JPH11347324A - Support for multi-type filter and method for producing the same - Google Patents

Support for multi-type filter and method for producing the same

Info

Publication number
JPH11347324A
JPH11347324A JP15447298A JP15447298A JPH11347324A JP H11347324 A JPH11347324 A JP H11347324A JP 15447298 A JP15447298 A JP 15447298A JP 15447298 A JP15447298 A JP 15447298A JP H11347324 A JPH11347324 A JP H11347324A
Authority
JP
Japan
Prior art keywords
support
cross
sintered body
type filter
extrusion direction
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
JP15447298A
Other languages
Japanese (ja)
Inventor
Yuji Hirano
裕司 平野
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Noritake Co Ltd
Original Assignee
Noritake Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Noritake Co Ltd filed Critical Noritake Co Ltd
Priority to JP15447298A priority Critical patent/JPH11347324A/en
Publication of JPH11347324A publication Critical patent/JPH11347324A/en
Withdrawn legal-status Critical Current

Abstract

(57)【要約】 【課題】微小粒子を用いて押出成形する場合であっても
所望の形状に簡単に押出成形し焼結して製造することが
できるマルチ型フィルター用支持体及びその製造方法を
提供する。また、押出方向に対して直角方向の断面の中
心部にキレ、ワレ等の欠陥がないマルチ型フィルター用
支持体及びその製造方法を提供する。 【解決手段】押出方向に対して直角方向の断面の中心部
を除く領域のみに孔を有する無機質粒子の成形体を焼成
して、無機質粒子の押出成形体の焼結体であって押出方
向に対して直角方向の断面の中心部22を除く領域のみ
に流路20を有するセラミックス多孔質焼結体のマルチ
型フィルター用支持体21を得る。
(57) Abstract: A support for a multi-type filter, which can be easily extruded into a desired shape and produced by sintering even when extruding using fine particles, and a method for producing the same. I will provide a. Further, the present invention provides a multi-type filter support having no defects such as cracks and cracks in the center of a cross section perpendicular to the extrusion direction and a method for producing the same. A sintered body of an inorganic particle extruded body obtained by firing a molded body of inorganic particles having holes only in a region excluding a center part of a cross section in a direction perpendicular to an extrusion direction, wherein the sintered body is formed in the extrusion direction. On the other hand, a support 21 for a multi-type filter made of a ceramic porous sintered body having a flow path 20 only in a region except for a central portion 22 of a cross section in a direction perpendicular to the cross direction is obtained.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は、セラミックフィル
ターに用いられるマルチ型支持体(マルチ型フィルター
用支持体)及びその製造方法に関し、特に構成原料が微
細粉末であり、従来の方法では成形が困難で製造しにく
い支持体に好適に適用することができる多孔性セラミッ
ク質焼結体を含むマルチ型フィルター用支持体及びその
製造方法に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a multi-type support (support for a multi-type filter) used for a ceramic filter and a method for producing the same. The present invention relates to a support for a multi-type filter including a porous ceramics sintered body which can be suitably applied to a support which is difficult to manufacture with a filter, and a method for manufacturing the same.

【0002】[0002]

【従来の技術】近年、液体中の固体成分を分離回収する
方法として、セラミック原料を緻密化しない程度に焼成
した多孔性セラミック質焼結体をフィルターとして用い
ることが注目されている。その利点として、耐薬品性、
耐熱性、耐久性に優れていることが挙げられる。また、
その補足性能は、構成体(多孔性セラミック質焼結体)
の原料粉体の粒径によってほぼ決定され、原料として使
用する無機質粉体粒子の寸法が小さいほど微少なごみを
取り除くことができる。
2. Description of the Related Art In recent years, as a method for separating and recovering a solid component in a liquid, attention has been paid to using a porous ceramic sintered body fired so as not to densify a ceramic raw material as a filter. Its advantages are chemical resistance,
It is excellent in heat resistance and durability. Also,
The supplemental performance is the structure (porous ceramic sintered body)
Is substantially determined by the particle size of the raw material powder, and finer dust can be removed as the size of the inorganic powder particles used as the raw material is smaller.

【0003】通常、セラミックフィルターは多層構造を
有しており、比較的粒径の大きい無機質粉体粒子を用い
て焼結させて成る支持体上に、比較的粒径の小さい無機
質粉体粒子を用いて焼結させて成るコーティング層が2
層あるいは3層と設けられている。前記コーティング層
のうちの最小粒子から成る層は濾過膜と呼ばれ、分離性
能はここで決定される。
[0003] Usually, a ceramic filter has a multi-layer structure, in which inorganic powder particles having a relatively small particle size are placed on a support sintered using inorganic powder particles having a relatively large particle size. Coating layer which is sintered by using
And three layers. The layer consisting of the smallest particles of the coating layer is called a filtration membrane, and the separation performance is determined here.

【0004】濾過液の透過性能の向上の為に、最小粒子
から成る濾過膜は極力薄いことが好ましいが、それを支
持する支持体部は一層であることが製造コストの点から
好ましい。しかし、濾過膜形成用坏土を支持体にコーテ
ィング(被覆)する際に、この支持体を構成する粉体粒
子の粒径と濾過膜形成用坏土に含まれる粉体粒子の粒径
との差が大きいと(支持体を構成する粉体粒子の粒径の
ほうが大きいと)、支持体の孔への濾過膜形成用坏土に
含まれる粉体粒子の吸込みが大きくなり濾過膜形成用坏
土のコーティング層を得ることが困難になるため、濾過
膜形成用坏土に含まれる粉体粒子の粒径が小さいほど支
持体も微小な粒径の粉体粒子で作らなければならなかっ
た。
[0004] In order to improve the permeation performance of the filtrate, it is preferable that the filtration membrane composed of the smallest particles is as thin as possible. However, it is preferable that the number of support members supporting the filtration membrane be one, from the viewpoint of production cost. However, when coating (coating) the kneaded material for forming a filtration membrane on a support, the particle size of the powder particles constituting the support and the particle size of the powder particles contained in the kneaded material for forming a filtration film are determined. When the difference is large (when the particle size of the powder particles constituting the support is larger), the suction of the powder particles contained in the filter film forming clay into the pores of the support increases, and Since it is difficult to obtain a soil coating layer, the smaller the particle size of the powder particles contained in the kneaded material for forming a filtration membrane, the more the support must be made of powder particles having a smaller particle size.

