JPS58190824A - Treatment of precipitate containing mercury - Google Patents

Treatment of precipitate containing mercury

Info

Publication number
JPS58190824A
JPS58190824A JP57072803A JP7280382A JPS58190824A JP S58190824 A JPS58190824 A JP S58190824A JP 57072803 A JP57072803 A JP 57072803A JP 7280382 A JP7280382 A JP 7280382A JP S58190824 A JPS58190824 A JP S58190824A
Authority
JP
Japan
Prior art keywords
mercury
flotation
precipitate
leaching
solution
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP57072803A
Other languages
Japanese (ja)
Other versions
JPH0236529B2 (en
Inventor
Toshiaki Yamauchi
山内 利秋
Masashi Hashimoto
橋本 昌司
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dowa Holdings Co Ltd
Original Assignee
Dowa Mining Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dowa Mining Co Ltd filed Critical Dowa Mining Co Ltd
Priority to JP57072803A priority Critical patent/JPS58190824A/en
Publication of JPS58190824A publication Critical patent/JPS58190824A/en
Publication of JPH0236529B2 publication Critical patent/JPH0236529B2/ja
Granted legal-status Critical Current

Abstract

PURPOSE:To concentrate mercury contained in a precipitate to a high grade in a high yield and to easily separate and recover it, by subjecting the precipitate to preliminary leaching and by concentrating the mercury in floated ore by conventional flotation. CONSTITUTION:A precipitate contg. low grade mercury is subjected to primary leaching in a soln. contg. an oxidizing agent or a ferrous sulfate soln. After carrying out solid-liq. separation as required, flotation is applied to concentrate the mercury in floated ore. The mercury compounds in the precipitate contg. mercury are easily separated by flotation by subjecting the precipitate to the primary leaching.

Description

【発明の詳細な説明】 本発明は含水銅殿物から水銀を分離回収する方法に関す
るもので、含水銅殿物をあらかじめ予備浸出を行なった
後に通常の浮遊選鉱により水銀を浮鉱中に濃縮させて分
離回収するものである。
DETAILED DESCRIPTION OF THE INVENTION The present invention relates to a method for separating and recovering mercury from hydrated copper precipitate, in which mercury is concentrated in floating ore by normal flotation after preliminary leaching of hydrated copper precipitate. The waste is separated and collected.

一般に銅、亜鉛、鉛等の非鉄金属製錬における一/− 原料鉱石は主として硫化鉱であり、その産出地域により
多少の違いはあるもほとんどの鉱石中には微量の水銀が
随伴している。この水銀は焙焼又は溶錬工程においてS
、5etPb等と共にメタリック又は酸化物の状態でガ
ス又はフユ〜ムとして揮発し、ガス処理の第1段階であ
るガス冷却洗浄工程においてダストと共に捕収され、含
水銅殿物として系外へ抜き出されている。
In general, the raw material ore used in the smelting of non-ferrous metals such as copper, zinc, and lead is mainly sulfide ore, and although there are some differences depending on the region where it is produced, most ores contain trace amounts of mercury. This mercury is S during the roasting or smelting process.
, 5etPb, etc., in the form of a metallic or oxide gas or fume, and is collected together with dust in the gas cooling and cleaning step, which is the first stage of gas treatment, and is extracted from the system as a hydrated copper precipitate. ing.

この穀物中の水銀含有率が高い場合には、例えば該穀物
を加熱処理して発生する水銀蒸気を冷却して粗水銀とし
、更に真空蒸留法で精製する公知の方法によって水銀を
回収することができるが、水銀含有率が低い場合(例え
ば7%以下)やAl+ Cu + P b g S e
等の有価金属成分を多く含む場合には、直接かような方
法で水銀回収を実施することは単に経済的見地だけでは
なく環境対策の面からも適切でない。
If the mercury content in this grain is high, it is possible to recover the mercury by a known method, for example, by heating the grain and cooling the mercury vapor generated to obtain crude mercury, and then refining it by vacuum distillation. However, if the mercury content is low (e.g. 7% or less) or Al + Cu + P b g S e
When mercury contains a large amount of valuable metal components such as mercury, it is not appropriate to directly recover mercury using such a method, not only from an economic standpoint but also from an environmental standpoint.

