JPH0936320A - Method of forming memory capacitor - Google Patents

Method of forming memory capacitor

Info

Publication number
JPH0936320A
JPH0936320A JP7183036A JP18303695A JPH0936320A JP H0936320 A JPH0936320 A JP H0936320A JP 7183036 A JP7183036 A JP 7183036A JP 18303695 A JP18303695 A JP 18303695A JP H0936320 A JPH0936320 A JP H0936320A
Authority
JP
Japan
Prior art keywords
sidewall
side wall
dummy pattern
forming
polysi
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP7183036A
Other languages
Japanese (ja)
Other versions
JP3432644B2 (en
JPH0936320A5 (en
Inventor
Masahiro Yamate
正浩 山手
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Oki Electric Industry Co Ltd
Original Assignee
Oki Electric Industry Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Oki Electric Industry Co Ltd filed Critical Oki Electric Industry Co Ltd
Priority to JP18303695A priority Critical patent/JP3432644B2/en
Publication of JPH0936320A publication Critical patent/JPH0936320A/en
Publication of JPH0936320A5 publication Critical patent/JPH0936320A5/ja
Application granted granted Critical
Publication of JP3432644B2 publication Critical patent/JP3432644B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

(57)【要約】 【目的】 円筒型メモリキャパシタの形成においてシリ
ンダ部分の脱落を防止する。 【構成】 MOSFET12を覆うSiO2絶縁膜20上に順次に、Si
N エッチングストッパ22及びpolySi下層電極材料を積層
し、然る後、下層電極材料上にSiO2ダミーパターン26を
形成する。次いでドライエッチングにより、ダミーパタ
ーン26を介して下層電極材料をエッチングして、オーバ
ーハング状の側壁28a を有する下層電極突起28を形成す
る。次いでダミーパターン26上にpolySiサイドウォール
形成材料を積層し、然る後、異方性エッチングによりサ
イドウォール形成材料をエッチングして、下層電極突起
28の側壁28a からダミーパターン26の側壁26a にわたる
領域に、サイドウォールを形成する。次いでダミーパタ
ーン26をエッチング除去する。この除去の際に、サイド
ウォールが下層電極突起28から剥離することがあって
も、サイドウォールはオーバーハング状の側壁28a に引
っ掛かるので、サイドウォールの脱落を防止できる。
(57) [Abstract] [Purpose] To prevent the cylinder part from falling off when forming a cylindrical memory capacitor. [Structure] Si is sequentially formed on the SiO 2 insulating film 20 covering the MOSFET 12.
An N etching stopper 22 and a polySi lower layer electrode material are laminated, and then a SiO 2 dummy pattern 26 is formed on the lower layer electrode material. Next, the lower layer electrode material is etched through the dummy pattern 26 by dry etching to form the lower layer electrode protrusion 28 having the overhang-shaped side wall 28a. Next, a polySi sidewall forming material is laminated on the dummy pattern 26, and thereafter, the sidewall forming material is etched by anisotropic etching to form a lower electrode projection.
A sidewall is formed in a region extending from the sidewall 28a of 28 to the sidewall 26a of the dummy pattern 26. Then, the dummy pattern 26 is removed by etching. At the time of this removal, even if the side wall is separated from the lower layer electrode protrusion 28, the side wall is caught by the overhang-shaped side wall 28a, so that the side wall can be prevented from falling off.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】この発明は、メモリキャパシタの
形成方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method for forming a memory capacitor.

【0002】[0002]

【従来の技術】DRAMにおいて、メモリキャパシタの
容量を増大させるための構造として円筒型のスタックト
キャパシタが提案されている。
2. Description of the Related Art In a DRAM, a cylindrical stacked capacitor has been proposed as a structure for increasing the capacity of a memory capacitor.

【0003】円筒型のスタックトキャパシタを形成する
場合、従来は、基板にメモリトランジスタとして形成し
たMOSトランジスタを層間絶縁膜で覆い、この層間絶
縁膜上にpolySi第一層を積層する。そしてこの第
一層上にSiO2 ダミーパターンを形成し、然る後、ダ
ミーパターン上にpolySi第二層を積層する。次い
で異方性エッチングにより、第二層をエッチングしてダ
ミーパターン側壁にpolySiサイドウォールを形成
し、さらにこれらダミーパターン及びサイドウォールを
介し第一層をエッチングしてpolySi下層電極を形
成する。次いでダミーパターンを除去した後、サイドウ
ォール上にキャパシタ絶縁膜及び上層電極を形成し、こ
れら下層電極、キャパシタ絶縁膜及び上層電極から成る
スタックトキャパシタを得る。
When forming a cylindrical stacked capacitor, conventionally, a MOS transistor formed as a memory transistor on a substrate is covered with an interlayer insulating film, and a polySi first layer is laminated on the interlayer insulating film. Then, a SiO 2 dummy pattern is formed on this first layer, and thereafter, a polySi second layer is laminated on the dummy pattern. Next, the second layer is etched by anisotropic etching to form a polySi sidewall on the sidewall of the dummy pattern, and the first layer is further etched through the dummy pattern and the sidewall to form a polySi lower layer electrode. Then, after removing the dummy pattern, a capacitor insulating film and an upper layer electrode are formed on the sidewalls to obtain a stacked capacitor including the lower layer electrode, the capacitor insulating film and the upper layer electrode.

【0004】[0004]

【発明が解決しようとする課題】しかしながら上述した
従来方法では、polySi下層電極を形成した後の工
程において、例えば洗浄、熱処理或は基板搬送といった
工程において、polySi下層電極の表面にSiO2
自然酸化膜を生じる。この自然酸化膜の発生を防止する
ことは困難であり、また下層電極表面の全面にわたって
完全に自然酸化膜を除去した状態で、サイドウォールを
形成することも困難である。
However, in the conventional method described above, SiO 2 is formed on the surface of the polySi lower layer electrode in a step after the polySi lower layer electrode is formed, for example, in a step such as cleaning, heat treatment or substrate transfer.
A natural oxide film is formed. It is difficult to prevent the formation of the natural oxide film, and it is also difficult to form the sidewall while the natural oxide film is completely removed over the entire surface of the lower electrode.

【0005】従って下層電極とサイドウォールとの間に
は不可避的に自然酸化膜が介在するので、SiO2 ダミ
ーパターンのエッチング除去時にSiO2 自然酸化膜が
エッチングされて、サイドウォールが下層電極から剥離
し易い。
Therefore, since the natural oxide film is inevitably interposed between the lower layer electrode and the side wall, the SiO 2 natural oxide film is etched when the SiO 2 dummy pattern is removed by etching, and the side wall is separated from the lower layer electrode. Easy to do.

【0006】しかも従来にあっては、ダミーパターン及
びサイドウォールを介し、異方性エッチングにより、p
olySi第一層をエッチングして、polySi下層
電極を形成するので、サイドウォールは、下層電極とは
下層電極の上面において密着することとなる。従ってサ
イドウォールは、下層電極から剥離すると、下層電極に
引っ掛からずにそのまま脱落してしまう。
Moreover, in the prior art, p is formed by anisotropic etching through the dummy pattern and the sidewall.
Since the polySi first layer is etched to form the polySi lower layer electrode, the sidewall is in close contact with the lower layer electrode on the upper surface of the lower layer electrode. Therefore, when the side wall is peeled off from the lower layer electrode, it is not caught by the lower layer electrode and is dropped off as it is.

【0007】サイドウォールの脱落した箇所では、キャ
パシタメモリの容量を増大させることができず、従って
歩留りの低下を招く。
At the location where the side wall is removed, the capacity of the capacitor memory cannot be increased, and therefore the yield is reduced.

【0008】この発明の目的は上述した従来の問題点を
解決するため、自然酸化膜が存在してもサイドウォール
の脱落が生じにくいメモリキャパシタの形成方法を提供
することにある。
An object of the present invention is to provide a method of forming a memory capacitor in which the sidewalls are unlikely to fall off even if a natural oxide film is present in order to solve the above-mentioned conventional problems.

【0009】[0009]

【課題を解決するための手段及び作用】この目的を達成
するため、請求項1記載の発明のメモリキャパシタの形
成方法は、基板に形成したメモリトランジスタ上に層間
絶縁膜を介して設けた下層電極と、下層電極上に順次に
設けたキャパシタ絶縁膜及び上層電極とを備えて成るメ
モリキャパシタを形成するに当り、層間絶縁膜上に下層
導電性膜を形成する工程と、下層導電性膜上にダミーパ
ターンを形成する工程と、ダミーパターンを介し下層導
電性膜をエッチングして、基板に覆い被さるようなオー
バーハング状の側壁を有する下層電極突起を形成する工
程と、下層電極突起の側壁からダミーパターンの側壁に
わたってサイドウォールを形成する工程と、ダミーパタ
ーンを除去した後、サイドウォール上にキャパシタ絶縁
膜及び上層電極を形成する工程とを含んで成ることを特
徴とする。
In order to achieve this object, in the method of forming a memory capacitor according to the present invention, a lower layer electrode provided on a memory transistor formed on a substrate via an interlayer insulating film. And a step of forming a lower conductive film on the interlayer insulating film in forming a memory capacitor including a capacitor insulating film and an upper electrode sequentially provided on the lower conductive film, and a step of forming a lower conductive film on the lower conductive film. A step of forming a dummy pattern, a step of etching the lower conductive film through the dummy pattern to form a lower layer electrode protrusion having an overhang-like side wall covering the substrate, and a dummy from the side wall of the lower layer electrode protrusion. A step of forming a sidewall over the side wall of the pattern, and after removing the dummy pattern, a capacitor insulating film and an upper layer electrode are formed on the sidewall. Characterized in that it comprises the step of forming.

【0010】このような形成方法によれば、下層電極突
起の側壁は基板に覆い被さるようにオーバーハング状に
傾斜しており、このオーバーハング状の側壁にサイドウ
ォールを形成する。従って何らかの要因によって、例え
ばサイドウォールと下層電極突起との間に介在する自然
酸化膜がエッチング除去されるといった要因によって、
サイドウォールが下層電極突起から剥離するようなこと
があっても、サイドウォールはオーバーハング状の側壁
に引っ掛かるので、サイドウォールが下層電極突起から
抜け落ちるのを防止できる。
According to such a forming method, the side wall of the lower layer electrode projection is inclined in an overhang shape so as to cover the substrate, and the side wall is formed on this overhang shape side wall. Therefore, due to some factor, for example, the natural oxide film existing between the sidewall and the lower electrode protrusion is removed by etching,
Even if the side wall is peeled off from the lower layer electrode protrusion, the side wall is caught on the overhang-shaped side wall, so that the side wall can be prevented from coming off from the lower layer electrode protrusion.

【0011】また請求項2記載のメモリキャパシタの形
成方法は、基板に形成したメモリトランジスタ上に層間
絶縁膜を介して設けた下層電極と、下層電極上に順次に
設けたキャパシタ絶縁膜及び上層電極とを備えて成るメ
モリキャパシタを形成するに当り、層間絶縁膜上にpo
lySi下層導電性膜を形成する工程と、polySi
下層導電性膜上にダミーパターンを形成する工程と、ダ
ミーパターン上にアモルファスSiサイドウォール形成
材料を形成する工程と、サイドウォール形成材料をダミ
ーパターンを介しエッチングしてpolySi下層電極
突起の側壁からダミーパターンの側壁にわたってサイド
ウォールを形成する工程と、アモルファスSiサイドウ
ォール形成材料を結晶化した後、ダミーパターンを除去
する工程とを含んで成ることを特徴とする。
According to a second aspect of the present invention, there is provided a method of forming a memory capacitor, in which a lower layer electrode provided on a memory transistor formed on a substrate via an interlayer insulating film, and a capacitor insulating film and an upper layer electrode sequentially provided on the lower electrode. In forming a memory capacitor comprising:
forming a polySi lower conductive film;
Forming a dummy pattern on the lower conductive film; forming an amorphous Si sidewall forming material on the dummy pattern; etching the sidewall forming material through the dummy pattern to form a dummy from the sidewall of the polySi lower electrode protrusion. The method is characterized by including a step of forming a sidewall over the side wall of the pattern, and a step of removing the dummy pattern after crystallizing the amorphous Si sidewall forming material.