【0005】[0005]

【発明が解決しようとする課題】しかしながら、微小粒
子(例えば、1次粒子の平均粒径が10μm以下)を用
いての押出成形には、困難な点があった。即ち、通常の
適度な使用量のバインダーや滑剤を配合して行う押出成
形は基本的に極めて困難であり、過剰な量のバインダー
や滑剤を配合しなければ、押出成形体の形状を決定する
押出成形用ダイ(以下、ダイという。)を通過すること
ができない。そのため、押出成形体(特に、所望の形状
の押出成形体)を簡単に得ることはできなかった。
However, extrusion using fine particles (for example, primary particles having an average particle size of 10 μm or less) has a difficulty. That is, it is basically extremely difficult to carry out extrusion molding by blending ordinary amounts of binders and lubricants, and unless excessive amounts of binders and lubricants are blended, extrusion molding which determines the shape of the extruded body is performed. It cannot pass through a molding die (hereinafter, die). Therefore, an extruded product (especially, an extruded product having a desired shape) cannot be easily obtained.

【0006】また、適度な量のバインダーや滑剤を配合
して押出成形が可能な場合であっても、得られた成形体
の押出方向に対して直角方向の断面の中心部の孔(押出
方向に平行な貫通孔)付近の隔壁にはキレ、ワレ等の欠
陥が生じていた。特に、押出方向に平行な貫通孔の数が
多い成形体の場合ほど、この傾向が著しい。
[0006] Even when extrusion molding can be performed by blending an appropriate amount of a binder or a lubricant, a hole at the center of a cross section perpendicular to the extrusion direction of the obtained molded body (extrusion direction). Defects such as cracks and cracks occurred in the partition near the through hole parallel to the hole). In particular, this tendency is more remarkable in a molded article having a large number of through holes parallel to the extrusion direction.

【0007】一方、過剰な量のバインダーや滑剤の配合
により押出成形体を得ることはできるが、前記過剰な量
のバインダーや滑剤の配合により押出成形体の保形性は
悪化するので、やはり所望の形状の成形体を得ることが
できなかった。なお、この場合であっても、得られた成
形体の押出方向に対して直角方向の断面の中心部の孔
(押出方向に平行な貫通孔)付近の隔壁にはキレ、ワレ
等の欠陥が生じる場合があった。特に、押出方向に平行
な貫通孔の数が多い成形体の場合ほど、この傾向が著し
い。
On the other hand, an extruded product can be obtained by blending an excessive amount of a binder or a lubricant, but the shape retention of the extruded product is deteriorated by blending the excessive amount of a binder or a lubricant. Could not be obtained. Even in this case, the partition near the center hole (through hole parallel to the extrusion direction) in the center of the cross section perpendicular to the extrusion direction of the obtained molded body has defects such as cracks and cracks. May have occurred. In particular, this tendency is more remarkable in a molded article having a large number of through holes parallel to the extrusion direction.

【0008】本発明は、上記従来技術の問題点を解決
し、微小粒子を用いて押出成形する場合であっても所望
の形状に簡単に押出成形し焼結して製造することができ
るマルチ型フィルター用支持体及びその製造方法を提供
することを目的とする。また、押出方向に対して直角方
向の断面の中心部にキレ、ワレ等の欠陥がないマルチ型
フィルター用支持体及びその製造方法を提供することを
目的とする。
The present invention solves the above-mentioned problems of the prior art, and even when extruding using fine particles, a multi-type mold which can be easily extruded into a desired shape and sintered. An object of the present invention is to provide a support for a filter and a method for producing the same. It is another object of the present invention to provide a support for a multi-type filter having no defects such as cracks and cracks in the center of a cross section perpendicular to the extrusion direction and a method for producing the same.

【0009】[0009]

【課題を解決するための手段】本発明者は、微小径粒子
(例えば、1次粒子の平均粒径が10μm以下)を含有
する坏土をダイを用いて押出成形する場合に、次の内容
を知見して本発明を完成するに至った。
Means for Solving the Problems The present inventor, when extruding a clay containing fine particles (for example, the average particle diameter of primary particles is 10 μm or less) using a die, has the following contents. The inventors have found that the present invention has been completed.

【0010】微小径粒子(例えば、1次粒子の平均粒径
が10μm以下)を含有する坏土を用いて押出成形する
場合、前記粒子間の隙間が小さいことからその隙間にバ
インダーがまんべんなく充填されることが難しいため、
原料(坏土)に与える応力を大きくするほど滑りにくく
なるというダイラタント挙動が発生しやすいので、多く
のバインダーや滑剤を配合しなければ、押出成形体の形
状を決定するダイを通過することができず、所望の形状
の成形体を得ることができない。
When extruding using a clay containing fine particles (for example, primary particles having an average particle diameter of 10 μm or less), the gaps between the particles are so small that the binder is evenly filled in the gaps. Because it is difficult to
As the stress applied to the raw material (kneaded clay) increases, the dilatant behavior, in which the material becomes less slippery, is likely to occur. Therefore, a molded article having a desired shape cannot be obtained.

