JPS6231114B2 - - Google Patents

Info

Publication number
JPS6231114B2
JPS6231114B2 JP1757781A JP1757781A JPS6231114B2 JP S6231114 B2 JPS6231114 B2 JP S6231114B2 JP 1757781 A JP1757781 A JP 1757781A JP 1757781 A JP1757781 A JP 1757781A JP S6231114 B2 JPS6231114 B2 JP S6231114B2
Authority
JP
Japan
Prior art keywords
paper
aqueous dispersion
self
carboxyl group
polyolefin resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
JP1757781A
Other languages
Japanese (ja)
Other versions
JPS57134556A (en
Inventor
Mutsuhiro Tanaka
Yukihiro Takada
Hiroyuki Hamasuna
Shiro Pponma
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsui Chemicals Inc
Original Assignee
Mitsui Petrochemical Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsui Petrochemical Industries Ltd filed Critical Mitsui Petrochemical Industries Ltd
Priority to JP1757781A priority Critical patent/JPS57134556A/en
Publication of JPS57134556A publication Critical patent/JPS57134556A/en
Publication of JPS6231114B2 publication Critical patent/JPS6231114B2/ja
Granted legal-status Critical Current

Description

【発明の詳細な説明】[Detailed description of the invention]

本発明は金属蒸着紙、更に詳しくは金属と紙と
の密着性および表面光沢が改良された金属蒸着紙
及びその製造方法に関する。 アルミニウム箔と紙との貼合品は、ラベルや包
装用に大量に使用されているが、近年紙にアルミ
ニウムを蒸着した所謂蒸着紙がアルミニウム箔と
の貼合品に比べて屈曲させてもピンホールが発生
し難く、またアルミニウム層が薄いので、柔らか
さ、折り目のつけ易さ等の紙の利点を損わないと
いう長所を有しているので、一部アルミニウム箔
との貼合品に代えての使用が検討されている。金
属蒸着紙としては基材となる紙に樹脂層を設け、
該樹脂層上に金属を蒸着したものと紙に直接金属
を蒸着したものとがあるが、後者は紙との密着性
が悪く、表面光沢の良いものが得られないので、
特殊な用途に限られており、金属蒸着紙としては
ほとんど前者が使用されている。紙に樹脂をコー
トするのは、表面の平滑性を良くし、光沢を高め
る、紙とアルミニウムとの密着性を良くする、蒸
着時、紙からの水分、ガスの放出を抑える等の為
であり、コート用樹脂としては溶液タイプが良い
とされ、一般にポリウレタン、アクリル、ポリア
ミド、ニトロセルロースなどをコートしたものが
使用されている。しかしながら溶液タイプは溶剤
の残留の問題があり、また紙とアルミニウムとの
密着性についても問題がある。紙とアルミニウム
との密着性が優れる蒸着紙の一つとして、出願人
等は先に自己水分散性ポリオレフイン系樹脂の水
性分散液を塗布したものを提案したが、表面光沢
の良いものを得るためには、少なくとも3回以上
塗布する必要があり、工程が煩雑であつた。本発
明は、その点に鑑みなされたもので、紙上にある
特定の異種の高分子を積層させた上にアルミニウ
ムを蒸着させたものが密着性と光沢の優れた蒸着
紙となり、しかもそれら異種の高分子材料は各一
度塗布するのみでも充分満足すべき蒸着紙が得ら
れることを見出したものである。 すなわち、本発明は紙の少なくとも一面に、カ
ルボキシル基変性スチレン・ブタジエン共重合体
からなるカルボキシル基含有ゴム層、自己水分散
