JPH09171802A - Battery case, manufacturing method thereof, and battery using the case - Google Patents

Battery case, manufacturing method thereof, and battery using the case

Info

Publication number
JPH09171802A
JPH09171802A JP8293197A JP29319796A JPH09171802A JP H09171802 A JPH09171802 A JP H09171802A JP 8293197 A JP8293197 A JP 8293197A JP 29319796 A JP29319796 A JP 29319796A JP H09171802 A JPH09171802 A JP H09171802A
Authority
JP
Japan
Prior art keywords
battery case
steel sheet
coating layer
organic
container
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP8293197A
Other languages
Japanese (ja)
Other versions
JP3200375B2 (en
Inventor
Satoru Matsuo
悟 松尾
Michifumi Nika
通文 丹花
Akio Miyaji
昭夫 宮地
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toyo Kohan Co Ltd
Original Assignee
Toyo Kohan Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toyo Kohan Co Ltd filed Critical Toyo Kohan Co Ltd
Priority to JP29319796A priority Critical patent/JP3200375B2/en
Publication of JPH09171802A publication Critical patent/JPH09171802A/en
Application granted granted Critical
Publication of JP3200375B2 publication Critical patent/JP3200375B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To prevent a film from being peeled after diameter contracting work with excellent conductivity, working property and adhesion by forming an organic material coated steel plate into a case by means of diameter contracting work, and then heating this case to carbonize the organic coating layer. SOLUTION: An organic material coated steel plate having a coating layer of an organic material on one surface of a steel plate is formed into a vessel having integrated body part and bottom part by means of diameter contracting work so that the organic material coating layer is situated on the inner surface side of the case. Thereafter, the case is heated to carbonize the organic material coating layer, whereby a battery case 1 is formed. The carbonized organic material coating layer of the battery case desirably has an electric resistance of 10Ω/cm or less. This steel plate is desirably formed of a surface treated steel plate having a layer consisting of a chromium hydrate oxide on the surface.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【発明の属する技術分野】本発明はアルカリマンガン電
池などの電池ケース、その製造方法及びその電池ケース
を用いた電池に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a battery case such as an alkaline manganese battery, a method for manufacturing the same, and a battery using the battery case.

【0002】[0002]

【発明が解決しようとする課題】アルカリマンガン電池
などの乾電池においては、内部抵抗が小さいことが望ま
しい。内部抵抗の中でも、活物質としての二酸化マンガ
ンと導電剤としての黒鉛を混合してペレットに成形され
た正極合剤と、正極缶とも呼ばれる電池ケースとの間の
接触抵抗が最も大きい。この接触抵抗を低減させる方法
として、電池ケース内面にスプレーなどにより導電性塗
料を塗布することが行われ、これにより、正極合剤中の
活物質/導電剤の比率を高めることが可能となり、電池
の長寿命化が達成されている。しかし、電池ケース内面
に導電性塗膜を形成させる方法は、スプレーノズルの目
詰まりによるトラブルを生じやすいこと、塗膜厚みが不
均一になりやすいこと、さらに、小さな電池ケース一つ
一つの内面に導電性塗料を塗布せねばならず、その低い
生産効率がコスト上昇をもたらすことなど、解決すべき
問題が残されている。
In dry batteries such as alkaline manganese batteries, it is desirable that the internal resistance be small. Among the internal resistances, the contact resistance between the positive electrode mixture formed by mixing manganese dioxide as an active material and graphite as a conductive agent into pellets and the battery case also called a positive electrode can is the largest. As a method of reducing this contact resistance, a conductive paint is applied to the inner surface of the battery case by spraying or the like, which makes it possible to increase the ratio of active material / conductive agent in the positive electrode mixture, Has been achieved. However, the method of forming a conductive coating film on the inner surface of the battery case is liable to cause troubles due to clogging of the spray nozzle, the coating film thickness tends to be uneven, and the inner surface of each small battery case There remains a problem to be solved, such as the fact that a conductive paint has to be applied, and its low production efficiency causes an increase in cost.

【0003】これらの問題を解決するために、表面処理
を施した金属板に導電性皮膜を被覆した後、電池ケース
に加工するプロセスが電池業界の一部で試みられている
が、工業的レベルでは今日に至るまで必ずしも成功して
いない。その主な理由の一つとして、導電性皮膜の剥落
をもたらすことなく被覆金属板を電池ケースに成形加工
することが困難であることが挙げられる。
In order to solve these problems, a process of coating a surface-treated metal plate with a conductive film and then processing it into a battery case has been attempted in a part of the battery industry, but at an industrial level. So far, it's not always successful. One of the main reasons for this is that it is difficult to form the coated metal plate into a battery case without causing the conductive coating to come off.

【0004】市販されているアルカリマンガン乾電池の
中には例えば、LR6(単3型)乾電池などのように、
極めて厳しい加工が施されて製造された電池ケースを用
いているものもある。これらの電池ケースの製造におい
ては、次のような加工が施される。まず、導電性皮膜を
被覆した金属板から円板上のブランクが打ち抜かれ、6
工程前後の絞り加工により、順次に内径の小さい缶に成
形される。最終的に内径13.8mmの電池ケースとな
るが、全工程の絞り比(ブランク径/絞り加工缶の内
径)は4.2にも達する。このような苛酷な加工が施さ
れた後も皮膜剥離を生じさせないためには、塗膜が十分
な加工性と、金属板に対する優れた密着力を兼備してい
ることが不可欠である。
Among the commercially available alkaline manganese dry batteries, for example, LR6 (AA) dry batteries,
Some use a battery case that is manufactured through extremely severe processing. In manufacturing these battery cases, the following processing is performed. First, a blank on a disk is punched out from a metal plate coated with a conductive film,
By the drawing process before and after the process, it is sequentially formed into a can with a small inner diameter. Although the battery case finally has an inner diameter of 13.8 mm, the drawing ratio (blank diameter / inner diameter of the drawn can) of all processes reaches 4.2. In order to prevent film peeling even after such severe processing, it is essential that the coating film has both sufficient workability and excellent adhesion to the metal plate.