【0011】また、押出成形しようとする成形体の孔
(マルチ型フィルター用支持体における流路に対応する
孔)の数が増すほど、そのような成形体を得るためのダ
イの形状が複雑になり、押出成形中に原料であるグリー
ン体(坏土)に大きな応力が生じ、坏土の流動性が減少
する。特に、押出成形体の押出方向に対して直角方向の
中心部でその傾向が顕著であるので、得られた成形体の
ほとんどが前記中心部の孔の付近の隔壁にて、キレ、ワ
レ等の欠陥を生じていた。
Further, as the number of holes (holes corresponding to the flow path in the support for a multi-type filter) of a molded article to be extruded increases, the shape of a die for obtaining such a molded article becomes more complicated. Thus, a large stress is generated in the green body (kneaded clay) as a raw material during extrusion molding, and the fluidity of the kneaded clay decreases. In particular, since the tendency is remarkable in the central part in the direction perpendicular to the extrusion direction of the extruded molded body, most of the obtained molded body is a partition wall near the hole in the central part, such as cracks, cracks, etc. Had defects.

【0012】即ち、本発明者は、従来の一般的なマルチ
型セラミックフィルター支持体の製造方法では、微細原
料粉末を含有する坏土の押出成形をする場合には、その
坏土にダイラタントな挙動があることから、構造が入り
組んでいるダイ中心部での坏土の流れが阻害されること
となり、多孔性セラミック質焼結体を製造するための成
形体の成形性が前記成形体の中心部(押出方向に対して
直角方向の断面の中心部)にて特に悪化し、欠陥の無い
成形体を得ることができなかったことを見出した。
That is, in the conventional method for manufacturing a multi-type ceramic filter support, when extruding a kneaded clay containing fine raw material powder, the present inventor has found that the kneaded clay has a dilatant behavior. Therefore, the flow of the clay at the center of the die where the structure is intricate is impeded, and the moldability of the compact for producing the porous ceramic sintered body is reduced by the central portion of the compact. (The center of the cross section in the direction perpendicular to the extrusion direction) particularly deteriorated, and it was found that a molded article having no defect could not be obtained.

【0013】本発明者は、本件に関して研究を重ねた結
果、上記欠陥が前記成形体の前記中心部の前記孔の付近
の隔壁に出る頻度が高いことから、ダイの中心部の構造
及び成形体の形状に着目し、ダイ中心部の坏土の流れを
高める為に、無機質粒子の成形体の形状を、押出方向に
対して直角方向の断面の中心部を除く領域のみに孔(マ
ルチ型フィルター用支持体における流路に対応する孔)
を有する形状とし前記中心部には孔を設けないようにす
ることにより、上記問題点を解決できるということを見
出し、本発明を完成するに至った。
As a result of repeated studies on the present case, the present inventor has found that the frequency of occurrence of the defect in the partition wall near the hole in the central portion of the molded body is high. In order to increase the flow of the clay at the center of the die, the shape of the compact of inorganic particles should be changed only in the region except the center of the cross section perpendicular to the extrusion direction (multi-type filter). Hole corresponding to the flow path in the support
It has been found that the above problem can be solved by adopting a shape having a shape and not providing a hole in the central portion, thereby completing the present invention.

【0014】本発明の第1の視点によれば、無機質粒子
の押出成形体の焼結体であって押出方向に対して直角方
向の断面の中心部を除く領域のみに流路を有するセラミ
ックス多孔質焼結体を含むマルチ型フィルター用支持体
により上記目的の少なくとも1を達成することができ
る。このマルチ型フィルター用支持体は、次のようにす
ることができる。
According to a first aspect of the present invention, there is provided a ceramic porous body which is a sintered body of an extruded body of inorganic particles and has a flow path only in a region except a central portion of a cross section perpendicular to an extrusion direction. At least one of the above objects can be achieved by a support for a multi-type filter including a porous sintered body. The support for the multi-type filter can be as follows.

【0015】前記セラミックス多孔質焼結体の押出方向
に対して直角方向における、前記セラミックス多孔質焼
結体の全断面積に占める前記中心部の断面積は、0.5
%以上にすることができる。前記セラミックス多孔質焼
結体は、平均粒径10μm以下の1次粒子の焼結体にす
ることができる。
[0015] The cross-sectional area of the central portion with respect to the total cross-sectional area of the ceramic porous sintered body in a direction perpendicular to the extrusion direction of the ceramic porous sintered body is 0.5.
%. The ceramic porous sintered body can be a sintered body of primary particles having an average particle size of 10 μm or less.

【0016】本発明の第2の視点によれば、押出方向に
対して直角方向の断面の中心部を除く領域のみに孔を有
する無機質粒子の成形体を焼成する焼成工程を含むマル
チ型フィルター用支持体の製造方法により、上記目的の
少なくとも1を達成することができる。このマルチ型フ
ィルター用支持体の製造方法は、次のようにすることが
できる。
According to a second aspect of the present invention, there is provided a multi-type filter for a multi-type filter including a firing step of firing a formed body of inorganic particles having holes only in a region except for a central portion of a cross section perpendicular to the extrusion direction. According to the method for producing the support, at least one of the above objects can be achieved. The method for producing the support for a multi-type filter can be as follows.

【0017】前記成形体の押出方向に対して直角方向に
おける、前記成形体の全断面積に占める前記中心部の断
面積を、0.5%以上にすることができる。前記無機質
粒子として、平均粒径10μm以下の1次粒子を用いる
ことができる。なお、本発明において数値範囲の記載
は、両端値のみならず、その中に含まれる全ての任意の
中間値を含むものとする。
[0017] The cross-sectional area of the central portion with respect to the total cross-sectional area of the molded body in a direction perpendicular to the extrusion direction of the molded body can be 0.5% or more. Primary particles having an average particle size of 10 μm or less can be used as the inorganic particles. In the present invention, the description of the numerical range includes not only both end values, but also all arbitrary intermediate values included therein.