性ポリオレフイン系樹脂および金属蒸着層を順次
形成させた金属蒸着紙及びその好適な製造方法と
して、紙の片面あるいは両面にカルボキシル基含
有ゴムの水性分散液を塗布し、その乾燥被膜上に
更に自己水分散性ポリオレフイン系樹脂の水性分
散液を塗布し、その乾燥被膜上に金属を真空蒸着
することにより製造する方法に係わる。 本発明で好適に用いられるカルボキシル基含有
ゴム及び自己水分散性ポリオレフイン系樹脂の水
性分散液は該変性ゴム及び樹脂の微粒子、例えば
粒径約0.01〜5μ程度の粒子が不連続相をなし水
に分散されたもので、水が連続相であり、一般に
ポリマーエマルジヨン、ポリマーラテツクス、ポ
リマーデイスパージヨンと呼ばれているものであ
る。 本発明で用いられるカルボキシル基含有ゴムと
はスチレン、ブタジエン、α,β―エチレン性不
飽和カルボン酸とを共重合したり、スチレン・ブ
タジエンの共重合体にα,β―エチレン性不飽和
カルボン酸をグラフト共重合したりしてスチレ
ン・ブチジエン共重合体中にカルボキシル基を導
入したものであり、このようなカルボキシル基変
性スチレン・ブタジエン共重合体は後述するアイ
オノマー樹脂からなる自己分散性ポリオレフイン
系樹脂との密着性が優れるので好ましい。変性に
使用されるα,β―エチレン性不飽和カルボン酸
としては、アクリル酸、メタアクリル酸、クロト
ン酸、マレイン酸等が挙げられる。 本発明で用いられる自己分散性ポリオレフイン
系樹脂とは、オレフインの単独重合体または相互
共重合体、オレフインとビニル化合物との共重合
体等で、これら重合体中に分散能を付与するカル
ボキシル基含有または形成性共単量体を共重合さ
せ、含有している。 好ましい自己分散性ポリオレフイン系樹脂は、
エチレンによつて代表されるオレフインとα,β
―エチレン性不飽和カルボン酸またはその誘導体
との共重合体、またはオレフイン重合体の不飽和
カルボン酸またはその誘導体のグラフト共重合体
であり、共重合体中の遊離のカルボキシル基は完
全にまたは部分的にナトリウム、カリウムなどの
アルカリ金属または亜鉛などのアルカリ土類金属
で中和されている。 α,β―エチレン性不飽和カルボン酸およびそ
の誘導体としては、アクリル酸、メタクリル酸、
クロトン酸、マレイン酸およびこれらの酸無水物
やけん化されてカルボキシル基を形成するエステ
ル、酸アミド、酸イミドなどが例示でき、これら
は共重合体中に約5〜45重量%、好ましくは約10
〜20重量%の割合で共重合されている。この共重
合割合がこれより少ないと水分散能が劣り、粒径
の小さい分散液が得られ難い。一方これより多い
共重合割合では、共重合体の融点が低すぎて被膜
が弱く、耐水性も低下する。グラフト共重合体の
場合には、その共重合割合は前記割合よりも一桁
程度少なくてもよい。 水性分散液が調製されるポリオレフイン系樹脂
としては、そこに蒸着されるアルミニウムなどの
金属に対する接着性の点などから、特にアイオノ
マー樹脂、α,β―不飽和カルボン酸グラフトポ
リオレフインなどが好んで用いられる。アイオノ
マー樹脂は、カルボキシル基の全部または一部が
ナトリウム、亜鉛などの金属でイオン化されてい
るため、水に対して容易に自己分散する性質を有
しているので、それ自体で水性分散液を形成し得
る。アイオノマー樹脂、例えばエチレン―メタク
リル酸共重合体のナトリウム塩の水性分散液は、
それ単独で用いられるだけではなく、そこに例え
ばエチレン―酢酸ビニル共重合体、ポリエチレン
などを均一に混合するだけで、本来自己分散性を
有しないポリオレフイン系樹脂との混合水性分散
液を形成することができ、かかる混合水性分散液
もまた自己分散性のポリオレフイン系樹脂水性分
散液として使用することができる。 α,β―不飽和カルボン酸グラフトポリオレフ
インは、その溶融物を塩基性物質を含有する加熱
水中に撹拌下に添加することによつて、容易にそ
の水性分散液を形成させることができる(特開昭
52―13539号公報参照)。この際、エチレン―酢酸
ビニル共重合体、ポリエチレンなどとの混合物を
同様に処理すると、これらの非自己分散性ポリオ
レフイン系樹脂との混合水性分散液を形成させる
ことができる。具体的には、例えば酸価約30〜
150のα,β―不飽和カルボン酸グラフトポリオ
レフイン50〜1重量部にエチレン―酢酸ビニル共
重合体、ポリエチレンなどを50〜99重量部混合
し、その溶融均一混合物を塩基性物質を含有する
加熱水中に撹拌しながら添加することにより、容
易に混合水性分散液を形成させることができる。
このように、非自己分散性ポリオレフイン系樹脂
との混合水性分散液も、アイオノマー樹脂の混合
