JPH088103A - Fe-Pt based alloy for permanent magnet having high coercive force and method for producing the same - Google Patents

Fe-Pt based alloy for permanent magnet having high coercive force and method for producing the same

Info

Publication number
JPH088103A
JPH088103A JP6159505A JP15950594A JPH088103A JP H088103 A JPH088103 A JP H088103A JP 6159505 A JP6159505 A JP 6159505A JP 15950594 A JP15950594 A JP 15950594A JP H088103 A JPH088103 A JP H088103A
Authority
JP
Japan
Prior art keywords
atomic
ordered
domains
coercive force
alloy
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP6159505A
Other languages
Japanese (ja)
Inventor
Naomasa Kimura
直正 木村
Mitsuya Hosoe
光矢 細江
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Honda Motor Co Ltd
Original Assignee
Honda Motor Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Honda Motor Co Ltd filed Critical Honda Motor Co Ltd
Priority to JP6159505A priority Critical patent/JPH088103A/en
Publication of JPH088103A publication Critical patent/JPH088103A/en
Pending legal-status Critical Current

Abstract

(57)【要約】 【目的】 高保磁力を有する永久磁石用Fe−Pt系合
金を提供する。 【構成】 Fe−Pt系合金は、Pt含有量が35原子
%≦Pt≦54原子%であり、残部が不可避不純物を含
むFeよりなる組成を有し、金属組織が、規則γ1 相よ
りなる多数の規則ドメインD1 ,D2 より構成され、ま
たそれら規則ドメインD1 ,D2 の平均径dが70Å≦
d≦350Åであり、さらに、相互に隣接し、且つ原子
配列の位相が反転関係にある両規則ドメインD1 ,D2
間に逆位相境界APBが存在する。この逆位相境界AP
Bが磁壁移動を妨げるピンニングサイトとなるので、保
磁力Hcが高められる。
(57) [Summary] [Object] To provide an Fe-Pt alloy for a permanent magnet having a high coercive force. [Structure] The Fe-Pt alloy has a Pt content of 35 atomic% ≤ Pt ≤ 54 atomic%, and has a composition in which the balance is Fe containing unavoidable impurities, and has a metallic structure of a regular γ 1 phase. It is composed of a large number of regular domains D 1 and D 2 , and the average diameter d of these regular domains D 1 and D 2 is 70Å ≦
d ≦ 350Å, and both ordered domains D 1 and D 2 that are adjacent to each other and in which the phases of the atomic arrangement are inverted
There is an antiphase boundary APB between them. This antiphase boundary AP
Since B becomes a pinning site that hinders domain wall movement, the coercive force Hc is increased.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は高保磁力を有する永久磁
石用Fe−Pt系合金およびその製造方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a Fe-Pt alloy for permanent magnets having a high coercive force and a method for producing the same.

【0002】[0002]

【従来の技術】従来、この種Fe−Pt系合金として
は、その金属組織が、不規則γ相よりなるマトリックス
と、そのマトリックス中に存在する規則γ1 相とより構
成されるものが知られている(特開昭57−17830
5号公報参照)。
2. Description of the Related Art Heretofore, as this type of Fe--Pt type alloy, one having a metal structure composed of a matrix of disordered γ phases and an ordered γ 1 phase existing in the matrix is known. (JP-A-57-17830)
(See Japanese Patent Publication No. 5).

【0003】[0003]

【発明が解決しようとする課題】しかしながら、従来の
Fe−Pt系合金は、その金属組織が不規則γ相から規
則γ1 相に変態する初期の状態にあって、針状の規則γ
1 相が層状に配列した多数の双晶を有するため、保磁力
が比較的低く、また低靱性であって機械加工性に欠け
る、といった問題がある。
However, the conventional Fe--Pt alloy has a needle-like regular γ in the initial state where the metal structure is transformed from the disordered γ phase to the ordered γ 1 phase.
Since one phase has a large number of twin crystals arranged in layers, there is a problem that the coercive force is relatively low, and the toughness is low and the machinability is poor.

【0004】本発明は前記に鑑み、双晶を含まない金属
組織を備えることによって高い保磁力と良好な機械加工
性を有し、また量産性の優れた前記永久磁石用Fe−P
t系合金およびその製造方法を提供することを目的とす
る。
In view of the above, the present invention has high coercive force and good machinability by providing a metallic structure not containing twins, and is excellent in mass productivity.
An object is to provide a t-based alloy and a method for producing the same.

