JPH09268317A - How to quench steel - Google Patents

How to quench steel

Info

Publication number
JPH09268317A
JPH09268317A JP10638796A JP10638796A JPH09268317A JP H09268317 A JPH09268317 A JP H09268317A JP 10638796 A JP10638796 A JP 10638796A JP 10638796 A JP10638796 A JP 10638796A JP H09268317 A JPH09268317 A JP H09268317A
Authority
JP
Japan
Prior art keywords
heating
steel material
quenching
steel
temperature
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP10638796A
Other languages
Japanese (ja)
Other versions
JP3542228B2 (en
Inventor
Michio Maruki
三千男 丸木
Koji Obayashi
巧治 大林
Takatoshi Suzuki
隆敏 鈴木
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Aisin AW Co Ltd
Toyota Central R&D Labs Inc
Original Assignee
Aisin AW Co Ltd
Toyota Central R&D Labs Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Aisin AW Co Ltd, Toyota Central R&D Labs Inc filed Critical Aisin AW Co Ltd
Priority to JP10638796A priority Critical patent/JP3542228B2/en
Publication of JPH09268317A publication Critical patent/JPH09268317A/en
Application granted granted Critical
Publication of JP3542228B2 publication Critical patent/JP3542228B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

(57)【要約】 【課題】 焼入れによる硬度向上効果を維持し,かつ,
残留応力を制御することができる,鋼材の焼入れ方法を
提供すること。 【解決手段】 鋼材に対して,第1加熱(A)と,これ
よりも高い温度の第2加熱(B)とをそれぞれ部分的に
互いに隣接させて実施し,その後急冷する鋼材の焼入れ
方法である。第1加熱は,鋼材のオーステナイト変態点
以上で鋼材の溶融温度以下の温度で行い,一方上記第2
加熱は,鋼材の表層が溶融する溶融温度以上の温度で行
う。第1加熱と第2加熱とは,鋼材における調質所望部
分に対して行うことが好ましい。また第1加熱及び第2
加熱は,高密度エネルギービームを照射することにより
行うことが好ましい。
(57) [Abstract] [Problem] To maintain the hardness improvement effect by quenching, and
To provide a quenching method for steel materials capable of controlling residual stress. SOLUTION: The quenching method for a steel material comprises first heating (A) and second heating (B) at a temperature higher than that of the steel material partially adjacent to each other, and then rapidly cooling. is there. The first heating is performed at a temperature above the austenite transformation point of the steel and below the melting temperature of the steel, while the above second
Heating is performed at a temperature above the melting temperature at which the surface layer of the steel material melts. The first heating and the second heating are preferably performed on a desired portion of the steel material for heat treatment. The first heating and the second
The heating is preferably performed by irradiating a high density energy beam.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【技術分野】本発明は,鋼材を焼入れによって高硬度化
すると共に,焼入れに伴う残留応力を制御する方法に関
する。
TECHNICAL FIELD The present invention relates to a method of increasing the hardness of a steel material by quenching and controlling a residual stress associated with the quenching.

【0002】[0002]

【従来技術】従来,鋼材の表面硬度を高くし,耐摩耗性
や疲労強度等を向上させるために,いわゆる焼入れ処理
が行われている。かかる焼入れ処理は,鋼材をオーステ
ナイト変態点以上の温度に加熱し,次いで急冷すること
により,オーステナイト相をマルテンサイト相に変態さ
せる。このマルテンサイトは,非常に硬く,鋼材の硬度
を高めるのに非常に効果的である。
2. Description of the Related Art Conventionally, so-called quenching treatment has been performed in order to increase the surface hardness of steel materials and improve wear resistance and fatigue strength. In the quenching treatment, the steel material is heated to a temperature above the austenite transformation point and then rapidly cooled to transform the austenite phase into the martensite phase. This martensite is very hard and very effective in increasing the hardness of steel.

【0003】一方,鋼材の表面層を急速に焼入れ処理す
る方法として,例えば,高密度エネルギービームを照射
して鋼材の表面層を急激に加熱し,次いで急冷する方法
が提案されている(特願平7−345160号)。そし
て,この提案においては,上記加熱を,鋼材の表層が溶
融するほどの高いエネルギーを用いて行えば,非常に優
れた焼入れ効果が得られることが示されている。
On the other hand, as a method for rapidly quenching the surface layer of a steel material, for example, a method of irradiating a high-density energy beam to rapidly heat the surface layer of the steel material and then rapidly cooling it has been proposed (Japanese Patent Application No. 2000-242242). No. 7-345160). Then, in this proposal, it is shown that a very excellent quenching effect can be obtained if the above heating is carried out with energy high enough to melt the surface layer of the steel material.

【0004】即ち,鋼材をその表層が溶融する温度以上
の温度で加熱し,その後急冷することにより,表層の溶
融部分だけでなく,その下層部分が比較的深い範囲でマ
ルテンサイト化され,高硬度の焼入れ硬化層を比較的深
く形成することができる。そのため,極めて優れた硬度
向上効果が得られる。
That is, by heating the steel material at a temperature higher than the temperature at which the surface layer melts and then rapidly cooling it, not only the molten portion of the surface layer but also the lower layer portion thereof become martensite in a relatively deep range, resulting in high hardness. The quench hardened layer can be formed relatively deeply. Therefore, an extremely excellent hardness improving effect can be obtained.

【0005】[0005]

【解決しようとする課題】しかしながら,上記焼入れ方
法においては,次の問題がある。即ち,上記鋼材の溶融
温度以上に加熱後急冷して焼入れする方法(以下,適宜
溶融焼入れという)によれば,優れた焼入れ効果が得ら
れる一方,表層の溶融層の再凝固時に引張残留応力が発
生する。
However, the above quenching method has the following problems. That is, according to the method of quenching after quenching after heating above the melting temperature of the above steel material (hereinafter appropriately referred to as melt quenching), while an excellent quenching effect is obtained, tensile residual stress during resolidification of the molten layer of the surface layer appear.

【0006】この引張残留応力は,焼入れ歪みを発生さ
せる原因となるだけでなく,焼き割れや破損等を引き起
こしやすく,有害である。この対策として,上記加熱を
鋼材のオーステナイト変態点以上で溶融温度以下の温度
で行いその後急冷する方法(以下,適宜,非溶融焼入れ
という)に変更することが考えられる。
This tensile residual stress is not only a cause of quenching strain, but also prone to quench cracking and damage, which is harmful. As a countermeasure against this, it is conceivable to change the above heating method to a method in which the temperature is higher than the austenite transformation point of the steel material and lower than the melting temperature and then rapidly cooled (hereinafter appropriately referred to as non-melt quenching).

【0007】しかし,この非溶融焼入れの場合には,表
層部分における引張残留応力は解消するが,逆に,通常
のオーステナイトからマルテンサイトへの変態による体
積膨張によって,表層に圧縮応力が発生してしまう。ま
た,溶融焼入れの場合よりも焼入れ硬化層が浅くなり,
硬度向上効果も減少してしまう。
However, in the case of this non-melting quenching, the tensile residual stress in the surface layer part is eliminated, but conversely, the compressive stress is generated in the surface layer due to the volume expansion due to the transformation from ordinary austenite to martensite. I will end up. Also, the quench hardening layer becomes shallower than in the case of melt quenching,
The hardness improving effect also decreases.

【0008】本発明は,かかる従来の問題点に鑑みてな
されたもので,焼入れによる硬度向上効果を維持し,か
つ,残留応力を制御することができる,鋼材の焼入れ方
法を提供しようとするものである。
The present invention has been made in view of the above conventional problems, and an object of the present invention is to provide a quenching method for a steel material capable of maintaining the hardness improving effect by quenching and controlling the residual stress. Is.

