着した(図13図示)。しかる後、ガラス支
持基板31を下方に移動させることにより、連結粒33
はポリイミド膜32から剥離した。こうした工程により
図5に示すように良品チップ34表面のパッド35上に
40μm径の球状をなすAuからなる連結粒33を固着
した。
Next, as shown in FIG. 12, the non-defective chip 34 produced by the above-described method was placed on the glass supporting substrate 31 so that the pads 35 on the surface thereof were aligned with the connecting grains 33 of the supporting substrate 31. This alignment is performed by the support substrate 3
Since 1 is made of transparent glass, the mark (not shown) formed on the polyimide film 32 from the back surface side of the support substrate 31 and the mark (not shown) provided on the back surface of the good chip 34 are matched. The non-defective chip 34 is moved so as to do so. Incidentally, 36 in FIG. 12 is a chip 34.
Is an interlayer insulating film for electrically insulating the pad 35 and the pad 35. Subsequently, the non-defective chip 34 and the glass support substrate 31 are pressure-contacted from the non-defective chip 34 side while being heated to 300 ° C. by the holding jig 37 having a heating mechanism.
The connecting particles 33 made of Au were brought into contact with the pad 35 made of Al on the surface of the non-defective chip 34 to form an Au-Al intermetallic compound and fixed (FIG. 13). Then, by moving the glass supporting substrate 31 downward, the connecting particles 33
Was peeled from the polyimide film 32. Through these steps, as shown in FIG. 5, the connecting particles 33 made of spherical Au having a diameter of 40 μm were fixed on the pad 35 on the surface of the good chip 34.

【0016】(V)次いで、前記(IV)の工程で作製し
た良品チップ34上に前記(I)〜(III)の工程により
作製した積層用半導体基板16を該チップ34のパッド
35上のAuからなる連結粒33と該半導体基板16の
連結孔17内のAuからなる連結粒24とが合致するよ
うに重ねた後、300℃に加熱しながら積層用半導体基
板16をチップ34に対して押し付けることにより連結
粒33、24を互いに固着した(図6図示)。つづい
て、積層された半導体基板16表面の所定のパッド1
2、13上に球状をなすAuの連結粒38を熱圧接して
固着した(図7図示)。
(V) Next, the stacking semiconductor substrate 16 manufactured by the steps (I) to (III) is placed on the non-defective chip 34 manufactured in the step (IV) by Au on the pad 35 of the chip 34. After connecting the connecting particles 33 made of (a) and the connecting particles 24 made of Au in the connecting holes 17 of the semiconductor substrate 16 so as to match each other, the stacking semiconductor substrate 16 is pressed against the chip 34 while being heated to 300 ° C. As a result, the connecting particles 33 and 24 were fixed to each other (shown in FIG. 6). Subsequently, a predetermined pad 1 on the surface of the stacked semiconductor substrates 16
The spherical connecting particles 38 of Au were fixed on the sheets 2 and 13 by thermocompression (see FIG. 7).

【0017】(VI)次いで、前記(I)〜 (III)と同様
な工程により複数枚の薄板状の積層用半導体基板を作製
し、これら半導体基板を前記図7により積層した半導体
基板16の上に前記(V)と同様な工程により順次積層
し、多層積み重ねた半導体装置(図示せず)を製造し
た。
(VI) Next, a plurality of thin plate-shaped semiconductor substrates for lamination are produced by the same steps as in (I) to (III), and these semiconductor substrates are laminated on the semiconductor substrate 16 shown in FIG. Then, a semiconductor device (not shown) was manufactured by sequentially stacking layers by the same process as (V).

【0018】以上のように本発明方法によれば、予めガ
ラス支持基板(例えば22)のポリイミド膜23上に複
数個のAuからなる連結粒24を所望の配列状態で仮固
定し、この支持基板22上にパッド13が形成された半
導体基板16を該パッド13が前記連結粒24に合致す
るように配置し、該連結粒24をパッド13に固着して
同パッド13に移行させることによって、複数個の連結
粒24を効率よく半導体基板16のパッド13に固着で
きる。しかも、良品チップ34のパッド35へのAuか
らなる連結粒33の固着もポリイミド膜32が被覆され
たガラス支持基板31を用いて同様に行なうため、複数
個の連結粒33を効率よく良品チップ34のパッド35
に固着できる。従って、半導体装置の生産性を著しく向
上できる。
As described above, according to the method of the present invention, a plurality of connecting particles 24 made of Au are temporarily fixed in advance in a desired arrangement on the polyimide film 23 of the glass supporting substrate (for example, 22). The semiconductor substrate 16 having the pad 13 formed on 22 is arranged so that the pad 13 is aligned with the connecting grain 24, and the connecting grain 24 is fixed to the pad 13 and transferred to the pad 13. The individual connecting particles 24 can be efficiently fixed to the pad 13 of the semiconductor substrate 16. Moreover, since the connecting particles 33 made of Au are fixed to the pads 35 of the non-defective chips 34 in the same manner by using the glass supporting substrate 31 covered with the polyimide film 32, the plurality of connecting particles 33 can be efficiently attached to the non-defective chips 34. The pad 35
Can stick to. Therefore, the productivity of the semiconductor device can be significantly improved.