水性分散液と同様に、自己分散性のポリオレフイ
ン系樹脂水性分散液として使用することができ
る。 非自己分散性のポリオレフイン系樹脂として挙
げられるのは、エチレン、プロピレン、1―ブテ
ン、4―メチル―1―ペンテンなどのα―オレフ
インの単独重合体または共重合体であり、例えば
ポリエチレン、ポリプロピレン、ポリ―1―ブテ
ン、ポリ―4―メチル―1―ペンテンなどの単独
重合体、またはエチレン―プロピレン共重合体、
エチレン―1―ブテン共重合体、プロピレン―1
―ブテン共重合体、エチレン―酢酸ビニル共重合
体またはそのけん化物などの共重合体が挙げら
れ、これらは単独でまたは2種以上の混合物とし
て使用することができる。 このようにして調製される自己分散性のポリオ
レフイン系樹脂水性分散液は、固形分濃度が約10
〜60重量%、好ましくは約20〜50重量%のときに
塗布に適した粘度を有し、また被膜にピンホール
が発生するのを防止することができる。その際、
必要ならば更に増粘剤を加えて粘度を調節し、紙
への浸透を最小限に抑えることも可能である。 これらのポリオレフイン系樹脂の水性分散液
は、自己分散性のポリオレフイン系樹脂から調製
されているので、そこに実質的に揮発性の添加
剤、特に界面活性剤を含有していない。乳化剤や
分散剤として作用する界面活性剤や重合時の各種
添加剤などの揮発性添加剤の存在は、金属蒸着の
際に必要とする高真空度を得ることを困難とさせ
るばかりではなく、金属蒸着面の光沢度に著しく
悪影響を及ぼす不均一被膜の形成をもたらし、更
には金属蒸着面の接着性や印刷適性などにも悪影
響を与えるので、その存在を最小限に留める配慮
が特に望まれる。 紙へのカルボキシル基含有ゴム及び自己分散性
ポリオレフイン系樹脂の水性分散液の塗布は、ス
プレー法、ロールコーター法、エアーナイフコー
ター法、マイヤーバーコーター法、ブレードコー
ター法、サイズプレスコーター法、カーテンコー
ター法など公知の方法で連続的かつ均一に行うこ
とができ、紙に対して約1〜20g/m2、好ましく
は約2〜10g/m2のゴムまたは樹脂の塗布量で塗
布する。またカルボキシル基含有ゴムの水性分散
液を塗布する場合、次いで塗布する自己分散性ポ
リオレフイン系樹脂層との密着性をよりよくする
為にカルボキシル基含有ゴムの水性分散液に一部
自己分散性ポリオレフイン系樹脂の水性分散液を
混入させてもよい。また自己分散性ポリオレフイ
ン系樹脂の水性分散液には、既に形成されている
被膜にはじかれるのを防止する為に、ノニオン系
界面活性剤、ポリビニルアルコール等を添加して
漏れ性を改善することができる。 塗布された各々の水性分散液の乾燥は、当該ゴ
ム及び樹脂の成膜温度以上、一般には当該ゴム及
び樹脂の軟化点または融点以上の温度で行われ
る。乾燥条件は、水性分散液中のゴム及び樹脂の
粒子の粒径によつても影響され、大きな粒径の場
合は比較的高温度で、また小さな粒径の場合には
比較的低温で乾燥される。そして、一般には100
℃以上の温度で数秒間〜数分間程度行われる。 形成される被膜の厚さは、紙の種類や用途など
に応じて、一般に約1〜30μ、好ましくは約2〜
15μ程度であり、この範囲内の厚さのものは水性
分散液中の固形分濃度および粒径を調節すること
によつて、容易に均一な被膜として得られる。 真空蒸着は、10-3〜10-5トール程度の高真空下
において、蒸着すべき金属をその融点以上に加熱
することにより行われる。蒸着金属材料として
は、アルミニウム、亜鉛、錫、金、銀、銅、クロ
ム、ニツケル、マンガン、ニツケル―クロム合金
等が用いられ、蒸着条件を調節することによつて
約100〜1000Å、好ましくは約300〜700Å程度の
金属蒸着膜を形成させる。形成された金属蒸着膜
のコート層を介しての紙への接着力は良好であ
り、セロハンテープ剥離試験にも十分に耐える程
度である。 本発明に係わる金属蒸着紙は、金属と紙との密
着性、光沢が優れ、菓子、タバコ、バター、コー
ヒー等の包装紙として、またラベル、金銀糸、ポ
スター等の装飾用としてそれぞれ有効に利用する
ことができる。そしてそれらの用途に応じて金属
蒸着面にエンボス加工を施したり、あるいは更に
金属蒸着層表面にトツプコートあるいは印刷する
こともできる。 次に実施例により、本発明を更に具体的に説明
するが、本発明はその要旨を越えない限りこれら
の実施例に制約されるものではない。 実施例 1 上質紙(坪量54g/m2)の片面にカルボキシル
基変性SBRラテツクス(Nipol 2570X5:日本ゼ
オン(株)製)(以下変性SBRと略す):濃度40重量
%を固形分として6g/m2ロール塗布し、120℃