【0009】[0009]

【課題の解決手段】請求項1の発明は,鋼材に対して,
第1加熱と,これよりも高い温度の第2加熱とをそれぞ
れ部分的に互いに隣接させて実施し,その後急冷する鋼
材の焼入れ方法であって,上記第1加熱は,鋼材のオー
ステナイト変態点以上で鋼材の溶融温度以下の温度で行
い,一方上記第2加熱は,鋼材の表層が溶融する溶融温
度以上の温度で行うことを特徴とする鋼材の焼入れ方法
にある。
The invention according to claim 1 relates to steel material,
A method for quenching a steel material in which first heating and second heating at a temperature higher than this are carried out partially adjacent to each other and then rapidly cooled, wherein the first heating is at least the austenite transformation point of the steel material. In the method for quenching steel, the second heating is performed at a temperature not lower than the melting temperature of the steel, while the second heating is performed at a temperature not lower than the melting temperature at which the surface layer of the steel melts.

【0010】本発明において最も注目すべきことは,上
記第1加熱と上記第2加熱とをそれぞれ部分的に互いに
隣接させて実施することである。即ち,鋼材のオーステ
ナイト変態点以上で鋼材の溶融温度以下の温度による第
1加熱を行った後急冷する,いわば「非溶融焼入れ」し
た部分と,鋼材の表層が溶融する溶融温度以上の温度に
よる第2加熱を行った後急冷する,いわば「溶融焼入
れ」部分とを,鋼材上に互いに隣接して形成することで
ある。
What is most noticeable in the present invention is that the first heating and the second heating are performed partially adjacent to each other. That is, the first heating at a temperature above the austenite transformation point of the steel material and below the melting temperature of the steel material is followed by rapid cooling, so to speak, "non-melt quenching", and 2 To form a so-called "melt-quenched" portion on a steel material, which is so-called "melt-quenched" after being heated and then rapidly cooled.

【0011】本発明において対象とする鋼材としては,
例えば,S50C,S23C,S10C等の炭素鋼,S
NCM,SCR,SCM等の合金鋼,SK,SKD,S
KH,SKS等の工具鋼など,焼入れ調質を行うもので
ある。
The steel material to which the present invention is applied includes
For example, carbon steel such as S50C, S23C, S10C, S
Alloy steel such as NCM, SCR, SCM, SK, SKD, S
It is used for quenching and tempering of tool steels such as KH and SKS.

【0012】上記第1加熱は,上記のごとく鋼材のオー
ステナイト変態点以上で鋼材の溶融温度以下の温度で行
う。即ち,第1加熱温度は,後述する図3に示した鉄−
炭素系平衡状態図における,γ(オーステナイト)領域
内の温度である。なお,δ(非溶融)領域内の温度もこ
れに含める。具体的には例えば組成がL1 の場合には,
P1 からP2 までの温度で行う。
As described above, the first heating is performed at a temperature above the austenite transformation point of the steel material and below the melting temperature of the steel material. That is, the first heating temperature is equal to that of the iron shown in FIG.
It is the temperature in the γ (austenite) region in the carbon system equilibrium diagram. The temperature in the δ (non-melting) region is also included in this. Specifically, for example, when the composition is L 1 ,
Perform at a temperature from P 1 to P 2 .

【0013】この第1加熱温度に加熱することにより,
鋼材の組成がオーステナイトとなり,これを急冷するこ
とにより,オーステナイトがマルテンサイトに変態し,
焼入れ硬化層となる。一方オーステナイト変態点以下の
温度(例えば上記P1 未満の温度)の場合には,加熱に
よるオーステナイト変態が不完全であるため,急冷によ
るマルテンサイト変態も不完全となる。
By heating to this first heating temperature,
The composition of steel becomes austenite, and by quenching it, austenite transforms to martensite,
It becomes a quench hardening layer. On the other hand, when the temperature is below the austenite transformation point (for example, the temperature below P 1 ), the austenite transformation due to heating is incomplete, so that the martensite transformation due to quenching is also incomplete.

【0014】また,上記第2加熱は,上記のごとく第1
加熱よりも高い温度であって,鋼材の表層が溶融する溶
融温度以上の温度で行う。即ち,第2加熱温度は,これ
も後述する図3に示した鉄−炭素系平衡状態図において
説明すると,鋼材の表層がγ相領域を超える温度であ
る。
The second heating is performed by the first heating as described above.
It is performed at a temperature higher than the heating temperature and higher than the melting temperature at which the surface layer of the steel material melts. That is, the second heating temperature is a temperature at which the surface layer of the steel material exceeds the γ phase region, which will be described later with reference to the iron-carbon system equilibrium diagram shown in FIG.

【0015】具体的には,例えば組成がL1 の場合に
は,表層がP2 点以上の温度となるように加熱する。た
だし,あくまでも溶融する領域は,鋼材の表層部分のみ
である。鋼材が全体的に溶融した場合には,全体の形状
等を維持することができないという問題がある。
Specifically, for example, when the composition is L 1 , heating is performed so that the surface layer has a temperature of P 2 point or higher. However, the only melting area is the surface layer of the steel. When the steel material is entirely melted, there is a problem that the overall shape cannot be maintained.

【0016】次に,本発明の作用につき説明する。本発
明の鋼材の焼入れ方法においては,上記第1加熱と第2
加熱とをそれぞれ部分的に互いに隣接させて実施する。
そのため,鋼材上には,上記溶融焼入れ部分と非溶融焼
入れ部分がそれぞれ部分的に互いに隣接して形成され
る。
Next, the operation of the present invention will be described. In the method for quenching steel according to the present invention, the first heating and the second
The heating and the partial heating are carried out partially adjacent to each other.
Therefore, the melt-quenched portion and the non-melt-quenched portion are formed on the steel material so as to be partially adjacent to each other.

【0017】ここで,上記非溶融焼入れ部分は,上記第
1加熱により溶融することなく処理されている。そのた
め,オーステナイトからマルテンサイトへの変態による
体積膨張によって表層に圧縮残留応力が発生している。
一方,上記溶融焼入れ部分は,上記第2加熱により鋼材
の表層が溶融するように処理されている。そのため,溶
融焼入れ部分の表層には,凝固収縮による引張残留応力
が発生している。
Here, the non-melt-quenched portion is processed by the first heating without melting. Therefore, compressive residual stress occurs in the surface layer due to volume expansion due to transformation from austenite to martensite.
On the other hand, the melt-quenched portion is treated so that the surface layer of the steel material is melted by the second heating. Therefore, tensile residual stress due to solidification shrinkage occurs in the surface layer of the melt-quenched portion.

【0018】即ち,鋼材上には,圧縮残留応力部分と引
張残留応力部分とが,互いに隣接して形成される。その
ため,焼入れ処理された鋼材全体でみれば,圧縮残留応
力と引張残留応力とが互いに緩和しあい,実質上残留応
力はほとんど解消される。それ故,残留応力に起因する
歪みの発生や,焼入れ後の置き割れ等の不具合を十分に
回避することができる。
That is, a compressive residual stress portion and a tensile residual stress portion are formed adjacent to each other on the steel material. Therefore, in the case of the quenched steel as a whole, the compressive residual stress and the tensile residual stress relax each other, and the residual stress is virtually eliminated. Therefore, it is possible to satisfactorily avoid the occurrence of strain due to the residual stress and the inconveniences such as the cracking after the quenching.

【0019】また上記第2加熱は,溶融する表層の下層
に,上記第1加熱の場合よりも深い範囲までオーステナ
イト相を形成する。そのため,第2加熱後急冷すること
により,上記第1加熱の場合に比べて深い範囲までマル
テンサイト化された焼入れ硬化層が形成される。即ち,
第2加熱による溶融焼入れの場合には,第1加熱による
非溶融焼入れの場合に比べて表面から深いところまで焼
入れ硬化層が形成され,硬度向上効果が非常に高くな
る。
Further, the second heating forms an austenite phase in the lower layer of the melted surface layer to a deeper range than in the case of the first heating. Therefore, by quenching after the second heating, a quench-hardened layer martensitic to a deeper range than in the case of the first heating is formed. That is,
In the case of the melt-quenching by the second heating, as compared with the case of the non-melt-quenching by the first heating, the quench-hardened layer is formed deeper from the surface, and the effect of improving the hardness becomes very high.