【0019】また、本実施例の方法により製造された半
導体装置は半導体素子等が形成された良品チップ34と
同素子が形成された積層用半導体基板16の間、更に各
積層用半導体基板16間を積層用半導体基板16の連結
孔17に対応するパッド13の露出部及び相手側のパッ
ド35にAuからなる連結粒33、24、38を介して
固着、積層するため、高集積度で多機能の三次元構造を
有する半導体装置を得ることができる。
In the semiconductor device manufactured by the method of this embodiment, the non-defective chips 34 having semiconductor elements and the like are provided between the semiconductor chips 16 for lamination and the semiconductor substrates 16 for lamination. Is fixed and laminated on the exposed portion of the pad 13 corresponding to the connecting hole 17 of the laminating semiconductor substrate 16 and the mating pad 35 via the connecting grains 33, 24, 38 made of Au. It is possible to obtain a semiconductor device having the three-dimensional structure.

【0020】更に、良品チップ34と積層用半導体基板
16及び各積層用半導体基板16間の積層は、Auから
なる連結粒33、24、38によりなされいるため、熱
ストレスを該Au粒33、24、38で吸収できるた
め、従来のSOI構造のようなクラック発生を防止でき
る。しかも、同様な理由により良品チップ34と積層用
半導体基板16の間、各半導体基板16の間に所望の隙
間を形成できるため、各基板間に熱がこもることなく、
放熱性が改善される。従って、高信頼性の三次元構造を
有する半導体装置を得ることができる。
Furthermore, since the non-defective chip 34 and the stacking semiconductor substrate 16 and the stacking between the stacking semiconductor substrates 16 are formed by the connecting grains 33, 24 and 38 made of Au, thermal stress is applied to the Au grains 33, 24. , 38, it is possible to prevent the occurrence of cracks as in the conventional SOI structure. Moreover, for the same reason, desired gaps can be formed between the non-defective chip 34 and the semiconductor substrate 16 for stacking, and between the semiconductor substrates 16, so that heat does not accumulate between the respective substrates.
The heat dissipation is improved. Therefore, a semiconductor device having a highly reliable three-dimensional structure can be obtained.

【0021】なお、上記実施例では連結粒の仮固定をガ
ラス支持基板上に半硬化状態のポリイミド膜を形成した
ものを用いて行なったが、これに限定されず、以下に説
明する図14〜図16に示す方法により行なってもよ
い。
In the above-mentioned embodiment, the temporary fixing of the connecting particles was carried out by using a glass supporting substrate on which a semi-cured polyimide film was formed. However, the present invention is not limited to this, and FIGS. You may perform by the method shown in FIG.

【0022】(1)図14に示すようにガラス支持基板
41にホ―ニング法等により所望の径及び深さの半円弧
状の凹部42を連結粒の配列位置に形成し、これら凹部
42に例えばAlからなる連結粒43を落下させ、仮固
定する。
(1) As shown in FIG. 14, semi-arcuate concave portions 42 having a desired diameter and depth are formed in the glass supporting substrate 41 by a honing method or the like at the positions where the connecting grains are arranged. For example, the connecting grains 43 made of Al are dropped and temporarily fixed.

【0023】(2)図15に示すようにガラス支持基板
41上に所望厚さのマイラ―等からなる有機膜44を張
付け、この有機膜44をレ―ザビ―ムにより溶解、分解
して穴45を連結粒の配列位置に形成し、これら穴45
に例えばAlからなる連結粒43を落下させ、仮固定す
る。なお、有機膜44には図示しない合せ用マ―クが付
されている。
(2) As shown in FIG. 15, an organic film 44 made of mylar or the like having a desired thickness is put on a glass supporting substrate 41, and the organic film 44 is melted and decomposed by a laser beam to form holes. 45 are formed in the arrangement position of the connecting grains, and these holes 45
Then, the connecting grains 43 made of, for example, Al are dropped and temporarily fixed. The organic film 44 is provided with a marking mark (not shown).

