JPH09201630A - Plate joining method - Google Patents
Plate joining methodInfo
- Publication number
- JPH09201630A JPH09201630A JP4528696A JP4528696A JPH09201630A JP H09201630 A JPH09201630 A JP H09201630A JP 4528696 A JP4528696 A JP 4528696A JP 4528696 A JP4528696 A JP 4528696A JP H09201630 A JPH09201630 A JP H09201630A
- Authority
- JP
- Japan
- Prior art keywords
- stem
- plate
- die
- plate material
- plate materials
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
(57)【要約】
【課題】複数枚の板材を確実かつ強固に連結することの
できる板材の接合方法を提供する。
【解決手段】先端に向かって小径となるテーパ状部3a
を有するステム3が進入可能な穴を有するダイ2上に、
積層状態にある2枚の板材S1,S2を載置し、ステム
3を前進させてテーパ状部3aにより各板材S1,S2
を押圧する。そして、まずステム3が接する板材S1を
打ち抜いてこれにステム3の移動方向に突出する筒状部
Pを成形し、さらにステム3を前進させることでダイ2
側の板材S2をダイ2の穴2aの周縁部付近で破断させ
る。このようにすると、各板材S1,S2に重合する筒
状部が成形されることがなく、板材S1の筒状部Pをか
しめることによって、2枚の板材S1,S2を確実かつ
強固に接合することができる。
(57) Abstract: [PROBLEMS] To provide a method for joining plate materials capable of reliably and firmly connecting a plurality of plate materials. SOLUTION: A tapered portion 3a having a diameter decreasing toward a tip.
On the die 2 having a hole through which the stem 3 having
Two plate materials S1 and S2 in a stacked state are placed, the stem 3 is moved forward, and each plate material S1 and S2 is moved by the tapered portion 3a.
Press. Then, first, the plate material S1 with which the stem 3 is in contact is punched out to form a tubular portion P protruding in the moving direction of the stem 3, and the stem 3 is further advanced to move the die 2
The side plate material S2 is broken near the periphery of the hole 2a of the die 2. In this way, the tubular portion that overlaps the respective plate materials S1 and S2 is not formed, and the tubular portion P of the plate material S1 is caulked to securely and firmly join the two plate materials S1 and S2. can do.
Description
【0001】[0001]
【発明の属する技術分野】本発明は、積層状態にある2
枚以上の複数の鋼板などの板材を一体に接合する板材の
接合方法に関する。BACKGROUND OF THE INVENTION 1. Field of the Invention
The present invention relates to a method for joining sheet materials such as one or more sheet materials such as a plurality of steel sheets.
【0002】[0002]
【従来の技術】従来、2枚以上の複数の鋼板などの板材
を接合するためには、溶接、リベット接合などの手段が
知られるが、最近ではより簡易的な手段として2枚の板
材をバーリング処理により打ち抜き、これによって各板
材に筒状部を成形し、この筒状部を巻き返すことによっ
て板材を互いに接合するバーリングかしめと称される接
合手段が用いられている。このバーリングかしめは、一
般に被接合対象となる2枚以上の板材を重ねた状態で打
ち抜き、図3(a)に示すように、それぞれの板材S
1’,S2’に互いに重合する筒状部P1,P2を形成
した後、図3(b)に示すように、この筒状部P1,P
2をかしめるべく巻き返して板材S1’,S2’を接合
するようになっている。2. Description of the Related Art Conventionally, means such as welding and rivet joining have been known for joining two or more sheet materials such as steel plates. Recently, however, a simpler means is to burring two sheet materials. A joining means called burring caulking is used in which a cylindrical portion is formed on each plate material by processing, thereby forming a cylindrical portion on each plate material, and the cylindrical members are rewound to join the plate materials to each other. This burring caulking is generally performed by punching in a state where two or more plate materials to be joined are stacked, and as shown in FIG.
After forming cylindrical portions P1 and P2 overlapping each other on 1 ′ and S2 ′, as shown in FIG.
The plate materials S1 'and S2' are joined by being rolled back to caulk 2.
【0003】[0003]
【発明が解決しようとする課題】上記バーリングかしめ
は、筒状部を巻き返すことによる引掛かりによって板材
を接合するようになっているが、一般にリベットかしめ
において知られるように、このように筒状部を巻き返し
た際の引掛かりによって板材を接合する場合には、引掛
かり量によって板材の結合力が大きく異なってくる。上
記バーリングかしめにおいては、各板材の筒状部が重合
して形成されているため、これを一体に巻き返すと接合
に直接影響する内側の筒状部の引掛かりが浅くなり、板
材を確実に接合することが困難となってしまう問題が発
生している。The burring caulking is such that the plate members are joined by catching by rewinding the cylindrical portion. When the plate members are joined by hooking at the time of rewinding, the joining force of the plate materials greatly differs depending on the amount of hooking. In the above burring caulking, since the tubular portions of each plate material are formed by superimposition, when they are rewound together, the hook of the inner tubular portion that directly affects the joining becomes shallower, and the plate materials are securely joined. There is a problem that it becomes difficult to do so.