【0018】[0018]

【発明の実施の形態】〔マルチ型フィルター用支持体〕 [セラミックス多孔質焼結体]本発明のマルチ型フィル
ター用支持体におけるセラミックス多孔質焼結体は、無
機質粒子の押出成形体の焼結体であって押出方向に対し
て直角方向の断面の中心部を除く領域のみに流路を有す
るものである。ここで、押出方向に対して直角方向の断
面の中心部とは、前記断面の重心を含む領域のことであ
る。前記流路は、通常は前記押出方向に対して平行に設
けられている。
BEST MODE FOR CARRYING OUT THE INVENTION [Support for Multi-Type Filter] [Ceramic Porous Sintered Body] The ceramic porous sintered body in the support for a multi-type filter of the present invention is obtained by sintering an extruded body of inorganic particles. The body has a flow path only in a region excluding the center of a cross section perpendicular to the extrusion direction. Here, the central portion of the cross section in the direction perpendicular to the extrusion direction is a region including the center of gravity of the cross section. The flow path is usually provided in parallel with the extrusion direction.

【0019】前記セラミックス多孔質焼結体の押出方向
に対して直角方向における、前記セラミックス多孔質焼
結体の全断面積(流路の断面の面積を含む)に占める前
記中心部の断面積は、好ましくは0.5%以上(より好
ましくは1.0〜20%、さらに好ましくは3.0〜1
5%)にする。
The cross-sectional area of the central portion occupying the total cross-sectional area (including the cross-sectional area of the flow path) of the ceramic porous sintered body in a direction perpendicular to the extrusion direction of the ceramic porous sintered body is , Preferably 0.5% or more (more preferably 1.0 to 20%, further preferably 3.0 to 1%).
5%).

【0020】前記セラミックス多孔質焼結体は、好まし
くは、平均粒径10μm以下(より好ましくは0.1〜
5μm、さらに好ましくは0.2〜3μm)の1次粒子
の焼結体にする。前記セラミックス多孔質焼結体は、好
ましくはアルミナを含有する無機質粒子の焼結体にす
る。
The ceramic porous sintered body preferably has an average particle size of 10 μm or less (more preferably 0.1 to 10 μm).
5 μm, more preferably 0.2 to 3 μm). The ceramic porous sintered body is preferably a sintered body of inorganic particles containing alumina.

【0021】前記流路の径は、例えば0.5〜10mm
にすることができ、好ましくは1〜5mm(より好まし
くは2〜4mm)にすることができる。前記セラミック
ス多孔質焼結体の体積(前記流路の体積を含む):前記
流路の体積の比は、例えば90〜60:10〜40にす
ることができ、好ましくは80〜63:20〜37(よ
り好ましくは75〜65:25〜35、さらに好ましく
は72〜68:28〜32)にすることができる。
The diameter of the flow path is, for example, 0.5 to 10 mm.
And preferably 1-5 mm (more preferably 2-4 mm). The ratio of the volume of the ceramic porous sintered body (including the volume of the flow path) to the volume of the flow path can be, for example, 90 to 60:10 to 40, and preferably 80 to 63:20. 37 (more preferably 75-65: 25-35, even more preferably 72-68: 28-32).

【0022】前記セラミックス多孔質焼結体の細孔率
(セラミックス多孔質焼結体において細孔が占める体
積、但し、流路の体積を除く)は、例えば25〜60体
積%にすることができ、好ましくは30〜50体積%
(より好ましくは35〜45体積%、さらに好ましくは
38〜42体積%)にすることができる。
The porosity of the ceramic porous sintered body (the volume occupied by the pores in the ceramic porous sintered body, excluding the volume of the flow path) can be, for example, 25 to 60% by volume. , Preferably 30 to 50% by volume
(More preferably 35 to 45% by volume, still more preferably 38 to 42% by volume).

【0023】マルチ型フィルター用支持体の「マルチ
型」とは、一般的には「長尺方向に平行な流路を複数持
った蓮根状の形」のことを指す。本発明のマルチ型フィ
ルター用支持体におけるセラミックス多孔質焼結体は、
好ましくはマルチ型にすることができるが、流路方向の
長さが、前記流路方向に対して直角方向の長さ以上のも
のだけでなく、前記流路方向に対して直角方向の長さよ
りも短いものも含まれるものとする。
The "multi-type" of the multi-type filter support generally means "a lotus root-like shape having a plurality of flow paths parallel to the longitudinal direction". Ceramic porous sintered body in the support for a multi-type filter of the present invention,
Preferably, it can be a multi-type, but the length in the flow direction is not only the length in the direction perpendicular to the flow direction or more, but also the length in the direction perpendicular to the flow direction. As well as short ones.

【0024】前記セラミックス多孔質焼結体における流
路の数は、必要に応じて任意の数に設定することがで
き、例えば数個〜100個程度にすることができる。セ
ラミックス多孔質焼結体における流路の径方向の断面の
形状は、必要に応じて任意の形状に設定することができ
るが、典型的には円形である。流路の径方向の断面の形
状が正方形等の多角形でかつ流路を隔てる隔壁の厚さが
均等である形状の場合は「ハニカム型」と呼ばれること
が多い。本発明のマルチ型フィルター用支持体における
セラミックス多孔質焼結体の形状は、このような「ハニ
カム型」にすることができる。
The number of channels in the ceramic porous sintered body can be set to an arbitrary number as required, and can be, for example, about several to about 100. The shape of the cross section in the radial direction of the flow path in the ceramic porous sintered body can be set to any shape as necessary, but is typically circular. When the cross section in the radial direction of the flow path is a polygon such as a square and the thickness of the partition wall separating the flow path is uniform, it is often called “honeycomb type”. The shape of the ceramic porous sintered body in the support for a multi-type filter of the present invention can be such a “honeycomb type”.

【0025】本発明のマルチ型フィルター用支持体は、
前記セラミックス多孔質焼結体と共に、前記セラミック
ス多孔質焼結体を保護ないし補強するための保護部ない
し補強部、あるいは濾過層を形成するための中間層を有
することができる。前記保護部ないし補強部あるいは前
記中間層の材質は、例えば、セラミックス、金属等にす
ることができる。
The support for a multi-type filter of the present invention comprises:
Along with the ceramic porous sintered body, the ceramic porous sintered body may include a protective portion or a reinforcing portion for protecting or reinforcing the ceramic porous sintered body, or an intermediate layer for forming a filtration layer. The material of the protection portion or the reinforcement portion or the intermediate layer can be, for example, ceramics, metal, or the like.