【0024】(3)図16に示すようにガラス支持基板
41の裏面にフェライト等からなる所望厚さの磁性薄膜
46を形成し、該支持基板41の表面にNi球47の表
面にAuメッキ膜48を施した連結粒43´を所望の配
列位置で載置する。この場合、連結粒43´は支持基板
41裏面に被覆された磁性薄膜46の磁力により同支持
基板41表面に仮固定される。
(3) As shown in FIG. 16, a magnetic thin film 46 made of ferrite or the like having a desired thickness is formed on the back surface of the glass support substrate 41, and the surface of the support substrate 41 is an Au plating film on the surface of the Ni sphere 47. The connecting grains 43 'subjected to 48 are placed at a desired arrangement position. In this case, the connecting particles 43 ′ are temporarily fixed on the surface of the support substrate 41 by the magnetic force of the magnetic thin film 46 coated on the back surface of the support substrate 41.

【0025】上記実施例では、半導体基板等のパッドへ
の連結粒の固着を該基板側に配置した押え治具の加熱機
構や超音波機構により行なったが、支持基板の載置台に
付加された加熱機構や超音波機構を用いて行なってもよ
い。
In the above-mentioned embodiment, the connecting grains are fixed to the pad of the semiconductor substrate or the like by the heating mechanism or ultrasonic mechanism of the holding jig arranged on the substrate side, but it is added to the mounting table of the supporting substrate. Alternatively, a heating mechanism or an ultrasonic mechanism may be used.

【0026】[0026]

【発明の効果】以上詳述した如く、本発明によれば半導
体基板の素子への多大な熱影響を与えることなく、複数
個の導電性連結粒を効率よく半導体基板のパッドに固着
でき、ひいては多機能化が可能な高集積度で高信頼性の
三次元構造の半導体装置の製造に有効に適用できる等顕
著な効果を有する。
As described above in detail, according to the present invention, a plurality of conductive connecting grains can be efficiently fixed to the pad of the semiconductor substrate without exerting a great thermal influence on the element of the semiconductor substrate, and by extension, It has remarkable effects such that it can be effectively applied to the manufacture of a semiconductor device having a highly integrated and highly reliable three-dimensional structure capable of multi-functionalization.

【図面の簡単な説明】[Brief description of drawings]

【図1】本発明の実施例における三次元構造の半導体装
置の製造工程を示す断面図。
FIG. 1 is a sectional view showing a manufacturing process of a semiconductor device having a three-dimensional structure according to an embodiment of the present invention.

【図2】本発明の実施例における三次元構造の半導体装
置の製造工程を示す断面図。
FIG. 2 is a cross-sectional view showing a manufacturing process of a semiconductor device having a three-dimensional structure according to an embodiment of the present invention.

【図3】本発明の実施例における三次元構造の半導体装
置の製造工程を示す断面図。
FIG. 3 is a cross-sectional view showing a manufacturing process of a semiconductor device having a three-dimensional structure according to an embodiment of the present invention.

【図4】本発明の実施例における三次元構造の半導体装
置の製造工程を示す断面図。
FIG. 4 is a sectional view showing a manufacturing process of a semiconductor device having a three-dimensional structure according to an embodiment of the present invention.

【図5】本発明の実施例における三次元構造の半導体装
置の製造工程を示す断面図。
FIG. 5 is a cross-sectional view showing a manufacturing process of a semiconductor device having a three-dimensional structure in an example of the present invention.

【図6】本発明の実施例における三次元構造の半導体装
置の製造工程を示す断面図。
FIG. 6 is a cross-sectional view showing a manufacturing process of a semiconductor device having a three-dimensional structure according to an embodiment of the present invention.

【図7】本発明の実施例における三次元構造の半導体装
置の製造工程を示す断面図。
FIG. 7 is a cross-sectional view showing a manufacturing process of a semiconductor device having a three-dimensional structure according to an embodiment of the present invention.

【図8】積層用半導体基板の連結孔のパッドにAuから
なる連結粒を固着する工程を示す断面図。
FIG. 8 is a cross-sectional view showing the step of fixing the connecting particles made of Au to the pads of the connecting holes of the stacking semiconductor substrate.