【0020】そして,本発明においては溶融焼入れ部分
を非溶融焼入れ部分と混在させて隣接配置する。そのた
め,鋼材全体を非溶融焼入れする場合に比べて,硬度向
上効果を高く維持することができる。それ故,高い硬度
向上効果を維持しつつ,上記残留応力の制御を図ること
ができる。
In the present invention, the melt-quenched portion and the non-melt-quenched portion are mixed and arranged adjacent to each other. Therefore, the hardness improving effect can be maintained higher than in the case where the entire steel material is non-melt-quenched. Therefore, it is possible to control the residual stress while maintaining a high hardness improving effect.

【0021】次に,請求項2の発明のように,上記第1
加熱と上記第2加熱とは,鋼材における調質所望部分の
みに対して行うことができる。ここでいう調質所望部分
とは,焼入れにより硬化したい部分をいう。これによ
り,製品の種類等に応じて,必要部分のみを硬化し,他
の部分には例えば比較的軟らかく粘り強い性質の部分を
残すことができる。
Next, as in the second aspect of the present invention, the first
The heating and the second heating can be performed only on the desired portion for heat treatment in the steel material. The desired portion for refining as used herein means a portion desired to be hardened by quenching. As a result, it is possible to cure only the necessary parts according to the type of product, etc., while leaving the other parts, for example, parts that are relatively soft and tenacious.

【0022】また,請求項3の発明のように,上記第1
加熱及び上記第2加熱は,鋼材に対して高密度エネルギ
ービームを照射することにより行うことが好ましい。こ
れにより,上記第1加熱及び第2加熱をレスポンス良
く,効率良く行うことができる。そのため,高い生産性
と安定した品質が得られる。この高密度エネルギービー
ムによる方法は,上記調質所望部分のみを部分的に焼入
れしたい場合に,特にその効果が大きい。
Further, as in the third aspect of the present invention, the first
The heating and the second heating are preferably performed by irradiating the steel material with a high-density energy beam. As a result, the first heating and the second heating can be performed efficiently with good response. Therefore, high productivity and stable quality can be obtained. The method using the high-density energy beam is particularly effective when it is desired to partially quench only the desired portion for refining.

【0023】上記高密度エネルギービームとしては,例
えば電子ビーム,レーザビーム,また,ビームではない
が高周波加熱などの高密度エネルギーがある。本発明で
は,これらを総称して高密度エネルギービームという。
なお,上記電子ビームは電子ビームガンに高電圧を印加
することにより発生させる。また,レーザ光は,レーザ
発振器に高電圧を印加することにより発生させる。
Examples of the high-density energy beam include electron beams, laser beams, and high-density energy such as high-frequency heating, which is not a beam. In the present invention, these are collectively called high-density energy beams.
The electron beam is generated by applying a high voltage to the electron beam gun. The laser light is generated by applying a high voltage to the laser oscillator.

【0024】次に,請求項4の発明のように,上記高密
度エネルギービームの照射は,上記第1加熱を行う第1
加熱用ビームと,上記第2加熱を行う第2加熱用ビーム
とを用いて,上記第1加熱用ビームによる第1加熱と,
上記第2加熱用ビームによる第2加熱とを同時に行う方
法がある。この場合には,上記第1加熱と第2加熱とを
同時に行うことができるため,トータルの処理時間を短
くして,サイクルタイムを短縮することができる。
Next, as in the invention of claim 4, the irradiation of the high-density energy beam is performed by the first heating for the first heating.
Using the heating beam and the second heating beam for performing the second heating, the first heating by the first heating beam;
There is a method of simultaneously performing the second heating by the second heating beam. In this case, since the first heating and the second heating can be performed at the same time, the total processing time can be shortened and the cycle time can be shortened.

【0025】また,請求項5の発明にように,上記高密
度エネルギービームは,1箇所のビーム発生源から発射
されたビームを,複数箇所に分配して照射することがで
きる。この場合には,1本の高密度エネルギービームを
偏向制御装置等により複数に分割する。これにより,1
本の高密度エネルギービームを,鋼材における所望する
複数部分に,同時に分配照射することができ,照射設備
を小型化することができる。
Further, as in the fifth aspect of the invention, the high-density energy beam can be irradiated by dividing the beam emitted from the beam generating source at one place into a plurality of places. In this case, one high-density energy beam is divided into a plurality of beams by a deflection control device or the like. This gives 1
The high-density energy beam of the book can be simultaneously distributed-irradiated to desired portions of the steel material, and the irradiation equipment can be downsized.

【0026】また,請求項6の発明のように,上記急冷
は,103 ℃/分以上の速度で行うことが好ましい。上
記103 ℃/分未満では,低炭素鋼ではマルテンサイト
変態が十分におこなわれないという問題がある。なお,
その上限は,速いほど良いが,鋼の熱伝導率により限定
されるものである。
As in the sixth aspect of the invention, it is preferable that the rapid cooling is performed at a rate of 10 3 ° C / min or more. Below 10 3 ° C / min, there is a problem that martensitic transformation is not sufficiently performed in low carbon steel. In addition,
The upper limit is better as it is faster, but it is limited by the thermal conductivity of steel.

【0027】[0027]

【発明の実施の形態】BEST MODE FOR CARRYING OUT THE INVENTION

実施形態例1 本発明の実施形態例にかかる鋼材の焼入れ方法につき,
図1〜図5を用いて説明する。即ち,本例の鋼材の焼入
れ方法は,図1(a)に示すごとく,被処理材としての
鋼材2(図2)に対して,第1加熱(A)と,これより
も高い温度の第2加熱(B)とをそれぞれ部分的に互い
に隣接させて行い,その後急冷する。
Embodiment 1 Regarding a method for quenching a steel material according to an embodiment of the present invention,
This will be described with reference to FIGS. That is, as shown in FIG. 1 (a), the quenching method of the steel material of this example is the same as that for the steel material 2 (FIG. 2) as the material to be treated, the first heating (A) and the first heating at a temperature higher than this. 2) Heating (B) is performed partially adjacent to each other, followed by quenching.

【0028】上記第1加熱は,鋼材のオーステナイト変
態点以上で鋼材の溶融温度以下の温度で行う。即ち,図
3に示した鉄−炭素系平衡状態図において,例えば組成
をL1 とすると,表層の温度がL1 線上におけるT1 点
になるまで加熱する。一方,第2加熱は,鋼材の表層が
溶融する溶融温度以上の温度で加熱する。即ち,例え
ば,図3において,表層の温度がL1 線上におけるT2
点になるまで加熱する。なお,部分的溶融のT2 ′点ま
での加熱もこの中に含まれる。
The first heating is carried out at a temperature above the austenite transformation point of the steel and below the melting temperature of the steel. That is, in the iron-carbon system equilibrium diagram shown in FIG. 3, when the composition is L 1 , for example, the surface layer is heated until the temperature reaches the T 1 point on the L 1 line. On the other hand, the second heating is performed at a temperature equal to or higher than the melting temperature at which the surface layer of the steel material melts. That is, for example, in FIG. 3, the temperature of the surface layer is T 2 on the L 1 line.
Heat to the point. The heating up to the T 2 ′ point of partial melting is also included in this.

【0029】なお,ここでは簡単の為,鉄−炭素2元系
平衡状態図で説明するが,これらの変態温度は鋼の成分
によって異なるばかりでなく,急速な加熱では変態温度
は高温側へ,急速な冷却では変態温度は低温側へ移行す
ることが知られており,具体的に鋼の変態温度の数値を
図3に示すごとく限定するものではない。
For the sake of simplicity, the iron-carbon binary system equilibrium diagram will be described here. However, not only these transformation temperatures differ depending on the composition of the steel, but also the transformation temperature increases to the high temperature side by rapid heating. It is known that the transformation temperature shifts to the low temperature side in rapid cooling, and the numerical value of the transformation temperature of steel is not specifically limited as shown in FIG.