【0005】[0005]

【課題を解決するための手段】本発明に係る高保磁力を
有する永久磁石用Fe−Pt系合金は、Pt含有量が3
5原子%≦Pt≦54原子%であり、残部が不可避不純
物を含むFeよりなる組成を有し、金属組織が、規則γ
1 相よりなる多数の規則ドメインより構成され、またそ
れら規則ドメインの平均径dが70Å≦d≦350Åで
あり、さらに、相互に隣接し、且つ原子配列の位相が反
転関係にある両規則ドメイン間に逆位相境界が存在する
ことを特徴とする。
The Fe-Pt alloy for a permanent magnet having a high coercive force according to the present invention has a Pt content of 3 or less.
5 atomic% ≤ Pt ≤ 54 atomic%, with the balance being Fe containing unavoidable impurities, and having a metallic structure of regular γ.
It is composed of a large number of ordered domains consisting of one phase, the average diameter d of these ordered domains is 70 Å ≤ d ≤ 350 Å, and the two ordered domains that are adjacent to each other and in which the phases of the atomic arrangement are in an inverted relationship Is characterized by the existence of an antiphase boundary.

【0006】本発明に係る前記永久磁石用Fe−Pt系
合金の製造方法は、Pt含有量が35原子%≦Pt≦5
4原子%であり、残部が不可避不純物を含むFeよりな
る合金組成の素材を鋳造する工程と、その素材に1次熱
処理を施して溶体化組織を有する中間体を得る工程と、
その中間体に2次熱処理を施して、規則γ1 相よりなる
多数の規則ドメインより構成され、またそれら規則ドメ
インの平均径dが70Å≦d≦350Åであり、さら
に、相互に隣接し、且つ原子配列の位相が反転関係にあ
る両規則ドメイン間に逆位相境界が存在する金属組織を
形成する工程と、を順次行うことを特徴とする。
In the method for producing the Fe—Pt alloy for permanent magnet according to the present invention, the Pt content is 35 atomic% ≦ Pt ≦ 5.
A step of casting a material having an alloy composition of 4 atomic% and the balance being Fe containing unavoidable impurities; a step of subjecting the material to a primary heat treatment to obtain an intermediate having a solution structure;
The intermediate is subjected to a secondary heat treatment to be composed of a large number of ordered domains consisting of ordered γ 1 phases, and the average diameter d of these ordered domains is 70Å ≦ d ≦ 350Å, and further, they are adjacent to each other, and It is characterized in that the step of forming a metallographic structure in which an antiphase boundary exists between the two ordered domains in which the phases of the atomic arrangement have an inversion relation is sequentially performed.

【0007】[0007]

【作用】組成および金属組織を前記のように特定する
と、高保磁力を有する永久磁石用Fe−Pt系合金を提
供することができる。この合金の高保磁力は、相互に隣
接し、且つ原子配列の位相が反転関係にある両規則ドメ
イン間に逆位相境界が在り、その逆位相境界が両規則ド
メイン間に亘る磁壁移動を妨げるピンニングサイトとな
っている、ということに起因するものと考えられる。
When the composition and the metal structure are specified as described above, it is possible to provide the Fe-Pt based alloy for a permanent magnet having a high coercive force. The high coercive force of this alloy has an anti-phase boundary between two ordered domains that are adjacent to each other and in which the phases of the atomic arrangement are in an inverted relationship, and the anti-phase boundary prevents the domain wall movement between the two ordered domains. It is considered that it is due to that.

【0008】また前記金属組織は双晶を含まないので、
Fe−Pt系合金の機械加工性は良好である。さらに金
属組織が、最終的に、安定相である規則γ1 相よりなる
多数の規則ドメインより構成されるようにすればよいの
で、Fe−Pt系合金の製造条件は比較的緩やかであ
り、したがってその合金は優れた量産性を有する。
Since the metal structure does not contain twins,
The Fe-Pt alloy has good machinability. Furthermore, since the final metallographic structure may be composed of a large number of ordered domains of the ordered γ 1 phase, which is a stable phase, the manufacturing conditions of the Fe—Pt-based alloy are relatively mild, and therefore, The alloy has excellent mass productivity.