【0004】[0004]
【課題を解決するための手段】本発明の板材の接合方法
では、先端に向かって小径となるテーパ状部を有するス
テムが進入可能な穴を有するダイ上に積層状態にある複
数枚の板材を載置し、ステムを前進させてテーパ状部に
より各板材を押圧し、まずステムが接する板材を打ち抜
いてこれにステムの移動方向に突出する筒状部を成形す
る。続いてステムをさらに前進させることで筒状部が成
形された板材以外の板材をダイの穴の周縁部付近で破断
させ、最終的に前記筒状部をかしめて各板材を一体に接
合するようになっている。この板材の接合方法によれ
ば、筒状部が各板材に重合して成形されることがないた
め、筒状部をかしめた時の引掛かり量を充分確保するこ
とができ、各板材を確実かつ強固に接合することが可能
である。According to the method of joining plate materials of the present invention, a plurality of plate materials laminated in a die having a hole into which a stem having a tapered portion having a small diameter toward the tip can enter can be obtained. The plate is placed, the stem is advanced, and each plate is pressed by the tapered portion. First, a plate in contact with the stem is punched out, and a cylindrical portion protruding in the moving direction of the stem is formed thereon. Subsequently, by further advancing the stem, a plate material other than the plate material with the cylindrical portion formed is broken near the periphery of the hole of the die, and finally the cylindrical portion is caulked to join the respective plate materials integrally. It has become. According to this plate material joining method, since the tubular portion is not formed by being superposed on each plate material, it is possible to secure a sufficient amount of catch when the tubular portion is crimped, and to secure each plate material. In addition, it is possible to firmly bond.
【0005】[0005]
【発明の実施の形態】以下、図面に基づき本発明の実施
の形態を説明する。図1(a)、(b)、(c)、
(d)において、1は板材を接合する工程の初期におい
て使用されるバーリング機構であり、鋼板などに代表さ
れる板材を2枚重ねて支持するダイ2と、このダイ2に
支持された板材S1,S2を打ち抜いてバーリング処理
を施す軸状のステム3とを有している。このバーリング
機構1におけるステム3の先端部は、その先端に向かっ
て徐々に小径となるテーパ状部3aに成形されており、
またダイ2には、ステム3が進入可能な穴2aが設けら
れている。Embodiments of the present invention will be described below with reference to the drawings. 1 (a), (b), (c),
In (d), reference numeral 1 denotes a burring mechanism used at an early stage of a step of joining plate materials, a die 2 for supporting two plate materials typified by a steel plate or the like, and a plate material S1 supported by the die 2. , S2, and a shaft-shaped stem 3 for performing a burring process. The tip of the stem 3 in the burring mechanism 1 is formed into a tapered portion 3a whose diameter gradually decreases toward the tip thereof.
The die 2 is provided with a hole 2a into which the stem 3 can enter.
【0006】図1(a)に示すようにダイ2上に支持さ
れた2枚の板材S1,S2は、ステム3の前進にともな
って図1(b)に示すようにダイ2の穴2a内に突出す
るべく変形する。この時、板材S1,S2はステム3の
テーパ状部3a外形に沿って変形するため、ステム3が
接する板材S1の方がダイ2側の板材S2よりも急峻な
形状に変形し、このことによって板材S1においては、
ステム3先端の周縁部が接する付近で極端に材料の流動
性が悪くなり、図1(c)に示すようにその部分で板材
S2よりも早く破断する。このようにしてステム3によ
って打ち抜かれた板材S1には、テーパ状を成す筒状部
Pが成形される。As shown in FIG. 1 (a), the two plate members S1 and S2 supported on the die 2 move in the hole 2a of the die 2 as shown in FIG. 1 (b) as the stem 3 advances. Deforms to project to. At this time, since the plates S1 and S2 are deformed along the outer shape of the tapered portion 3a of the stem 3, the plate S1 in contact with the stem 3 is deformed to a steeper shape than the plate S2 on the die 2 side. In the plate material S1,
The fluidity of the material becomes extremely poor near the periphery of the distal end of the stem 3, and as shown in FIG. 1 (c), the material breaks earlier than the plate S2 at that portion. In the plate material S1 punched by the stem 3 in this manner, a cylindrical portion P having a tapered shape is formed.