【0005】予め導電性皮膜を被覆した金属板を絞り加
工して電池ケースを成形する一例として、特開平6−3
42653号公報による方法が開示されている。これ
は、絶縁性のクロメート皮膜に導電性を付与するため
に、カーボンブラックを含有させたクロメート処理液に
金属板を浸漬し、皮膜の密着力を向上させるクロメート
皮膜を形成させた後、エポキシ樹脂などを主剤とする導
電性塗料を塗布したものである。しかし、この金属板を
絞り加工した場合、黒鉛やカーボンブラックなどの粉体
を添加した熱硬化性のエポキシ樹脂を塗料として用いて
いるために皮膜も展延性に欠け、加工性が低下すること
は否めず、絞り加工時に皮膜にクラックが生じることは
避けられない。また、皮膜剥離を皆無にすることも困難
であると思われる。このように、予め導電性皮膜を被覆
した金属板を加工して電池ケースとすることには、未だ
に改善の余地が残されている。
As an example of forming a battery case by drawing a metal plate coated with a conductive film in advance, Japanese Patent Laid-Open No. 6-3
A method according to Japanese Patent No. 42653 is disclosed. This is because in order to impart conductivity to the insulative chromate film, the metal plate is dipped in a chromate treatment liquid containing carbon black to form a chromate film that improves the adhesion of the film, and then the epoxy resin. It is the one to which a conductive paint whose main ingredient is is applied. However, when this metal plate is drawn, since the thermosetting epoxy resin to which powder such as graphite or carbon black is added is used as the paint, the film also lacks spreadability and the workability does not deteriorate. Inevitably, cracking of the coating is inevitable during drawing. It also seems difficult to eliminate the peeling of the film. As described above, there is still room for improvement in processing a metal plate coated with a conductive film in advance to form a battery case.

【0006】本発明においては、導電性に優れ、かつ電
池ケースに縮径加工される際に、加工性、および密着力
に優れ、縮径加工後に皮膜剥離が生じることのない電池
ケースを提供することを課題としている。なお、ここで
いう縮径加工とは一段または多段の絞り加工、薄肉化絞
り加工、絞りしごき加工などであり、容器の径および高
さ、皮膜の強度、密着性などを考慮し、最適な加工方法
が選択される。
The present invention provides a battery case which is excellent in conductivity, has excellent workability and adhesiveness when the battery case is subjected to diameter reduction processing, and does not cause film peeling after the diameter reduction processing. That is the issue. It should be noted that the diameter reduction process here means a single-stage or multi-stage drawing process, a thinning process, a drawing and ironing process, etc., and it is the optimum process considering the diameter and height of the container, the strength of the film, the adhesion, etc. The method is selected.

【0007】[0007]

【課題を解決するための手段】本発明においては、下記
に示すように、有機物を被覆した金属板を電池ケースに
縮径加工した後加熱し、被覆物層を炭化させることによ
り、上記の課題が解決されることが判明した。
In the present invention, as described below, the metal plate coated with an organic material is subjected to a diameter reduction process in a battery case and then heated to carbonize the coating layer, whereby the above-mentioned problems are solved. Was found to be resolved.

【0008】本発明の電池ケースは、鋼板の片面に有機
物の被覆層を設けた有機物被覆鋼板を、有機物被覆層が
容器の内面側となるようにして、縮径加工法を用いて容
器の胴部と底部が一体となって成形される容器に成形し
た後、容器を加熱し有機物被覆層を炭化させたことを特
徴とする電池ケースであり、炭化させた有機物被覆層の
電気抵抗が10Ω/cm以下であることを特徴とし、ま
た鋼板が、クロム水和酸化物からなる層を有している
か、あるいは下層が金属クロム、上層がクロム水和酸化
物からなる二層を有しているか、あるいはまた表面にニ
ッケルめっき層を有しているか、または表面にニッケル
めっき層を有し、さらにその上にクロム水和酸化物から
なる層を有しているか、さらにまたは表面にニッケルめ
っき層を有し、さらにその上に下層が金属クロム、およ
び上層がクロム水和酸化物からなる二層を有する表面処
理鋼板であることを特徴としている。
In the battery case of the present invention, an organic material-coated steel sheet having an organic material coating layer provided on one surface of the steel sheet is used so that the organic material coating layer is on the inner surface side of the container, and the body of the container is subjected to a diameter reduction processing method. The battery case is characterized in that the container and the bottom are integrally molded, and then the container is heated to carbonize the organic coating layer. The carbonized organic coating layer has an electric resistance of 10Ω / Whether the steel sheet has a layer made of chromium hydrated oxide, or has a lower layer made of metallic chromium and an upper layer has two layers made of chromium hydrated oxide, Alternatively, it has a nickel plating layer on its surface, or has a nickel plating layer on its surface, and further has a layer made of hydrated chromium oxide on it, or has a nickel plating layer on its surface. And then It is characterized in that the lower layer is chromium metal thereon, and the upper layer is a surface treated steel sheet having a double layer consisting of hydrated chromium oxide.

【0009】また本発明は上記の被覆される有機物被覆
層が、溶媒に溶解、または溶媒中に分散させた有機樹脂
塗料を鋼板上に塗装積層するか、または加熱溶融した樹
脂を鋼板上に押し出して積層するか、または有機樹脂フ
ィルムを、接着剤を介してまたは接着剤を介さずに直接
鋼板上に熱圧着して積層することにより形成されること
を特徴とし、被覆鋼板を成形して得られる容器を非酸化
雰囲気又はわずかな酸素分圧を有する雰囲気で400〜
900℃に加熱し、有機被覆物被覆層を炭化することが
望ましい。さらにまた本発明の電池は、上記のようにし
て得られた電池ケースに、正極合剤、導電剤及び負極ゲ
ルを充填してなることを特徴としている。
In the present invention, the above organic coating layer to be coated is formed by coating and laminating an organic resin paint dissolved or dispersed in a solvent on a steel plate, or extruding a heat-melted resin on the steel plate. It is characterized in that it is formed by thermocompression-bonding an organic resin film directly onto a steel sheet with or without an adhesive, and forming a coated steel sheet by molding. The container to be heated in a non-oxidizing atmosphere or an atmosphere having a slight oxygen partial pressure of 400
It is desirable to heat to 900 ° C. to carbonize the organic coating layer. Furthermore, the battery of the present invention is characterized in that the battery case obtained as described above is filled with a positive electrode mixture, a conductive agent and a negative electrode gel.