【0009】ただし、組成において、Pt含有量がPt
<35原子%であるか、またはPt>54原子%である
と、前記金属組織を得ることができない。また規則ドメ
インの平均径dがd<70Åであるか、またはd>35
0Åであると、保磁力が急激に低下する。
However, in the composition, the Pt content is Pt.
If it is <35 atomic% or Pt> 54 atomic%, the above metal structure cannot be obtained. Also, the average diameter d of the ordered domain is d <70Å, or d> 35
When it is 0Å, the coercive force drops sharply.

【0010】前記製造方法によれば、前記永久磁石用F
e−Pt系合金を容易に量産することが可能である。
According to the manufacturing method, the F for permanent magnet is
It is possible to easily mass-produce the e-Pt-based alloy.

【0011】[0011]

【実施例】永久磁石用Fe−Pt系合金は、組成上、P
t含有量が35原子%≦Pt≦54原子%であり、残部
が不可避不純物を含むFeよりなる。その合金の金属組
織は、図1に示すように規則γ1 相よりなる多数の規則
ドメインD1 ,D2 より構成され、それら規則ドメイン
D1 ,D2 の平均径(最長部位の長さの平均値)dは7
0Å≦d≦350Åに設定される。白色の規則ドメイン
D1 と斜線を施された規則ドメインD2 とは、原子配列
の位相が反転関係にあり、相互に隣接する両規則ドメイ
ンD1 ,D2 間には逆位相境界APBが存在する。
[Examples] Fe-Pt alloys for permanent magnets have a composition of P
The t content is 35 atomic% ≦ Pt ≦ 54 atomic%, and the balance is Fe containing unavoidable impurities. As shown in FIG. 1, the metal structure of the alloy is composed of a large number of ordered domains D 1 and D 2 consisting of ordered γ 1 phase, and the average diameter of these ordered domains D 1 and D 2 (the length of the longest part is Average value) d is 7
It is set to 0Å ≦ d ≦ 350Å. The white ordered domain D 1 and the hatched ordered domain D 2 have an inverted atomic arrangement phase, and an antiphase boundary APB exists between the adjacent ordered domains D 1 and D 2. To do.

【0012】図2はFe−Pt系合金の規則格子におけ
る逆位相境界APBを示すもので、Fe原子配列および
Pt原子配列の位相がそれぞれ反転している境界が逆位
相境界APBである。
FIG. 2 shows the antiphase boundary APB in the ordered lattice of the Fe-Pt system alloy, and the boundaries at which the phases of the Fe atomic arrangement and the Pt atomic arrangement are inverted are the antiphase boundaries APB.

【0013】永久磁石用Fe−Pt系合金において、組
成および金属組織を前記のように特定すると、その保磁
力Hcを高めることができる。この場合、各規則ドメイ
ンD1 ,D2 内には多数の磁区が存在するが、原子配列
の位相が反転関係にあると共に相隣る両規則ドメインD
1 ,D2 間に亘る磁壁移動は逆位相境界APBにより妨
げられ、この逆位相境界APBの、磁壁移動に対するピ
ンニングサイト化によりFe−Pt系合金の保磁力Hc
が高められるものと考えられる。
In the Fe--Pt alloy for permanent magnets, the coercive force Hc can be increased by specifying the composition and the metal structure as described above. In this case, although a large number of magnetic domains exist in each of the ordered domains D 1 and D 2 , both of the ordered domains D which are in the inversion relation of the atomic arrangement and are adjacent to each other.
The domain wall movement between 1 and D 2 is hindered by the antiphase boundary APB, and the coercive force Hc of the Fe—Pt-based alloy is generated due to the antiphase boundary APB becoming a pinning site for the domain wall movement.
Is considered to be increased.

【0014】また金属組織は双晶を含まないので、Fe
−Pt系合金は良好な機械加工性を有する。さらに金属
組織が、最終的に、安定相である規則γ1 相よりなる多
数の規則ドメインより構成されるようにすればよいの
で、Fe−Pt系合金の製造条件は比較的緩やかであ
り、したがってその合金は優れた量産性を有する。
Further, since the metal structure does not contain twins, Fe
-Pt-based alloys have good machinability. Furthermore, since the final metallographic structure may be composed of a large number of ordered domains of the ordered γ 1 phase, which is a stable phase, the manufacturing conditions of the Fe—Pt-based alloy are relatively mild, and therefore, The alloy has excellent mass productivity.