【0007】その後、さらにステム3が前進すると、テ
ーパ状部によって板材S1の筒状部Pが押し拡げられ、
ダイ2の穴2aの周縁部との隙間が徐々に狭まる。した
がって、ステム3の前進によって押し伸ばされる板材S
2は、ダイ2の穴2aの周縁部付近で徐々に材料の流動
性が悪くなり、最終的に図1(d)に示すように、ダイ
2の穴2aの周縁部付近で破断する。このバーリング機
構1において、ステム3はテーパ状部3aとダイ2の穴
2aの周縁部との間に板材S1の筒状部Pが挟まれた状
態で停止するようになっており、板材S1の筒状部Pが
ダイ2の穴2aの周縁部で破断することがないように設
定されている。Thereafter, when the stem 3 is further advanced, the cylindrical portion P of the plate S1 is pushed and expanded by the tapered portion.
The gap between the die 2 and the periphery of the hole 2a gradually narrows. Therefore, the plate material S pushed and stretched by the advance of the stem 3
The material 2 gradually deteriorates in the fluidity of the material near the periphery of the hole 2a of the die 2 and finally breaks near the periphery of the hole 2a of the die 2 as shown in FIG. In the burring mechanism 1, the stem 3 stops in a state where the tubular portion P of the plate S1 is sandwiched between the tapered portion 3a and the peripheral edge of the hole 2a of the die 2, and the stem 3 The cylindrical portion P is set so as not to be broken at the peripheral portion of the hole 2 a of the die 2.
【0008】前述のようにしてバーリング機構1により
バーリング処理が施された2枚の板材S1,S2は、板
材S1の筒状部Pがステム3によって押し拡げられて板
材S2の破断部分に圧着している関係から、そのままで
も簡易的な接合状態となっている。このことにより、2
枚の板材S1,S2を予め仮止めしておくことができ、
複数箇所に同様のバーリング処理を施して板材S1,S
2を接合する場合、あるいは板材の形状を正確に合致さ
せて接合しなければならない場合などの作業性を向上し
ている。The two plate members S1 and S2, which have been subjected to the burring process by the burring mechanism 1 as described above, are pressed and spread on the broken portion of the plate member S2 by the cylindrical portion P of the plate member S1 being pushed and expanded by the stem 3. Therefore, a simple joining state is obtained as it is. As a result, 2
The sheet materials S1 and S2 can be temporarily fixed in advance,
A similar burring process is performed on a plurality of places to make the plate materials S1, S
In this case, the workability is improved in the case of joining the two or in the case where the shape of the plate material must be accurately matched and joined.
【0009】このようにバーリング処理が完了すると、
図2(a)、(b)に示すかしめ機構4によって板材S
1の筒状部Pをかしめるかしめ作業が行われる。このか
しめ機構4は、板材S1,S2を支持するアンビル5
と、アンビル5に板材S1,S2を押し付ける押圧部材
6とを有しており、アンビル5先端は、前記ステム3の
先端形状と同じくテーパ状部5aに成形されている。か
しめ作業は、板材S1の筒状部Pを突出端側からアンビ
ル5のテーパ状部5aに嵌合させ(図2(a))、押圧
部材6により板材S1,S2を押圧することにより、板
材S1の筒状部Pを板材S2に接するように巻き返して
行われる(図2(b))。このかしめ作業時、板材S2
には板材S1にあるような筒状部Pが成形されていない
ため、板材S1の筒状部Pを巻き返した時に、板材S2
への引掛かり量を充分確保することができ、板材S1,
S2を確実かつ強固に接合することが可能である。When the burring process is completed as described above,
The plate material S is formed by the caulking mechanism 4 shown in FIGS.
A caulking operation of caulking the cylindrical portion P is performed. The caulking mechanism 4 includes an anvil 5 that supports the plate materials S1 and S2.
And a pressing member 6 for pressing the plate members S1 and S2 against the anvil 5, and the tip of the anvil 5 is formed into a tapered portion 5 a like the tip shape of the stem 3. The caulking operation is performed by fitting the tubular portion P of the plate material S1 from the protruding end side to the tapered portion 5a of the anvil 5 (FIG. 2A), and pressing the plate materials S1 and S2 by the pressing member 6. This is performed by winding back the cylindrical portion P of S1 so as to be in contact with the plate material S2 (FIG. 2B). During this caulking operation, the sheet material S2
Is not formed with the cylindrical portion P as in the plate member S1, and when the cylindrical portion P of the plate member S1 is rewound, the plate member S2 is formed.
To the plate material S1,
It is possible to securely and firmly join S2.