【0012】アモルファスSiサイドウォール形成材料
の結晶化を行なった後にサイドウォールを形成しても良
いし、或は、サイドウォールを形成した後にアモルファ
スSiサイドウォール形成材料の結晶化を行なっても良
い。
The side wall may be formed after crystallization of the amorphous Si side wall forming material, or the amorphous Si side wall forming material may be crystallized after forming the side wall.

【0013】このような形成方法によれば、ダミーパタ
ーン上にアモルファスSiサイドウォール形成材料を積
層する。次に、アモルファスSiサイドウォール形成材
料を結晶化(再結晶化或は多結晶化)して、polyS
iサイドウォール形成材料を形成する。次に、poly
Siサイドウォール形成材料をダミーパターンを介しエ
ッチングして、polySiサイドウォールを形成す
る。次に、ダミーパターンを除去する。
According to such a forming method, the amorphous Si sidewall forming material is laminated on the dummy pattern. Next, the amorphous Si sidewall forming material is crystallized (recrystallized or polycrystallized) to obtain polyS.
An i-sidewall forming material is formed. Next, poly
The Si sidewall forming material is etched through the dummy pattern to form the polySi sidewall. Next, the dummy pattern is removed.

【0014】或は、ダミーパタン上にアモルファスSi
サイドウォール形成材料を積層する。次に、アモルファ
スSiサイドウォール形成材料をダミーパターンを介し
エッチングして、アモルファスSiサイドウォールを形
成する。このサイドウォールは下層電極突起の側壁から
ダミーパターンの側壁にかけて残存させたアモルファス
Siサイドウォール形成材料である。次に、アモルファ
スSiサイドウォールを結晶化(再結晶化或は多結晶
化)して、polySiサイドウォールを形成する。次
に、ダミーパターンを除去する。
Alternatively, amorphous Si is formed on the dummy pattern.
A sidewall forming material is laminated. Next, the amorphous Si sidewall forming material is etched through the dummy pattern to form amorphous Si sidewalls. This side wall is an amorphous Si side wall forming material left over from the side wall of the lower electrode projection to the side wall of the dummy pattern. Next, the amorphous Si sidewall is crystallized (recrystallized or polycrystallized) to form a polySi sidewall. Next, the dummy pattern is removed.

【0015】このようにアモルファスSiのサイドウォ
ール形成材料或はサイドウォールを結晶化して、pol
ySiのサイドウォール形成材料或はサイドウォールを
形成した場合、この結晶化は、下層電極突起の側壁表層
のpolySiを種結晶として進行し、従ってこの結晶
化によってpolySi下層電極と一体になったpol
ySiのサイドウォール形成材料或はサイドウォールを
得ることができる。
In this way, the amorphous silicon sidewall forming material or the sidewall is crystallized, and pol
When a sidewall forming material or a sidewall of ySi is formed, this crystallization proceeds with polySi on the side wall surface layer of the lower electrode projection as a seed crystal, and therefore, this crystallization causes the pol integrated with the polySi lower electrode to be integrated.
A ySi sidewall forming material or a sidewall can be obtained.

【0016】polySi下層電極突起の側壁表層がS
iO2 自然酸化膜で覆われていたとしても、アモルファ
スSiのサイドウォール形成材料或はサイドウォールを
結晶化する際に、SiO2 自然酸化膜が結晶化されpo
lySi膜になると考えられる。従ってその側壁表層の
SiO2 自然酸化膜を必ずしも完全にエッチング除去せ
ずとも、下層電極突起と一体になったpolySiのサ
イドウォール形成材料或はサイドウォールを得ることが
できる。
The sidewall surface layer of the polySi lower electrode projection is S
Even if it is covered with the iO 2 natural oxide film, when the amorphous Si sidewall forming material or the sidewall is crystallized, the SiO 2 natural oxide film is crystallized and po.
It is considered to be a lySi film. Therefore, even if the SiO 2 natural oxide film on the side wall surface layer is not necessarily completely removed by etching, it is possible to obtain the sidewall forming material or sidewall of polySi integrated with the lower layer electrode protrusion.

【0017】またSiO2 自然酸化膜の結晶化(再結晶
化或は多結晶化)が生じなかったとしても、下層電極突
起の側壁表層の少なくとも一部を露出するように、Si
O2自然酸化膜を除去してあれば、露出する側壁表層に
おいてpolySi下層電極突起と一体になったpol
ySiのサイドウォール形成材料或はサイドウォールを
得ることができる。下層電極突起の側壁表層の自然酸化
膜の全てを完全に除去した状態で、アモルファスSiサ
イドウォール形成材料を積層することは困難であるが、
polySi下層電極突起の側壁表層の少なくとも一部
を露出するように、SiO2 自然酸化膜を除去した状態
で、アモルファスSiサイドウォール形成材料を積層す
ることは容易である。
Even if the SiO 2 natural oxide film does not crystallize (recrystallize or polycrystallize), at least a part of the side wall surface layer of the lower electrode protrusion is exposed so that Si is exposed.
If the O 2 natural oxide film is removed, the poly that is integrated with the polySi lower electrode protrusion on the exposed side wall surface layer.
A ySi sidewall forming material or a sidewall can be obtained. It is difficult to stack the amorphous Si sidewall forming material in a state where all of the native oxide film on the side wall surface layer of the lower layer electrode protrusion is completely removed.
It is easy to stack the amorphous Si sidewall forming material in a state where the SiO 2 natural oxide film is removed so that at least a part of the sidewall surface layer of the polySi lower electrode projection is exposed.

【0018】このように下層電極と一体になったサイド
ウォール形成材料或はサイドウォールを形成し、その
後、ダミーパターンを除去することにより、サイドウォ
ールの剥離や脱落を減少させることができる。
By forming the sidewall forming material or the sidewall integrated with the lower electrode in this way and then removing the dummy pattern, peeling or dropping of the sidewall can be reduced.

【0019】[0019]

【実施例】図1〜図6は請求項1記載の発明の第一実施
例の説明に供する工程図である。発明の理解を助けるた
め、以下の説明では、メモリトランジスタの形成工程の
説明と共に、この実施例のメモリキャパシタの形成工程
について説明する。
DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS FIG. 1 to FIG. 6 are process drawings for explaining the first embodiment of the invention described in claim 1. In order to facilitate understanding of the invention, the following description will be given of the process of forming the memory transistor, and the process of forming the memory capacitor of this embodiment.

【0020】(基板にメモリトランジスタを形成する工
程)この実施例では、メモリトランジスタ12としてM
OSFETを形成するものであって、p−Si基板10
の(100)主面10aに、選択酸化法(LOCOS法
とも称す)によりSiO2 フィールド酸化膜14を形成
する(図1(A))。SiO2 フィールド酸化膜14
は、素子分離領域の主面10a表層を覆うと共に、素子
形成予定領域の主面10a表層を露出する窓14aを有
する。素子形成予定領域は、メモリトランジスタ12を
形成する予定の領域である。
(Process of Forming Memory Transistor on Substrate) In this embodiment, M is used as the memory transistor 12.
A p-Si substrate 10 for forming an OSFET
A SiO 2 field oxide film 14 is formed on the (100) main surface 10a of FIG. 1 by a selective oxidation method (also referred to as LOCOS method) (FIG. 1 (A)). SiO 2 field oxide film 14
Has a window 14a which covers the surface of the main surface 10a of the element isolation region and exposes the surface of the main surface 10a of the element formation planned region. The element formation planned area is an area where the memory transistor 12 is to be formed.

【0021】次いで素子形成予定領域の主面10aに、
熱酸化法によりゲート絶縁膜形成用の絶縁膜16として
SiO2 膜を形成し、然る後、この絶縁膜16上に、C
VD法によりゲート電極形成用の導電性膜18としてド
ープトpolySi膜を積層する(図1(B))。この
ドープトpolySi膜が含有する不純物は、当該導電
性膜に電極としての導電性を付与するための不純物であ
る。
Then, on the main surface 10a of the device formation region,
A SiO 2 film is formed as the insulating film 16 for forming the gate insulating film by the thermal oxidation method, and then C is formed on the insulating film 16.
A doped polySi film is laminated as the conductive film 18 for forming the gate electrode by the VD method (FIG. 1B). The impurity contained in the doped polySi film is an impurity for imparting conductivity as an electrode to the conductive film.

【0022】次いでフォトリソ及びエッチング技術によ
り、ゲート電極形成用のドープトpolySi導電性膜
18をエッチングして、素子形成予定領域にドープトp
olySiゲート電極121を形成する。ゲート電極1
21下側の主面10aの表層部分が、メモリトランジス
タ12のチャネル領域122として機能する。然る後、
ドープトpolySiゲート電極121をマスクとして
異方性エッチングにより、ゲート絶縁膜形成用のSiO
2 絶縁膜16をエッチングする。このエッチングによ
り、ドープトpolySiゲート電極121側部に隣接
するソース予定領域及びドレイン予定領域の主面10a
を露出させて、ドープトpolySiゲート電極121
直下にSiO2 ゲート絶縁膜123を形成する(図2
(A))。ゲート絶縁膜123は、ゲート電極121直
下に残存させたSiO2 絶縁膜16から成る。
Then, the doped polySi conductive film 18 for forming the gate electrode is etched by photolithography and etching techniques to dope p in the region where the device is to be formed.
The oliSi gate electrode 121 is formed. Gate electrode 1
The surface layer portion of the main surface 10a on the lower side of 21 functions as the channel region 122 of the memory transistor 12. After that,
Anisotropy etching is performed using the doped polySi gate electrode 121 as a mask to form SiO for forming a gate insulating film.
2 The insulating film 16 is etched. By this etching, the main surface 10a of the planned source region and the planned drain region adjacent to the side of the doped polySi gate electrode 121 is formed.
Exposing the doped polySi gate electrode 121
The SiO 2 gate insulating film 123 is formed immediately below (see FIG. 2).
(A)). The gate insulating film 123 is made of the SiO 2 insulating film 16 left under the gate electrode 121.

【0023】次いでゲート電極121を介しソース予定
領域及びドレイン予定領域に不純物を導入して、ゲート
電極121側部にソース領域124及びドレイン領域1
25を形成し、メモリトランジスタ12を得る(図2
(B))。ここでは、ソース予定領域及びドレイン予定
領域に不純物イオンを注入して、n+ −Siソース領域
124及びn+ −Siドレイン領域125を形成する。
Then, impurities are introduced into the planned source region and the planned drain region through the gate electrode 121, and the source region 124 and the drain region 1 are provided on the side of the gate electrode 121.
25 to obtain the memory transistor 12 (see FIG. 2).
(B)). Here, impurity ions are implanted into the planned source region and the planned drain region to form the n + -Si source region 124 and the n + -Si drain region 125.

【0024】メモリトランジスタ12は、チャネル領域
122と、チャネル領域122を挟みチャネル領域12
2に隣接させて設けたソース領域124及びドレイン領
域125と、チャネル領域122上に順次に設けたゲー
ト絶縁膜123及びゲート電極121とを備えて成る。
The memory transistor 12 has a channel region 122 and the channel region 12 with the channel region 122 sandwiched therebetween.
2 includes a source region 124 and a drain region 125 that are provided adjacent to each other, and a gate insulating film 123 and a gate electrode 121 that are sequentially provided on the channel region 122.