【0015】前記Fe−Pt系合金の製造に当っては、
Pt含有量が35原子%≦Pt≦54原子%であり、残
部が不可避不純物を含むFeよりなる合金組成の素材を
鋳造する工程と、その素材に1次熱処理を施して溶体化
組織を有する中間体を得る工程と、その中間体に2次熱
処理を施して、規則γ1 相よりなる多数の規則ドメイン
D1 ,D2 より構成され、またそれら規則ドメイン
D1 ,D2 の平均径dが70Å≦d≦350Åであり、
さらに、相互に隣接し、且つ原子配列の位相関係が反転
関係にある両規則ドメインD1 ,D2 間に逆位相境界A
PBが存在する金属組織を形成する工程と、を順次行
う。
In manufacturing the Fe--Pt alloy,
An intermediate step of casting a material having an alloy composition of Pt content of 35 atomic% ≤ Pt ≤ 54 atomic% and the balance being Fe containing inevitable impurities, and performing a primary heat treatment on the material to have a solution structure. The step of obtaining a body and the second intermediate heat treatment of the intermediate body are composed of a large number of ordered domains D 1 and D 2 having an ordered γ 1 phase, and the average diameter d of these ordered domains D 1 and D 2 is 70Å ≦ d ≦ 350Å,
Further, the antiphase boundary A between the two ordered domains D 1 and D 2 which are adjacent to each other and in which the phase relation of the atomic arrangement is in the inversion relation.
The step of forming a metallographic structure in which PB is present is sequentially performed.

【0016】前記1次熱処理としては溶体化処理が適用
され、その溶体化処理は、真空中、または不活性ガス中
にて、処理温度T1 を1100℃≦T1 ≦1500℃
に、また処理時間t1 を0.1時間≦t1 ≦10時間に
それぞれ設定して行われる。この溶体化処理は、主とし
て、均質な溶体化組織を有する中間体を得るために行わ
れ、処理温度T1 および処理時間t1 が前記範囲を逸脱
すると、所期の目的を達成することができない。好まし
くは、処理温度T1 は1200℃≦T1 ≦1350℃で
あり、また処理時間t1 は0.5時間≦t1 ≦2時間で
ある。
A solution treatment is applied as the first heat treatment, and the solution treatment is performed in vacuum or in an inert gas at a treatment temperature T 1 of 1100 ° C. ≦ T 1 ≦ 1500 ° C.
And the processing time t 1 is set to 0.1 hour ≦ t 1 ≦ 10 hours. This solution treatment is mainly performed in order to obtain an intermediate having a homogeneous solution structure, and if the treatment temperature T 1 and the treatment time t 1 deviate from the above ranges, the intended purpose cannot be achieved. . Preferably, the treatment temperature T 1 is 1200 ° C. ≦ T 1 ≦ 1350 ° C., and the treatment time t 1 is 0.5 hour ≦ t 1 ≦ 2 hours.

【0017】2次熱処理は、前記金属組織を得るため
に、図3に示すFe−Pt状態図においてスピノーダル
オーダリング曲線で囲まれる斜線を付した領域(FeP
t)内で行われる。この2次熱処理領域(FePt)に
はスピノーダルオーダリング曲線上も含まれる。
In the secondary heat treatment, in order to obtain the above metal structure, a hatched region (FeP surrounded by a spinodal ordering curve in the Fe-Pt phase diagram shown in FIG. 3).
within t). The secondary heat treatment region (FePt) also includes a spinodal ordering curve.