【0010】[0010]

【発明の実施の形態】本発明においては、予め有機物を
被覆した鋼板を縮径加工して電池ケースとした後加熱し
て、有機物層を炭化させ、炭化後の被覆層の電気抵抗を
10Ω/cm以下とすることにより、導電性に優れ、か
つ電池ケースに縮径加工される際に、加工性、および密
着力に優れ、縮径加工後に塗膜剥離が生じることのない
電池ケースが得られる。
BEST MODE FOR CARRYING OUT THE INVENTION In the present invention, a steel sheet previously coated with an organic material is reduced in diameter to form a battery case and then heated to carbonize the organic material layer, and the electrical resistance of the carbonized coating layer is 10Ω / When it is not more than cm, it is possible to obtain a battery case which is excellent in conductivity and is excellent in workability and adhesion when the battery case is subjected to the diameter reduction processing and does not cause peeling of the coating film after the diameter reduction processing. .

【0011】本発明の電池ケースに適用する鋼板として
は耐食性、鋼板に被覆される有機物皮膜の加工性、およ
び密着性の観点から、板厚が0.18〜0.32mmの鋼
板の表面に電解クロム酸処理などにより3〜30mg/
m2 (クロムとして)の量のクロム水和酸化物からなる
層を形成させた鋼板、下層が150〜300g/m2の
量の金属クロム、上層が3〜30mg/m2 (クロムと
して)の量のクロム水和酸化物からなる二層を形成させ
た鋼板、あるいは上記の板厚を有する鋼板に電気めっき
などの方法を用いて10〜30g/m2 の量のニッケル
めっきを施した鋼板、または上記の板厚を有する鋼板に
上記の量のニッケルめっきを施した後、電解クロム酸処
理などにより3〜30mg/m2 (クロムとして)の量
のクロム水和酸化物からなる層を形成させた鋼板、さら
にまたは、上記の板厚を有する鋼板に上記の量のニッケ
ルめっきを施した後、電解クロム酸処理などによりその
上に下層が150〜300g/m2 の量の金属クロム、
上層が3〜30mg/m2(クロムとして)の量のクロ
ム水和酸化物からなる二層を形成させた鋼板であること
により、縮径加工直後、および加熱炭化後の皮膜の密着
性を向上させるためより好ましい。
As a steel sheet applied to the battery case of the present invention, from the viewpoints of corrosion resistance, workability of an organic film coated on the steel sheet, and adhesion, the surface of the steel sheet having a thickness of 0.18 to 0.32 mm is electrolyzed. 3-30 mg / due to chromic acid treatment
steel sheet with a layer formed of chromium hydrated oxide in an amount of m 2 (as chromium), metallic chromium in an amount of 150 to 300 g / m 2 in the lower layer, and 3 to 30 mg / m 2 (as chromium) in the upper layer. Steel plate on which two layers of hydrated chromium oxide are formed, or a steel plate having a plate thickness as described above, which has been plated with nickel in an amount of 10 to 30 g / m 2 using a method such as electroplating, Alternatively, a steel plate having the above plate thickness is plated with the above amount of nickel, and then a layer of chromium hydrate oxide of 3 to 30 mg / m 2 (as chromium) is formed by electrolytic chromic acid treatment or the like. Steel plate, or further, after the above-mentioned amount of nickel plating is applied to a steel plate having the above-mentioned plate thickness, a lower layer is formed with an amount of metallic chromium of 150 to 300 g / m 2 by electrolytic chromic acid treatment or the like,
Improving the adhesion of the coating immediately after the diameter reduction processing and after the heat carbonization by the steel sheet having the upper layer formed with the two layers of the hydrated chromium oxide in an amount of 3 to 30 mg / m 2 (as chromium) It is more preferable because

【0012】上記の鋼板は上記した種々の表面処理を施
した後に、0.1〜1.0μmの中心線平均粗さを有して
いることも、鋼板に被覆される有機物皮膜の加工性、お
よび密着性の観点からこのましい。中心線平均粗さが
0.1μm以下では被覆される有機物皮膜に与えるアン
カー効果が十分ではなく、有機物を被覆した鋼板を縮径
加工する際、または縮径加工した後に、有機物皮膜が剥
離しやすく、好ましくない。一方、中心線平均粗さが
1.0μm以上では、絞り加工時に工具との摩擦によ
り、有機被膜が剥離しやすくなるので好ましくない。
The above steel sheet has a center line average roughness of 0.1 to 1.0 μm after being subjected to the above-mentioned various surface treatments. And it is preferable from the viewpoint of adhesion. When the center line average roughness is 0.1 μm or less, the anchor effect given to the organic film to be coated is not sufficient, and the organic film is likely to peel off when the steel sheet coated with the organic material is subjected to the diameter reduction process or after the diameter reduction process. , Not preferable. On the other hand, when the center line average roughness is 1.0 μm or more, it is not preferable because the organic coating film is easily peeled off due to friction with the tool during drawing.