【0025】(メモリトランジスタを層間絶縁膜で覆う
工程)次にこの実施例では、メモリトランジスタ12上
に、CVD法によりSiO2 層間絶縁膜20を積層し
て、メモリトランジスタ12をSiO2 層間絶縁膜20
で覆う(図3(A))。
(Process of Covering Memory Transistor with Interlayer Insulating Film) Next, in this embodiment, the SiO 2 interlayer insulating film 20 is laminated on the memory transistor 12 by the CVD method to form the memory transistor 12 with the SiO 2 interlayer insulating film. 20
(Fig. 3 (A)).

【0026】(層間絶縁膜上に下層導電性膜を形成する
工程)次にこの実施例では、SiO2 層間絶縁膜20上
に、CVD法によりSiNエッチングストッパ22を積
層する。然る後、フォトリソ及びエッチング技術を用い
て、SiNエッチングストッパ22及びSiO2 層間絶
縁膜20にコンタクトホール22a及び20aを形成す
る(図3(B))。コンタクトホール22a及び20a
を、メモリトランジスタ12のソース領域124に対応
する領域に形成する。
(Step of Forming Lower Conductive Film on Interlayer Insulating Film) Next, in this embodiment, the SiN etching stopper 22 is laminated on the SiO 2 interlayer insulating film 20 by the CVD method. After that, contact holes 22a and 20a are formed in the SiN etching stopper 22 and the SiO 2 interlayer insulating film 20 by using photolithography and etching techniques (FIG. 3B). Contact holes 22a and 20a
Are formed in a region corresponding to the source region 124 of the memory transistor 12.

【0027】SiNエッチングストッパ22は、後工程
においてダミーパターンをウエットエッチングして除去
するときに、下層電極の下側のSiO2 層間絶縁膜20
がエッチングされるのを防止するためのものである。
The SiN etching stopper 22 is used for the SiO 2 interlayer insulating film 20 below the lower electrode when the dummy pattern is removed by wet etching in a later process.
To prevent the etching.

【0028】次いでSiNエッチングストッパ22上
に、ドープトpolySi下層導電性膜24を形成する
(図4(A))。ドープトpolySi下層導電性膜2
4は、コンタクトホール22a及び20aを介し、ソー
ス領域124と電気的に接続する。下層導電性膜24と
して形成するドープトpolySi膜は、当該導電性膜
24に電極としての導電性を付与するための不純物を含
有する。
Next, a doped polySi lower conductive film 24 is formed on the SiN etching stopper 22 (FIG. 4A). Doped polySi lower conductive film 2
4 is electrically connected to the source region 124 through the contact holes 22a and 20a. The doped polySi film formed as the lower conductive film 24 contains impurities for imparting conductivity to the conductive film 24 as an electrode.

【0029】ここではシランガスを用いた低圧CVD法
により膜厚2000Å程度のアンドープpolySi膜
を積層し、然る後、イオン打ち込みエネルギーを60K
eV及びイオン注入量を1.0×1016ions/cm
2 として、アンドープpolySi膜にPイオンを注入
して、ドープトpolySi膜を形成する。
Here, an undoped polySi film having a film thickness of about 2000 Å is laminated by a low pressure CVD method using silane gas, and thereafter, ion implantation energy is set to 60K.
eV and ion implantation dose of 1.0 × 10 16 ions / cm
2 , P ions are implanted into the undoped polySi film to form a doped polySi film.

【0030】(下層導電性膜上にダミーパターンを形成
する工程)次にこの実施例では、ドープトpolySi
下層導電性材料24上に、CVD法により、ダミーパタ
ーン形成用のパターン材料として膜厚5000Å程度の
SiO2 膜を積層する。然る後、フォトリソ及びエッチ
ング技術を用い、異方性エッチングにより、SiO2パ
ターン材料をエッチングして、ダミーパターン26を形
成する(図4(B))。異方性エッチングによりダミー
パターン26を形成するので、ダミーパターン26の側
壁は基板10の主面10aに対しほぼ垂直に切り立った
壁となる。
(Step of Forming Dummy Pattern on Lower Conductive Film) Next, in this embodiment, doped polySi is used.
A SiO 2 film having a film thickness of about 5000 Å is laminated on the lower conductive material 24 by a CVD method as a pattern material for forming a dummy pattern. Then, the SiO 2 pattern material is etched by anisotropic etching using photolithography and etching techniques to form a dummy pattern 26 (FIG. 4B). Since the dummy pattern 26 is formed by anisotropic etching, the side wall of the dummy pattern 26 becomes a wall which is substantially vertical to the main surface 10a of the substrate 10.

【0031】主面10aの法線方向から見たときのダミ
ーパターン26の形状は、円、四角形、多角形或はその
ほかの任意好適な形状とすることができるが、ここでは
円形状とする。
The shape of the dummy pattern 26 when viewed from the direction normal to the main surface 10a may be a circle, a quadrangle, a polygon, or any other suitable shape, but here, it is a circular shape.

【0032】(ダミーパターンを介し下層導電性膜をエ
ッチングして、基板に覆い被さるようなオーバーハング
状の側壁を有する下層電極突起を形成する工程)次にこ
の実施例では、ドライエッチングにより、SiO2 ダミ
ーパターング26を介し下層導電性膜24をエッチング
して、基板10の主面10aに覆い被さるようなオーバ
ーハング状の側壁28aを有するドープトpolySi
下層電極突起28を形成する(図5(A))。このよう
なオーバーハング状の側壁28aの形成は、ドライエッ
チングのエッチング条件例えばエッチングガスの組成を
調整することにより、達成できる。例えば、Cl2 及び
SF6 の混合ガスをエッチングガスとして用いることが
できる。
(Step of etching lower conductive film through dummy pattern to form lower electrode projection having overhang-shaped side wall covering substrate) Next, in this embodiment, SiO 2 is formed by dry etching. 2 The lower conductive film 24 is etched through the dummy pattern 26 to form a doped polySi having an overhanging side wall 28a which covers the main surface 10a of the substrate 10.
The lower electrode protrusion 28 is formed (FIG. 5A). The formation of such overhanging side walls 28a can be achieved by adjusting the etching conditions for dry etching, for example, the composition of the etching gas. For example, a mixed gas of Cl 2 and SF 6 can be used as an etching gas.

【0033】ここでは、ドープトpolySi下層電極
突起28は逆テーパ状(逆円錐台状)の柱状突起であ
り、従ってこの突起28の周回り全周にわたってオーバ
ーハング状の側壁28aを形成している。オーバーハン
グ状の側壁28aと主面10aの法線Hとが成す角度α
(図5(A))は、後述するサイドウォールが下層電極
突起28から剥離したときにサイドウォールを側壁28
に引っ掛けてサイドウォールの脱落を防止できる程度で
あればよい。
Here, the doped polySi lower layer electrode protrusion 28 is a columnar protrusion having an inverse taper shape (inverted truncated cone shape), and therefore, an overhanging side wall 28a is formed over the entire circumference of the protrusion 28. Angle α formed by the overhang-shaped side wall 28a and the normal line H of the main surface 10a
(FIG. 5A) shows that when a sidewall described later is separated from the lower electrode projection 28, the sidewall
As long as it can be hooked on the wall to prevent the sidewall from falling off.

【0034】またメモリトランジスタ12及びメモリキ
ャパシタの配設密度を高めるため、ドープトpolyS
i下層電極突起28を、主面10aの法線方向から見て
ソース領域124と重なり合う位置に形成する。下層電
極突起28は、コンタクトホール22a及び20a内に
残存する下層導電性膜24を介して、ソース領域124
と電気的に接続する。
In order to increase the arrangement density of the memory transistors 12 and the memory capacitors, the doped polyS is used.
The i lower-layer electrode protrusion 28 is formed at a position overlapping the source region 124 when viewed in the normal direction of the main surface 10a. The lower layer electrode protrusion 28 is formed on the source region 124 through the lower layer conductive film 24 remaining in the contact holes 22a and 20a.
To be electrically connected to.

【0035】尚、後述するサイドウォールが下層電極突
起28から剥離したときにサイドウォールを側壁28a
に引っ掛けてサイドウォールの脱落を防止できるのであ
れば、下層電極突起28の側壁28aの一部をオーバー
ハング状の側壁28aとし残りの側壁28aを主面10
aに対しほぼ垂直な壁としても良い。また場合によって
は、下層電極突起28を、主面10aの法線方向から見
てソース領域124と重なり合わない位置に形成しても
構わない。
When the side wall, which will be described later, is separated from the lower electrode projection 28, the side wall 28a is formed.
If it is possible to prevent the side wall from falling off by hooking it on the upper surface of the lower electrode projection 28, a part of the side wall 28a of the lower layer electrode protrusion 28 is formed as an overhang-shaped side wall 28a, and the remaining side wall 28a is used as the main surface 10.
The wall may be substantially vertical to a. In some cases, the lower-layer electrode protrusion 28 may be formed at a position where it does not overlap the source region 124 when viewed in the normal direction of the main surface 10a.

【0036】次いで通常行なわれる如く洗浄処理を行な
う。この洗浄処理により、下層電極突起28の自然酸化
膜(図示せず)が除去される。後述するサイドウォール
と下層電極突起28との間に自然酸化膜が介在し、この
自然酸化膜がエッチングされてサイドウォールが下層電
極突起28から剥離することがあったとしても、サイド
ウォールはオーバーハング状の側壁28aに引っ掛かる
のでサイドウォールが下層電極突起28から脱落するの
を防止できる。従って下層電極突起28の自然酸化膜を
下層電極突起28全面にわたって完全に除去できなくて
も良い。
Then, a cleaning process is performed as usual. By this cleaning process, the natural oxide film (not shown) of the lower electrode protrusion 28 is removed. Even if a natural oxide film is present between the sidewall and the lower electrode projection 28, which will be described later, and the natural oxide film is etched and the sidewall is separated from the lower electrode projection 28, the sidewall is overhanged. Since it is caught on the side wall 28 a, it is possible to prevent the side wall from falling off the lower electrode projection 28. Therefore, the natural oxide film of the lower layer electrode protrusion 28 may not be completely removed over the entire surface of the lower layer electrode protrusion 28.

【0037】(下層電極突起の側壁からダミーパターン
の側壁にわたってサイドウォールを形成する工程)次に
この実施例では、サイドウォール形成材料30として膜
厚1000Å程度のアンドープpolySi膜を、低圧
CVD法により、ダミーパターン26上に積層する(図
5(B))。
(Step of Forming Sidewalls from Sidewalls of Lower-Layer Electrode Protrusions to Sidewalls of Dummy Pattern) Next, in this embodiment, an undoped polySi film having a film thickness of about 1000Å is formed as the sidewall forming material 30 by a low pressure CVD method. It is stacked on the dummy pattern 26 (FIG. 5B).

【0038】次いで熱処理を行なって、ドープトpol
ySi下層電極突起28が含有する不純物を拡散及び活
性化させる。ここでは、p−Si基板10を、窒素雰囲
気中に保持して850℃で15分間加熱することによ
り、不純物を拡散及び活性化させる。
Then, heat treatment is performed to make the doped pol.
The impurities contained in the ySi lower layer electrode protrusions 28 are diffused and activated. Here, the p-Si substrate 10 is held in a nitrogen atmosphere and heated at 850 ° C. for 15 minutes to diffuse and activate the impurities.

【0039】次いで異方性エッチングにより、下層電極
突起28の側壁28a及びダミーパターン26の側壁2
6aのサイドウォール形成材料30は残存させるように
して、サイドウォール形成材料30をエッチング除去
し、これにより下層電極突起28の側壁28aからダミ
ーパターン26の側壁26aにわたってサイドウォール
32を形成する(図6(A))。サイドウォール32
は、側壁28a及び26aに残存させたサイドウォール
形成材料30から成る。
Next, by anisotropic etching, the side wall 28a of the lower layer electrode protrusion 28 and the side wall 2 of the dummy pattern 26 are formed.
The side wall forming material 30 of 6a is left as it is, and the side wall forming material 30 is removed by etching, thereby forming a side wall 32 from the side wall 28a of the lower layer electrode protrusion 28 to the side wall 26a of the dummy pattern 26 (FIG. 6). (A)). Sidewall 32
Is made of the side wall forming material 30 left on the side walls 28a and 26a.