のオーブン中で60秒間乾燥し、次いで下記自己分
散性ポリオレフイン系樹脂の25重量%水性分散液
(A)にポリビニルアルコール(商品名NL―05日
本合成化学(株)製)の10重量%水溶液を前記樹脂に
対して1重量%(固形分として)添加したものを
固形分として4g/m2ロール塗布し、120℃のオ
ーブン中で60秒間乾燥した。その後10-4トールに
調整した真空蒸着装置内において、前記乾燥塗布
面にアルミニウム層が約500Åの厚さになるよう
に真空蒸着させた。 塗布した自己分散性ポリオレフイン系樹脂の水
性分散液(A)は次のようなものである。 (A) エチレン―メタクリル酸共重合体のナトリウ
ム塩(メタクリル酸含量15重量%、中和度59モ
ル%、密度0.95g/cm3)を水中に粒径約0.1μ
の大きさで分散させたもの。 得られたアルミニウム蒸着紙の蒸着面にセロハ
ンテープを貼り、その後それを引き剥して蒸着面
の接着性を調べた結果、アルミニウムの剥離は認
められなかつた。 また、蒸着面の光沢度をJIS Z 8741(測定角
度45゜)により測定した。結果を第1表に示す。 実施例 2〜4 実施例1で用いたカルボキシル基変性SBRラテ
ツクスの代わりに、カルボキシル基変性SBRラテ
ツクス/自己分散性ポリオレフイン系樹脂の水性
分散液=7/3(重量比)からなる混合水性分散液
(濃度35重量%)を用いて各分散液の塗布量を第
1表の如くする以外は実施例1と同様に行つた。
結果を第1表に示す。 比較例 1 実施例1で用いたカルボキシル基変性SBRラテ
ツクスを用いずに、自己分散性ポリオレフイン系
樹脂を二回塗布する以外は、実施例1と同様に行
つた。結果を第1表に示す。 実施例5および比較例2〜6 模造紙の片面に第2表に示す各種エマルジヨ
ン・ラテツクスを固形分として5.5g/m2塗布し
て120℃のオーブン中で乾燥後、実施例1と同じ
ポリビニルアルコール含有自己分散性ポリオレフ
イン系樹脂水性分散液(A)を固形分として3
g/m2塗布し、120℃のオーブン中で乾燥した。
その後、実施例1と同様にアルミニウムを真空蒸
着し、実施例1と同様に蒸着面の密着性と光沢度
を測定した。結果を第2表に示す。尚、同表にお
いて密着性は、実施例1の方法においてアルミニ
ウムが剥離しなかつたものが〇、一部でもアルミ
ニウムが剥離したものを×として標示した。
The present invention relates to metallized paper, and more particularly to metallized paper with improved adhesion between metal and paper and surface gloss, and a method for producing the same. Products laminated with aluminum foil and paper are used in large quantities for labels and packaging, but in recent years so-called vapor-deposited paper, which is paper with aluminum vapor-deposited, is more stable when bent than products laminated with aluminum foil. It is difficult to form holes, and since the aluminum layer is thin, it has the advantage of not detracting from the advantages of paper such as softness and ease of creases. The use of all is being considered. For metallized paper, a resin layer is provided on the base paper,
There are two types: one in which the metal is vapor-deposited on the resin layer and one in which the metal is vapor-deposited directly on the paper, but the latter has poor adhesion to the paper and does not provide a good surface gloss.