かかる低品位水銀含有物中の水銀を濃縮させる方法とし
て、浮遊選鉱を直接適用することも試みられているが、
水銀の浮遊性が悪く、歩留りゃ製品品位が低くて適切な
方法とは言えず、未だ工業的規模で実施し得るような方
法はないのが実情である。この浮遊性の悪い理由は、穀
物中の水銀の形態がメタリック或いはHgSの如く共存
するS、Cu 、 Seなどと結合して(Hg−Cu)
x・(S−8e)y のような複雑な化合物を形成して
いるためと考えられる。
Direct application of flotation has been attempted as a method of concentrating mercury in such low-grade mercury-containing materials;
The mercury has poor buoyancy and the yield and product quality are low, making this method unsuitable, and the reality is that there is still no method that can be implemented on an industrial scale. The reason for this poor buoyancy is that the form of mercury in grains is metallic or combined with coexisting S, Cu, Se, etc., such as HgS (Hg-Cu).
This is thought to be due to the formation of a complex compound such as x·(S-8e)y.

そこで、本発明者等は上記のような低品位水銀含有穀物
から水銀を回収すべく研究・検討した結果、含水銅殿物
を浮遊選鉱法で水銀を濃縮回収するに先立って、酸化剤
を含む溶液或いは硫酸第1鉄溶液で予備浸出した後、直
接あるいは固液分離後に浮選すると、浮鉱中に水銀が極
めて良好に濃縮されるという知見を得た。
Therefore, as a result of research and consideration to recover mercury from the above-mentioned low-grade mercury-containing grains, the present inventors discovered that prior to concentrating and recovering mercury from the hydrated copper precipitate using the flotation method, it was found that It has been found that mercury can be very well concentrated in the floating ore by flotation either directly or after solid-liquid separation after preliminary leaching with a solution or ferrous sulfate solution.

これは、浮選の前処理として含酸止剤溶液又は硫酸第1
鉄溶液で予備浸出を行なうと、前記のような複雑な形態
の水銀化合物が分解され、比較的単純な形態の水銀化合
物となって浮選分離が容易になるためであると推測され
る。
This can be used as a pre-treatment for flotation using an acid-containing anti-acid solution or sulfuric acid
It is presumed that this is because pre-leaching with an iron solution decomposes the complex forms of mercury compounds as described above, converting them into relatively simple forms of mercury compounds, making flotation separation easier.

予備浸出溶液として使用する酸化剤は硫酸第2鉄をはじ
め過酸化水素、C,t2又はCt化合物、過マンガン酸
塩、硝酸又は硝酸塩等が適用される。
As the oxidizing agent used as the preliminary leaching solution, ferric sulfate, hydrogen peroxide, C, t2 or Ct compounds, permanganate, nitric acid or nitrates, etc. are used.

以下、本発明の実施例を比較例と共に説明する。Examples of the present invention will be described below along with comparative examples.

なお、ここに使用した供試試料はCu、 Pb 、Zn
、F6等の硫化精鉱の焙焼又は溶錬により発生した含水
銀802ガスを湿式で冷却洗浄する際に発生した含水銅
殿物である。
The test samples used here were Cu, Pb, and Zn.
This is a hydrated copper precipitate generated during wet cooling and cleaning of hydrated silver 802 gas generated by roasting or smelting of sulfide concentrates such as , F6, etc.

比較例/ 含水銀穀物バルブをγ濾過後に水でリノクルプして、そ
のまま直接浮選を行なった結果を第1表に示す。
Comparative Example/Table 1 shows the results of mercury-containing grain bulbs being gamma-filtered, then linocruped with water, and then directly flotated.

浮選条件: plI 2.1.〜3.3; 、 温度3
0℃、ノクルブ濃度23%1時間 粗選75分。
Flotation conditions: plI 2.1. ~3.3; , temperature 3
0℃, Nokurubu concentration 23% 1 hour, rough selection 75 minutes.

精選j分 浮選剤 気泡剤]) OW 2 !; 0番(商品名)
≠0 ?/を 第  /  表 比較例λ 含水銀穀物パルプを濾過・リパルプ後そのまま温度り0
℃でψ時間加熱処理した後に直接浮選した結果を第2表
に示す。
Carefully selected flotation agent, foaming agent]) OW 2! ; No. 0 (product name)
≠0? /Table Comparative Example λ After filtration and repulping of mercury-containing grain pulp, the temperature is 0.
The results of direct flotation after heat treatment at °C for ψ hours are shown in Table 2.