【0018】スピノーダルオーダリング曲線は、実験に
より求められたものであり、Fe−Pt状態図において
Pt含有量をX軸に、また温度をY軸にそれぞれとった
とき、8座標、即ち、a1 (35,400)、a2 (4
3.5,1020)、a3 (46,1180)、a
4 (48,1260)、a5 (49.5,1290)、
a6 (50,1260)、a7 (51.5,780)、
a8 (54,400)を結ぶ曲線として表わされる。故
に、2次熱処理領域(FePt)は、座標a1 →a2 →
a3 →a4 →a5 →a6 →a7 →a8 →a1 を結んで得
られる略二等辺三角形をなす領域であり、したがって処
理温度T2 は400℃≦T2 ≦1290℃に設定され、
またPt含有量は、処理温度T2 =400℃にて35原
子%≦Pt≦54原子%であるが、処理温度T2 の上昇
に伴いそのPt含有量の許容範囲は狭められる。
The spinodal ordering curve is obtained by experiments, and when the Pt content is on the X axis and the temperature is on the Y axis in the Fe-Pt phase diagram, 8 coordinates, that is, a 1 ( 35,400), a 2 (4
3.5, 1020), a 3 (46, 1180), a
4 (48,1260), a 5 (49.5,1290),
a 6 (50,1260), a 7 (51.5,780),
It is represented as a curve connecting a 8 (54,400). Therefore, the secondary heat treatment area (FePt) has coordinates a 1 → a 2 →
a 3 → a 4 → a 5 → a 6 → a 7 → a 8 → a 1 is an approximately isosceles triangular region obtained, and therefore the processing temperature T 2 is 400 ° C. ≦ T 2 ≦ 1290 ° C. Is set,
Further, the Pt content is 35 atomic% ≦ Pt ≦ 54 atomic% at the processing temperature T 2 = 400 ° C., but the allowable range of the Pt content is narrowed as the processing temperature T 2 rises.

【0019】処理時間t2 は、後述するように、保磁力
Hcに影響を与える規則ドメインの平均径dとの関係か
ら0.5時間≦t2 ≦50時間、好ましくは1時間≦t
2 ≦20時間に設定される。
As will be described later, the treatment time t 2 is 0.5 hours ≦ t 2 ≦ 50 hours, preferably 1 hour ≦ t, from the relationship with the average diameter d of the ordered domains that influence the coercive force Hc.
2 ≤ 20 hours.

【0020】なお、35原子%≦Pt≦54原子%にお
いて、スピノーダルオーダリング曲線で規定される2次
熱処理領域(FePt)を外れた温度域で2次熱処理を
行うと、Fe−Pt系合金の金属組織が、図4に示すよ
うに層状双晶組織となる。この場合、相互に隣接し、且
つ原子配列の位相が反転関係にある両針状規則γ1 相A
1 ,A2 間には逆位相境界APBが存在するが、その逆
位相境界APBは直線状に長く延びているので、その逆
位相境界APBに沿った磁壁移動が発生し、その結果、
保磁力Hcは低くなる。また層状双晶組織を有するFe
−Pt系合金は脆く、薄板状等に切断加工することが困
難である。
When 35 atomic% ≤ Pt ≤ 54 atomic%, the secondary heat treatment is performed in a temperature range outside the secondary heat treatment range (FePt) defined by the spinodal ordering curve, the metal of the Fe-Pt alloy is obtained. The structure becomes a layered twin structure as shown in FIG. In this case, both needle-like rules γ 1 phase A which are adjacent to each other and in which the phases of the atomic arrangement are in the inversion relation.
An antiphase boundary APB exists between 1 and A 2 , but since the antiphase boundary APB extends linearly long, domain wall movement occurs along the antiphase boundary APB, and as a result,
The coercive force Hc becomes low. Fe having a layered twin structure
-Pt-based alloys are brittle, and it is difficult to cut them into thin plates.

【0021】以下、具体例について説明する。Hereinafter, specific examples will be described.

【0022】Fe−Pt系合金を製造するに当り、Fe
およびPtをPt含有量が35原子%≦Pt≦54原子
%の範囲で変化するように秤量し、次いで各秤量物をア
ルミナ製るつぼ内に投入して、高周波溶解炉を用いて溶
解し、その後各種組成の素材を鋳造した。
In producing the Fe-Pt alloy, Fe
And Pt are weighed so that the Pt content changes in the range of 35 atomic% ≤ Pt ≤ 54 atomic%, then each weighed material is put into an alumina crucible and melted using a high frequency melting furnace, and then Materials of various compositions were cast.

【0023】1次熱処理工程では、各素材に、不活性ガ
ス中、処理温度T1 =1300℃、処理時間t1 =1時
間、急冷の条件で溶体化処理を施して各種中間体を得
た。
In the primary heat treatment step, each material was subjected to solution treatment in an inert gas under the conditions of a treatment temperature T 1 = 1300 ° C., a treatment time t 1 = 1 hour, and a rapid cooling to obtain various intermediates. .

【0024】2次熱処理工程では、各中間体に、処理時
間t2 をt2 =10時間に設定し、また処理温度T2 を
400℃≦T2 ≦1000℃の範囲内で変化させた熱処
理を施して、各種Fe−Pt系合金を得た。
In the secondary heat treatment step, the heat treatment was carried out by setting the treatment time t 2 to t 2 = 10 hours and changing the treatment temperature T 2 within the range of 400 ° C. ≦ T 2 ≦ 1000 ° C. for each intermediate. Then, various Fe—Pt based alloys were obtained.