It is limited to special uses, and the former is mostly used as metallized paper. The purpose of coating paper with resin is to improve the surface smoothness and gloss, improve the adhesion between the paper and aluminum, and suppress the release of moisture and gas from the paper during vapor deposition. It is said that a solution type is best as a coating resin, and those coated with polyurethane, acrylic, polyamide, nitrocellulose, etc. are generally used. However, the solution type has the problem of residual solvent and also has problems with the adhesion between paper and aluminum. As a type of metallized paper that has excellent adhesion between paper and aluminum, the applicant and others previously proposed a paper coated with an aqueous dispersion of self-water dispersible polyolefin resin, but in order to obtain a paper with good surface gloss, It was necessary to apply the coating at least three times, and the process was complicated. The present invention was made in view of this point, and it is possible to create a vapor-deposited paper with excellent adhesion and gloss by laminating specific different types of polymers on paper and vapor-depositing aluminum on top. It has been discovered that a sufficiently satisfactory vapor-deposited paper can be obtained by applying the polymeric material only once. That is, the present invention provides metallized paper in which a carboxyl group-containing rubber layer made of a carboxyl group-modified styrene-butadiene copolymer, a self-water dispersible polyolefin resin, and a metallization layer are sequentially formed on at least one surface of the paper, and its preferred embodiments. As a manufacturing method, an aqueous dispersion of a carboxyl group-containing rubber is coated on one or both sides of paper, an aqueous dispersion of a self-water-dispersible polyolefin resin is further coated on the dry coating, and metal is coated on the dry coating. It relates to a method of manufacturing by vacuum evaporation. The aqueous dispersion of the carboxyl group-containing rubber and self-water dispersible polyolefin resin preferably used in the present invention is composed of fine particles of the modified rubber and resin, e.g., particles with a particle size of about 0.01 to 5 μm, forming a discontinuous phase and dispersing into water. It is a dispersed material in which water is the continuous phase and is commonly referred to as a polymer emulsion, polymer latex, or polymer dispersion. The carboxyl group-containing rubber used in the present invention is produced by copolymerizing styrene, butadiene, α,β-ethylenically unsaturated carboxylic acid, or by copolymerizing styrene/butadiene copolymer with α,β-ethylenically unsaturated carboxylic acid. A carboxyl group is introduced into a styrene/butadiene copolymer by graft copolymerization of It is preferable because it has excellent adhesion with Examples of the α,β-ethylenically unsaturated carboxylic acid used for modification include acrylic acid, methacrylic acid, crotonic acid, and maleic acid. The self-dispersing polyolefin resin used in the present invention is a homopolymer or mutual copolymer of olefin, a copolymer of olefin and a vinyl compound, etc., and these polymers contain carboxyl groups that impart dispersibility. Alternatively, a forming comonomer is copolymerized and contained. Preferred self-dispersing polyolefin resins are:
Olefins represented by ethylene and α,β
- copolymers with ethylenically unsaturated carboxylic acids or derivatives thereof, or graft copolymers of unsaturated carboxylic acids or derivatives thereof of olefin polymers, in which the free carboxyl groups in the copolymer are completely or partially It is generally neutralized with alkali metals such as sodium and potassium or alkaline earth metals such as zinc. α,β-Ethylenically unsaturated carboxylic acids and their derivatives include acrylic acid, methacrylic acid,
Examples include crotonic acid, maleic acid, their acid anhydrides, esters, acid amides, and acid imides which are saponified to form carboxyl groups, and these are contained in the copolymer in an amount of about 5 to 45% by weight, preferably about 10% by weight.