【0013】上記の表面処理を施した鋼板の片面に被覆
する有機物としては、ロジン、アスファルト、ピッチな
どからなるワニス、ポリビニルアセタール、ポリビニル
ブチラール、ポリ酢酸ビニル、ポリアクリル酸エステル
などの合成樹脂、ポリクロロプレン、スチレンブタジエ
ン樹脂、ブタジエン−アクリロニトリル樹脂、イソプレ
ンスチレン樹脂、イソプレンイソブチレン樹脂などのゴ
ム系樹脂などの有機樹脂の1種または2種以上を主剤と
し、必要に応じてこれらの有機樹脂に可塑剤等を添加し
た有機溶媒系塗料、水性塗料、エマルジョン塗料のいず
れかの有機樹脂塗料を塗布し乾燥させたもの、あるいは
ポリエチレン、ポリプロピレン、エチレン−プロピレン
共重合体、エチレン−酢酸ビニル共重合体、エチレン−
アクリル酸共重合体、ポリエチレンテレフタレート、ポ
リブチレンテレフタレート、エチレンテレフタレート−
イソフタレート共重合体、ブチレンテレフタレート−イ
ソフタレート共重合体、6-ナイロン、6,6−ナイロ
ン、6,10−ナイロン、ポリカーボネート、ポリウレ
タン、アイオノマー樹脂、ポリアクリロニトリル、アク
リロニトリル−ブタジエン−スチレン共重合体などの樹
脂を加熱溶融し、鋼板上に直接押し出して積層したも
の、あるいは上記の樹脂をフィルムに成形加工した後、
これらのフィルムを直接鋼板上に加熱圧着したもの、も
しくはこれらのフィルムを接着剤を介して鋼板上に加熱
圧着したものなどが本発明に適用することができる。鋼
板上に形成された後の有機物層の厚さは10〜50μm
であることが好ましい。10μm以下では有機物被覆鋼
板を縮径加工する際に有機物層にクラックが生じやす
く、50μm以上では縮径加工し加熱を施した後も皮膜
の厚さが厚く、内部抵抗を小さくすることができない。
なお、これらの塗料や樹脂、もしくは樹脂フィルムに、
加工性や密着性を著しく損なわない範囲で黒鉛、カ−ボ
ンブラック、アセチレンブラックなどの導電性を有する
粉末を添加しても差し支えない。
Examples of the organic substance coated on one surface of the steel sheet subjected to the above-mentioned surface treatment include varnish consisting of rosin, asphalt, pitch, etc., polyvinyl acetal, polyvinyl butyral, polyvinyl acetate, polyacrylic acid ester and other synthetic resins, poly One or more organic resins such as chloroprene, styrene-butadiene resin, butadiene-acrylonitrile resin, isoprene-styrene resin, isoprene-isobutylene resin, and other organic resins are used as the main agent, and if necessary, plasticizers are added to these organic resins. An organic solvent-based paint containing any of the above, a water-based paint, or an emulsion paint applied and dried, or polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ethylene-
Acrylic acid copolymer, polyethylene terephthalate, polybutylene terephthalate, ethylene terephthalate-
Isophthalate copolymer, butylene terephthalate-isophthalate copolymer, 6-nylon, 6,6-nylon, 6,10-nylon, polycarbonate, polyurethane, ionomer resin, polyacrylonitrile, acrylonitrile-butadiene-styrene copolymer, etc. After heating and melting the resin of, and extruding directly on a steel plate and laminating it, or after molding the above resin into a film,
Those obtained by directly heat-pressing these films on a steel plate, or those obtained by heat-pressing these films on a steel plate via an adhesive agent can be applied to the present invention. The thickness of the organic material layer formed on the steel plate is 10 to 50 μm.
It is preferred that If the thickness is 10 μm or less, cracks are likely to occur in the organic material layer when the organic-coated steel sheet is subjected to diameter reduction processing, and if the thickness is 50 μm or more, the thickness of the coating is large even after the diameter reduction processing and heating, and the internal resistance cannot be reduced.
In addition, these paints and resins, or resin film,
It is possible to add a conductive powder such as graphite, carbon black or acetylene black as long as the workability and adhesion are not significantly impaired.

【0014】上記のようにして得られた、鋼板の片面に
有機物の被覆層を設けた有機物被覆鋼板は、有機物被覆
層が容器の内面側となるようにして、縮径加工法を用い
て容器の胴部と凸部を有する底部が一体として成形され
る。この有機物被覆鋼板を本発明の目的とする電池ケー
スに成形するを縮径加工法としては、複数の段階からな
る絞り加工を施し、各段階の絞り加工毎に容器の径が縮
小される多段の絞り加工、または、上記の絞り加工時に
引張力を作用させて容器の壁厚みを減少させる薄肉化絞
り加工、または、1段もしくは複数段の絞り加工を施し
て容器の径を所定のものとした後、しごき加工を施して
容器の壁厚みを減少させる絞りしごき加工などを適用す
ることができる。
The organic substance-coated steel sheet obtained as described above, in which the organic substance coating layer is provided on one surface of the steel sheet, is prepared by reducing the diameter of the container by making the organic substance coating layer on the inner surface side of the container. The body and the bottom having the protrusion are integrally molded. As a method for reducing the diameter of forming the organic matter-coated steel sheet into a battery case for the purpose of the present invention, a drawing process including a plurality of steps is performed, and the diameter of the container is reduced in each step of the drawing process. Drawing, or thinning to reduce the wall thickness of the container by applying a tensile force during the above drawing, or one or more steps of drawing to make the container have a predetermined diameter. After that, squeezing and ironing for reducing the wall thickness of the container by performing ironing can be applied.

【0015】上記のようにして有機物を被覆した鋼板を
胴部と凸部を有する底部が一体となった容器に成形した
後、容器を真空中、窒素ガスなどの非酸化性雰囲気、あ
るいは燃焼を生じない程度の極くわずかな酸素分圧を有
する雰囲気中で、400〜900℃の温度で、長くとも
3時間加熱して有機物被覆層を炭化させ、炭化後の被覆
層の電気抵抗を10Ω/cm以下とする。加熱温度が4
00℃以下では長時間加熱しても有機物被覆層が十分に
炭化せず、炭化後の被覆層の電気抵抗は10Ω/cm以
上となり、電池とした場合の内部抵抗が高くなり、高い
放電電流が得られにくい。一方、900℃以上の温度で
容器を加熱すると短時間の加熱でも鋼板が極端に軟化
し、わずかの衝撃を受けても容器に凹凸が生じやすくな
るため、加熱温度の上限を900℃とし、できるだけ短
時間加熱することが好ましい。より好ましい加熱条件は
500〜800℃の温度で、2時間〜10分である。こ
のようにして、導電性に優れた電池ケースを得ることが
できる。
After the steel sheet coated with the organic substance is formed into a container in which the body and the bottom having the protrusions are integrated as described above, the container is placed in a vacuum, a non-oxidizing atmosphere such as nitrogen gas, or burned. In an atmosphere having a very small oxygen partial pressure that does not occur, the organic coating layer is carbonized by heating at a temperature of 400 to 900 ° C. for at most 3 hours, and the electrical resistance of the coating layer after carbonization is 10 Ω / cm or less. Heating temperature is 4
If the temperature is lower than 00 ° C, the organic coating layer is not sufficiently carbonized even after being heated for a long time, the electrical resistance of the coating layer after carbonization is 10 Ω / cm or more, the internal resistance of the battery is high, and high discharge current is high. Hard to get. On the other hand, if the container is heated at a temperature of 900 ° C. or higher, the steel sheet will be extremely softened even by heating for a short time, and unevenness will easily occur in the container even with a slight impact. Therefore, the upper limit of the heating temperature is set to 900 ° C. It is preferable to heat for a short time. More preferable heating conditions are a temperature of 500 to 800 ° C. and a time of 2 hours to 10 minutes. In this way, a battery case with excellent conductivity can be obtained.