【0025】表1は、Fe−Pt系合金の例1〜8にお
けるPt含有量、2次熱処理における処理温度T2 、金
属組織、保磁力Hcおよび厚さ300μmの薄板を得る
場合の切断加工性を示す。
Table 1 shows the Pt content in Examples 1 to 8 of Fe-Pt type alloys, the processing temperature T 2 in the secondary heat treatment, the metal structure, the coercive force Hc, and the cutting workability when obtaining a thin plate having a thickness of 300 μm. Indicates.

【0026】[0026]

【表1】 例1〜8は、それらの組成と2次熱処理の処理温度T2
との関係において、図3に点(1)〜(8)として示さ
れている。
[Table 1] Examples 1 to 8 are those compositions and the treatment temperature T 2 of the secondary heat treatment.
In relation to, the points (1) to (8) are shown in FIG.

【0027】[0027]

【外1】 反射)であり、その金属組織は、規則γ1 相よりなる多
数の規則ドメインより構成される。図中、白色部分の規
則ドメインと黒色部分の規則ドメインとでは原子配列の
位相が反転関係にあり、それら白色部分の規則ドメイン
と黒色部分の規則ドメインの境界が逆位相境界APBで
ある。白色部分の規則ドメインおよび黒色部分の規則ド
メインにおいて、大きな島状になっている所は、それぞ
れ原子配列の位相が同一である複数の規則ドメインが隣
接していることを示し、これら規則ドメインの平均径d
はd=200Åである。
[Outer 1] Reflection), and its metallic structure is composed of a large number of ordered domains composed of ordered γ 1 phases. In the figure, the phase of the atomic arrangement is inverted between the white regular domain and the black regular domain, and the boundary between the white regular domain and the black regular domain is the antiphase boundary APB. The large islands in the white and black ordered domains indicate that multiple ordered domains with the same atomic arrangement phase are adjacent to each other. Diameter d
Is d = 200Å.

【0028】表1から明らかなように、例3は高い保磁
力Hcを有し、また切断加工性も良好である。これは、
表1および図3,5に示すように例3においてはPt含
有量が39.5原子%であって35原子%≦Pt≦54
原子%の範囲にあること、2次熱処理の処理温度T2 が
600℃であってスピノーダルオーダリング曲線で規定
される2次熱処理領域(FePt)に設定されているこ
と、金属組織が、規則γ1 相よりなる多数の規則ドメイ
ンより構成されていること、規則ドメインの平均径dが
200Åであって70Å≦d≦350Åの範囲にあるこ
と、相互に隣接し、且つ原子配列の位相が反転関係にあ
る両規則ドメイン間に逆位相境界APBが存在すること
に起因する。
As is clear from Table 1, Example 3 has a high coercive force Hc and good cutting workability. this is,
As shown in Table 1 and FIGS. 3 and 5, in Example 3, the Pt content was 39.5 atomic% and 35 atomic% ≦ Pt ≦ 54.
In the range of atomic%, the processing temperature T 2 of the second heat treatment is set in the secondary heat treatment region (FePt) to a 600 ° C. defined by spin nodal ordering curve, metal structure, rules gamma 1 It is composed of many regular domains consisting of phases, the average diameter d of the regular domains is 200 Å and 70 Å ≤ d ≤ 350 Å, adjacent to each other, and the phases of the atomic arrangement are in an inverted relationship. This is due to the existence of an antiphase boundary APB between certain rule domains.

【0029】例3に関する理由と同一の理由から、例
1,5,7,8も高い保磁力Hcと良好な切断加工性を
有する。
For the same reason as in Example 3, Examples 1, 5, 7 and 8 also have high coercive force Hc and good cutting workability.

【0030】[0030]

【外2】 反射)であり、その金属組織は層状双晶組織であること
が判る。したがって、表1に示すように例2はその保磁
力Hcが低く、また切断加工性も悪い。例2に関する理
由と同一の理由から、例4,6は保磁力Hcが低く、ま
た難切断加工性である。
[Outside 2] It is understood that the metallic structure is a layered twin structure. Therefore, as shown in Table 1, the coercive force Hc of Example 2 is low and the cutting workability is also poor. For the same reason as in Example 2, Examples 4 and 6 have low coercive force Hc and are difficult to cut.