It is copolymerized at a rate of ~20% by weight. If the copolymerization ratio is less than this, the water dispersibility will be poor and it will be difficult to obtain a dispersion with small particle size. On the other hand, if the copolymerization ratio is higher than this, the melting point of the copolymer will be too low, resulting in a weak coating and poor water resistance. In the case of a graft copolymer, the copolymerization ratio may be about one order of magnitude smaller than the above ratio. As the polyolefin resin from which the aqueous dispersion is prepared, ionomer resins, α,β-unsaturated carboxylic acid graft polyolefins, etc. are particularly preferably used from the viewpoint of adhesion to metals such as aluminum deposited thereon. . Ionomer resin has the property of easily self-dispersing in water because all or part of its carboxyl groups are ionized with metals such as sodium and zinc, so it forms an aqueous dispersion by itself. It is possible. An aqueous dispersion of an ionomer resin, such as the sodium salt of ethylene-methacrylic acid copolymer,
Not only can it be used alone, but by uniformly mixing it with ethylene-vinyl acetate copolymer, polyethylene, etc., it can form a mixed aqueous dispersion with a polyolefin resin that does not inherently have self-dispersibility. Such a mixed aqueous dispersion can also be used as a self-dispersing polyolefin resin aqueous dispersion. An aqueous dispersion of α,β-unsaturated carboxylic acid-grafted polyolefin can be easily formed by adding the melt into heated water containing a basic substance under stirring (JP-A Akira
(Refer to Publication No. 52-13539). At this time, by similarly treating a mixture with ethylene-vinyl acetate copolymer, polyethylene, etc., it is possible to form a mixed aqueous dispersion with these non-self-dispersing polyolefin resins. Specifically, for example, an acid value of about 30~
50 to 1 part by weight of α,β-unsaturated carboxylic acid grafted polyolefin No. 150 is mixed with 50 to 99 parts by weight of ethylene-vinyl acetate copolymer, polyethylene, etc., and the molten homogeneous mixture is poured into heated water containing a basic substance. A mixed aqueous dispersion can be easily formed by adding the mixture with stirring.