【0040】尚、下層電極突起28の不純物を拡散及び
活性化させるための熱処理によって、下層電極突起28
の側壁近傍部分のサイドウォール形成材料30にも不純
物が拡散されるので、導電性を有するサイドウォール3
2を形成でき、サイドウォール32を下層電極として機
能させることができる。サイドウォール32への不純物
拡散量が下層電極として機能させるには不十分な場合
は、サイドウォール32に別途不純物を添加すれば良
い。
The heat treatment for diffusing and activating the impurities of the lower layer electrode protrusions 28 is performed.
Since the impurities are diffused also into the sidewall forming material 30 in the vicinity of the side wall of the
2 can be formed, and the sidewall 32 can function as a lower layer electrode. If the amount of impurities diffused into the sidewalls 32 is insufficient to function as the lower layer electrode, impurities may be added to the sidewalls 32 separately.

【0041】(ダミーパターンを除去した後、サイドウ
ォール上にキャパシタ絶縁膜及び上層電極を形成する工
程)次にこの実施例では、下層電極突起28及びサイド
ウォール32は実質的にエッチングしないように、選択
的に、ダミーパターン26をエッチング除去する(図6
(B))。
(Step of Forming Capacitor Insulating Film and Upper Layer Electrode on Sidewalls After Removing Dummy Pattern) Next, in this embodiment, the lower layer electrode protrusions 28 and the sidewalls 32 are substantially not etched. The dummy pattern 26 is selectively removed by etching (FIG. 6).
(B)).

【0042】ここでは、下層電極突起28はドープトp
olySi、サイドウォール32はドープト若しくはア
ンンドープpolySi、及び、ダミーパターン28は
SiO2 から成るので、任意好適な組成のエッチャント
例えば希フッ酸を用いてウエットエッチングを行なうこ
とにより、ダミーパターン28を選択的にエッチング除
去できる。
Here, the lower electrode projection 28 is made of doped p.
Since the polySi and the sidewalls 32 are made of doped or undoped polySi, and the dummy pattern 28 is made of SiO 2 , the dummy pattern 28 is selectively etched by performing wet etching using an etchant having any suitable composition such as dilute hydrofluoric acid. Can be removed by etching.

【0043】次いでサイドウォール32上に順次に、キ
ャパシタ絶縁膜形成用の絶縁膜34及び上層電極形成用
の導電性膜36を形成する(図7(A))。
Next, an insulating film 34 for forming a capacitor insulating film and a conductive film 36 for forming an upper electrode are sequentially formed on the sidewall 32 (FIG. 7A).

【0044】ここでは、基板面全面にわたる領域上に、
低圧CVD法により膜厚100Å程度のSiN絶縁膜3
4を積層する。次いで、このSiN絶縁膜34上に、低
圧CVD法により膜厚2000Å程度のアンドープpo
lySi膜を積層する。然る後、このアンドープpol
ySi膜に、気相拡散法により不純物を拡散させて、ド
ープトpolySi膜から成る導電性膜36を得る。ド
ープトpolySi導電性膜36は、当該膜36に電極
としての導電性を付与するための不純物を含有する。例
えば、POCl3 の蒸気中にp−Si基板10を保持し
て、気相拡散により、PをアンドープpolySi膜中
に拡散させて、ドープトpolySi導電性膜36を形
成すれば良い。
Here, on the region over the entire surface of the substrate,
SiN insulating film 3 with a film thickness of about 100Å by low pressure CVD method
4 is laminated. Then, on the SiN insulating film 34, an undoped po having a film thickness of about 2000Å is formed by a low pressure CVD method.
A lySi film is laminated. After that, this undoped pol
Impurities are diffused in the ySi film by a vapor phase diffusion method to obtain a conductive film 36 made of a doped polySi film. The doped polySi conductive film 36 contains impurities for giving the film 36 conductivity as an electrode. For example, the p-Si substrate 10 may be held in the vapor of POCl 3 , and P may be diffused into the undoped polySi film by vapor phase diffusion to form the doped polySi conductive film 36.

【0045】次いでホトリソ及びエッチング技術を用い
て、ドープトpolySi導電性膜36及びSiN絶縁
膜34を順次にエッチングして、ドープトpolySi
上層電極38及びSiNキャパシタ絶縁膜40を形成
し、メモリキャパシタ42を得る(図7(B))。
Then, the doped polySi conductive film 36 and the SiN insulating film 34 are sequentially etched by using a photolithography and etching technique to obtain the doped polySi.
The upper electrode 38 and the SiN capacitor insulating film 40 are formed, and the memory capacitor 42 is obtained (FIG. 7B).

【0046】メモリキャパシタ42は、基板10に形成
したメモリトランジスタ12上に層間絶縁膜20を介し
て設けた下層電極突起28と、この下層電極突起28上
に順次に設けたキャパシタ絶縁膜40及び上層電極38
とを備えて成る。
The memory capacitor 42 includes a lower layer electrode protrusion 28 provided on the memory transistor 12 formed on the substrate 10 with the interlayer insulating film 20 interposed therebetween, a capacitor insulating film 40 and an upper layer electrode sequentially provided on the lower layer electrode protrusion 28. Electrode 38
And.

【0047】この実施例によれば、下層電極突起28は
逆円錐台状の柱状突起であり、従って下層電極突起28
はその側壁まわり全周にわたってオーバーハング状の側
壁28aを有する。これがため、ダミーパターン26の
エッチング除去の際に、サイドウォール32と下層電極
突起28の側壁28aとの間に介在する自然酸化膜がエ
ッチングされて、サイドウォール32が側壁28aから
剥離することがあったとしても、サイドウォール32は
オーバーハング状の側壁28aに引っ掛かるのでサイド
ウォール32が側壁28aから抜け落ちるのを防止でき
る。これがためメモリキャパシタ42を歩留り良く形成
できる。
According to this embodiment, the lower electrode projection 28 is a columnar projection having an inverted truncated cone shape, and therefore the lower electrode projection 28 is formed.
Has an overhanging side wall 28a over the entire circumference thereof. Therefore, when the dummy pattern 26 is removed by etching, the natural oxide film interposed between the side wall 32 and the side wall 28a of the lower electrode protrusion 28 may be etched and the side wall 32 may be separated from the side wall 28a. Even if it does, since the side wall 32 is caught by the overhang-shaped side wall 28a, it is possible to prevent the side wall 32 from falling off from the side wall 28a. Therefore, the memory capacitor 42 can be formed with high yield.

【0048】図8〜図10は請求項1記載の発明の第二
実施例の説明に供する工程図である。以下に述べる第二
実施例の説明では、主として上述した請求項1記載の発
明の第一実施例と相違する点につき説明し、上述した請
求項1記載の発明の第一実施例と同様の点についてはそ
の詳細な説明を省略する。
8 to 10 are process drawings for explaining the second embodiment of the invention described in claim 1. In the description of the second embodiment described below, the points different from the first embodiment of the invention described in claim 1 will be mainly described, and the same points as the first embodiment of the invention described in claim 1 will be described. The detailed description thereof will be omitted.

【0049】層間絶縁膜20上に下層導電性膜24を形
成する工程までは、上述した請求項1記載の発明の第一
実施例と同様である。
The steps up to the step of forming the lower conductive film 24 on the interlayer insulating film 20 are the same as those in the first embodiment of the invention described in claim 1.

【0050】(下層導電性膜上にダミーパターンを形成
する工程)この実施例では、下層導電性材料24側から
順次に配置した第一層261及び第二層262から成る
2層構造のダミーパターン26を形成する(図8
(A))。
(Step of Forming Dummy Pattern on Lower Conductive Film) In this embodiment, a dummy pattern having a two-layer structure comprising a first layer 261 and a second layer 262 which are sequentially arranged from the lower conductive material 24 side. 26 (FIG. 8)
(A)).

【0051】ここではCVD法により、ドープトpol
ySi下層導電性膜24上に順次に、膜厚5000Å程
度のNSG(Nonedope Silicate G
lass)第一層形成材料及び膜厚500Å程度のSi
N第二層形成材料を積層し、然る後、フォトリソ及びエ
ッチング技術を用い、異方性エッチングによりSiN第
二層形成材料及びNSG第一層形成材料をエッチングし
て、SiN第二層262及びNSG第一層261から成
る2層構造のダミーパターン26を得る。
Here, the doped pol is used by the CVD method.
NSG (None ope Silicate G) having a film thickness of about 5000 Å is sequentially formed on the ySi lower conductive film 24.
first) material for forming the first layer and Si having a film thickness of about 500Å
The N second layer forming material is laminated, and thereafter, the SiN second layer forming material and the NSG first layer forming material are etched by anisotropic etching using photolithography and etching techniques, and the SiN second layer 262 and A dummy pattern 26 having a two-layer structure composed of the NSG first layer 261 is obtained.

【0052】異方性エッチングにより、SiN第二層2
62及びNSG第一層261を形成するので、これら各
層262及び261の側壁は基板10の主面10aに対
しほぼ垂直に切り立った壁となる。
By anisotropic etching, the SiN second layer 2 is formed.
Since 62 and the NSG first layer 261 are formed, the side walls of each of the layers 262 and 261 are vertical walls that are substantially perpendicular to the main surface 10a of the substrate 10.

【0053】(ダミーパターンを介し下層導電性膜をエ
ッチングして、基板に覆い被さるようなオーバーハング
状の側壁を有する下層電極突起を形成する工程)次にこ
の実施例では、2層構造のダミーパターング26を介し
て、ドライエッチングによりドープトpolySi下層
導電性膜24をエッチングして、p−Si基板10の主
面10aに覆い被さるようなオーバーハング状の側壁2
8aを有するドープトpolySi下層電極突起28を
形成する(図8(B))。
(Step of etching lower conductive film through dummy pattern to form lower electrode projection having overhang-shaped side wall covering substrate) Next, in this embodiment, a dummy having a two-layer structure is formed. The doped polySi lower conductive film 24 is dry-etched through the pattern 26 to form an overhang-shaped side wall 2 that covers the main surface 10a of the p-Si substrate 10.
A doped polySi lower layer electrode protrusion 28 having 8a is formed (FIG. 8B).

【0054】次にこの実施例では、ダミーパターン26
のSiN第二層262をマスクに用いて、NSG第一層
261をアンダーカットして、ダミーパターン26の側
壁26aに凹部26bを形成する(図9(A))。ここ
では、ふっ酸をエッチャントに用いたウエットエッチン
グにより、NSG第一層261をアンダーカットする。
Next, in this embodiment, the dummy pattern 26
Using the SiN second layer 262 as a mask, the NSG first layer 261 is undercut to form a recess 26b in the side wall 26a of the dummy pattern 26 (FIG. 9A). Here, the NSG first layer 261 is undercut by wet etching using hydrofluoric acid as an etchant.

【0055】(下層電極突起の側壁からダミーパターン
の側壁にわたってサイドウォールを形成する工程)次に
この実施例では、アンドープpolySiサイドウォー
ル形成材料30を、2層構造のダミーパターン26上に
積層する(図9(B))。
(Step of Forming Sidewall from Sidewall of Lower Layer Electrode Protrusion to Sidewall of Dummy Pattern) Next, in this embodiment, an undoped polySi sidewall forming material 30 is laminated on the dummy pattern 26 having a two-layer structure ( FIG. 9B).

【0056】次いで熱処理を行なって、ドープトpol
ySi下層電極突起28が含有する不純物を拡散及び活
性化させる。
Next, heat treatment is performed to make the doped pol.
The impurities contained in the ySi lower layer electrode protrusions 28 are diffused and activated.