【0030】上記第1加熱を行った部分は,図1,図5
に示すごとく,その後の急冷により,ある程度の焼入れ
硬化層29を有する非溶融焼入れ部分Aとなり,上記第
2加熱を行った部分は,その後の急冷により,非溶融焼
入れ部分Aよりも深い焼入れ硬化層29を有する溶融焼
入れ部分Bとなる。
The portion subjected to the first heating is shown in FIGS.
As shown in (4), the subsequent quenching results in a non-melting quenching portion A having a certain degree of quenching hardening layer 29, and the portion subjected to the second heating is a quenching hardening layer deeper than the non-melting quenching portion A by the subsequent quenching. This is a melt-quenched portion B having 29.

【0031】また,本例における上記第1加熱及び第2
加熱は,図2に示すごとく,鋼材2の調質所望部分20
に対して,高密度エネルギービーム11,12を照射す
ることにより行っている。つまり,図2(a)に示すご
とく,高密度エネルギービーム発生源1より,発射した
高密度エネルギービーム10を2種類の出力のビーム1
1,12に順次切り換えながら,これを鋼材2の調質所
望部分20に照射する。
The first heating and the second heating in this example
As shown in FIG. 2, heating is performed on the desired portion 20 of the steel material 2.
The irradiation is performed by irradiating the high-density energy beams 11 and 12. That is, as shown in FIG. 2A, the high-density energy beam 10 emitted from the high-density energy beam source 1 is converted into a beam 1 of two types of outputs.
This is applied to the desired heat treatment portion 20 of the steel material 2 while sequentially switching to 1 and 12.

【0032】上記2種類の出力の高密度エネルギービー
ム11,12は,第1加熱用ビーム11と第2加熱用ビ
ーム12の2種類であって,これらは,一定時間間隔で
切り換えるようにしてある。また,図2に示すごとく,
両ビーム11,12の照射は,鋼材2を,同図の矢印方
向へ移動させながら行う。
The above-mentioned two types of high-density energy beams 11 and 12 having two kinds of output are the first heating beam 11 and the second heating beam 12, and these are switched at fixed time intervals. . Also, as shown in FIG.
The irradiation of both beams 11 and 12 is performed while moving the steel material 2 in the arrow direction in the figure.

【0033】これにより,図1,図2に示すごとく,上
記第1加熱用ビーム11によって加熱された部分が,そ
の後の急冷によって非溶融焼入れ部分Aとなり,第2加
熱用ビーム12によって加熱された部分がその後の急冷
によって溶融焼入れ部分Bとなる。また,これらの急冷
は,上記加熱が表層部だけであるため,加熱完了後の自
己放冷によって十分に速い冷却速度で行うことができ
る。
As a result, as shown in FIGS. 1 and 2, the portion heated by the first heating beam 11 becomes a non-melt-quenched portion A by the subsequent rapid cooling and is heated by the second heating beam 12. The part becomes the melt-quenched part B by the subsequent rapid cooling. Further, these rapid cooling can be performed at a sufficiently high cooling rate by self-cooling after completion of heating, because the above heating is performed only on the surface layer portion.

【0034】上記のごとく,本例においては,非溶融焼
入れ部分Aと溶融焼入れ部分Bとが互いに隣接して交互
に形成される。そのため,図4に示すごとく,この焼入
れによる調質を行った部分の残留応力状態は,非溶融焼
入れ部分Aが圧縮残留応力状態81(図4(a)),溶
融焼入れ部分Bが引張残留応力状態82(図4(b))
となり,連続的にみれば,これらが交互に存在してサイ
ンカーブ状83(図4(c))になっている。
As described above, in this example, the non-melt-quenched portion A and the melt-quenched portion B are alternately formed adjacent to each other. Therefore, as shown in FIG. 4, the residual stress state of the portion that has been tempered by quenching is as follows: the non-melt-quenched portion A has a compressive residual stress state 81 (FIG. 4 (a)), and the melt-quenched portion B has a tensile residual stress. State 82 (Fig. 4 (b))
Therefore, when viewed continuously, these are alternately present and have a sine curve shape 83 (FIG. 4C).

【0035】即ち,焼入れを施した調質部分は,全体的
にみれば残留応力がほぼ解消した状態が実現する。それ
故,焼入れ処理後に残留応力に起因する歪みの発生や置
き割れ等の不具合を防止することができる。
That is, in the tempered portion that has been hardened, the residual stress is almost eliminated as a whole. Therefore, after the quenching treatment, it is possible to prevent the occurrence of strains caused by the residual stress and the problems such as cracks caused by placement.

【0036】また,図5(c)に示すごとく,本例にお
いて得られた焼入れ硬化層29は,浅い部分と深い部分
とが交互に存在する。即ち,上記非溶融焼入れ部分Aは
焼入れ硬化層29が浅く(図5(a)),溶融焼入れ部
分Bは焼入れ硬化層29が深く(図5(b)),これら
が交互に配置されている(図5(c))。この溶融焼入
れ部分Bにおける深い焼入れ硬化層29の存在により,
鋼材2の硬度を非常に高いレベルに維持することができ
る。
Further, as shown in FIG. 5 (c), the quench-hardened layer 29 obtained in this example has alternating shallow and deep portions. That is, the quench-hardened layer 29 is shallow in the non-melt-quenched portion A (FIG. 5A), and the quench-hardened layer 29 is deep in the melt-quenched portion B (FIG. 5B), and these are alternately arranged. (FIG.5 (c)). Due to the presence of the deep quench-hardened layer 29 in the melt-quenched portion B,
The hardness of the steel material 2 can be maintained at a very high level.

【0037】実施形態例2 本例においては,図6に示すごとく,実施形態例1と同
様の焼入れ装置及び方法によって,鋼材2の調質所望部
分20に,非溶融焼入れ部分Aと溶融焼入れ部分Bとを
縦横に互いに隣接配置し,全体的に市松模様状に設け
た。
Embodiment 2 In this embodiment, as shown in FIG. 6, a non-melt-quenched portion A and a melt-quenched portion A are applied to a desired tempered portion 20 of a steel material 2 by the same quenching apparatus and method as in the first embodiment. B and B are vertically and horizontally adjacent to each other, and are provided in a checkered pattern as a whole.

【0038】この場合には,実施形態例1における高密
度エネルギービーム11,12の照射を,鋼材2に対し
て複数列順次実施する。得られた調質部分は,縦横いず
れの方向においても,上述した図4(c)に示すような
残留応力状態と,図5(c)に示すような焼入れ硬化層
29の分布が得られる。そのため,実施形態例1におけ
る効果を一層向上させることができる。
In this case, irradiation of the high-density energy beams 11 and 12 in the first embodiment is sequentially performed on the steel material 2 in a plurality of columns. In the obtained tempered portion, the residual stress state as shown in FIG. 4C and the distribution of the quench-hardened layer 29 as shown in FIG. 5C are obtained in both the vertical and horizontal directions. Therefore, the effect of the first embodiment can be further improved.

【0039】実施形態例3 本例は,図7,図8に示すごとく,上記実施形態例1に
示した鋼材の焼入れ方法において,鋼材2を回転させな
がら,該鋼材2におけるリング状の調質所望部分20
(図8)に対して,高密度エネルギービーム11,12
を連続的に照射する熱処理装置及び方法を示すものであ
る。
Embodiment 3 In this embodiment, as shown in FIGS. 7 and 8, in the quenching method for the steel material shown in the embodiment 1, the steel material 2 is rotated while the ring-shaped heat treatment is performed. Desired portion 20
In contrast to (FIG. 8), high-density energy beams 11 and 12
It shows a heat treatment apparatus and method for continuously irradiating the.