【0031】次に、前記1次熱処理工程を経て得られ
た、前記例2と同一組成(Fe−39.5原子%Pt)
の中間体を選定し、その中間体に対する2次熱処理の処
理温度T2 をT2 =600℃に設定すると共に処理時間
t2 を0.25時間≦t2 ≦100時間の範囲で変化さ
せ、得られたFe−Pt系合金における規則ドメインの
平均径dと保磁力Hcとの関係を調べたところ、表2の
結果を得た。なお、各Fe−Pt系合金の金属組織は、
その組成および2次熱処理の処理温度T2 に起因して、
前記同様に規則γ1 相よりなる多数の規則ドメインより
構成される。
Next, the same composition (Fe-39.5 atomic% Pt) as in Example 2 obtained through the first heat treatment step was obtained.
Is selected, the treatment temperature T 2 of the secondary heat treatment for the intermediate is set to T 2 = 600 ° C., and the treatment time t 2 is changed within the range of 0.25 hours ≦ t 2 ≦ 100 hours, When the relationship between the average diameter d of the ordered domains and the coercive force Hc in the obtained Fe-Pt-based alloy was examined, the results shown in Table 2 were obtained. The metallic structure of each Fe-Pt alloy is
Due to its composition and the treatment temperature T 2 of the secondary heat treatment,
Similar to the above, it is composed of a number of ordered domains consisting of ordered γ 1 phases.

【0032】[0032]

【表2】 表2において、例21 は処理時間t2 =0であることか
ら中間体そのものであり、また例25 は前記例2と同一
である。
[Table 2] In Table 2, Example 2 1 is the intermediate itself because the treatment time t 2 = 0, and Example 25 is the same as Example 2 above.

【0033】図7は、表2における規則ドメインの平均
径dと保磁力Hcとの関係をグラフ化したものである。
図中、各点(21 )〜(28 )は各例21 〜28 に対応
する。表2および図7から明らかなように、処理時間t
2 を長く設定すると、それに伴い規則ドメインの平均径
dが大きくなるが、保磁力Hcは規則ドメインの平均径
d=200Åにおいて最大となる。
FIG. 7 is a graph showing the relationship between the average diameter d of the ordered domains in Table 2 and the coercive force Hc.
In the figure, points (2 1 ) to (2 8 ) correspond to examples 2 1 to 2 8 . As is clear from Table 2 and FIG. 7, the processing time t
When 2 is set to be long, the average diameter d of the ordered domains increases accordingly, but the coercive force Hc becomes maximum at the average diameter d of the ordered domains d = 200Å.

【0034】高性能な永久磁石用材料には、保磁力Hc
がHc≧3.0kOeであることが要求され、そのため
には規則ドメインの平均径dを70Å≦d≦350Åに
設定することが必要である。この場合、最も性能の良い
永久磁石用Fe−Pt系合金を得るためには規則ドメイ
ンの平均径dを200Åに設定すればよい。
Coercive force Hc is used for high-performance permanent magnet materials.
Is required to be Hc ≧ 3.0 kOe, and for that purpose, it is necessary to set the average diameter d of the ordered domain to 70Å ≦ d ≦ 350Å. In this case, the average diameter d of the ordered domains may be set to 200Å in order to obtain the best performance Fe-Pt alloy for permanent magnets.

【0035】[0035]

【発明の効果】本発明によれば、前記のように構成する
ことによって高い保磁力と良好な機械加工性を有し、ま
た量産性の優れた永久磁石用Fe−Pt系合金を提供す
ることができる。
According to the present invention, it is possible to provide an Fe-Pt-based alloy for a permanent magnet, which has a high coercive force and good machinability and is excellent in mass productivity by having the above-mentioned constitution. You can

【0036】さらに本発明によれば、前記特性を備えた
永久磁石用Fe−Pt系合金を容易に量産することが可
能な製造方法を提供することができる。
Further, according to the present invention, it is possible to provide a manufacturing method capable of easily mass-producing the Fe-Pt alloy for permanent magnets having the above-mentioned characteristics.

【図面の簡単な説明】[Brief description of drawings]

【図1】実施例に係るFe−Pt系合金の金属組織を示
す説明図である。
FIG. 1 is an explanatory diagram showing a metal structure of an Fe—Pt-based alloy according to an example.