【0057】次いで異方性エッチングにより、ドープト
polySi下層電極突起28の側壁28a及びダミー
パターン26の側壁26aのサイドウォール形成材料3
0は残存させるようにして、サイドウォール形成材料3
0をエッチング除去し、これにより下層電極突起28の
側壁28aからダミーパターン26の側壁26aにわた
ってサイドウォール32を形成する(図10(A))。
Next, by anisotropic etching, the side wall forming material 3 for the side wall 28a of the doped polySi lower electrode projection 28 and the side wall 26a of the dummy pattern 26 is formed.
0 is allowed to remain, and the sidewall forming material 3
0 is removed by etching, whereby a sidewall 32 is formed from the sidewall 28a of the lower electrode protrusion 28 to the sidewall 26a of the dummy pattern 26 (FIG. 10A).

【0058】上述したようにダミーパターン26の側壁
26aには凹部26bを形成してあるので、この凹部2
6bに対応する箇所で湾曲したサイドウォール32を形
成できる。
As described above, since the recess 26b is formed on the side wall 26a of the dummy pattern 26, the recess 2
The curved sidewall 32 can be formed at a location corresponding to 6b.

【0059】(ダミーパターンを除去した後、サイドウ
ォール上にキャパシタ絶縁膜及び上層電極を形成する工
程)次にこの実施例では、下層電極突起28及びサイド
ウォール32は実質的にエッチングしないように、選択
的に、ダミーパターン26をエッチング除去する(図1
0(B))。
(Step of Forming Capacitor Insulating Film and Upper Layer Electrode on Sidewalls After Removing Dummy Pattern) Next, in this embodiment, the lower layer electrode projections 28 and the sidewalls 32 are substantially not etched. The dummy pattern 26 is selectively removed by etching (see FIG. 1).
0 (B)).

【0060】ここでは、ダミーパターン26のSiN第
一層261を、りん酸をエッチャントに用いたウエット
エッチングによりエッチング除去し、然る後、ダミーパ
ターン26のNSG第二層262を、ふっ酸をエッチャ
ントに用いたウエットエッチングによりエッチング除去
する。
Here, the SiN first layer 261 of the dummy pattern 26 is etched and removed by wet etching using phosphoric acid as an etchant, and then the NSG second layer 262 of the dummy pattern 26 is etched with hydrofluoric acid. It is removed by the wet etching used in the above.

【0061】次いで図示せずも、SiO2 サイドウォー
ル32上に順次に、キャパシタ絶縁膜形成用のSiN絶
縁膜及び上層電極形成用のドープトpolySi導電性
膜を形成し、然る後、これらドープトpolySi導電
性膜及びSiN絶縁膜を順次にエッチングして、ドープ
トpolySi上層電極及びSiNキャパシタ絶縁膜を
形成する。
Next, although not shown, a SiN insulating film for forming a capacitor insulating film and a doped polySi conductive film for forming an upper layer electrode are sequentially formed on the SiO 2 sidewall 32, and thereafter, these doped polySi films are formed. The conductive film and the SiN insulating film are sequentially etched to form a doped polySi upper electrode and a SiN capacitor insulating film.

【0062】この実施例によれば、下層電極突起28は
逆円錐台状の柱状突起であり、従って下層電極突起28
はその側壁まわり全周にわたってオーバーハング状の側
壁28aを有する。これがため、ダミーパターン26の
エッチング除去の際に、サイドウォール32と下層電極
突起28の側壁28aとの間に介在する自然酸化膜がエ
ッチングされて、サイドウォール32が側壁28aから
剥離することがあったとしても、サイドウォール32は
オーバーハング状の側壁28aに引っ掛かるのでサイド
ウォール32が側壁28aから抜け落ちるのを防止でき
る。これがためメモリキャパシタ42を歩留り良く形成
できる。
According to this embodiment, the lower-layer electrode protrusion 28 is an inverted truncated cone columnar protrusion, and therefore the lower-layer electrode protrusion 28 is formed.
Has an overhanging side wall 28a over the entire circumference thereof. Therefore, when the dummy pattern 26 is removed by etching, the natural oxide film interposed between the side wall 32 and the side wall 28a of the lower electrode protrusion 28 may be etched and the side wall 32 may be separated from the side wall 28a. Even if it does, since the side wall 32 is caught by the overhang-shaped side wall 28a, it is possible to prevent the side wall 32 from falling off from the side wall 28a. Therefore, the memory capacitor 42 can be formed with high yield.

【0063】さらにこの実施例によれば、ダミーパター
ン26の側壁26aに凹部26bを形成し、この凹部2
6bに対応する箇所で湾曲したサイドウォール32を形
成する。従ってこの湾曲したサイドウォール32上にキ
ャパシタ絶縁膜及び上層電極を形成することにより、キ
ャパシタ面積が増大し、これがためより一層キャパシタ
容量を増大させることができる。
Further, according to this embodiment, the recess 26b is formed in the side wall 26a of the dummy pattern 26, and the recess 2 is formed.
A curved sidewall 32 is formed at a location corresponding to 6b. Therefore, by forming the capacitor insulating film and the upper layer electrode on the curved sidewall 32, the capacitor area is increased, which can further increase the capacitor capacitance.

【0064】図11〜図13は請求項1記載の発明の第
三実施例の説明に供する工程図である。以下に述べる第
三実施例の説明では、主として上述した請求項1記載の
発明の第一実施例と相違する点につき説明し、上述した
請求項1記載の発明の第一実施例と同様の点については
その詳細な説明を省略する。
11 to 13 are process drawings for explaining the third embodiment of the invention according to claim 1. In the following description of the third embodiment, the points different from the first embodiment of the invention described in claim 1 described above will be mainly described, and the same points as the first embodiment of the invention described in claim 1 described above The detailed description thereof will be omitted.

【0065】層間絶縁膜20上に下層導電性膜24を形
成する工程までは、上述した請求項1記載の発明の第一
実施例と同様である。
The steps up to the step of forming the lower conductive film 24 on the interlayer insulating film 20 are the same as those in the first embodiment of the invention described in claim 1.

【0066】(下層導電性膜上にダミーパターンを形成
する工程)この実施例では、下層導電性膜24上に、エ
ッチングレートの異なる第一層形成材料及び第二層形成
材料を交互に積層し、これら形成材料をエッチングし
て、第一層441及び第二層442を順次に形成し、こ
れら第一層441及び第二層442から成る多層構造の
ダミーパターン44を形成する。第一層形成材料及び第
二層形成材料のエッチングレートの差を利用することに
より、側壁44aに凹部44bを有するダミーパターン
44を形成する。
(Step of Forming Dummy Pattern on Lower Conductive Film) In this embodiment, the first layer forming material and the second layer forming material having different etching rates are alternately laminated on the lower conductive film 24. Then, these forming materials are etched to sequentially form a first layer 441 and a second layer 442, and a dummy pattern 44 having a multi-layer structure including the first layer 441 and the second layer 442 is formed. By utilizing the difference in etching rate between the first layer forming material and the second layer forming material, the dummy pattern 44 having the recess 44b on the side wall 44a is formed.

【0067】ここでは、ドープトpolySi下層導電
性膜24上に順次に、NSG第一層形成材料、PSG
(Phospho−Silicate Glass)第
二層形成材料及びNSG第一層形成材料を積層する。然
る後、フォトリソ及びエッチング技術によりこれら形成
材料をエッチングして、NSG第一層441、PSG第
二層442及びNSG第一層441を順次に形成し、こ
れらNSG第一層441及びPSG第二層442から成
る3層構造のダミーパターン44を形成する(11
(A))。このエッチングは自然酸化膜の除去も兼ね
る。
Here, the NSG first layer forming material and PSG are sequentially formed on the doped polySi lower conductive film 24.
(Phospho-Silicate Glass) The second layer forming material and the NSG first layer forming material are laminated. After that, these forming materials are etched by a photolithography and etching technique to sequentially form the NSG first layer 441, the PSG second layer 442 and the NSG first layer 441, and the NSG first layer 441 and the PSG second layer 441. A dummy pattern 44 having a three-layer structure including the layer 442 is formed (11
(A)). This etching also serves to remove the natural oxide film.

【0068】エッチャントとして例えばフッ酸を用いた
ウエットエッチングでは、PSG第二層形成材料のエッ
チングレートはNSG第一層形成材料のエッチングレー
トよりも速くなるので、側壁44aに凹部44bを有す
るダミーパターン44を形成できる。
In wet etching using, for example, hydrofluoric acid as an etchant, since the etching rate of the PSG second layer forming material is higher than that of the NSG first layer forming material, the dummy pattern 44 having the recess 44b on the side wall 44a is formed. Can be formed.

【0069】ダミーパターン44の形状従って第一層4
41及び第二層442の形状を、主面10aの法線方向
から見て円形状とする。
The shape of the dummy pattern 44 and therefore the first layer 4
The shapes of 41 and the second layer 442 are circular when viewed from the direction normal to the main surface 10a.

【0070】尚、ダミーパターン44の第一層441及
び第二層442の積層個数はそれぞれ、少なくとも1個
とすることができる。
The first layer 441 and the second layer 442 of the dummy pattern 44 may each be laminated at least one.

【0071】(ダミーパターンを介し下層導電性膜をエ
ッチングして、基板に覆い被さるようなオーバーハング
状の側壁を有する下層電極突起を形成する工程)次にこ
の実施例では、ダミーパターン44を介して、ドライエ
ッチングによりドープトpolySi下層導電性膜24
をエッチングして、p−Si基板10の主面10aに覆
い被さるようなオーバーハング状の側壁28aを有する
ドープトpolySi下層電極突起28を形成する(図
11(B))。
(Step of etching lower conductive film via dummy pattern to form lower electrode projection having overhang-like side wall covering substrate) Next, in this embodiment, dummy pattern 44 is used. Then, the doped polySi lower conductive film 24 is formed by dry etching.
Is etched to form a doped polySi lower electrode projection 28 having an overhanging side wall 28a which covers the main surface 10a of the p-Si substrate 10 (FIG. 11B).

【0072】(下層電極突起の側壁からダミーパターン
の側壁にわたってサイドウォールを形成する工程)次に
この実施例では、アンドープpolySiサイドウォー
ル形成材料48を、ダミーパターン44上に積層する
(図12(A))。
(Step of Forming Sidewall from Sidewall of Lower Layer Electrode Protrusion to Sidewall of Dummy Pattern) Next, in this embodiment, an undoped polySi sidewall forming material 48 is laminated on the dummy pattern 44 (FIG. 12A). )).

【0073】次いで熱処理を行なって、ドープトpol
ySi下層電極突起28が含有する不純物を拡散及び活
性化させる。
Next, heat treatment is performed to make the doped pol.
The impurities contained in the ySi lower layer electrode protrusions 28 are diffused and activated.

【0074】次いで異方性エッチングにより、ドープト
polySi下層電極突起28の側壁28a及びダミー
パターン44の側壁44aのサイドウォール形成材料4
8は残存させるようにして、サイドウォール形成材料4
8をエッチング除去し、これにより下層電極突起28の
側壁28aからダミーパターン44の側壁44aにわた
ってサイドウォール50を形成する(図13)。
Next, by anisotropic etching, the side wall forming material 4 for the side wall 28a of the doped polySi lower electrode protrusion 28 and the side wall 44a of the dummy pattern 44 is formed.
8 is left so that the sidewall forming material 4
8 is removed by etching, thereby forming a sidewall 50 from the sidewall 28a of the lower layer electrode protrusion 28 to the sidewall 44a of the dummy pattern 44 (FIG. 13).

【0075】上述したようにダミーパターン44の側壁
44aには凹部44bを形成してあるので、この凹部4
4bに対応する箇所に凸部を有するサイドウォール50
を形成できる。
As described above, since the recess 44b is formed in the side wall 44a of the dummy pattern 44, the recess 4 is formed.
Sidewall 50 having a convex portion at a position corresponding to 4b
Can be formed.