浮選条件はpH0,9〜/、lI−でその他は比較例/
と同じである。
The flotation conditions were pH 0.9~/, lI-, and the rest were comparative examples/
is the same as

1− 第  2  表 比較例1と比較して改善が認められるが、水銀実収率が
低い。
1-Table 2 Improvement is observed compared to Comparative Example 1, but the actual mercury yield is low.

実施例/ 含水銀穀物バルブを涙過後、ケーキを硫酸第2鉄溶液で
予備酸化浸出した後に浮選した結果を第3表に示す。
Example/ After filtration of hydrated silver grain bulbs, the cake was pre-oxidized and leached with ferric sulfate solution followed by flotation. The results are shown in Table 3.

予備浸出条件二Fθ3+濃度、? j ?/l 、液温
9θ℃9時間弘時間、攪拌300r pm、パルプ濃度23〜30% 浮選条件: pH/J〜2.0.温度SO℃、パルプ濃
度23〜30%、その他は比較 例/に同じ。
Pre-leaching conditions 2 Fθ3+ concentration, ? j? flotation conditions: pH/J~2.0. Temperature SO°C, pulp concentration 23-30%, and other conditions were the same as in Comparative Example.

  − 第  3  表 実施例! 実施例/の予備浸出における硫酸第2鉄溶液のFe3+
濃度をs o y71に上げ、更に浮選時のpHを/、
/〜/、了にした場合の結果を第グ表に示す。
- Table 3 Examples! Fe3+ of ferric sulfate solution in preliminary leaching of Example/
The concentration was increased to so y71, and the pH during flotation was increased to /,
Table G shows the results when /~/ and END are selected.

第  ≠  表 実施例3 実施例/の予備浸出における硫酸第2鉄溶液のFea+
濃度を/ 00 fit−llにし、浮選時のpHを0
、り〜/、jにした場合の結果を第5表に示す。
Table ≠ Example 3 Fea+ of ferric sulfate solution in preliminary leaching of Example/
The concentration was set to /00 fit-ll, and the pH during flotation was set to 0.
Table 5 shows the results when , ri~/, j.

第  j  表 実施例/〜3で分るように硫酸第2鉄溶液中のFe3+
濃度が高い程、水銀の浮選効率が良くなっている。
Fe3+ in ferric sulfate solution as seen in Table j Example/~3
The higher the concentration, the better the flotation efficiency of mercury.

実施例≠ 含水銀穀物バルブをγ濾過後ケーキをH202溶液で予
備浸出した後に浮選した結果を第2表に示す。
Example ≠ Table 2 shows the results of flotation after gamma filtration of the mercury-containing grain bulb and pre-leaching the cake with H202 solution.

予備浸出条件: H2O2a度30cx、/ / I 
OOct、 。
Pre-leaching conditions: H2O2a degree 30cx, / / I
OOct, .

ケーキjOθノ、液温りOCで 弘時間、攪拌300rpm。Cake jOθノ, liquid temperature OC Hiro time, stirring 300 rpm.

パルプ濃度約、23% 浮選条件:pH3゜j、浮選時間 浮鉱/。2゜3とも
5分、その他は実施例/に同 じ。
Pulp concentration: approx. 23% Flotation conditions: pH 3゜J, flotation time Flotation/. 5 minutes for both 2° and 3, otherwise the same as Example/.

第  2  表 実施例j 各水銀獲物バルブをl濾過後ケーキをHNOs溶液で予
備浸出した後に浮選した結果を第7表に示す。
Table 2 Example j The results of flotation after pre-leaching the cake after filtration with HNOs solution for each mercury prey bulb are shown in Table 7.

予備浸出条件: HNOs濃度30cC//l00cc
。
Pre-leaching conditions: HNOs concentration 30cC//l00cc
.

ケーキ5ooy 、液温9θ℃で 弘時間、攪拌300rpm、パ ーター ルブ濃度約2≠% 浮選条件: pIT O,ll−〜O,S 、その他は
実施例弘に同じ。
Cake 5ooy, liquid temperature 9θ°C, time, stirring 300 rpm, Partalbe concentration about 2≠% Flotation conditions: pIT O,ll-~O,S, other conditions are the same as in Example Hiro.