In this way, a mixed aqueous dispersion with a non-self-dispersing polyolefin resin can also be used as a self-dispersing polyolefin resin aqueous dispersion, similar to a mixed aqueous dispersion of an ionomer resin. Examples of non-self-dispersing polyolefin resins include homopolymers or copolymers of α-olefins such as ethylene, propylene, 1-butene, and 4-methyl-1-pentene, such as polyethylene, polypropylene, Homopolymers such as poly-1-butene and poly-4-methyl-1-pentene, or ethylene-propylene copolymers,
Ethylene-1-butene copolymer, propylene-1
Examples include copolymers such as -butene copolymer, ethylene-vinyl acetate copolymer, and saponified products thereof, and these can be used alone or in a mixture of two or more. The self-dispersing polyolefin resin aqueous dispersion prepared in this manner has a solid content concentration of approximately 10
When the amount is about 60% by weight, preferably about 20 to 50% by weight, it has a viscosity suitable for coating and can prevent pinholes from forming in the film. that time,
If necessary, additional thickeners can be added to adjust the viscosity and minimize penetration into the paper. Since these aqueous dispersions of polyolefin resins are prepared from self-dispersing polyolefin resins, they do not substantially contain volatile additives, particularly surfactants. The presence of volatile additives, such as surfactants that act as emulsifiers and dispersants, and various additives during polymerization, not only makes it difficult to obtain the high degree of vacuum required during metal deposition, but also makes it difficult to obtain the high degree of vacuum necessary for metal deposition. Since it causes the formation of a non-uniform film that has a significant negative effect on the glossiness of the metal-deposited surface, and also has an adverse effect on the adhesion and printability of the metal-deposited surface, it is particularly desirable to minimize its presence. The aqueous dispersion of carboxyl group-containing rubber and self-dispersible polyolefin resin can be applied to paper using a spray method, roll coater method, air knife coater method, Mayer bar coater method, blade coater method, size press coater method, or curtain coater. The rubber or resin coating can be carried out continuously and uniformly by a known method such as the method, and the amount of rubber or resin applied to the paper is about 1 to 20 g/m 2 , preferably about 2 to 10 g/m 2 . In addition, when applying an aqueous dispersion of a carboxyl group-containing rubber, some self-dispersing polyolefin resin is added to the aqueous dispersion of a carboxyl group-containing rubber in order to improve adhesion to the self-dispersing polyolefin resin layer that is applied next. An aqueous dispersion of resin may also be incorporated. Furthermore, in order to prevent the aqueous dispersion of self-dispersing polyolefin resin from being repelled by the already formed film, nonionic surfactants, polyvinyl alcohol, etc. may be added to improve leakage. can. Drying of each applied aqueous dispersion is carried out at a temperature equal to or higher than the film-forming temperature of the rubber or resin, generally at a temperature equal to or higher than the softening point or melting point of the rubber or resin. Drying conditions are also influenced by the particle size of the rubber and resin particles in the aqueous dispersion, with large particle sizes being dried at relatively high temperatures and small particle sizes being dried at relatively low temperatures. Ru. And generally 100
It is carried out for several seconds to several minutes at a temperature of ℃ or higher. The thickness of the film formed is generally about 1 to 30 μm, preferably about 2 to 30 μm, depending on the type of paper and its use.
The thickness is approximately 15 μm, and a uniform film having a thickness within this range can be easily obtained by adjusting the solid content concentration and particle size in the aqueous dispersion. Vacuum deposition is performed by heating the metal to be deposited above its melting point under a high vacuum of about 10 -3 to 10 -5 Torr. As the metal material for vapor deposition, aluminum, zinc, tin, gold, silver, copper, chromium, nickel, manganese, nickel-chromium alloy, etc. are used, and by adjusting the vapor deposition conditions, the thickness of about 100 to 1000 Å, preferably about A metal vapor deposition film of about 300 to 700 Å is formed. The adhesion of the formed metal vapor-deposited film to the paper through the coating layer is good, and it can sufficiently withstand a cellophane tape peeling test. The metallized paper according to the present invention has excellent adhesion between metal and paper and has excellent gloss, and can be effectively used as wrapping paper for confectionery, cigarettes, butter, coffee, etc., and for decorative purposes such as labels, gold and silver thread, and posters. can do. Depending on the application, the metal-deposited surface can be embossed, or the metal-deposited layer can be top-coated or printed. Next, the present invention will be explained in more detail with reference to Examples, but the present invention is not limited to these Examples unless the gist thereof is exceeded. Example 1 Carboxyl group-modified SBR latex (Nipol 2570X5: manufactured by Nippon Zeon Co., Ltd.) (hereinafter abbreviated as modified SBR): 6 g/ m2 with solid content at a concentration of 40% by weight was coated on one side of high-quality paper (basis weight 54 g/m 2 ). m 2 rolls applied, 120℃
Then, a 10% by weight aqueous solution of polyvinyl alcohol (trade name NL-05 manufactured by Nippon Gosei Kagaku Co., Ltd.) was added to the 25% by weight aqueous dispersion (A) of the following self-dispersing polyolefin resin. A 1% by weight (solid content) added to the resin was applied to a roll of 4 g/m 2 as a solid content, and dried in an oven at 120°C for 60 seconds. Thereafter, an aluminum layer was vacuum-deposited to a thickness of about 500 Å on the dry coating surface in a vacuum evaporation apparatus adjusted to 10 −4 Torr. The applied aqueous dispersion (A) of self-dispersing polyolefin resin is as follows. (A) Sodium salt of ethylene-methacrylic acid copolymer (methacrylic acid content 15% by weight, degree of neutralization 59 mol%, density 0.95g/cm 3 ) was added to water with a particle size of approximately 0.1μ.