【0026】前記保護部ないし補強部あるいは前記中間
層の前記セラミックスは、多孔質セラミックスにするこ
とができ、好ましくは、支持体を形成する無機質粒子の
粒子径よりも小さい無機質粒子で形成されたセラミック
ス(特に、多孔質セラミックス)であり、前記多孔質セ
ラミックスは、支持体が気孔を有する場合は当該気孔の
径よりも小さい径の気孔を有する多孔質セラミックスに
することができる。
The ceramic of the protective portion or the reinforcing portion or the intermediate layer may be a porous ceramic, preferably a ceramic formed of inorganic particles smaller than the particle size of the inorganic particles forming the support. (Especially, porous ceramics). When the support has pores, the porous ceramics may be porous ceramics having pores smaller in diameter than the pores.

【0027】前記保護部ないし補強部あるいは前記中間
層は、例えば、前記セラミックス多孔質焼結体の表面を
被覆するように層状に設けることができ、あるいは、前
記セラミックス多孔質焼結体のエッジ部に前記エッジ部
を被覆するように設けることができる。
The protective portion, the reinforcing portion, or the intermediate layer may be provided in a layer shape so as to cover the surface of the ceramic porous sintered body, or may be provided at the edge portion of the ceramic porous sintered body. To cover the edge portion.

【0028】〔マルチ型フィルター用支持体の製造方
法〕本発明のマルチ型フィルター用支持体の製造方法で
は、押出方向に対して直角方向の断面の中心部を除く領
域のみに孔を有する無機質粒子の成形体を焼成する焼成
工程を含む。前記焼成工程の前には、前記特定の無機質
粒子の成形体の原料の坏土を製造する坏土製造工程、前
記坏土製造工程で得られた坏土を用いて前記特定の無機
質粒子の成形体を成形する成形工程を設けることができ
る。
[Method for Producing Multi-Type Filter Support] In the method for producing a multi-type filter support of the present invention, the inorganic particles having pores only in a region excluding the center of the cross section perpendicular to the extrusion direction. And a baking step of baking the molded body. Prior to the firing step, a kneaded clay manufacturing step of manufacturing a kneaded clay of a raw material of the molded body of the specific inorganic particle, and molding of the specific inorganic particle using the kneaded clay obtained in the kneaded clay manufacturing step A molding step for molding the body can be provided.

【0029】[坏土製造工程]坏土は、主成分である無
機質粒子と、前記無機質粒子を成形するための結合剤で
ある有機質バインダーと、押出成形を容易に行うための
滑剤等の各種添加剤を混合して製造することができる。
[Knead clay manufacturing process] The kneaded clay includes various additions of inorganic particles as a main component, an organic binder as a binder for forming the inorganic particles, and a lubricant for facilitating extrusion molding. It can be manufactured by mixing agents.

【0030】坏土の主成分となる無機質粒子としては、
好ましくはアルミナを用いることができる。前記無機質
粒子として、好ましくは、平均粒径10μm以下(より
好ましくは1〜5μm、さらに好ましくは2〜4μm
)の1次粒子である無機質粒子を用いる。
The inorganic particles that are the main components of the clay include:
Preferably, alumina can be used. The inorganic particles preferably have an average particle size of 10 μm or less (more preferably 1 to 5 μm, and still more preferably 2 to 4 μm).
Inorganic particles, which are the primary particles, are used.

【0031】本発明の効果は、平均粒径が10μm以下
の無機質粒子を用いた場合に顕著になる。即ち、平均粒
径が10μmを越える場合には、その無機質粒子(原料
粉末)の粒子間隙間が十分に大きいことから、前記隙間
にバインダーや滑剤が充填されることとなり、ダイの中
心部のピンや支持部を取り除かなくとも成形時における
坏土の流れは十分スムーズであり、所望の形状の成形体
が得られる。
The effect of the present invention is remarkable when inorganic particles having an average particle size of 10 μm or less are used. That is, when the average particle size exceeds 10 μm, the gap between the inorganic particles (raw material powder) is sufficiently large, so that the gap is filled with a binder or a lubricant, and the pin at the center of the die is formed. The flow of the clay at the time of molding is sufficiently smooth without removing the support and the supporting portion, and a molded body having a desired shape can be obtained.

【0032】坏土における無機質粒子の重量:無機質粒
子を成形するための結合剤の重量:押出成形を容易に行
うための添加剤の重量の比は、好ましくは97〜80:
1〜7:2〜13(より好ましくは95〜82:2〜
6:3〜12、さらに好ましくは90〜88:3〜4:
7〜8)にする。
The ratio of the weight of the inorganic particles in the kneaded clay: the weight of the binder for forming the inorganic particles: the weight of the additive for facilitating the extrusion molding is preferably from 97 to 80:
1-7: 2-13 (more preferably 95-82: 2-
6: 3 to 12, more preferably 90 to 88: 3 to 4:
7-8).

【0033】[成形工程]成形工程は、前記坏土製造工
程で得られた坏土を用いて本発明の製造方法で特定する
無機質粒子の成形体、即ち、押出方向に対して直角方向
の断面の中心部を除く領域のみに孔(マルチ型フィルタ
ー用支持体における流路に対応する孔)を有する無機質
粒子の成形体を押出成形する成形工程である。ここで、
押出方向に対して直角方向の断面の中心部とは、前記断
面の重心を含む領域のことである。前記孔は、通常は前
記成形体の押出方向に対して平行に設けられている。
[Molding Step] The forming step is performed by using the kneaded clay obtained in the above-mentioned kneaded clay manufacturing step to form a formed body of inorganic particles specified by the manufacturing method of the present invention, that is, a cross section perpendicular to the extrusion direction. This is a molding step of extruding a molded body of inorganic particles having holes (holes corresponding to the flow path in the support for a multi-type filter) only in the region excluding the central part of the above. here,
The center of the cross section perpendicular to the extrusion direction is a region including the center of gravity of the cross section. The hole is usually provided in parallel with the extrusion direction of the molded body.