【0016】[0016]

【実施例】以下、実施例にて本発明をさらに詳細に説明
する。表1〜2に本発明の実施範囲を説明する実験に用
いた鋼板を示す。鋼板に金属クロム、およびまたは水和
酸化物を形成させる場合は、電解クロム酸処理によりそ
れぞれ所定の量の皮膜を形成させた。ニッケルめっきは
通常のワット浴を用い通常の条件で電気めっきした。ニ
ッケルめっき層の上にさらに金属クロム、およびまたは
水和酸化物を形成させる場合は、電解クロム酸処理によ
りそれぞれ所定の量の皮膜を形成させた。ついでこれら
の鋼板の片面に、以下のA〜Dに示す3種類の方法によ
り、有機物皮膜を形成させた。
The present invention will be described in more detail with reference to the following examples. Tables 1 and 2 show the steel sheets used in the experiments for explaining the scope of the present invention. When forming metallic chromium and / or hydrated oxides on the steel sheet, electrolytic chromic acid treatment was performed to form a predetermined amount of a film. The nickel plating was performed by using a normal Watt bath and electroplating under normal conditions. When further forming metallic chromium and / or hydrated oxide on the nickel plating layer, a predetermined amount of film was formed by electrolytic chromic acid treatment. Then, an organic film was formed on one surface of each of the steel plates by the following three kinds of methods shown in A to D.

【0017】A:鋼板を280℃に加熱し、ポリエチレ
ンテレフタレート88モル%、ポリエチレンイソフタレ
ート12モル%からなる共重合ポリエステル樹脂(融
点:229℃)の二軸延伸フィルム(厚さ:25μm)
を接触させ圧着した。 B:上記の共重合ポリエステル樹脂にカーボンブラック
を10重量%含有させた以外はAと同様のフィルムを、
Aと同様にして圧着した。 C:ポリエチレンテレフタレート(融点:255℃)を
加熱溶融し、Tダイから鋼板上に直接押出し、積層し
た。 D:ポリビニルブチラール100重量部、フタル酸ジブ
チルを50重量部、エポキシ樹脂30重量部からなる樹
脂をイソプロパノールに溶解し、鋼板上にロールコート
法により塗布し、200℃で3分間加熱乾燥し焼き付け
た。
A: Biaxially stretched film (thickness: 25 μm) of a copolyester resin (melting point: 229 ° C.) made of 88 mol% polyethylene terephthalate and 12 mol% polyethylene isophthalate by heating a steel plate to 280 ° C.
Were contacted and crimped. B: A film similar to A except that the above copolyester resin contained 10% by weight of carbon black,
It pressure-bonded like A. C: Polyethylene terephthalate (melting point: 255 ° C.) was melted by heating, directly extruded from a T die onto a steel plate, and laminated. D: 100 parts by weight of polyvinyl butyral, 50 parts by weight of dibutyl phthalate, and 30 parts by weight of epoxy resin were dissolved in isopropanol, coated on a steel sheet by a roll coating method, heated and dried at 200 ° C. for 3 minutes, and baked. .

【0018】上記のようにして得られた有機物被覆鋼板
から58mm径のブランクを打ち抜き、有機物被覆面が
ケースの内面側となるようにして、6段階からなる絞り
加工(最終絞り比4.2)により、13.8mm径の円筒
状の電池ケース(缶)に縮径成形した。絞り加工した後
の電池ケースの、いわゆる耳を切り落とす前の有機物皮
膜の剥離程度を肉眼観察により、以下に示す評価基準で
評価した。 評点 ◎:剥離が全く認められない。 ○:剥離が殆ど認められない。(缶上端部にわずかな剥離が認められる。) △:缶上部の一部に剥離が認められる。 ×:缶のかなりの部分に剥離が認められる。 結果を表1〜2に示す。
A blank with a diameter of 58 mm was punched out from the organic substance-coated steel sheet obtained as described above, and the organic substance-coated surface was the inner surface side of the case, and drawing was performed in 6 stages (final drawing ratio 4.2). Then, the diameter was reduced to a cylindrical battery case (can) having a diameter of 13.8 mm. The degree of peeling of the organic film of the battery case after the drawing process before the so-called ear was cut off was evaluated by visual observation according to the following evaluation criteria. Rating ⊚: No peeling is observed. ◯: Peeling is hardly observed. (Slight peeling is observed at the top of the can.) Δ: Peeling is observed at part of the top of the can. X: Peeling is observed in a considerable part of the can. The results are shown in Tables 1 and 2.