【0010】なお、本発明の実施の形態においては、板
材を2枚重ねて接合する例について説明したが、何もこ
れに限定されるものではなく、板材が2枚以上の複数枚
積層された状態にあっても、作用効果は同様であり、ス
テムが当接する板材のみに筒状部を成形して各板材を良
好に接合することができる。In the embodiment of the present invention, an example in which two plate materials are overlapped and joined is described, but the present invention is not limited to this, and two or more plate materials are laminated. Even in the state, the operation and effect are the same, and the tubular portion can be formed only on the plate member with which the stem abuts, and the plate members can be joined well.
【0011】[0011]
【発明の効果】以上説明したように、本発明の板材の接
合方法は、まず、テーパ状部を有するステムの前進によ
りステムの当接する板材を打ち抜いてこれに筒状部を成
形し、続いてステムをさらに前進させることで筒状部と
ダイの穴との隙間を狭め、このダイの穴の周縁部付近で
ダイ側の板材を破断させているため、ダイ側の板材には
従来のような筒状部が成形されることがなく、このこと
によって筒状部を巻き返した際の引掛かり部分を寸法的
に十分確保することができ、板材を確実、強固に接合す
ることができる等の効果を得ることができる。また、ダ
イ側の板材に筒状部が成形されないことで、かしめを行
った場合に巻き返し部分の厚さを格段に薄くすることが
可能であり、このことによって突出部分を少なくして見
栄えの良い製品を提供することができる等の効果を得る
こともできる。As described above, according to the method of joining plate materials according to the present invention, first, a plate material to be brought into contact with the stem is punched out by advancing the stem having a tapered portion, and a tubular portion is formed therefrom. By further advancing the stem, the gap between the cylindrical part and the hole in the die is narrowed, and the plate material on the die side is broken near the periphery of the hole in the die. The tubular portion is not formed, and thus, the catch portion when the tubular portion is rewound can be sufficiently secured in dimension, and the plate material can be securely and firmly joined. Can be obtained. Further, since the cylindrical portion is not formed on the plate material on the die side, it is possible to remarkably reduce the thickness of the rewinding portion when caulking is performed, thereby reducing the protruding portion and improving the appearance. It is also possible to obtain effects such as being able to provide a product.
【図1】本発明に係る板材の接合方法のバーリング処理
を示す動作説明図である。FIG. 1 is an operation explanatory view showing a burring process of a method of joining plate materials according to the present invention.
【図2】本発明に係る板材の接合方法のかしめ作業を示
す動作説明図である。FIG. 2 is an operation explanatory view showing a caulking operation of the plate material joining method according to the present invention.
【図3】従来例の説明図である。FIG. 3 is an explanatory diagram of a conventional example.
1 バーリング機構 2 ダイ 2a 穴 3 ステム 3a テーパ状部 4 かしめ機構 5 アンビル 5a テーパ状部 6 押圧部材 S1 板材 S2 板材 P 筒状部 Reference Signs List 1 burring mechanism 2 die 2a hole 3 stem 3a tapered part 4 caulking mechanism 5 anvil 5a tapered part 6 pressing member S1 plate S2 plate S cylindrical
Claims (3)
するステムが進入可能な穴を有するダイ上に、積層状態
にある複数枚の板材を載置し、 ステムを前進させてテーパ状部により各板材を押圧し、 まずステムが接する板材を打ち抜いてこれにステムの移
動方向に突出する筒状部を成形し、 続いてステムをさらに前進させることで筒状部が成形さ
れた板材以外の板材をダイの穴の周縁部付近で破断さ
せ、 最終的に前記筒状部をかしめて各板材を一体に接合する
ことを特徴とする板材の接合方法。1. A plurality of plate materials in a stacked state are placed on a die having a hole into which a stem having a tapered portion having a smaller diameter toward the tip can enter, and the stem is advanced by tapering the stem. By pressing each plate material, first punching the plate material that the stem contacts, forming a cylindrical part protruding in the moving direction of the stem, and then further moving the stem forward, other than the plate material with the cylindrical part formed A plate material joining method, wherein a plate material is broken near a peripheral portion of a hole of a die, and finally, the tubular portion is caulked to join the respective plate materials together.
広げ、ダイの穴の周縁部との隙間を狭めることによりダ
イ側の板材をダイの穴の周縁部付近で破断させることを
特徴とする請求項1に記載の板材の接合方法。2. The method according to claim 1, wherein the tapered portion of the stem pushes and expands the cylindrical portion, thereby narrowing a gap between the die and the peripheral edge of the die hole to break the plate material on the die side near the peripheral edge of the die hole. The method for joining plate materials according to claim 1.
1または請求項2に記載の板材の接合方法。3. The method for joining plate materials according to claim 1, wherein the number of plate materials is two.