【0034】前記無機質粒子の成形体は、前記成形体の
中心部に孔を形成しない形状のダイ(例えば、前記成形
体の中心部に対応する部分に孔形成用のピンを具備しな
いダイ)を用いて押出成形して得ることができる。
[0034] The molded body of the inorganic particles includes a die having no hole at the center of the molded body (for example, a die having no pin for forming a hole at a portion corresponding to the center of the molded body). And can be obtained by extrusion molding.

【0035】前記成形体の押出方向に対して直角方向に
おける、前記成形体の全断面積(孔の断面の面積を含
む)に占める前記中心部の断面積は、好ましくは、0.
5%以上(より好ましくは1.0〜20%、さらに好ま
しくは3.0〜15%)にする。
The cross-sectional area of the central portion occupying the total cross-sectional area (including the cross-sectional area of the hole) in the direction perpendicular to the extrusion direction of the molded body is preferably 0.1 mm.
5% or more (more preferably 1.0 to 20%, further preferably 3.0 to 15%).

【0036】前記孔の径は、例えば0.5〜10mmに
することができ、好ましくは1〜5mm(より好ましく
は2〜4mm)にすることができる。前記成形体の体積
(前記孔の体積を含む):前記孔の体積の比は、例えば
90〜60:10〜40にすることができ、好ましくは
80〜63:20〜37(より好ましくは75〜65:
25〜35)にすることができる。
The diameter of the hole can be, for example, 0.5 to 10 mm, preferably 1 to 5 mm (more preferably, 2 to 4 mm). The ratio of the volume of the molded body (including the volume of the hole) to the volume of the hole can be, for example, 90 to 60:10 to 40, preferably 80 to 63:20 to 37 (more preferably 75 to 60:37). ~ 65:
25 to 35).

【0037】[焼成工程]本発明の製造方法における焼
成工程では、押出方向に対して直角方向の断面の中心部
を除く領域のみに孔を有する無機質粒子の成形体を焼成
する。焼成温度及び焼成時間は、使用する材料にもよる
が、例えば1000〜1800℃で、1〜4時間行うこ
とができる。
[Firing Step] In the firing step in the production method of the present invention, a formed body of inorganic particles having holes only in a region excluding the center of the cross section perpendicular to the extrusion direction is fired. The firing temperature and the firing time depend on the material used, but can be, for example, 1000 to 1800 ° C. for 1 to 4 hours.

【0038】機質粒子としてアルミナ粒子を用いた場合
は、好ましくは1200〜1800℃(より好ましくは
1300〜1700℃、さらに好ましくは1400〜1
600℃)で、好ましくは0.5〜5時間(より好まし
くは1〜4時間、さらに好ましくは2〜3時間)行うこ
とができる。
When alumina particles are used as the material particles, they are preferably from 1200 to 1800 ° C. (more preferably from 1300 to 1700 ° C., further preferably from 1400 to 1800 ° C.).
(600 ° C.), preferably for 0.5 to 5 hours (more preferably for 1 to 4 hours, more preferably for 2 to 3 hours).

【0039】[0039]

【実施列】以下、本発明の実施例を図面を参照して説明
する。なお、図面において各部の寸法比等は図示の都合
上、実際の寸法比と必ずしも完全には一致しない。
Embodiments of the present invention will be described below with reference to the drawings. In the drawings, the dimensional ratios and the like of each part do not always completely match the actual dimensional ratios for the sake of illustration.

【0040】[実施例]まず、主成分としての純度99
%、平均粒径3μmのアルミナ粒子(AL−45−H、
昭和電工製)89重量部、助剤としての有機バインダー
(メトロース 60SH−4000、信越化学工業製)
3.5重量部、滑剤(ユニルーブ、日本油脂製)4重量
部、ワックス(マクセロンM、中京油脂製)3.5重量部
とを、双腕式ニーダーを用いて混合して坏土(グリーン
体)を得た。
[Example] First, purity 99 as a main component
%, Alumina particles having an average particle size of 3 μm (AL-45-H,
89 parts by weight, organic binder as auxiliary agent
(Metroose 60SH-4000, manufactured by Shin-Etsu Chemical Co., Ltd.)
3.5 parts by weight, 4 parts by weight of a lubricant (Unilube, manufactured by Nippon Yushi) and 3.5 parts by weight of wax (Maxelon M, manufactured by Chukyo Yushi) are mixed using a double-arm kneader to form a clay (green body). ) Got.

【0041】次に真空押出成形機を用いて前記杯土の成
形を行い中心部(押出方向に対して直角方向の断面の中
心部)に流路のない生成形体を作成した。この成形体を
得る際に用いたダイの支持部1及びピン2の配置を図1
に示す。成形体に貫通孔(マルチ型フィルター用支持体
における流路に対応する貫通孔)を形成する為に、図1
にはピン2が同心円上に配設されているが、このピンを
支える支持部及びピンがダイの支持部の中心部(成形体
の前記中心部に対応)には無い。このようにダイ中央部
を取り除くことにより、坏土の流れを良くし、真空押出
成形機のスクリューによって押し出されてきた坏土がダ
イ中心部においてもスムーズに流れることとなり、成形
体の成形性を高めることができ、所望の形状の生成形体
を得ることができる。
Next, the potting material was formed using a vacuum extruder to produce a formed body having no flow path at the center (the center of the cross section perpendicular to the extrusion direction). FIG. 1 shows the arrangement of the support portion 1 and the pin 2 of the die used to obtain this molded product.
Shown in In order to form a through-hole (a through-hole corresponding to the flow path in the support for the multi-type filter) in the molded body, FIG.
Has a pin 2 disposed concentrically, but the supporting portion for supporting the pin and the pin are not located at the center of the supporting portion of the die (corresponding to the center of the molded body). By removing the center of the die in this way, the flow of the kneaded clay is improved, and the kneaded clay extruded by the screw of the vacuum extrusion molding machine flows smoothly even in the center of the die, and the formability of the formed body is improved. Can be increased to obtain a desired shape of the formed form.