【0019】上記の絞り加工を施した後に有機物皮膜の
剥離が認められなかった電池ケースについて、0.2to
rr程度の真空度を有する真空炉中で表3〜5に示す加熱
条件で後加熱を実施し、有機物層を炭化させた。そして
後加熱により炭化した有機物皮膜の密着強度を鉛筆硬度
法を用いて評価した。すなわち、加熱処理を施した電池
ケース(缶)の側壁の一ヶ所をを切り裂いて開缶し、缶
内面の炭化した皮膜に硬度Fの鉛筆を1kgの荷重をか
けて45度の角度で接触させて引っかいた際に生じる皮
膜の剥離程度を、肉眼観察により、以下に示す評価基準
で評価した。 評点 ◎:剥離が全く生じない。 ○:剥離が殆ど生じない。(缶上端部でのみ、わずかに剥離が生じる。) △:缶上部の一部で剥離が生じる。 ×:缶のかなりの部分で剥離が生じる。 結果を表3〜5に示す。
With respect to the battery case in which the peeling of the organic film was not observed after the above drawing process, 0.2 to
Post-heating was carried out under the heating conditions shown in Tables 3 to 5 in a vacuum furnace having a vacuum degree of about rr to carbonize the organic material layer. Then, the adhesion strength of the organic film carbonized by post-heating was evaluated using the pencil hardness method. That is, one side wall of a battery case (can) that has been subjected to heat treatment is torn open to open the can, and a pencil of hardness F is applied to the carbonized coating on the inside of the can at a 45 degree angle with a load of 1 kg. The degree of peeling of the film caused by scratching was evaluated by visual observation according to the following evaluation criteria. Rating ◎: Peeling does not occur at all. ◯: Peeling hardly occurs. (Peeling slightly occurs only at the upper end of the can.) Δ: Peeling occurs at a part of the upper part of the can. X: Peeling occurs in a considerable part of the can. The results are shown in Tables 3 to 5.

【0020】後加熱後の電池ケース(缶)の側壁の一ヶ
所を切り裂いて開缶し、底部を除去した後側壁部を平坦
にレベリングし、表面抵抗計(三菱油化(株)製、プロ
ーブ:2mm径の平坦なもの)を用い、1cmの間隔で
炭化した有機物皮膜の電気抵抗を測定した。結果を表3
〜5に示す。
After the post-heating, one side wall of the battery case (can) was cut open to open the can, the bottom part was removed, and the side wall was leveled flat, and a surface resistance meter (Mitsubishi Yuka Co., Ltd., probe : 2 mm diameter flat) was used to measure the electric resistance of the carbonized organic film at an interval of 1 cm. Table 3 shows the results
Are shown in FIGS.

【0021】図1に示すように、上記に示した絞り加工
を施した後も有機物皮膜の剥離が殆ど認められず、かつ
その後に後加熱を施して剥離が認められなかった電池ケ
ース10に、正極合剤11として正極活物質である電解
二酸化マンガンと、導電剤である黒鉛とを水酸化カリウ
ム電解液で混練したもの、および負極ゲル12として酸
化亜鉛を飽和させた水酸化カリウムの電解液にゲル化剤
を添加し、これに亜鉛粒を加えたものを作成した。この
正極合剤11を、ビニロン・ビニヨン製の不織布からな
るセパレータ16と電池ケース10の間に充填した。引
き続き、負極ゲル12を、集電体13とセパレータ16
の間に挿入した。これに負極キャップ14、集電体1
3、およびガスケット15を電池ケース10内に装着
し、電池ケース開放端部をかしめて電池1を作成し、温
度60℃、湿度95%で4週間の経時を施した後、電
圧、内部抵抗、および短絡電流を測定した。内部抵抗は
正極と負極の間にACミリオームテスタを接続し、1K
Hzの周波数で交流インピーダンス法により測定した。
結果を表3〜5に示す。
As shown in FIG. 1, in the battery case 10 in which peeling of the organic film was scarcely observed even after the above-mentioned drawing process was performed, and peeling was not observed after the post-heating, A positive electrode mixture 11 obtained by kneading electrolytic manganese dioxide, which is a positive electrode active material, and graphite, which is a conductive agent, with a potassium hydroxide electrolyte solution, and a negative electrode gel 12 which is an electrolyte solution of potassium hydroxide saturated with zinc oxide. A gelling agent was added, and zinc particles were added to this to prepare a gelling agent. The positive electrode mixture 11 was filled between the separator 16 made of non-woven vinylon vinylon and the battery case 10. Subsequently, the negative electrode gel 12 is applied to the current collector 13 and the separator 16
Inserted between. In addition to this, the negative electrode cap 14 and the current collector 1
3, the gasket 15 was mounted in the battery case 10, and the open end of the battery case was caulked to prepare the battery 1, which was subjected to 4 weeks of aging at a temperature of 60 ° C. and a humidity of 95%, and then the voltage, internal resistance, And the short circuit current was measured. For internal resistance, connect an AC milliohm tester between the positive and negative electrodes and
It was measured by the AC impedance method at a frequency of Hz.
The results are shown in Tables 3 to 5.

【0022】[0022]

【表1】 注) −:処理無し[Table 1] Note) −: No treatment

【0023】[0023]

【表2】 [Table 2]

【0024】[0024]

【表3】 注 −:測定せず[Table 3] Note-: Not measured

【0025】[0025]

【表4】 [Table 4]

【0026】[0026]

【表5】 [Table 5]

【0027】[0027]

【発明の効果】本発明の鋼板の片面に有機物の被覆層を
設けた有機物被覆鋼板を、有機物被覆層が容器の内面側
となるようにして、縮径加工法を用いて容器の胴部と底
部が一体となって成形される容器に成形した後、容器を
加熱し有機物被覆層を炭化させたことを特徴とする電池
ケースは、電池ケースに絞り加工される際に、加工性、
および密着力に優れ絞り加工後に塗膜剥離が生じること
がなく、得られた電池ケースを加熱して有機物皮膜を炭
化させても皮膜が剥離せず、かつ皮膜導電性に優れてい
る。そのため、本発明の被覆金属板を用いて製造された
電池は、内部抵抗が小さく、優れた放電特性を示す。
EFFECTS OF THE INVENTION An organic substance-coated steel sheet having an organic substance coating layer provided on one side of the steel sheet of the present invention is used as a body part of a container by using a diameter reduction processing method such that the organic substance coating layer is on the inner surface side of the container. After molding into a container in which the bottom part is integrally molded, the battery case characterized by heating the container to carbonize the organic coating layer, when drawn into a battery case, processability,
Also, the adhesiveness is excellent, the coating film does not peel off after drawing, the coating does not peel off even when the obtained battery case is heated to carbonize the organic material film, and the film conductivity is excellent. Therefore, the battery manufactured using the coated metal plate of the present invention has a small internal resistance and exhibits excellent discharge characteristics.