【0076】(ダミーパターンを除去した後、サイドウ
ォール上にキャパシタ絶縁膜及び上層電極を形成する工
程)次にこの実施例では、下層電極突起28及びサイド
ウォール50は実質的にエッチングしないように、選択
的に、ダミーパターン44をエッチング除去する(図1
3(B))。
(Step of Forming Capacitor Insulating Film and Upper Layer Electrodes on Sidewalls After Removing Dummy Pattern) Next, in this embodiment, the lower layer electrode protrusions 28 and the side walls 50 are not substantially etched. The dummy pattern 44 is selectively removed by etching (see FIG. 1).
3 (B)).

【0077】ここでは、ダミーパターン44のNSG第
一層441及びPSG第二層442を、ふっ酸をエッチ
ャントに用いたウエットエッチングによりエッチング除
去する。
Here, the NSG first layer 441 and the PSG second layer 442 of the dummy pattern 44 are removed by wet etching using hydrofluoric acid as an etchant.

【0078】次いで図示せずも、サイドウォール50上
に順次に、キャパシタ絶縁膜形成用のSiN絶縁膜及び
上層電極形成用のドープトpolySi導電性膜を形成
し、然る後、これらドープトpolySi導電性膜及び
SiN絶縁膜を順次にエッチングして、ドープトpol
ySi上層電極及びSiNキャパシタ絶縁膜を形成す
る。
Next, although not shown, a SiN insulating film for forming a capacitor insulating film and a doped polySi conductive film for forming an upper layer electrode are sequentially formed on the sidewall 50, and thereafter, these doped polySi conductive films are formed. The film and the SiN insulating film are sequentially etched to obtain a doped pol.
An ySi upper layer electrode and a SiN capacitor insulating film are formed.

【0079】この実施例によれば、下層電極突起28は
逆円錐台状の柱状突起であり、従って下層電極突起28
はその側壁まわり全周にわたってオーバーハング状の側
壁28aを有する。これがため、ダミーパターン44の
エッチング除去の際に、サイドウォール50と下層電極
突起28の側壁28aとの間に介在する自然酸化膜がエ
ッチングされて、サイドウォール50が側壁28aから
剥離することがあったとしても、サイドウォール50は
オーバーハング状の側壁28aに引っ掛かるのでサイド
ウォール50が側壁28aから抜け落ちるのを防止でき
る。これがためメモリキャパシタを歩留り良く形成でき
る。
According to this embodiment, the lower layer electrode protrusions 28 are columnar protrusions having an inverted truncated cone shape, and therefore the lower layer electrode protrusions 28 are formed.
Has an overhanging side wall 28a over the entire circumference thereof. Therefore, when the dummy pattern 44 is removed by etching, the natural oxide film interposed between the sidewall 50 and the side wall 28a of the lower electrode protrusion 28 may be etched and the side wall 50 may be peeled off from the side wall 28a. Even if the sidewall 50 is caught on the overhang-shaped side wall 28a, the sidewall 50 can be prevented from falling off from the side wall 28a. Therefore, the memory capacitor can be formed with high yield.

【0080】さらにこの実施例によれば、ダミーパター
ン44の側壁44aに凹部44bを形成し、この凹部4
4bに対応する箇所に凸部を有するサイドウォール50
を形成する。従ってこの凸部を有するサイドウォール5
0上にキャパシタ絶縁膜及び上層電極を形成することに
より、キャパシタ面積が増大し、これがためより一層キ
ャパシタ容量を増大させることができる。
Further, according to this embodiment, the recess 44b is formed in the side wall 44a of the dummy pattern 44, and the recess 4 is formed.
Sidewall 50 having a convex portion at a position corresponding to 4b
To form Therefore, the sidewall 5 having this convex portion
By forming the capacitor insulating film and the upper layer electrode on 0, the capacitor area is increased, which can further increase the capacitor capacitance.

【0081】図14〜図18は請求項2記載の発明の実
施例の説明に供する工程図である。基板にメモリトラン
ジスタを形成する工程は請求項1記載の発明の第一実施
例と同様であるので、その説明を省略する。
14 to 18 are process diagrams for explaining the embodiment of the invention described in claim 2. Since the step of forming the memory transistor on the substrate is the same as that of the first embodiment of the invention described in claim 1, its description is omitted.

【0082】(メモリトランジスタを層間絶縁膜で覆う
工程)この実施例では、メモリトランジスタ12上に、
CVD法によりSiO2 層間絶縁膜20を積層して、メ
モリトランジスタ12をSiO2 層間絶縁膜20で覆う
(図14(A))。
(Step of Covering Memory Transistor with Interlayer Insulating Film) In this embodiment, on the memory transistor 12,
The SiO 2 interlayer insulating film 20 is stacked by the CVD method, and the memory transistor 12 is covered with the SiO 2 interlayer insulating film 20 (FIG. 14A).

【0083】(層間絶縁膜上にpolySi下層導電性
膜を形成する工程)次にこの実施例では、SiO2 層間
絶縁膜20上に、CVD法によりSiNエッチングスト
ッパ22を積層する。然る後、フォトリソ及びエッチン
グ技術を用いて、SiNエッチングストッパ22及びS
iO2 層間絶縁膜20にコンタクトホール22a及び2
0aを形成する(図14(B))。コンタクトホール2
2a及び20aを、メモリトランジスタ12のソース領
域124に対応する領域に形成する。
(Step of Forming PolySi Lower Layer Conductive Film on Interlayer Insulating Film) Next, in this embodiment, the SiN etching stopper 22 is laminated on the SiO 2 interlayer insulating film 20 by the CVD method. After that, the SiN etching stopper 22 and the S
Contact holes 22a and 2 are formed in the SiO 2 interlayer insulating film 20.
0a is formed (FIG. 14B). Contact hole 2
2a and 20a are formed in a region corresponding to the source region 124 of the memory transistor 12.

【0084】SiNエッチングストッパ22は、後工程
においてドープトpolySi下層導電性膜24をドラ
イエッチングして下層電極突起を形成するときに、Si
O2層間絶縁膜20がドライエッチングされるのを防止
するためのものである。
The SiN etching stopper 22 is formed of Si when the doped polySi lower conductive film 24 is dry-etched to form lower electrode protrusions in a later step.
This is for preventing the O 2 interlayer insulating film 20 from being dry-etched.

【0085】次いでSiNエッチングストッパ22上
に、ドープトpolySi下層導電性膜24を形成する
(図15(A))。ドープトpolySi下層導電性膜
24は、コンタクトホール22a及び20aを介し、ソ
ース領域124と電気的に接続する。下層導電性膜24
として形成するドープトpolySi膜は、当該導電性
膜24に電極としての導電性を付与するための不純物を
含有する。
Next, a doped polySi lower conductive film 24 is formed on the SiN etching stopper 22 (FIG. 15A). The doped polySi lower conductive film 24 is electrically connected to the source region 124 through the contact holes 22a and 20a. Lower conductive film 24
The doped polySi film formed as described above contains impurities for imparting conductivity as an electrode to the conductive film 24.

【0086】ここではシランガスを用いた低圧CVD法
により膜厚2000Å程度のアンドープpolySi膜
を積層し、然る後、イオン打ち込みエネルギーを60K
eV及びイオン注入量を1.0×1016ions/cm
2 として、アンドープpolySi膜にPイオンを注入
して、ドープトpolySi膜を形成する。
Here, an undoped polySi film having a film thickness of about 2000 Å is laminated by a low pressure CVD method using silane gas, and then ion implantation energy is set to 60 K.
eV and ion implantation dose of 1.0 × 10 16 ions / cm
2 , P ions are implanted into the undoped polySi film to form a doped polySi film.

【0087】(polySi下層導電性膜上にダミーパ
ターンを形成する工程)次にこの実施例では、ドープト
polySi下層導電性材料24上に、CVD法によ
り、ダミーパターン形成用のパターン材料として膜厚5
000Å程度のSiO2 膜を積層する。然る後、フォト
リソ及びエッチング技術を用い、異方性エッチングによ
り、SiO2 パターン材料をエッチングして、ダミーパ
ターン26を形成する(図15(B))。異方性エッチ
ングによりダミーパターン26を形成するので、ダミー
パターン26の側壁は基板10の主面10aに対しほぼ
垂直に切り立った壁となる。
(Step of Forming Dummy Pattern on PolySi Lower Layer Conductive Film) Next, in this embodiment, a film thickness of 5 is formed as a pattern material for forming a dummy pattern on the doped polySi lower layer conductive material 24 by the CVD method.
A SiO 2 film of about 000Å is laminated. Then, the SiO 2 pattern material is etched by anisotropic etching using photolithography and etching techniques to form a dummy pattern 26 (FIG. 15B). Since the dummy pattern 26 is formed by anisotropic etching, the side wall of the dummy pattern 26 becomes a wall which is substantially vertical to the main surface 10a of the substrate 10.

【0088】主面10aの法線方向から見たときのダミ
ーパターン26の形状は、円、四角形、多角形或はその
ほかの任意好適な形状とすることができるが、ここでは
円形状とする。
The shape of the dummy pattern 26 when viewed from the direction normal to the main surface 10a may be a circle, a quadrangle, a polygon, or any other suitable shape, but here it is a circular shape.

【0089】(ダミーパターンを介しpolySi下層
導電性膜をエッチングして、polySi下層電極突起
を形成する工程)次にこの実施例では、異方性エッチン
グにより、SiO2 ダミーパターング26を介しドープ
トpolySi下層導電性膜24をエッチングして、ド
ープトpolySi下層電極突起28を形成する(図1
6(A))。
(Step of Forming PolySi Lower Layer Electrode Protrusion by Etching PolySi Lower Layer Conductive Film Through Dummy Pattern) Next, in this embodiment, anisotropic poly-Si 2 is used to form doped polySi through the SiO 2 dummy pattern 26. The lower conductive film 24 is etched to form the doped polySi lower electrode projections 28 (FIG. 1).
6 (A)).

【0090】異方性エッチングにより、ドープトpol
ySi下層電極突起28を形成するので、下層電極突起
28の側壁28aは基板10の主面10aに対しほぼ垂
直に切り立った形状となる。
By anisotropic etching, the doped pol is used.
Since the ySi lower layer electrode protrusions 28 are formed, the sidewalls 28a of the lower layer electrode protrusions 28 have a shape that is substantially vertical to the main surface 10a of the substrate 10.

【0091】メモリトランジスタ12及びメモリキャパ
シタの配設密度を高めるため、ドープトpolySi下
層電極突起28を、主面10aの法線方向から見てソー
ス領域124と重なり合う位置に形成する。下層電極突
起28は、コンタクトホール22a及び20a内に残存
する下層導電性膜24を介して、ソース領域124と電
気的に接続する。
In order to increase the arrangement density of the memory transistor 12 and the memory capacitor, the doped polySi lower electrode protrusion 28 is formed at a position overlapping the source region 124 when viewed in the normal direction of the main surface 10a. The lower layer electrode protrusion 28 is electrically connected to the source region 124 via the lower layer conductive film 24 remaining in the contact holes 22a and 20a.

【0092】尚、場合によっては、下層電極突起28
を、主面10aの法線方向から見てソース領域124と
重なり合わない位置に形成しても構わない。
In some cases, the lower electrode projection 28
May be formed at a position which does not overlap with the source region 124 when viewed from the direction normal to the main surface 10a.

【0093】次いで通常行なわれる如く洗浄処理を行な
う。この洗浄処理により、下層電極突起28の自然酸化
膜(図示せず)が除去される。尚、下層電極突起28の
側壁28aの自然酸化膜を、側壁28a全面にわたって
完全に除去できなくても良い。
Then, a cleaning process is performed as usual. By this cleaning process, the natural oxide film (not shown) of the lower electrode protrusion 28 is removed. The native oxide film on the side wall 28a of the lower layer electrode protrusion 28 may not be completely removed over the entire side wall 28a.