【図9】積層用半導体基板の連結孔のパッドにAuから
なる連結粒を固着する工程を示す断面図。
FIG. 9 is a cross-sectional view showing a step of fixing connecting grains made of Au to the pads of the connecting holes of the semiconductor substrate for lamination.

【図10】積層用半導体基板の連結孔のパッドにAuか
らなる連結粒を固着する工程を示す断面図。
FIG. 10 is a cross-sectional view showing a step of fixing the connecting particles made of Au to the pads of the connecting holes of the stacking semiconductor substrate.

【図11】既に作製された積層用半導体基板と電気的に
接続される良品チップのパッドにAuからなる連結粒を
固着する工程を示す断面図。
FIG. 11 is a cross-sectional view showing a step of fixing the connecting grains made of Au to the pads of the non-defective chip which is electrically connected to the already manufactured laminated semiconductor substrate.

【図12】既に作製された積層用半導体基板と電気的に
接続される良品チップのパッドにAuからなる連結粒を
固着する工程を示す断面図。
FIG. 12 is a cross-sectional view showing a step of fixing the connecting particles made of Au to the pads of the non-defective chip which is electrically connected to the already manufactured laminated semiconductor substrate.

【図13】既に作製された積層用半導体基板と電気的に
接続される良品チップのパッドにAuからなる連結粒を
固着する工程を示す断面図。
FIG. 13 is a cross-sectional view showing the step of fixing the connecting particles made of Au to the pads of the non-defective chip that is electrically connected to the already manufactured stacking semiconductor substrate.

【図14】本発明の他の実施例を示す断面図。FIG. 14 is a sectional view showing another embodiment of the present invention.

【図15】本発明の他の実施例を示す断面図。FIG. 15 is a sectional view showing another embodiment of the present invention.

【図16】本発明の他の実施例を示す断面図。FIG. 16 is a sectional view showing another embodiment of the present invention.

【図17】従来の半導体基板のパッドに連結粒を固着す
る工程を示す断面図。
FIG. 17 is a cross-sectional view showing a step of fixing connecting particles to a pad of a conventional semiconductor substrate.

【符号の説明】[Explanation of symbols]

11…シリコンウェハ、12、13、35…パッド、1
6…積層用半導体基板、17…連結孔、22、31、4
1…ガラス支持基板、23、32…ポリイミド膜、2
4、33、38、43、43´…連結粒、34…良品チ
ップ、42…凹部、44…有機膜、45…穴、46…磁
性薄膜。
11 ... Silicon wafer, 12, 13, 35 ... Pad, 1
6 ... Laminating semiconductor substrate, 17 ... Connection holes, 22, 31, 4
1 ... Glass support substrate, 23, 32 ... Polyimide film, 2
4, 33, 38, 43, 43 '... Connected grain, 34 ... Good chip, 42 ... Recess, 44 ... Organic film, 45 ... Hole, 46 ... Magnetic thin film.

フロントページの続き (51)Int.Cl.6 識別記号 庁内整理番号 FI 技術表示箇所 H01L 27/00 301 C Continuation of front page (51) Int.Cl. 6 Identification number Office reference number FI technical display location H01L 27/00 301 C

Claims (1)

【特許請求の範囲】[Claims] 【請求項1】 Auからなる球状の導電性連結粒を形成
する工程と、支持基板上の所望位置に前記連結粒を複数
個配列、固定する工程と、半導体素子が少なくとも形成
され、かつ表面にパッドが形成された半導体基板を前記
支持基板上にその連結粒と該半導体基板のパッドとが合
致するように配置する工程と、前記連結粒を前記半導体
基板のパッドに前記連結粒および前記パッドを溶融させ
ることなく圧接させ、パッド側に移行させる工程とを具
備したことを特徴とする半導体装置の製造方法。
1. A step of forming spherical conductive connecting particles made of Au, a step of arranging and fixing a plurality of the connecting particles at a desired position on a supporting substrate, and at least a semiconductor element being formed on the surface of the semiconductor element. A step of arranging the semiconductor substrate on which the pad is formed on the support substrate so that the connecting grains and the pad of the semiconductor substrate match, and connecting the connecting grain to the pad of the semiconductor substrate. A method of manufacturing a semiconductor device, comprising the step of bringing the semiconductor device into pressure contact without being melted and transferring it to the pad side.
JP7218891A 1995-08-28 1995-08-28 Method for manufacturing semiconductor device Expired - Fee Related JP2755927B2 (en)