【0028】すなわち、本発明は、前記の炭化させた有
機物被覆層の電気抵抗が10Ω/cm以下であることを
特徴としており、皮膜導電性に優れている。また、本発
明は、前記鋼板がその表面にクロム水和酸化物からなる
層を有することを特徴としており、電池ケースに絞り加
工される際に、加工性、および密着力に優れ絞り加工後
に塗膜剥離が生じることがなく、得られた電池ケースを
加熱して有機物皮膜を炭化させても皮膜が剥離すること
がない。あるいはまた、本発明は、前記鋼板がその表面
に下層が金属クロム、上層がクロム水和酸化物からなる
二層を有することを特徴としており、電池ケースに絞り
加工される際に、加工性、および密着力に優れ、絞り加
工後に塗膜剥離が生じることがなく、得られた電池ケー
スを加熱して有機物皮膜を炭化させても皮膜が剥離する
ことがない。
That is, the present invention is characterized in that the carbonized organic coating layer has an electric resistance of 10 Ω / cm or less, and is excellent in film conductivity. Further, the present invention is characterized in that the steel sheet has a layer made of a hydrated chromium oxide on the surface thereof, and when it is drawn into a battery case, it is excellent in workability and adhesion and is applied after drawing. No film peeling occurs, and the film does not peel even if the obtained battery case is heated to carbonize the organic film. Alternatively, the present invention is characterized in that the steel sheet has two layers on the surface of which a lower layer is metallic chrome and an upper layer is made of hydrated chromium oxide. Also, the adhesive strength is excellent, the coating film does not peel off after drawing, and the coating does not peel off even when the obtained battery case is heated to carbonize the organic film.

【0029】あるいはまた、本発明は、前記鋼板がその
表面にニッケルめっき層を有することを特徴としてお
り、電池ケースに絞り加工される際に、加工性、および
密着力に優れ、絞り加工後に塗膜剥離が生じることがな
く、得られた電池ケースを加熱して有機物皮膜を炭化さ
せても皮膜が剥離することがない。あるいはまた、本発
明は、前記鋼板がその表面にニッケルめっき層を有し、
さらにその上にクロム水和酸化物からなる層を有するこ
とを特徴としており、電池ケースに絞り加工される際
に、加工性、および密着力に優れ、絞り加工後に塗膜剥
離が生じることがなく、得られた電池ケースを加熱して
有機物皮膜を炭化させても皮膜が剥離することがない。
あるいはまた、本発明は、前記鋼板がその表面にニッケ
ルめっき層を有し、さらにその上に下層が金属クロム、
上層がクロム水和酸化物からなる二層を有することを特
徴としており、電池ケースに絞り加工される際に、加工
性、および密着力に優れ、絞り加工後に塗膜剥離が生じ
ることがない。
Alternatively, the present invention is characterized in that the steel sheet has a nickel plating layer on the surface thereof, which is excellent in workability and adhesion when drawn into a battery case and is applied after drawing. No film peeling occurs, and the film does not peel even if the obtained battery case is heated to carbonize the organic film. Alternatively, in the present invention, the steel sheet has a nickel plating layer on its surface,
Furthermore, it is characterized by having a layer made of hydrated chromium oxide on it, and when it is drawn into a battery case, it has excellent workability and adhesion, and it does not cause film peeling after drawing. Even if the obtained battery case is heated to carbonize the organic film, the film does not peel off.
Alternatively, in the present invention, the steel sheet has a nickel plating layer on its surface, and the lower layer further has a metal chromium layer thereon,
It is characterized in that the upper layer has two layers of hydrated chromium oxide, and when it is drawn into a battery case, it is excellent in workability and adhesion, and the coating film does not peel off after drawing.

【0030】さらに、本発明は、前記有機物被覆層が、
溶媒に溶解、または溶媒中に分散させた有機樹脂塗料を
鋼板に塗装し積層するか、または加熱溶融した樹脂を鋼
板上に押し出して積層するか、または有機樹脂フィルム
を接着剤を介して、または接着剤を介さずに直接鋼板上
に熱圧着して積層することにより形成されることを特徴
としており、加工性、および密着力に優れ、絞り加工後
に塗膜剥離が生じることがなく、得られた電池ケースを
加熱して有機物皮膜を炭化させても皮膜が剥離すること
がない。また、本発明は、前記容器を400〜900℃
に加熱し、前記有機物被覆層を炭化することを特徴とし
ており、得られた電池ケースを加熱して有機物皮膜を炭
化させても皮膜が剥離することがない。
Further, in the present invention, the organic coating layer comprises
Dissolved in a solvent, or coated with an organic resin paint dispersed in a solvent on a steel sheet to be laminated, or extruding a heat-melted resin onto a steel sheet to laminate, or an organic resin film via an adhesive, or It is characterized in that it is formed by laminating by thermocompression bonding directly on a steel plate without using an adhesive, and it has excellent workability and adhesion, and it is obtained without peeling of the coating film after drawing. Even if the battery case is heated to carbonize the organic film, the film does not peel off. Moreover, this invention is 400-900 degreeC of the said container.
It is characterized in that the organic material coating layer is carbonized by heating to the above, and even if the obtained battery case is heated to carbonize the organic material film, the film is not peeled off.

【0031】さらにまた、本発明は、前記の電池ケース
に正極合剤、導電剤及び負極ゲルを充填してなる電池で
あり、内部抵抗が小さく、優れた放電特性を示す。
Furthermore, the present invention is a battery in which the above-mentioned battery case is filled with a positive electrode mixture, a conductive agent and a negative electrode gel, and has a small internal resistance and excellent discharge characteristics.

【図面の簡単な説明】[Brief description of the drawings]

【図1】電池の構造を示す概略図である。FIG. 1 is a schematic diagram showing the structure of a battery.