【0094】(ダミーパターン上にアモルファスSiサ
イドウォール形成材料を形成する工程)次にこの実施例
では、ダミーパターン26上に、低圧CVD法により、
膜厚1000Å程度のノンドープアモルファスSiサイ
ドウォール形成材料46を積層する(図16(B))。
成膜温度は560℃程度とする。
(Step of Forming Amorphous Si Sidewall Forming Material on Dummy Pattern) Next, in this embodiment, the dummy pattern 26 is formed on the dummy pattern 26 by the low pressure CVD method.
A non-doped amorphous Si sidewall forming material 46 having a film thickness of about 1000 Å is laminated (FIG. 16B).
The film forming temperature is about 560 ° C.

【0095】(アモルファスSiサイドウォール形成材
料を結晶化する工程)次にこの実施例では、熱処理を行
なってアモルファスSiサイドウォール形成材料46を
結晶化(多結晶化或は再結晶化)して、polySiサ
イドウォール形成材料48を形成する(図17
(A))。
(Step of Crystallizing Amorphous Si Sidewall Forming Material) Next, in this embodiment, heat treatment is performed to crystallize (polycrystallize or recrystallize) the amorphous Si sidewall forming material 46, A polySi sidewall forming material 48 is formed (FIG. 17).
(A)).

【0096】ここではpolySiサイドウォール形成
材料48を形成するための熱処理はドープトpolyS
i下層電極突起28が含有する不純物を拡散及び活性化
させるための熱処理を兼ねる。例えばp−Si基板10
を、窒素雰囲気中に保持して850℃で15分間加熱す
ることにより熱処理を行なって、polySiサイドウ
ォール形成材料48の形成と不純物の拡散及び活性化と
を行なう。
Here, the heat treatment for forming the polySi sidewall forming material 48 is performed by using doped polyS.
i Also serves as a heat treatment for diffusing and activating the impurities contained in the lower layer electrode protrusions 28. For example, p-Si substrate 10
Is heat-treated by holding it in a nitrogen atmosphere and heating it at 850 ° C. for 15 minutes to form the polySi sidewall forming material 48 and diffuse and activate the impurities.

【0097】アモルファスSiサイドウォール形成材料
46を結晶化することにより、ドープトpolySi下
層電極突起28と一体化したpolySiサイドウォー
ル形成材料48を形成でき、従って下層電極突起28と
サイドウォール形成材料48との密着性を向上できる。
By crystallizing the amorphous Si sidewall forming material 46, it is possible to form the polySi sidewall forming material 48 integrated with the doped polySi lower electrode projection 28, and thus the lower electrode projection 28 and the sidewall forming material 48 are formed. Adhesion can be improved.

【0098】尚、熱処理によって、下層電極突起28に
対応する部分のサイドウォール形成材料48にも不純物
が拡散されるので、後述するサイドウォール50として
導電性を有するサイドウォールを形成できる。サイドウ
ォール形成材料48を形成するための熱処理と、下層電
極突起28が含有する不純物を拡散及び活性化させるた
めの熱処理とはそれぞれ別工程で行なうようにしても良
い。
Since the impurities are also diffused into the sidewall forming material 48 in the portion corresponding to the lower electrode protrusion 28 by the heat treatment, a conductive sidewall can be formed as the sidewall 50 described later. The heat treatment for forming the sidewall forming material 48 and the heat treatment for diffusing and activating the impurities contained in the lower layer electrode protrusions 28 may be performed in separate steps.

【0099】(サイドウォール形成材料をダミーパター
ンを介しエッチングしてpolySi下層電極突起の側
壁からダミーパターンの側壁にわたってサイドウォール
を形成する工程)次にこの実施例では、異方性エッチン
グにより、下層電極突起28の側壁28a及びダミーパ
ターン26の側壁26aのサイドウォール形成材料48
は残存させるようにして、サイドウォール形成材料48
をエッチング除去し、これにより下層電極突起28の側
壁28aからダミーパターン26の側壁26aにわたっ
てサイドウォール50を形成する(図17(B))。サ
イドウォール50は、側壁28a及び26aに残存させ
たサイドウォール形成材料48から成る。
(Step of Etching Sidewall Forming Material Through Dummy Pattern to Form Sidewall from Sidewall of PolySi Lower Layer Electrode Protrusion to Sidewall of Dummy Pattern) Next, in this embodiment, the lower layer electrode is formed by anisotropic etching. Sidewall forming material 48 for the side wall 28a of the protrusion 28 and the side wall 26a of the dummy pattern 26
The sidewall forming material 48
Are removed by etching, thereby forming a sidewall 50 from the sidewall 28a of the lower layer electrode protrusion 28 to the sidewall 26a of the dummy pattern 26 (FIG. 17B). The sidewall 50 is made of the sidewall forming material 48 left on the sidewalls 28a and 26a.

【0100】(ダミーパターンを除去する工程)次にこ
の実施例では、下層電極突起28及びサイドウォール5
0は実質的にエッチングしないように、選択的に、ダミ
ーパターン26をエッチング除去する(図18
(A))。
(Step of Removing Dummy Pattern) Next, in this embodiment, the lower electrode projection 28 and the sidewall 5 are formed.
The dummy pattern 26 is selectively etched away so that 0 does not substantially etch (FIG. 18).
(A)).

【0101】ここでは、下層電極突起28はドープトp
olySi、サイドウォール50はドープト若しくはア
ンンドープpolySi、及び、ダミーパターン28は
SiO2 から成るので、任意好適な組成のエッチャント
例えばフッ酸を用いてウエットエッチングを行なうこと
により、ダミーパターン28を選択的にエッチング除去
できる。
Here, the lower electrode projection 28 is made of doped p.
Since the polySi and the sidewalls 50 are made of doped or undoped polySi and the dummy pattern 28 is made of SiO 2 , the dummy pattern 28 is selectively etched by performing wet etching using an etchant having any suitable composition such as hydrofluoric acid. Can be removed.

【0102】(ダミーパターンの除去後、サイドウォー
ル上にキャパシタ絶縁膜及び上層電極を形成する工程)
次にこの実施例では、サイドウォール50上に順次に、
キャパシタ絶縁膜形成用の絶縁膜34及び上層電極形成
用の導電性膜36を形成する(図19(A))。
(Step of forming capacitor insulating film and upper layer electrode on sidewall after removal of dummy pattern)
Next, in this embodiment, the sidewalls 50 are sequentially
An insulating film 34 for forming a capacitor insulating film and a conductive film 36 for forming an upper electrode are formed (FIG. 19A).

【0103】ここでは、サイドウォール50上に、低圧
CVD法により膜厚100Å程度のSiN絶縁膜34を
積層する。次いで、このSiN絶縁膜34上に、低圧C
VD法により膜厚2000Å程度のアンドープpoly
Si膜を積層する。然る後、このアンドープpolyS
i膜に、気相拡散法により不純物を拡散させて、ドープ
トpolySi膜から成る導電性膜36を得る。ドープ
トpolySi導電性膜36は、当該膜36に電極とし
ての導電性を付与するための不純物を含有する。例え
ば、POCl3 の蒸気中にp−Si基板10を保持し
て、気相拡散により、PをアンドープpolySi膜中
に拡散させて、ドープトpolySi導電性膜36を形
成すれば良い。
Here, the SiN insulating film 34 having a film thickness of about 100 Å is laminated on the sidewall 50 by the low pressure CVD method. Then, a low voltage C is formed on the SiN insulating film 34.
Undoped poly with a film thickness of about 2000Å by VD method
A Si film is laminated. After that, this undoped polyS
Impurities are diffused in the i film by a vapor phase diffusion method to obtain a conductive film 36 made of a doped polySi film. The doped polySi conductive film 36 contains impurities for giving the film 36 conductivity as an electrode. For example, the p-Si substrate 10 may be held in the vapor of POCl 3 , and P may be diffused into the undoped polySi film by vapor phase diffusion to form the doped polySi conductive film 36.

【0104】次いでホトリソ及びエッチング技術を用い
て、ドープトpolySi導電性膜36及びSiN絶縁
膜34を順次にエッチングして、ドープトpolySi
上層電極38及びSiNキャパシタ絶縁膜40を形成
し、メモリキャパシタ52を得る(図19)。
Then, the doped polySi conductive film 36 and the SiN insulating film 34 are sequentially etched by using a photolithography and etching technique to obtain the doped polySi.
The upper electrode 38 and the SiN capacitor insulating film 40 are formed to obtain the memory capacitor 52 (FIG. 19).

【0105】メモリキャパシタ52は、基板10に形成
したメモリトランジスタ12上に層間絶縁膜20を介し
て設けた下層電極突起28と、この下層電極突起28上
に順次に設けたキャパシタ絶縁膜40及び上層電極38
とを備えて成る。
The memory capacitor 52 is composed of a lower layer electrode protrusion 28 provided on the memory transistor 12 formed on the substrate 10 with the interlayer insulating film 20 interposed therebetween, and a capacitor insulating film 40 and an upper layer electrode sequentially provided on the lower layer electrode protrusion 28. Electrode 38
And.

【0106】この実施例によれば、ダミーパターン26
上にアモルファスSiサイドウォール形成材料46を積
層した後、アモルファスSiサイドウォール形成材料4
6を結晶化してpolySiサイドウォール形成材料4
8を形成するので、polySiサイドウォール形成材
料48と下層電極突起28との密着強度を高めることが
できる。従ってこのpolySiサイドウォール形成材
料48を異方性エッチングによりエッチングしてサイド
ウォール50を形成することにより、下層電極突起28
との密着強度の高いサイドウォール50を得ることがで
きる。これがためサイドウォール50は、下層電極突起
28から剥離しにくくなるので、メモリキャパシタ52
を歩留り良く形成できる。
According to this embodiment, the dummy pattern 26
After stacking the amorphous Si sidewall forming material 46 on top, the amorphous Si sidewall forming material 4
6 is crystallized to form a polySi sidewall forming material 4
8 is formed, the adhesion strength between the polySi sidewall forming material 48 and the lower layer electrode protrusion 28 can be increased. Therefore, this polySi sidewall forming material 48 is etched by anisotropic etching to form sidewalls 50, whereby the lower layer electrode protrusions 28 are formed.
It is possible to obtain the sidewall 50 having high adhesion strength with. For this reason, the sidewall 50 is less likely to be peeled off from the lower layer electrode protrusion 28, so that the memory capacitor 52 is removed.
Can be formed with high yield.

【0107】尚、この実施例では主面10aに対し垂直
に切り立った形状の側壁28aを有する下層電極突起2
8を形成するようにしたが、これに代えて請求項1記載
の発明の第一実施例と同様に、基板10の主面10aに
覆い被さるようなオーバーハング状の側壁28aを有す
る下層電極突起28を形成するようにしても良い。オー
バーハング状とすることにより、より一層の歩留り向上
を望める。このようなオーバーハング状の側壁28aの
形成は、ドライエッチングのエッチング条件例えばエッ
チングガスの組成を調整することにより、達成できる。
In this embodiment, the lower layer electrode projection 2 having the side wall 28a which is vertically raised with respect to the main surface 10a.
However, instead of this, as in the first embodiment of the invention described in claim 1, a lower layer electrode projection having an overhanging side wall 28a which covers the main surface 10a of the substrate 10 is formed. 28 may be formed. With the overhang shape, further improvement in yield can be expected. The formation of such overhanging side walls 28a can be achieved by adjusting the etching conditions for dry etching, for example, the composition of the etching gas.

