JPS61245962A - 鋳造金属の品質向上方法 - Google Patents

鋳造金属の品質向上方法

Info

Publication number
JPS61245962A
JPS61245962A JP7317085A JP7317085A JPS61245962A JP S61245962 A JPS61245962 A JP S61245962A JP 7317085 A JP7317085 A JP 7317085A JP 7317085 A JP7317085 A JP 7317085A JP S61245962 A JPS61245962 A JP S61245962A
Authority
JP
Japan
Prior art keywords
molten metal
electromagnetic force
crystal grains
mold
manner
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP7317085A
Other languages
English (en)
Inventor
Masaru Takahashi
勝 高橋
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to JP7317085A priority Critical patent/JPS61245962A/ja
Publication of JPS61245962A publication Critical patent/JPS61245962A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 本発明は鋳造金属の品質向上方法に関するものである。
従来の鋳造金属は密度に均質を欠ぐとともに鋳巣や割れ
等発生の欠点があり鋳造品の品質を低下させていた。
本発明は従来のこれらの欠点を改善向上させ得るもので
あり、鋳造中の溶湯の金属原子および初期結晶粒に特定
方向へ電磁気力が発生する如くフレミング左手法則に従
った方向へ磁力線と電流を流通し電磁気力を連続加え、
溶湯の深度に比例する内部圧力と密度を助長し気泡や不
純物を排出し鋳巣の発生防止と結晶粒良質成長を醸成す
るとともに薄肉細径複雑形状の鋳造を特徴とする鋳造金
属の品質向上方法である。
本発明は非鉄金属材の外枠の中に鋳型を置きコ字形電磁
石を外枠又は鋳型の長辺側に近接しNS極を対向に据置
き固定し磁力線を最短距離で溶湯全体又は局部に通じる
、電極二個は極面中心点を結ぶ線が磁力線と直角に交差
し溶湯の両端に密接対向して取付は固定し電磁気力制御
装置を介し特定方向へ電磁気力が発生する如く直流電源
を接続したものである。
溶湯全体暑こ電磁気力を作用させる方法の実施例を第1
図により説明すると、非鉄材外枠1の中に鋳型2をl!
1き短辺内側に方向し耐熱材電極a4を鋳型2の内面に
それぞれ固定取付けし、線輪5を巻いたコ字形電磁石6
を外枠1の長辺両側にNS極を対向し据付台7.8に固
定取付けし、直流′iltI7ji9、IOと電磁気力
制御スイッチ11.12を接続準備し、@ @ 13を
注入すると同時にスイッチ11.12を閉となし溶@1
31こ下方向へ電磁気力を発生させ、m0全体が凝固終
了まで連続して通電する方法からなるものであり、電磁
気力が溶湯原子および初期結晶粒全体に作用し溶湯内部
の重力圧力に加わり溶湯深度に比例した内部圧力となり
気泡や不純物を溶湯外面方向へ排出するとともに細部番
こ溶湯を送り均質化1こ作用し鋳巣発生を防止する。ま
た結晶粒成長円滑を助長し割れ発生を防止する等の鋳造
方法である。
溶湯の局部に電磁気力を作用させる方法の実施例を第2
図および第3図により説明すると、外枠14の中こと逆
A型の鋳型15を置き、横桟16の内面と下に耐熱電極
17.18を$ $ 19に密接する如く取付けし、線
輪20を巻いた電磁石21に延長磁極2Z23を取付延
長し下方先端近くが電極17.18と直角に交差し、横
桟16の内部溶@19を囲む形に取付は固定する。
線輪20と″IIL橋17.18にそれぞれ直流を流し
俗−を湯口24から注入すると、溶湯が横桟16を充填
しフレミング左手法則の方向へ電磁気力が連続作用し溶
湯19を左方向へ圧送し水平横桟や縦部との三叉部にお
ける鋳巣の発生を防止するものである。延長磁極222
3の先端には溶湯との間に断熱材を置き磁極材の温度上
昇を防止する。第2図第3図では直流[ISiと制御ス
イッチは第1図に同様のため省略しtこ。
本発明は金属鋳造の宿命である鋳巣や密度不均質等欠陥
の発生を防止し得るものであり、鋳造品の不合格が減少
し製品歩留まりの向上と従来鋳造困難とされた形状製品
も可能となり、また比重の軽い非鉄金属の鋳造には多発
欠陥防止の効果大なるものがある。
【図面の簡単な説明】
第1図は本発明を溶湯全体へ作用させる方法の斜視図、
第2図は本発明を溶湯局部に作用させる方法の斜視図、
第3図は第2図の1−1断面図である。

Claims (1)

    【特許請求の範囲】
  1. 鋳造中の溶湯の金属原子および初期結晶粒に特定方向へ
    電磁気力が発生する如くフレミング左手法則に従った方
    向へ磁力線と電流を流通し電磁気力を連続加え、溶湯の
    深度に比例する内部圧力と密度を助長し気泡や不純物を
    排出し鋳巣の発生防止と結晶粒良質成長を醸成するとと
    もに薄肉細径複雑形状の鋳造を特徴とする鋳造金属の品
    質向上方法。
JP7317085A 1985-04-05 1985-04-05 鋳造金属の品質向上方法 Pending JPS61245962A (ja)