【符号の説明】 1 電池 10 電池ケース 11 正極合剤 12 負極ゲル 13 集電体 14 負極キャップ 15 ガスケット 16 セパレータ[Explanation of reference numerals] 1 battery 10 battery case 11 positive electrode mixture 12 negative electrode gel 13 current collector 14 negative electrode cap 15 gasket 16 separator

Claims (12)

【特許請求の範囲】[Claims] 【請求項1】 鋼板の片面に有機物の被覆層を設けた有
機物被覆鋼板を、有機物被覆層が容器の内面側となるよ
うにして、縮径加工法を用いて容器の胴部と底部が一体
となって成形される容器に成形した後、該容器を加熱し
該有機物被覆層を炭化させたことを特徴とする電池ケー
ス。
1. An organic substance-coated steel sheet having an organic substance coating layer provided on one surface of a steel plate, wherein the organic substance coating layer is on the inner surface side of the container, and the body and bottom of the container are integrated by a diameter reduction method. A battery case characterized in that after being molded into a container to be molded as described above, the container is heated to carbonize the organic coating layer.
【請求項2】 前記鋼板が、その表面にクロム水和酸化
物からなる層を有する表面処理鋼板である、請求項1に
記載の電池ケース。
2. The battery case according to claim 1, wherein the steel sheet is a surface-treated steel sheet having a layer made of hydrated chromium oxide on the surface thereof.
【請求項3】 前記鋼板が、その表面に下層が金属クロ
ム、上層がクロム水和酸化物からなる二層を有する表面
処理鋼板である、請求項1に記載の電池ケース。
3. The battery case according to claim 1, wherein the steel sheet is a surface-treated steel sheet having two layers on the surface of which a lower layer is metallic chrome and an upper layer is hydrated chromium oxide.
【請求項4】 前記鋼板が、その表面にニッケルめっき
層を有する表面処理鋼板である、請求項1に記載の電池
ケース。
4. The battery case according to claim 1, wherein the steel plate is a surface-treated steel plate having a nickel plating layer on the surface thereof.
【請求項5】 前記鋼板が、その表面にニッケルめっき
層を有し、さらにその上にクロム水和酸化物からなる層
を有する表面処理鋼板である、請求項1に記載の電池ケ
ース。
5. The battery case according to claim 1, wherein the steel sheet is a surface-treated steel sheet having a nickel plating layer on its surface and further having a layer made of hydrated chromium oxide on the nickel plating layer.
【請求項6】 前記鋼板が、その表面にニッケルめっき
層を有し、さらにその上に下層が金属クロム、上層がク
ロム水和酸化物からなる二層を有する表面処理鋼板であ
る、請求項1に記載の電池ケース。
6. The surface-treated steel sheet, wherein the steel sheet has a nickel plating layer on the surface thereof, and further has a lower layer of metallic chromium and an upper layer of two layers of hydrated chromium oxide thereon. Battery case described in.
【請求項7】 前記の炭化させた有機物被覆層の電気抵
抗が10Ω/cm以下であることを特徴とする、請求項
1〜6のいずれかに記載の電池ケース。
7. The battery case according to claim 1, wherein the carbonized organic coating layer has an electric resistance of 10 Ω / cm or less.
【請求項8】 前記有機物被覆層が、請求項2〜6のい
ずれかに記載の表面処理鋼板上に、溶媒に溶解または溶
媒中に分散させた有機樹脂塗料を塗装積層し形成させた
ものである、請求項1〜7のいずれかに記載の電池ケー
ス。
8. The organic coating layer is formed by coating and laminating an organic resin coating material dissolved or dispersed in a solvent on the surface-treated steel sheet according to claim 2. The battery case according to any one of claims 1 to 7.
【請求項9】 前記有機物被覆層が、請求項2〜6のい
ずれかに記載の表面処理鋼板上に、加熱溶融した樹脂を
押し出して積層し形成したものである、請求項1〜7の
いずれかに記載の電池ケース。
9. The organic coating layer is formed by extruding and laminating a heat-melted resin on the surface-treated steel sheet according to any one of claims 2 to 6 to form the organic coating layer. The battery case described in Crab.
【請求項10】 前記有機物被覆層が、請求項2〜6の
いずれかに記載の表面処理鋼板上に、有機樹脂フィルム
を、接着剤を介してまたは接着剤を介さずに熱圧着して
積層し形成したものである、請求項1〜7のいずれかに
記載の電池ケース。
10. The organic coating layer is formed by laminating an organic resin film on the surface-treated steel sheet according to claim 2 by thermocompression bonding with or without an adhesive. The battery case according to any one of claims 1 to 7, wherein the battery case is formed by forming.
【請求項11】 鋼板の片面に有機物の被覆層を設けた
有機物被覆鋼板を、有機物被覆層が容器の内面側となる
ようにして、縮径加工法を用いて容器の胴部と底部が一
体となって成形される容器に成形した後、該容器を非酸
化雰囲気又はわずかな酸素分圧を有する雰囲気で400
〜900℃に加熱し、前記有機物被覆層を炭化すること
を特徴とする電池ケースの製造方法。
11. An organic substance-coated steel sheet having an organic substance coating layer provided on one side of a steel plate, wherein the organic substance coating layer is on the inner surface side of the container, and the body and bottom of the container are integrated by using a diameter reduction processing method. After being molded into a container to be molded into a container, the container is heated in a non-oxidizing atmosphere or an atmosphere having a slight oxygen partial pressure to 400
A method for manufacturing a battery case, which comprises heating to ˜900 ° C. to carbonize the organic coating layer.
【請求項12】 請求項1〜10のいずれかに記載の電
池ケースに正極合剤、導電剤及び負極ゲルを充填してな
る電池。
12. A battery obtained by filling the battery case according to any one of claims 1 to 10 with a positive electrode mixture, a conductive agent and a negative electrode gel.
JP29319796A 1995-10-20 1996-10-16 Battery case, manufacturing method thereof, and battery using the case Expired - Fee Related JP3200375B2 (en)