【0040】本例における,被処理材としての鋼材2
は,トルクコンバータ用部品のロックアップクラッチピ
ストンである。このピストンは皿状をなしている(図
7,図10参照)。そして,その一部分にリング状の焼
入れ調質を施す(図8)。上記熱処理装置は,図7に示
すごとく,鋼材2を入れる加工室19と,該加工室19
内に上記高密度エネルギービーム10を照射するビーム
発生源1と,該ビーム発生源1からの高密度エネルギー
ビーム10を,第1加熱用ビーム11と第2加熱ビーム
12とに切り換える偏向コイル111,112とを有す
る。
Steel material 2 as the material to be treated in this example
Is a lock-up clutch piston that is a component for a torque converter. This piston has a dish shape (see FIGS. 7 and 10). Then, a ring-shaped quenching temper is applied to a part of it (Fig. 8). As shown in FIG. 7, the heat treatment apparatus includes a processing chamber 19 in which the steel material 2 is inserted, and the processing chamber 19
A beam generating source 1 for irradiating the high density energy beam 10 therein, and a deflection coil 111 for switching the high density energy beam 10 from the beam generating source 1 into a first heating beam 11 and a second heating beam 12, And 112.

【0041】また,加工室19内を減圧する真空排気装
置16と,上記偏向コイル111,112における高密
度エネルギービームの高速偏向制御装置110とを有す
る。上記偏向コイル111,112に流す電流の周波数
及び波形を変えることにより,高密度エネルギービーム
10の出力を任意に変更し,第1加熱用ビーム11と第
2加熱用ビーム12とに切り換えることができる。ま
た,上記加工室19の下部には,上記鋼材2の載置台1
5を回転させるための回転モータ150を有する。これ
らの装置は,総合制御装置17によりコントロールされ
る。
Further, it has a vacuum exhaust device 16 for reducing the pressure in the processing chamber 19, and a high-speed deflection control device 110 for the high-density energy beams in the deflection coils 111, 112. The output of the high-density energy beam 10 can be arbitrarily changed by changing the frequency and the waveform of the current passed through the deflection coils 111 and 112, and the beam can be switched between the first heating beam 11 and the second heating beam 12. . In addition, at the lower part of the processing chamber 19, the mounting table 1 for the steel material 2 is provided.
It has a rotary motor 150 for rotating 5. These devices are controlled by the general controller 17.

【0042】そして,上記熱処理装置により,鋼材の焼
入れを実施するに当たっては,まず上記回転モータ15
0を駆動させて,上記鋼材2を図8の矢印方向に約8m
/分の速度で回転させておく。また,真空排気装置16
により,加工室19内を真空状態にする。
When the steel material is quenched by the heat treatment apparatus, first the rotary motor 15 is used.
0 to drive the above steel material 2 about 8 m in the direction of the arrow in FIG.
Rotate at a speed of / minute. In addition, the vacuum exhaust device 16
Thus, the processing chamber 19 is evacuated.

【0043】そして,図7,図8に示すごとく,鋼材2
に対してまず高密度エネルギービーム10を第1加熱用
ビーム11(1.0KW)として0.5秒間照射し,次
いで,高密度エネルギービーム10の出力を上げて第2
加熱用ビーム12(3.0KW)として1.5秒間照射
する。さらに同一サイクルで,第1加熱用ビーム11に
よる照射と第2加熱用ビーム12による照射を連続して
切り換えながら行う。
Then, as shown in FIG. 7 and FIG.
First, the high-density energy beam 10 is irradiated as the first heating beam 11 (1.0 kW) for 0.5 seconds, and then the output of the high-density energy beam 10 is increased to the second.
Irradiation is performed for 1.5 seconds as a heating beam 12 (3.0 KW). Further, in the same cycle, the irradiation with the first heating beam 11 and the irradiation with the second heating beam 12 are continuously switched.

【0044】上記高密度エネルギービーム11,12の
照射を受けた部分は,照射完了後,自己放冷により即座
に急冷される。つまり,図9(a)に示すごとく,第1
加熱用ビーム11を受けた部分の表層は,オーステナイ
ト変態点T4 以上で融点T5以下の温度31に急速に加
熱後,マルテンサイト変態点T3 以下に急冷されるとい
うヒートパターンとなる。一方,図9(b)に示すごと
く,第2加熱用ビーム12を受けた部分の表層は,融点
T5 以上の温度32に急速に加熱後,マルテンサイト変
態点T3 以下に急冷されるというヒートパターンとな
る。
The parts irradiated with the high-density energy beams 11 and 12 are rapidly cooled by self-cooling after the irradiation is completed. That is, as shown in FIG. 9A, the first
The surface layer of the portion receiving the heating beam 11 has a heat pattern in which it is rapidly heated to a temperature 31 above the austenite transformation point T 4 and below the melting point T 5 and then rapidly cooled below the martensite transformation point T 3 . On the other hand, as shown in FIG. 9B, the surface layer receiving the second heating beam 12 is rapidly heated to a temperature 32 higher than the melting point T 5 and then rapidly cooled to a temperature below the martensitic transformation point T 3. It becomes a heat pattern.

【0045】このように,交互に第1加熱と第2加熱を
繰り返しながら,鋼材2が1回転した時点で,リング状
の焼入れ処理が完了する。即ち,鋼材2には,図8に示
すごとく,非溶融焼入れ部分Aと溶融焼入れ部分Bとが
互いに隣接してリング状に形成される。したがって,本
例においても,実施形態例1と同様の効果が得られる。
As described above, the ring-shaped quenching process is completed when the steel material 2 makes one rotation while alternately repeating the first heating and the second heating. That is, as shown in FIG. 8, in the steel material 2, the non-melt-quenched portion A and the melt-quenched portion B are formed adjacent to each other in a ring shape. Therefore, also in this example, the same effect as that of the first embodiment can be obtained.

【0046】実施形態例4 本例は,実施形態例1及び3に示した鋼材の焼入れ方法
及び装置を用いた具体例である。即ち,本例における被
処理品としての鋼材は,図10に示すごとく,トルクコ
ンバータに用いるロックアップクラッチピストン41で
ある。
Embodiment 4 This embodiment is a concrete example using the steel quenching method and apparatus shown in Embodiments 1 and 3. That is, the steel material as the article to be processed in this example is the lockup clutch piston 41 used in the torque converter as shown in FIG.

【0047】このロックアップクラッチピストン41
は,トルクコンバータにおいて,伝達トルクの変動を吸
収するためのダンパ装置に部分的にかしめ固定されるも
のである。なお,同図の符号43は取付用穴である。そ
して,上記ダンパ装置は,図10に示すごとく,タービ
ンライナと一体に回転させられるドリブンプレート51
及びスプリング52,53等からなる。
This lockup clutch piston 41
In the torque converter, is partially caulked and fixed to a damper device for absorbing fluctuations in transmission torque. Reference numeral 43 in the figure is a mounting hole. As shown in FIG. 10, the damper device includes a driven plate 51 that is rotated integrally with the turbine liner.
And springs 52, 53 and the like.

【0048】ここで,図10に示すごとくスプリング5
2はロックアップクラッチピストン41の円周方向にお
ける8箇所に配設された第1ステージ用のものであり,
またスプリング53はロックアップクラッチピストン4
1の円周方向における4箇所に配設された第2ステージ
用のものであって,このスプリング53はスプリング5
2内に一つ置きに配設される。なお,前記スプリング5
3はスプリング52より径が小さく,かつ短く設定さ
れ,スプリング52の捩れ角が設定値になって伝達トル
クが屈曲点トルクに到達した後に撓み始める。
Here, as shown in FIG. 10, the spring 5
2 is for the first stage, which is arranged at eight locations in the circumferential direction of the lockup clutch piston 41,
Further, the spring 53 is the lockup clutch piston 4
1 for the second stage, which is arranged at four locations in the circumferential direction of 1, and this spring 53 is
Every two of them are arranged in two. In addition, the spring 5
3 has a diameter smaller than that of the spring 52 and is set to be shorter. The torsion angle of the spring 52 reaches a set value, and the transmitted torque starts to bend after reaching the bending point torque.