【0108】この場合にも、ドープトpolySi下層
電極突起28は逆テーパ状(逆円錐台状)の柱状突起と
し、この突起28の周回り全周にわたってオーバーハン
グ状の側壁28aを形成するのが好ましい。オーバーハ
ング状の側壁28aと主面10aの法線Hとが成す角度
α(図5(A)参照)は、サイドウォール50が下層電
極突起28から剥離したときにサイドウォールを側壁2
8に引っ掛けてサイドウォールの脱落を防止できる程度
であれば良い。
Also in this case, it is preferable that the doped polySi lower layer electrode protrusion 28 is a columnar protrusion having an inverse taper shape (inverse truncated cone shape), and an overhanging side wall 28a is formed all around the periphery of the protrusion 28. . The angle α formed by the overhang-shaped side wall 28a and the normal line H of the main surface 10a (see FIG. 5A) indicates that when the side wall 50 is separated from the lower layer electrode protrusion 28, the side wall 2 is formed.
It suffices that it can be hooked on No. 8 to prevent the sidewall from falling off.

【0109】またサイドウォール50が下層電極突起2
8から剥離したときにサイドウォールを側壁28aに引
っ掛けてサイドウォールの脱落を防止できるのであれ
ば、下層電極突起28の側壁28aの一部をオーバーハ
ング状の側壁28aとし残りの側壁28aを主面10a
に対しほぼ垂直な壁としても良い。
Further, the sidewall 50 is the lower electrode projection 2
If it is possible to prevent the side wall from falling off by catching the side wall on the side wall 28a when peeled from 8, the side wall 28a of the lower layer electrode protrusion 28 is made to be an overhang-shaped side wall 28a and the remaining side wall 28a is the main surface. 10a
However, the wall may be almost vertical.

【0110】発明は上述した実施例にのみ限定されるも
のではなく、従って各構成成分の形成材料、形成方法、
積層個数、寸法、形状或はそのほかの条件を、発明の趣
旨の範囲内で任意好適に変更できる。
The invention is not limited to the above-mentioned embodiments, and therefore, the forming material of each constituent, the forming method,
The number of stacked layers, the size, the shape, or other conditions can be arbitrarily changed within the scope of the gist of the invention.

【0111】[0111]

【発明の効果】上述した説明からも明らかなように、請
求項1記載の発明のメモリキャパシタの形成方法によれ
ば、下層電極突起の側壁は基板に覆い被さるようにオー
バーハング状に傾斜しており、このオーバーハング状の
側壁にサイドウォールを形成する。従ってサイドウォー
ルが下層電極突起から剥離するようなことがあっても、
サイドウォールはオーバーハング状の側壁に引っ掛かる
ので、サイドウォールが下層電極突起から抜け落ちるの
を防止できる。これがためメモリキャパシタの歩留りを
向上できる。
As is apparent from the above description, according to the method of forming a memory capacitor of the first aspect of the present invention, the side wall of the lower layer electrode protrusion is inclined in an overhang shape so as to cover the substrate. A sidewall is formed on the overhanging side wall. Therefore, even if the side wall is peeled from the lower layer electrode protrusion,
Since the side wall is caught on the overhang-shaped side wall, it is possible to prevent the side wall from coming off from the lower layer electrode protrusion. Therefore, the yield of the memory capacitor can be improved.

【0112】また請求項2記載のメモリキャパシタの形
成方法によれば、アモルファスSiサイドウォール形成
材料を結晶化した後に、ダミーパターンを除去する。従
ってダミーパターン除去の際には、polySi下層電
極突起の側壁と一体になったpolySiサイドウォー
ルが形成されている。従って下層電極突起とサイドウォ
ールとの密着性を向上させた状態で、サイドウォールを
除去できるので、サイドウォールは下層電極突起から剥
離しにくくなる。これがためメモリキャパシタの歩留り
を向上できる。
According to the method of forming a memory capacitor of the second aspect, the dummy pattern is removed after the amorphous Si sidewall forming material is crystallized. Therefore, at the time of removing the dummy pattern, the polySi sidewall that is integrated with the sidewall of the polySi lower layer electrode protrusion is formed. Therefore, the side wall can be removed in a state where the adhesion between the lower layer electrode protrusion and the side wall is improved, so that the side wall is less likely to be separated from the lower layer electrode protrusion. Therefore, the yield of the memory capacitor can be improved.

【図面の簡単な説明】[Brief description of drawings]

【図1】(A)及び(B)は請求項1記載の発明の第一
実施例の説明に供する工程図である。
1A and 1B are process drawings for explaining a first embodiment of the invention according to claim 1. FIG.

【図2】(A)及び(B)は請求項1記載の発明の第一
実施例の説明に供する工程図である。
2 (A) and (B) are process drawings provided for explaining a first embodiment of the invention according to claim 1. FIG.

【図3】(A)及び(B)は請求項1記載の発明の第一
実施例の説明に供する工程図である。
3 (A) and 3 (B) are process drawings for explaining the first embodiment of the invention according to claim 1. FIG.

【図4】(A)及び(B)は請求項1記載の発明の第一
実施例の説明に供する工程図である。
4 (A) and 4 (B) are process drawings for explaining the first embodiment of the invention according to claim 1. FIG.

【図5】(A)及び(B)は請求項1記載の発明の第一
実施例の説明に供する工程図である。
5 (A) and 5 (B) are process drawings for explaining the first embodiment of the invention according to claim 1. FIG.

【図6】(A)及び(B)は請求項1記載の発明の第一
実施例の説明に供する工程図である。
6 (A) and 6 (B) are process drawings for explaining the first embodiment of the invention according to claim 1. FIG.

【図7】(A)及び(B)は請求項1記載の発明の第一
実施例の説明に供する工程図である。
7 (A) and 7 (B) are process drawings for explaining the first embodiment of the invention according to claim 1. FIG.

【図8】(A)及び(B)は請求項1記載の発明の第二
実施例の説明に供する工程図である。
8 (A) and 8 (B) are process drawings for explaining a second embodiment of the invention according to claim 1. FIG.

【図9】(A)及び(B)は請求項1記載の発明の第二
実施例の説明に供する工程図である。
9 (A) and 9 (B) are process drawings for explaining a second embodiment of the invention according to claim 1. FIG.

【図10】(A)及び(B)は請求項1記載の発明の第
二実施例の説明に供する工程図である。
10 (A) and 10 (B) are process drawings for explaining the second embodiment of the invention according to claim 1. FIG.

【図11】(A)及び(B)は請求項1記載の発明の第
三実施例の説明に供する工程図である。
11 (A) and (B) are process drawings for explaining a third embodiment of the invention according to claim 1. FIG.

【図12】(A)及び(B)は請求項1記載の発明の第
三実施例の説明に供する工程図である。
12 (A) and (B) are process drawings for explaining a third embodiment of the invention according to claim 1. FIG.

【図13】請求項1記載の発明の第三実施例の説明に供
する工程図である。
FIG. 13 is a process drawing for explaining a third embodiment of the invention according to claim 1;

【図14】(A)及び(B)は請求項2記載の発明の実
施例の説明に供する工程図である。
14 (A) and 14 (B) are process drawings for explaining the embodiment of the invention described in claim 2. FIG.

【図15】(A)及び(B)は請求項2記載の発明の実
施例の説明に供する工程図である。
15 (A) and 15 (B) are process drawings for explaining an embodiment of the invention described in claim 2. FIG.

【図16】(A)及び(B)は請求項2記載の発明の実
施例の説明に供する工程図である。
16 (A) and 16 (B) are process drawings for explaining the embodiment of the invention described in claim 2. FIG.

【図17】(A)及び(B)は請求項2記載の発明の実
施例の説明に供する工程図である。
17 (A) and 17 (B) are process drawings for explaining the embodiment of the invention described in claim 2. FIG.

【図18】(A)及び(B)は請求項2記載の発明の実
施例の説明に供する工程図である。
18 (A) and 18 (B) are process drawings for explaining an embodiment of the invention described in claim 2. FIG.

【図19】請求項2記載の発明の実施例の説明に供する
工程図である。
FIG. 19 is a process chart for explaining the embodiment of the invention according to claim 2;

【符号の説明】[Explanation of symbols]

12:メモリトランジスタ 20:層間絶縁膜 26、44:ダミーパターン 28:下層電極突起 28a:オーバーハング状の側壁 32、50:サイドウォール 38:上層電極 40:キャパシタ絶縁膜 42、52:メモリキャパシタ 46:アモルファスSiサイドウォール形成材料 48:polySiサイドウォール形成材料 12: Memory transistor 20: Interlayer insulating film 26, 44: Dummy pattern 28: Lower layer electrode protrusion 28a: Overhang side wall 32, 50: Side wall 38: Upper layer electrode 40: Capacitor insulating film 42, 52: Memory capacitor 46: Amorphous Si sidewall forming material 48: PolySi sidewall forming material

Claims (2)

【特許請求の範囲】[Claims] 【請求項1】 基板に形成したメモリトランジスタ上に
層間絶縁膜を介して設けた下層電極と、該下層電極上に
順次に設けたキャパシタ絶縁膜及び上層電極とを備えて
成るメモリキャパシタを形成するに当り、 層間絶縁膜上に下層導電性膜を形成する工程と、 前記下層導電性膜上にダミーパターンを形成する工程
と、 前記ダミーパターンを介し下層導電性膜をエッチングし
て、前記基板に覆い被さるようなオーバーハング状の側
壁を有する下層電極突起を形成する工程と、 前記下層電極突起の側壁からダミーパターンの側壁にわ
たってサイドウォールを形成する工程と、 ダミーパターンを除去した後、サイドウォール上にキャ
パシタ絶縁膜及び上層電極を形成する工程とを含んで成
ることを特徴とするメモリキャパシタの形成方法。
1. A memory capacitor comprising a lower layer electrode provided on a memory transistor formed on a substrate via an interlayer insulating film, and a capacitor insulating film and an upper electrode sequentially provided on the lower electrode. First, the step of forming a lower conductive film on the interlayer insulating film, the step of forming a dummy pattern on the lower conductive film, and the etching of the lower conductive film through the dummy pattern, Forming a lower layer electrode protrusion having an overhanging side wall that covers the substrate; forming a sidewall from the side wall of the lower layer electrode protrusion to the side wall of the dummy pattern; And a step of forming a capacitor insulating film and an upper layer electrode.
【請求項2】 基板に形成したメモリトランジスタ上に
層間絶縁膜を介して設けた下層電極と、該下層電極上に
順次に設けたキャパシタ絶縁膜及び上層電極とを備えて
成るメモリキャパシタを形成するに当り、 層間絶縁膜上にpolySi下層導電性膜を形成する工
程と、 前記polySi下層導電性膜上にダミーパターンを形
成する工程と、 前記ダミーパターン上にアモルファスSiサイドウォー
ル形成材料を形成する工程と、 サイドウォール形成材料をダミーパターンを介しエッチ
ングして前記polySi下層電極突起の側壁からダミ
ーパターンの側壁にわたってサイドウォールを形成する
工程と、 アモルファスSiサイドウォール形成材料を結晶化した
後、ダミーパターンを除去する工程とを含んで成ること
を特徴とするメモリキャパシタの形成方法。
2. A memory capacitor including a lower layer electrode provided on a memory transistor formed on a substrate via an interlayer insulating film, and a capacitor insulating film and an upper electrode sequentially provided on the lower electrode. First, a step of forming a polySi lower conductive film on the interlayer insulating film, a step of forming a dummy pattern on the polySi lower conductive film, and a step of forming an amorphous Si sidewall forming material on the dummy pattern. And a step of etching a sidewall forming material through a dummy pattern to form a sidewall from a sidewall of the polySi lower electrode protrusion to a sidewall of the dummy pattern, and after crystallizing the amorphous Si sidewall forming material, forming the dummy pattern And a step of removing. The method of forming the Pashita.
JP18303695A 1995-07-19 1995-07-19 Memory capacitor and method of forming memory capacitor Expired - Fee Related JP3432644B2 (en)