【図2】Fe−Pt系合金の規則格子における逆位相境
界を示す説明図である。
FIG. 2 is an explanatory diagram showing antiphase boundaries in an ordered lattice of Fe—Pt alloy.

【図3】Fe−Pt状態図である。FIG. 3 is an Fe—Pt phase diagram.

【図4】比較例に係るFe−Pt系合金の金属組織を示
す説明図である。
FIG. 4 is an explanatory diagram showing a metal structure of a Fe—Pt-based alloy according to a comparative example.

【図5】実施例に係るFe−Pt系合金の金属組織を示
す顕微鏡写真である。
FIG. 5 is a micrograph showing a metal structure of an Fe—Pt-based alloy according to an example.

【図6】比較例に係るFe−Pt系合金の金属組織を示
す顕微鏡写真である。
FIG. 6 is a micrograph showing a metal structure of a Fe—Pt alloy according to a comparative example.

【図7】規則ドメインの平均径と保磁力との関係を示す
グラフである。
FIG. 7 is a graph showing the relationship between the average diameter of ordered domains and the coercive force.

【符号の説明】[Explanation of symbols]

D1 ,D2 規則ドメイン APB 逆位相境界D 1 , D 2 Regular domain APB Antiphase boundary

Claims (2)

【特許請求の範囲】[Claims] 【請求項1】 Pt含有量が35原子%≦Pt≦54原
子%であり、残部が不可避不純物を含むFeよりなる組
成を有し、金属組織が、規則γ1 相よりなる多数の規則
ドメイン(D1 ,D2 )より構成され、またそれら規則
ドメイン(D1 ,D2 )の平均径dが70Å≦d≦35
0Åであり、さらに、相互に隣接し、且つ原子配列の位
相が反転関係にある両規則ドメイン(D1 ,D2 )間に
逆位相境界(APB)が存在することを特徴とする、高
保磁力を有する永久磁石用Fe−Pt系合金。
1. A Pt content of 35 atomic% ≤ Pt ≤ 54 atomic%, a balance of Fe containing unavoidable impurities, and a metallic structure having a large number of ordered domains (ordered γ 1 phases). D 1 , D 2 ) and the average diameter d of the ordered domains (D 1 , D 2 ) is 70Å ≦ d ≦ 35.
High coercive force, which is characterized in that an antiphase boundary (APB) exists between both ordered domains (D 1 and D 2 ) that are 0Å and are adjacent to each other and in which the phases of the atomic arrangement are in an inversion relation. Fe-Pt based alloy for permanent magnets.
【請求項2】 Pt含有量が35原子%≦Pt≦54原
子%であり、残部が不可避不純物を含むFeよりなる合
金組成の素材を鋳造する工程と、その素材に1次熱処理
を施して溶体化組織を有する中間体を得る工程と、その
中間体に2次熱処理を施して、規則γ1 相よりなる多数
の規則ドメイン(D1 ,D2 )より構成され、またそれ
ら規則ドメイン(D1 ,D2 )の平均径dが70Å≦d
≦350Åであり、さらに、相互に隣接し、且つ原子配
列の位相が反転関係にある両規則ドメイン(D1 ,
D2 )間に逆位相境界(APB)が存在する金属組織を
形成する工程と、を順次行うことを特徴とする、高保磁
力を有する永久磁石用Fe−Pt系合金の製造方法。
2. A step of casting a raw material of an alloy composition having a Pt content of 35 atomic% ≦ Pt ≦ 54 atomic% and the balance being Fe containing inevitable impurities, and subjecting the raw material to a primary heat treatment to form a solution. A step of obtaining an intermediate having a chemical structure and a secondary heat treatment of the intermediate to form a large number of ordered domains (D 1 , D 2 ) composed of an ordered γ 1 phase, and the ordered domains (D 1 , D 2 ) has an average diameter d of 70Å ≦ d
≦ 350Å, and both regular domains (D 1 ,
A method for producing an Fe-Pt-based alloy for a permanent magnet having a high coercive force, which comprises sequentially performing a step of forming a metal structure having an antiphase boundary (APB) between D 2 ).
JP6159505A 1994-06-17 1994-06-17 Fe-Pt based alloy for permanent magnet having high coercive force and method for producing the same Pending JPH088103A (en)