【0049】従って,フロントカバーから摩擦材を介し
て伝達された回転は前記ダンパ装置を介してタービンハ
ブに伝達されるが,この際,スプリング52,53が収
縮して回転伝達時における伝達トルクの変動を吸収す
る。また,“エンジンの出力トルクの急激な変動”が図
示しない変速装置に伝達されることによって起きる振
動,騒音等を防止する役目を担っている。
Therefore, the rotation transmitted from the front cover via the friction material is transmitted to the turbine hub via the damper device. At this time, the springs 52 and 53 contract to transmit the transmission torque during the rotation transmission. Absorb fluctuations. In addition, it also plays a role of preventing vibration, noise, and the like caused by the transmission of "rapid changes in the output torque of the engine" to a transmission (not shown).

【0050】ところで,前記ロックアップクラッチピス
トン41の正駆動時(ロックアップクラッチ装置が係合
状態に置かれてロックアップクラッチピストン41が図
10における反時計回り方向に回転する時)及び逆駆動
時(エンジンブレーキ時等でロックアップクラッチピス
トン41が図10における時計回り方向に回転する時)
には前記スプリング52が圧縮されるので,このスプリ
ング52がロックアップクラッチピストン41の平板部
411と繰り返し摺動しがちとなる。
By the way, during the normal drive of the lock-up clutch piston 41 (when the lock-up clutch device is placed in the engaged state and the lock-up clutch piston 41 rotates counterclockwise in FIG. 10) and during the reverse drive. (When the lock-up clutch piston 41 rotates clockwise in FIG. 10 due to engine braking, etc.)
Since the spring 52 is compressed, the spring 52 tends to repeatedly slide on the flat plate portion 411 of the lockup clutch piston 41.

【0051】そのため,ロックアップクラッチピストン
41の平板部411にはスプリング52との摺動による
摩擦が生じるという問題がある。そして,ロックアップ
クラッチピストン41は上記スプリング52と接触する
ドーナツ状のスプリング受け40の部分(図10のハッ
チング部分)を有している。
Therefore, there is a problem in that the flat plate portion 411 of the lockup clutch piston 41 causes friction due to sliding with the spring 52. The lock-up clutch piston 41 has a donut-shaped spring receiver 40 portion (hatched portion in FIG. 10) that contacts the spring 52.

【0052】このロックアップクラッチピストンのスプ
リング受け40は,耐摩耗性等が要求される。そのた
め,そのスプリング受け部分(厚み3mm)に,部分的
に焼入れ処理を施す必要がある。上記部品の材質は,S
23Cである。
The spring receiver 40 of the lockup clutch piston is required to have wear resistance and the like. Therefore, it is necessary to partially quench the spring receiving portion (thickness: 3 mm). The material of the above parts is S
23C.

【0053】また,焼入れ処理を行うに当たっては,上
記第1加熱,第2加熱には実施形態例1,3に示した高
密度エネルギービームとしての電子ビームを用いた。上
記電子ビーム発生装置は,最大5KWの出力を有し,第
1加熱用ビームとしての1.0KWの電子ビームと第2
加熱用ビームとしての3.0KWの電子ビームとを交互
に切り換えて出力することができる。この切り換えはパ
ワーのレベルを制御又はパルス制御することにより行
う。
Further, in carrying out the quenching treatment, the electron beam as the high-density energy beam shown in the first and third embodiments was used for the first heating and the second heating. The electron beam generator has a maximum output of 5 KW and a 1.0 KW electron beam as a first heating beam and a second heating beam.
A 3.0 KW electron beam as a heating beam can be alternately switched and output. This switching is performed by controlling the power level or pulse control.

【0054】そして,上記部品は,10rpmにて回転
させ,その半径127mmの位置に実施形態例1,3に
示すごとく,第1加熱用ビーム11と第2加熱用ビーム
12とを交互に照射した。即ち,電子ビームの照射は,
約8m/分の送り速度で行った。
Then, the above component was rotated at 10 rpm, and the first heating beam 11 and the second heating beam 12 were alternately irradiated to the position having a radius of 127 mm as shown in the first and third embodiments. . That is, the electron beam irradiation is
The feed rate was about 8 m / min.

【0055】また,第1加熱用ビーム11と第2加熱用
ビーム12との切り換えタイミングは,第1加熱用ビー
ム11の照射時間を0.5秒,第2加熱用ビーム12の
照射時間を1.5秒として,これを順次繰り返した。上
記第1加熱用ビーム11及び第2加熱用ビーム12は,
図11に示すごとく,ともにその偏向軌跡はX方向5m
m,Y方向10mmである。そして,部品の回転によっ
て,電子ビームの軌跡は矢印H方向に移動する。
The switching timing between the first heating beam 11 and the second heating beam 12 is such that the irradiation time of the first heating beam 11 is 0.5 seconds and the irradiation time of the second heating beam 12 is 1 second. This was repeated sequentially for 0.5 second. The first heating beam 11 and the second heating beam 12 are
As shown in FIG. 11, the deflection locus is 5 m in the X direction.
It is 10 mm in the m and Y directions. The trajectory of the electron beam moves in the direction of arrow H as the component rotates.

【0056】このように加熱された部分は,加熱直後に
鋼材2の自己放冷により十分に急冷され,焼入れられ
る。その結果,上記部品は,上記のスプリング受け部分
がリング状に焼入れられたマルテンサイトの焼入れ硬化
層を有し,一方,他の部分はフェライト・パーライト組
成のままの状態であった。さらに,上記焼入れ硬化層
は,上記第1加熱部と第2加熱部とに対応して交互に焼
入れ深さが変化していると共に,残留応力も引張残留応
力と圧縮残留応力が交互に分布していた。
Immediately after heating, the portion thus heated is sufficiently quenched by self-cooling of the steel material 2 and quenched. As a result, the above-mentioned component had a quench-hardened layer of martensite in which the above-mentioned spring receiving portion was quenched in a ring shape, while the other portions remained in the ferrite-pearlite composition. Further, in the quench-hardened layer, the quenching depth changes alternately corresponding to the first heating part and the second heating part, and the residual stress also has tensile residual stress and compressive residual stress alternately distributed. Was there.

【0057】実施形態例5 本例は,図12に示すごとく,実施形態例4における部
品に対して,上記非溶融焼入れ部分Aと溶融焼入れ部分
Bとを縦横に交互に設けて市松模様状に配置した。この
場合の高密度エネルギービームは,実施形態例3に示し
た電子ビーム発生装置により発生させ,上記偏向コイル
111,112によって,2つの電子ビーム101,1
02に分配した。
Embodiment 5 In this embodiment, as shown in FIG. 12, the non-melt-quenched portion A and the melt-quenched portion B are alternately provided in the vertical and horizontal directions with respect to the component of the fourth embodiment to form a checkerboard pattern. I placed it. The high-density energy beam in this case is generated by the electron beam generator shown in the third embodiment, and two electron beams 101, 1 are generated by the deflection coils 111, 112.
Distributed in 02.

【0058】分配された電子ビーム101,102は,
それぞれ,一定間隔毎に低出力の第1加熱用ビームと高
出力の第2加熱用ビームとに切り替わるようにしてあ
る。即ち,一方の電子ビーム101が第1加熱用ビーム
として低出力状態にある場合には,他方の電子ビーム1
02はその間高出力の第2加熱用ビームとして高出力状
態になっている。次いで,一方の電子ビーム101が第
2加熱用ビームとしての高出力に切り替わったとき,他
方の電子ビーム102は第1加熱用ビームとしての低出
力に切り替わる。
The distributed electron beams 101 and 102 are
Each of them is switched to a low-power first heating beam and a high-power second heating beam at regular intervals. That is, when one electron beam 101 is in a low output state as the first heating beam, the other electron beam 1
In the meantime, 02 is in a high output state as a high output second heating beam. Next, when one electron beam 101 is switched to a high output as the second heating beam, the other electron beam 102 is switched to a low output as the first heating beam.