【0042】そして得られた生成形体を電気炉にて14
50℃で2時間焼成し、図2に示す外径30mm、長さ
500mmその内部に内径2mmの流路20を90本有
した、アルミナ多孔質焼結体21を得た。前記90本の
流路は、成形体の押出方向(前記焼結体21の長手方
向)に対して直角方向の断面の中心部22を除く領域の
みに形成されている。
Then, the obtained shaped body was placed in an electric furnace for 14 hours.
It was fired at 50 ° C. for 2 hours to obtain a porous alumina sintered body 21 having 90 channels 20 having an outer diameter of 30 mm, a length of 500 mm and an inner diameter of 2 mm as shown in FIG. The 90 channels are formed only in the region excluding the central portion 22 in the cross section perpendicular to the extrusion direction of the molded body (the longitudinal direction of the sintered body 21).

【0043】このアルミナ多孔質焼結体をその長手方向
に50mm間隔に10等分に切断し、その切断面9個所
における亀裂や割れ等の欠陥の有無を調べた。その結
果、いずれの断面にも欠陥は全くなかった。即ち、欠陥
数は0であり、欠陥のある断面の数は0であった。前記
中心部22に流路を設けない形状を採用したことによ
り、欠陥の全くない多数の流路を持ったアルミナ多孔質
焼結体を得ることができた。
This alumina porous sintered body was cut into 10 equal parts in the longitudinal direction at 50 mm intervals, and the presence or absence of defects such as cracks and cracks at nine cut surfaces was examined. As a result, no defect was found in any of the cross sections. That is, the number of defects was 0, and the number of cross sections having a defect was 0. By adopting a shape in which no flow path is provided in the central portion 22, an alumina porous sintered body having many flow paths without any defect could be obtained.

【0044】[比較例]図3に示すようにピン32を配
置したダイの支持部31を用いた従来の成形方法を用い
て成形体を得た。なお、成形に用いた坏土は、実施例の
ものと同様のものを用いてある。上記実施例に対して、
この比較例(従来の製造方法)では、図3のダイの支持
部およびピンの配置に示すように、微細粉末体(平均粒
径3μmのアルミナ粒子)を含有する坏土がダイ中央部
においてもスムーズに移動する手段を講じていないた
め、ダイから受ける応力の影響を大きく受けることとな
り、得られた成形体の中央部にて割れや亀裂等の欠陥を
生じることとなった。
Comparative Example As shown in FIG. 3, a molded product was obtained by a conventional molding method using the support portion 31 of the die on which the pins 32 were arranged. The kneaded material used for the molding was the same as that of the example. For the above embodiment,
In this comparative example (conventional manufacturing method), as shown in the arrangement of the support portion and the pins of the die in FIG. 3, the clay containing the fine powder (alumina particles having an average particle size of 3 μm) is also formed in the center of the die. Since no means for moving smoothly was taken, it was greatly affected by the stress received from the die, and defects such as cracks and cracks occurred in the center of the obtained molded body.

【0045】上記実施例と同一組成の坏土を用いて成形
されると共に91個の流路を持った生成形体を電気炉に
て1450℃で2時間焼成し、図4に示す外径30m
m、長さ500mm、その内部に内径2mmの流路4
0、42を91本有した、アルミナ多孔質焼結体41を
得た。この焼結体は、成形時の押出方向(前記焼結体4
1の長手方向)に対して直角方向の断面の中心部に流路
42を形成している。
A molded body formed using a clay having the same composition as that of the above embodiment and having 91 channels was fired in an electric furnace at 1450 ° C. for 2 hours, and the outer diameter shown in FIG.
m, length 500 mm, flow path 4 having an inner diameter of 2 mm inside thereof
An alumina porous sintered body 41 having 91 pieces of 0 and 42 was obtained. This sintered body is extruded in the extrusion direction during molding (the sintered body 4).
The flow path 42 is formed at the center of the cross section in the direction perpendicular to the (longitudinal direction of one).

【0046】前記焼結体41について上記実施例と同様
にその長手方向に50mm間隔に10等分に切断し、そ
の切断面9個所における亀裂や割れ等の欠陥の有無を調
べた。その結果、欠陥数は21であり、欠陥のある断面
の数は8であった。前記中心部に流路42を設ける形状
としたために、前記中心部の流路を形成するためのピン
や支持部から大きな応力を受けることとなり、アルミナ
多孔質焼結体の前記中心部(中心部の隔壁)には多くの
欠陥が生じることとなった。
The sintered body 41 was cut into 10 equal parts in the longitudinal direction at intervals of 50 mm in the same manner as in the above embodiment, and nine cut surfaces were examined for the presence of defects such as cracks and cracks. As a result, the number of defects was 21, and the number of defective cross sections was 8. Since the flow path 42 is provided in the central portion, a large stress is applied from a pin or a support portion for forming the flow path in the central portion, and the central portion (central portion) of the alumina porous sintered body is received. Partition wall) has many defects.

【0047】[0047]

【発明の効果】請求項1〜3のマルチ型フィルター用支
持体は、無機質粒子の押出成形体の焼結体であって押出
方向に対して直角方向の断面の中心部を除く領域のみに
流路を有するセラミックス多孔質焼結体を含むので、次
の基本的効果を奏することができる。
The support for a multi-type filter according to any one of claims 1 to 3 is a sintered body of an extruded body of inorganic particles and flows only in a region excluding a central portion of a cross section perpendicular to the extrusion direction. Since the ceramic porous sintered body having the passage is included, the following basic effects can be obtained.