第  7  表 実施例乙 含水銀穀物パルプを濾過後ケーキを硫酸第1鉄溶液で予
備浸出した後に浮選した結果を第g表に示す。
Table 7 Example B The mercury-containing grain pulp was filtered and the cake was pre-leached with a ferrous sulfate solution and then flotated. The results are shown in Table g.

予備浸出条件: P e 804 q 71−120濃
度り00f//どOO匡水、ケーキ5ooy 。
Pre-leaching conditions: P e 804 q 71-120 concentration 00 f//do oo water, cake 5 ooy.

液温り0℃で弘時間、攪拌30 0rpm、パルプ濃度約23% //)− 浮選条件:pII2゜3〜2.夕、その他は実施例tに
同じ。
Liquid temperature: 0°C, stirring time: 300 rpm, pulp concentration: approximately 23% //) - Flotation conditions: pII2°3-2. The evening and other details were the same as in Example t.

第  K  表 以上の実施例からも判るように、硫酸第2鉄その他の酸
化剤溶液又は硫酸第1鉄溶液により予備浸出を行なう本
発明法によれば、浮選効率が著しく向」ニジ、低品位水
銀含有穀物から水銀を浮鉱として高実収率で浮選分離回
収することができる。
As can be seen from the examples shown in Table K, the flotation efficiency is significantly improved by the method of the present invention in which preliminary leaching is performed with a solution of ferric sulfate or other oxidizing agent or a solution of ferrous sulfate. Mercury can be separated and recovered as floating ore from high-grade mercury-containing grains at a high yield.

なお、酸化剤として硫酸第2鉄、過酸化水素、硝酸のほ
か、過マンガン酸塩、Ct塩、その他の硝酸塩を使用し
た場合にも同様の傾向を示したことを付言しておく。
It should be added that similar trends were observed when ferric sulfate, hydrogen peroxide, nitric acid, permanganate, Ct salt, and other nitrates were used as oxidizing agents.

手  続  補  正  書 (自発 ン昭和 57年
 5月29日 L 事件の表示 特願昭37−7:2ど03号 2 発明の名称 含水銀穀物の処理方法 a 補正をする者 事件との関係    偶゛許lB願人 氏名(名称)  IEJ和鉱業株式会社表代理人 住所 東京都千代田区神田淡路町λ丁目≠番地明細書の
[発明の詳細な説明]の欄 6 補正の内容 明細書3 F’4を行目に「の如く共存する」とあるを
[の如く単純な形態ではなく、共存する」と補正する。
Procedural Amendment (Spontaneous, May 29, 1980) Indication of Case Patent Application No. 2-03, 1977-7 Title of Invention Method for Processing Mercury-Containing Grains a Person Making Amendment Relationship to Case Incident Applicant's name (Name) IEJ Wa Mining Co., Ltd. Representative agent address λ-chome, Kanda-Awaji-cho, Chiyoda-ku, Tokyo ≠ Address Column 6 of [Detailed description of the invention] of the address specification Statement of contents of the amendment 3 F' In line 4, the phrase ``coexist as in'' is corrected to ``coexist not in a simple form like ''.

以上that's all

Claims (3)

【特許請求の範囲】[Claims] (1)含水銅殿物を予備浸出した後、通常の浮遊選鉱に
より水銀を浮鉱として濃縮分離回収することを特徴とす
る含水銅殿物の処理方法。
(1) A method for treating hydrated copper precipitates, which comprises preliminary leaching of hydrated copper precipitates, and then concentrating and separating and recovering mercury as floating ore through ordinary flotation.
(2)前記予備浸出液は酸化剤溶液であり、該酸化剤は
硫酸第2鉄、過酸化水素、N03塩、Ct塩、過マンガ
ン酸塩から選ばれる少なくとも一種である特許請求の範
囲第1項記載の含水銅殿物の処理方法。
(2) The preliminary leaching solution is an oxidizing agent solution, and the oxidizing agent is at least one selected from ferric sulfate, hydrogen peroxide, N03 salt, Ct salt, and permanganate. The method for treating hydrated copper precipitates described above.
(3)  前記予備浸出液は硫酸第1鉄溶液である特許
請求の範囲第1項記載の含水銅殿物の処理方法。
(3) The method for treating hydrated copper precipitates according to claim 1, wherein the preliminary leachate is a ferrous sulfate solution.
JP57072803A 1982-04-30 1982-04-30 Treatment of precipitate containing mercury Granted JPS58190824A (en)