【0059】本例においては,上記第1加熱用ビームの
出力は1.0KW,第2加熱用ビームの出力は3.0K
Wとし,それぞれ1秒ごとに切り換えた。この場合,図
12に示すごとく,部品には,その1回転によって,2
列の焼入れ部分が一度に形成される。そして,その隣の
外周側にもう1回転焼入れ部分を形成する。その結果,
図12に示すごとく,横方向4列のリング状調質部が形
成され非溶融焼入れ部分Aと溶融焼入れ部分Bとが縦横
に交互に分布して市松模様状に配置された。
In this example, the output of the first heating beam is 1.0 KW, and the output of the second heating beam is 3.0 KW.
It was set to W and was switched every 1 second. In this case, as shown in FIG. 12, the component has two
Quenched portions of the row are formed at one time. Then, another rotation-quenched portion is formed on the outer peripheral side next to it. as a result,
As shown in FIG. 12, four rows of ring-shaped heat-refined portions were formed, and the non-melt-quenched portions A and the melt-quenched portions B were alternately distributed vertically and horizontally and arranged in a checkered pattern.

【0060】尚,本例においては,上記2つの電子ビー
ムをそれぞれ隣接して照射したが,これを離して行うこ
とにより,2箇所の調質所望部分を同時に焼入れ処理す
ることもできる。更に電子ビームは3つ以上であっても
良い。この場合には,トータルの処理時間を短縮するこ
とができる。
In this example, the above two electron beams were irradiated adjacent to each other, but by performing the irradiation apart from each other, it is possible to simultaneously perform quenching treatment on the two desired parts for refining. Further, the number of electron beams may be three or more. In this case, the total processing time can be shortened.

【0061】実施形態例6 本例は,実施形態例5における2つの電子ビーム10
1,102を照射する場合の,電子ビームの照射軌跡の
1例を図13に示す。本例では,電子ビームは,2つの
円偏向軌跡C1 ,C2 に従って照射される。この場合,
各円偏向軌跡C1 ,C2 によってそれぞれ被熱処理領域
25,26に電子ビームが照射され,その間中,被熱処
理部材はその中心軸回りに回転させられる。従って,被
熱処理領域25.26における電子ビームの軌跡は矢印
H方向に移動する。
Sixth Embodiment The present example is the same as the two electron beams 10 in the fifth embodiment.
FIG. 13 shows an example of the irradiation trajectory of the electron beam when irradiating 1, 102. In this example, the electron beam is irradiated according to the two circular deflection trajectories C 1 and C 2 . in this case,
The circular deflection loci C 1 and C 2 irradiate the heat-treated regions 25 and 26 with electron beams, respectively, and the member to be heat-treated is rotated about its central axis during the period. Therefore, the trajectory of the electron beam in the heat-treated region 25.26 moves in the direction of arrow H.

【0062】なお,各円偏向軌跡C1 ,C2 は,x軸方
向及びy軸方向において正弦波の偏向波形を発生させ,
その偏向の組合せによって形成される。また,各円偏向
軌跡C1 ,C2 を切り換え,隣接する被熱処理領域2
5,26において交互に電子ビームを照射するために,
図14のような偏向波形w1 が発生させられ,該偏向波
形w1 と前記y軸方向における偏向波形とが重ねられ
る。
The circular deflection loci C 1 and C 2 generate sinusoidal deflection waveforms in the x-axis direction and the y-axis direction,
It is formed by the combination of the deflections. In addition, the circular deflection loci C 1 and C 2 are switched so that the adjacent heat-treated region 2
In order to irradiate the electron beams alternately at 5 and 26,
Deflection waveform w 1 is caused to occur as in FIG. 14, a deflection waveform deflection waveform w 1 and in the y-axis direction are overlapped.

【0063】従って,電圧VE が正の値を採る時間t1
の間に被熱処理領域25に電子ビームが照射され,電圧
VE が負の値を採る時間t2 の間に被熱処理領域26に
電子ビームが照射される。また,前記偏向波形w1 の時
間t1 ,t2 の長さを調整することにより,各被熱処理
領域25,26への照射エネルギーを調整することがで
きる。
Therefore, the time t 1 at which the voltage V E takes a positive value
Is irradiated electron beam to be heat-treated region 25 between, the voltage V E electron beam is irradiated to the heat treatment area 26 during the time t 2 to a negative value. Further, by adjusting the lengths of the deflection waveform w 1 for the times t 1 and t 2 , it is possible to adjust the irradiation energy to the heat-treated regions 25 and 26.

【0064】実施形態例7 本例は,図15に示すごとく,被熱処理領域27,28
へ電子ビームを照射する場合の別例を示している。この
場合には,二つの面偏向軌跡C3 ,C4 によって電子ビ
ームが照射される。つまり,各面偏向軌跡C3 ,C4 に
よってそれぞれ被熱処理領域27,28に電子ビームが
照射され,その間中,被処理部材はその中心軸回りに回
転させられる。従って,この場合も被熱処理領域27,
28における電子ビームの軌跡は矢印H方向に移動す
る。
Embodiment 7 In this embodiment, as shown in FIG.
9 shows another example in which an electron beam is irradiated to the light source. In this case, the electron beam is irradiated by two surface deflection trajectories C 3 and C 4 . That is, the electron beam is applied to the regions to be heat-treated 27 and 28 by the respective surface deflection trajectories C 3 and C 4 , during which the member to be processed is rotated around its central axis. Therefore, also in this case, the heat treatment region 27,
The trajectory of the electron beam at 28 moves in the direction of arrow H.

【0065】なお,各面偏向軌跡C3 ,C4 はx軸方向
及びy軸方向において三角波の偏向電圧を発生させるこ
とによって形成される。また,各面偏向軌跡C3 ,C4
を切り換え,被熱処理領域27,28において電子ビー
ムを照射するために,図16に示すような偏向波形w1
と前記x軸方向及びy軸方向における三角波とが重ねら
れる。勿論,円偏向と面偏向とを組み合わせたり,線,
楕円等の軌跡をたどるように電子ビームを偏向させるこ
ともできる。その他は,実施形態例6と同様である。
The surface deflection loci C 3 and C 4 are formed by generating a triangular wave deflection voltage in the x-axis direction and the y-axis direction. Also, each surface deflection locus C 3 , C 4
In order to irradiate the electron beam in the regions to be heat-treated 27 and 28, a deflection waveform w 1 as shown in FIG.
And the triangular waves in the x-axis direction and the y-axis direction are superimposed. Of course, combining circular and surface deflection,
The electron beam can be deflected so as to follow a locus such as an ellipse. Others are the same as those in the sixth embodiment.

【0066】ところで,上記実施形態例ではトルクコン
バータのロックアップクラッチピストンを処理する例を
説明したが,その外,例えば多板摩擦係合装置における
プレート摺動部,部材同士又はスナップリング等による
結合部,オイルポンププレート,シールリング等,表層
部を全部又は部分的に硬化させる必要がある鋼部材であ
れば,いずれのものであっても本発明を適用することが
できる。
By the way, in the above embodiment, an example of processing the lock-up clutch piston of the torque converter has been described, but in addition to this, for example, plate sliding parts in the multi-plate friction engagement device, members or snap rings or the like are coupled. The present invention can be applied to any steel member, such as parts, oil pump plates, seal rings, etc., for which the surface layer part needs to be wholly or partially hardened.

【0067】[0067]

【発明の効果】本発明によれば,焼入れによる硬度向上
効果を維持し,かつ,残留応力を制御することができ
る,鋼材の焼入れ方法を提供することができる。
According to the present invention, it is possible to provide a quenching method for a steel material, which can maintain the hardness improving effect by quenching and control the residual stress.

【図面の簡単な説明】[Brief description of drawings]

【図1】実施形態例1における,(a)焼入れパター
ン,(b)残留応力パターンを示す説明図。
FIG. 1 is an explanatory view showing (a) a quenching pattern and (b) a residual stress pattern in a first embodiment.