【0048】微小粒子を用いて押出成形する場合であっ
ても所望の形状に容易に押出成形し焼結して製造するこ
とができる。また、押出方向に対して直角方向の断面の
中心部にキレ、ワレ等の欠陥がないように製造すること
ができる。
Even in the case of extrusion molding using fine particles, it can be easily extruded into a desired shape and sintered. Further, it can be manufactured such that there is no defect such as cracks or cracks in the center of the cross section perpendicular to the extrusion direction.

【0049】請求項2〜3のマルチ型フィルター用支持
体は、前記それぞれの請求項に記載の構成をさらに具備
するので、上記基本的効果がより一層顕著である。
Since the multi-type filter supports of claims 2 and 3 are further provided with the constitutions described in the respective claims, the above-mentioned basic effects are more remarkable.

【0050】請求項4〜6のマルチ型フィルター用支持
体の製造方法は、押出方向に対して直角方向の断面の中
心部を除く領域のみに孔を有する無機質粒子の成形体を
焼成する焼成工程を含むので、次の基本的効果を奏する
ことができる。
The method of manufacturing a support for a multi-type filter according to claims 4 to 6, wherein the firing step of firing the inorganic particle compact having pores only in a region except for a central portion of a cross section perpendicular to the extrusion direction. Therefore, the following basic effects can be obtained.

【0051】微小粒子を用いて押出成形する場合であっ
ても所望の形状に容易に押出成形し焼結してマルチ型フ
ィルター用支持体を製造することができる。また、押出
方向に対して直角方向の断面の中心部にキレ、ワレ等の
欠陥がないマルチ型フィルター用支持体を製造すること
ができる。
Even in the case of extrusion molding using fine particles, it can be easily extruded into a desired shape and sintered to produce a multi-type filter support. In addition, it is possible to manufacture a support for a multi-type filter having no defects such as cracks and cracks at the center of a cross section perpendicular to the extrusion direction.

【0052】請求項5〜6のマルチ型フィルター用支持
体の製造方法は、前記それぞれの請求項に記載の構成を
さらに具備するので、上記基本的効果がより一層顕著で
ある。
The method for manufacturing a support for a multi-type filter according to claims 5 to 6 further includes the constitution described in each of the above claims, so that the above-mentioned basic effects are further remarkable.

【図面の簡単な説明】[Brief description of the drawings]

【図1】図1は、実施例の成形体を得る際に用いたダイ
の支持部及びピンの配置を示す図(ピンの先端部がわか
ら視た図)である。
FIG. 1 is a view showing the arrangement of a die supporting portion and pins used for obtaining a molded article of an example (a view in which a tip of a pin is seen).

【図2】図2は、実施例のアルミナ多孔質焼結体の斜視
図である。
FIG. 2 is a perspective view of an alumina porous sintered body of an example.

【図3】図3は、比較例の成形体を得る際に用いたダイ
の支持部及びピンの配置を示す図(ピンの先端部がわか
ら視た図)である。
FIG. 3 is a diagram showing the arrangement of pins and pins of a die used for obtaining a molded body of a comparative example (a view in which the tip of the pin is seen).

【図4】図4は、比較例のアルミナ多孔質焼結体の斜視
図である。
FIG. 4 is a perspective view of a porous alumina sintered body of a comparative example.

Claims (6)

【特許請求の範囲】[Claims] 【請求項1】無機質粒子の押出成形体の焼結体であって
押出方向に対して直角方向の断面の中心部を除く領域の
みに流路を有するセラミックス多孔質焼結体を含むこと
を特徴とするマルチ型フィルター用支持体。
1. A sintered body of an extruded body of inorganic particles, comprising a ceramic porous sintered body having a flow path only in a region excluding a central portion of a cross section perpendicular to an extrusion direction. Support for a multi-type filter.
【請求項2】前記セラミックス多孔質焼結体の押出方向
に対して直角方向における、前記セラミックス多孔質焼
結体の全断面積に占める前記中心部の断面積は、0.5
%以上であることを特徴とする請求項1に記載のマルチ
型フィルター用支持体。
2. A cross-sectional area of the central portion of the cross-sectional area of the ceramic porous sintered body in a direction perpendicular to an extrusion direction of the ceramic porous sintered body is 0.5%.
% Or more, the support for a multi-type filter according to claim 1.
【請求項3】前記セラミックス多孔質焼結体は、平均粒
径10μm以下の1次粒子の焼結体であることを特徴と
する請求項1〜2のいずれかに記載のマルチ型フィルタ
ー用支持体。
3. The support for a multi-type filter according to claim 1, wherein the ceramic porous sintered body is a sintered body of primary particles having an average particle diameter of 10 μm or less. body.
【請求項4】押出方向に対して直角方向の断面の中心部
を除く領域のみに孔を有する無機質粒子の成形体を焼成
する焼成工程を含むことを特徴とするマルチ型フィルタ
ー用支持体の製造方法。
4. A method for producing a support for a multi-type filter, comprising a firing step of firing a formed body of inorganic particles having holes only in a region excluding a central portion of a cross section perpendicular to the extrusion direction. Method.
【請求項5】前記成形体の押出方向に対して直角方向に
おける、前記成形体の全断面積に占める前記中心部の断
面積を、0.5%以上にすることを特徴とする請求項4
に記載のマルチ型フィルター用支持体の製造方法。
5. A cross-sectional area of said central portion with respect to a total cross-sectional area of said molded body in a direction perpendicular to an extrusion direction of said molded body is set to 0.5% or more.
3. The method for producing a support for a multi-type filter according to item 1.
【請求項6】前記無機質粒子として、平均粒径10μm
以下の1次粒子である無機質粒子を用いることを特徴と
する請求項4〜5のいずれかに記載のマルチ型フィルタ
ー用支持体の製造方法。
6. The inorganic particles have an average particle size of 10 μm.
The method for producing a support for a multi-type filter according to any one of claims 4 to 5, wherein inorganic particles that are the following primary particles are used.
JP15447298A 1998-06-03 1998-06-03 Support for multi-type filter and method for producing the same Withdrawn JPH11347324A (en)