Dispersed in size. Cellophane tape was attached to the vapor-deposited surface of the obtained aluminum vapor-deposited paper, and then it was peeled off to examine the adhesion of the vapor-deposited surface. As a result, no peeling of the aluminum was observed. In addition, the glossiness of the vapor-deposited surface was measured according to JIS Z 8741 (measurement angle: 45°). The results are shown in Table 1. Examples 2 to 4 Instead of the carboxyl group-modified SBR latex used in Example 1, a mixed aqueous dispersion of carboxyl group-modified SBR latex/self-dispersible polyolefin resin aqueous dispersion = 7/3 (weight ratio) was used. The same procedure as in Example 1 was carried out except that the coating amount of each dispersion was changed as shown in Table 1 using (concentration: 35% by weight).
The results are shown in Table 1. Comparative Example 1 The same procedure as in Example 1 was carried out except that the carboxyl group-modified SBR latex used in Example 1 was not used and the self-dispersing polyolefin resin was applied twice. The results are shown in Table 1. Example 5 and Comparative Examples 2 to 6 The various emulsion latexes shown in Table 2 were coated on one side of imitation paper at a solid content of 5.5 g/m 2 and dried in an oven at 120°C. Alcohol-containing self-dispersible polyolefin resin aqueous dispersion (A) as solid content: 3
g/m 2 and dried in an oven at 120°C.
Thereafter, aluminum was vacuum deposited in the same manner as in Example 1, and the adhesion and gloss of the deposited surface were measured in the same manner as in Example 1. The results are shown in Table 2. In the same table, the adhesion is shown as ○ if the aluminum did not peel off using the method of Example 1, and × if the aluminum peeled off even partially.

【表】【table】

【表】【table】

【表】【table】

Claims (1)

【特許請求の範囲】 1 紙の少なくとも一面に、カルボキシル基変性
スチレン・ブタジエン共重合体からなるカルボキ
シル基含有ゴム層、自己水分散性ポリオレフイン
系樹脂層および金属蒸着層を順次形成させてなる
金属蒸着紙。 2 紙の少なくとも一面に、カルボキシル基変性
スチレン・フタジエン共重合体からなるカルボキ
シル基含有ゴムの水性分散液を塗布し、該ゴムの
成膜温度以上で乾燥し、該乾燥被覆上に自己水分
散性ポリオレフイン系樹脂の水性分散液を塗布
し、該樹脂の成膜温度以上で乾燥した後、その被
覆上に金属層を真空蒸着させることを特徴とする
金属蒸着紙の製造方法。
[Scope of Claims] 1. Metal vapor deposition, in which a carboxyl group-containing rubber layer made of a carboxyl group-modified styrene-butadiene copolymer, a self-water dispersible polyolefin resin layer, and a metal vapor deposition layer are sequentially formed on at least one surface of paper. paper. 2. Apply an aqueous dispersion of a carboxyl group-containing rubber made of a carboxyl group-modified styrene-phtadiene copolymer to at least one surface of the paper, dry it at a temperature equal to or higher than the film forming temperature of the rubber, and apply self-water-dispersible dispersion onto the dry coating. 1. A method for producing metal-deposited paper, which comprises applying an aqueous dispersion of a polyolefin resin, drying the dispersion at a temperature higher than the film-forming temperature of the resin, and then vacuum-depositing a metal layer on the coating.
JP1757781A 1981-02-10 1981-02-10 Metallic vapor deposited paper and its manufacture Granted JPS57134556A (en)