【図2】実施形態例1における,高密度エネルギービー
ムの照射状態を示す,(a)側面図,(b)平面図。
FIG. 2A is a side view and FIG. 2B is a plan view showing an irradiation state of a high-density energy beam in the first embodiment.

【図3】鉄−炭素系平衡状態図,及び第1加熱,第2加
熱温度を示す説明図。
FIG. 3 is an iron-carbon system equilibrium diagram and an explanatory diagram showing first heating temperature and second heating temperature.

【図4】実施形態例1における,(a)非溶融焼入れ部
分,(b)溶融焼入れ部分,(c)全体,の残留応力状
態を示す説明図。
FIG. 4 is an explanatory view showing residual stress states of (a) non-melt-quenched portion, (b) melt-quenched portion, and (c) whole in the first embodiment.

【図5】実施形態例1における,(a)非溶融焼入れ部
分,(b)溶融焼入れ部分,(c)全体,の焼入れ硬化
層の形成状態を示す説明図。
5A and 5B are explanatory views showing a formation state of a quench-hardened layer of (a) non-melt-quenched portion, (b) melt-quenched portion, and (c) whole in the first embodiment.

【図6】実施形態例2における,焼入れパターンを示す
説明図。
FIG. 6 is an explanatory view showing a quenching pattern according to the second embodiment.

【図7】実施形態例3における,熱処理装置の説明図。FIG. 7 is an explanatory diagram of a heat treatment apparatus according to a third embodiment.

【図8】実施形態例3における,高密度エネルギービー
ムの照射状態を示す説明図。
FIG. 8 is an explanatory diagram showing an irradiation state of a high-density energy beam according to the third embodiment.

【図9】実施形態例3における,(a)非溶融焼入れ部
分,(b)溶融焼入れ部分,のヒートパターンを示す説
明図。
FIG. 9 is an explanatory diagram showing heat patterns of (a) non-melt-quenched portion and (b) melt-quenched portion in Embodiment 3;

【図10】実施形態例4における,ロックアップクラッ
チピストンの説明図。
FIG. 10 is an explanatory diagram of a lockup clutch piston according to the fourth embodiment.

【図11】実施形態例4における,電子ビームの照射部
の軌跡の一例を示す説明図。
FIG. 11 is an explanatory diagram showing an example of a trajectory of an electron beam irradiation unit in the fourth embodiment.

【図12】実施形態例5における,高密度エネルギービ
ームの照射状態を示す説明図。
FIG. 12 is an explanatory diagram showing an irradiation state of a high-density energy beam according to the fifth embodiment.

【図13】実施形態例6における,電子ビームの照射部
の軌跡の一例を示す説明図。
FIG. 13 is an explanatory diagram showing an example of a trajectory of an electron beam irradiation unit in the sixth embodiment.

【図14】実施形態例6における,電子ビーム照射の偏
向波形例を示す説明図。
FIG. 14 is an explanatory diagram showing an example of a deflection waveform of electron beam irradiation in the sixth embodiment.

【図15】実施形態例7における,電子ビームの照射部
の軌跡の他の例を示す説明図。
FIG. 15 is an explanatory diagram showing another example of the trajectory of the electron beam irradiation unit in the seventh embodiment.

【図16】実施形態例7における,電子ビーム照射の偏
向波形例を示す説明図。
FIG. 16 is an explanatory diagram showing an example of a deflection waveform of electron beam irradiation in the seventh embodiment.

【符号の説明】[Explanation of symbols]

1...高密度エネルギービームの発生源, 10...高密度エネルギービーム, 11...第1加熱用ビーム, 12...第2加熱用ビーム, 2...鋼材, 20...調質所望部分, 29...焼入れ硬化層, A...非溶融焼入れ部分(第1加熱部分), B...溶融焼入れ部分(第2加熱部分), 1. . . Source of high-density energy beam, 10. . . High-density energy beam, 11. . . First heating beam, 12. . . Second heating beam, 2. . . Steel, 20. . . Desired portion for tempering, 29. . . Quench hardened layer, A. . . Non-melt-quenched portion (first heating portion), B. . . Melting and quenching part (second heating part),

フロントページの続き (72)発明者 大林 巧治 愛知県安城市藤井町高根10番地 アイシ ン・エィ ダブリュ株式会社内 (72)発明者 鈴木 隆敏 愛知県愛知郡長久手町大字長湫字横道41番 地の1 株式会社豊田中央研究所内Front page continuation (72) Takuji Obayashi, Takuji Obayashi, 10 Takane, Fujii-cho, Anjo City, Aichi Prefecture, Aisin AW Co., Ltd. (72) Inventor, Takatoshi Suzuki, Aichi-gun, Nagachite-cho, Aichi-gun 1 Inside Toyota Central Research Institute

Claims (6)

【特許請求の範囲】[Claims] 【請求項1】 鋼材に対して,第1加熱と,これよりも
高い温度の第2加熱とをそれぞれ部分的に互いに隣接さ
せて実施し,その後急冷する鋼材の焼入れ方法であっ
て,上記第1加熱は,鋼材のオーステナイト変態点以上
で鋼材の溶融温度以下の温度で行い,一方上記第2加熱
は,鋼材の表層が溶融する溶融温度以上の温度で行うこ
とを特徴とする鋼材の焼入れ方法。
1. A quenching method for a steel material, which comprises first heating a steel material and second heating at a temperature higher than the first heating material partially adjacent to each other, and then rapidly cooling the steel material. 1. A quenching method for steel products, characterized in that 1 heating is carried out at a temperature not lower than the austenite transformation point of the steel product and not higher than the melting temperature of the steel product, while said second heating is carried out at a temperature not lower than the melting temperature at which the surface layer of the steel product melts. .
【請求項2】 請求項1において,上記第1加熱と上記
第2加熱とは,鋼材における調質所望部分のみに対して
行うことを特徴とする鋼材の焼入れ方法。
2. The method for quenching a steel material according to claim 1, wherein the first heating and the second heating are performed only on a desired portion of the steel material for heat treatment.
【請求項3】 請求項1又は2において,上記第1加熱
及び上記第2加熱は,鋼材に対して高密度エネルギービ
ームを照射することにより行うことを特徴とする鋼材の
焼入れ方法。
3. The method for quenching a steel material according to claim 1, wherein the first heating and the second heating are performed by irradiating the steel material with a high-density energy beam.
【請求項4】 請求項3において,上記高密度エネルギ
ービームの照射は,上記第1加熱を行う第1加熱用ビー
ムと,上記第2加熱を行う第2加熱用ビームとを用い
て,上記第1加熱用ビームによる第1加熱と,上記第2
加熱用ビームによる第2加熱とを同時に行うことを特徴
とする鋼材の焼入れ方法。
4. The irradiation of the high-density energy beam according to claim 3, wherein the first heating beam for performing the first heating and the second heating beam for performing the second heating are used. 1st heating with 1 heating beam, and 2nd above
A method of quenching a steel material, characterized in that the second heating with a heating beam is performed at the same time.
【請求項5】 請求項3又は4において,上記高密度エ
ネルギービームは,1箇所のビーム発生源から発射され
たビームを,複数箇所に分配して照射することを特徴と
する鋼材の焼入れ方法。
5. The method for quenching steel according to claim 3 or 4, wherein the high-density energy beam is a beam emitted from a beam generating source at one location and is distributed to a plurality of locations for irradiation.
【請求項6】 請求項1〜5のいずれか1項において,
上記急冷は,103 ℃/分以上の速度で行うことを特徴
とする鋼材の焼入れ方法。
6. The method according to any one of claims 1 to 5,
A quenching method for a steel material, wherein the rapid cooling is performed at a rate of 10 3 ° C / min or more.
JP10638796A 1996-04-02 1996-04-02 How to harden steel Expired - Fee Related JP3542228B2 (en)