JPS63242534A - Packaging material with metal evaporated layer - Google Patents

Packaging material with metal evaporated layer

Info

Publication number
JPS63242534A
JPS63242534A JP7733387A JP7733387A JPS63242534A JP S63242534 A JPS63242534 A JP S63242534A JP 7733387 A JP7733387 A JP 7733387A JP 7733387 A JP7733387 A JP 7733387A JP S63242534 A JPS63242534 A JP S63242534A
Authority
JP
Japan
Prior art keywords
film
vapor
deposited layer
packaging material
deposited
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP7733387A
Other languages
Japanese (ja)
Inventor
克昭 清水
岡野 滋
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toppan Inc
Original Assignee
Toppan Printing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toppan Printing Co Ltd filed Critical Toppan Printing Co Ltd
Priority to JP7733387A priority Critical patent/JPS63242534A/en
Publication of JPS63242534A publication Critical patent/JPS63242534A/en
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明は、レトルト殺菌時及びレトルト殺菌後の食品の
保存性の優れたレトルト殺菌に耐える金属蒸着層を有す
る包装材料に関するものである。
DETAILED DESCRIPTION OF THE INVENTION [Industrial Application Field] The present invention relates to a packaging material having a metal vapor-deposited layer that can withstand retort sterilization and has excellent preservation of foods during and after retort sterilization.

〔従来技術とその問題点〕[Prior art and its problems]

従来から、食品、医薬品等の包装用材料としては、包装
する食品等の酸化及び芳香の飛散、浸透性液の浸透によ
る変質を防止するため、ガスバリヤ性、水蒸気バリヤ性
の優れたものが要求されていた。ガスバリヤ性及び防湿
性の優れた材料として、アルミニウム箔があり、また、
紫外線等の光線遮断性が必要な場合においても、アルミ
ニウム箔を介在させて、積層材料を構成しているが、こ
の構成の概略は、外側より接着剤を介してアルミニウム
箔の保護N/アルニウム箔/シーラントとなるポリオレ
フィン樹脂層の最低でも3層構成となる。そのため、積
層材料の製造方法が複雑になるうえ、アルミニウム箔を
介在させるため柔軟性に劣り、内容物の充填適性も悪(
、コストが高くなる等の欠点があった。さらに、アルミ
ニウム箔は耐屈曲性に劣り、レトルト殺菌用積層材料に
使用される9μ厚程度のものでは、製袋時、レトルト殺
菌時、流通の各段階における使用時にピンホールの発生
が多々見られる。
Traditionally, packaging materials for foods, pharmaceuticals, etc. have been required to have excellent gas barrier and water vapor barrier properties in order to prevent deterioration due to oxidation of the packaged food, scattering of aromas, and penetration of penetrating liquids. was. Aluminum foil is a material with excellent gas barrier and moisture proof properties, and
Even in cases where light shielding properties such as ultraviolet rays are required, a laminated material is constructed with aluminum foil intervening. /Contains at least three layers of polyolefin resin layers that serve as a sealant. As a result, the manufacturing method for laminated materials is complicated, and since the aluminum foil is involved, the flexibility is poor, and the suitability for filling the contents is poor (
However, there were disadvantages such as high cost. Furthermore, aluminum foil has poor bending resistance, and when used as a laminated material for retort sterilization with a thickness of about 9 μm, pinholes often occur during bag making, retort sterilization, and use at each stage of distribution.

そこで、耐屈曲性も良く、安価であるアルミニラム蒸着
フィルムを積層材料の構成要素として用いる事が考えら
れるが、アルミニウム蒸着は、基材となるプラスチック
フィルムとの密着性が、ボイル等の加熱により劣化する
事が欠点であり、レトルト殺菌用積層材料には適さない
ものとされていた。
Therefore, it is possible to use aluminum vapor-deposited film, which has good bending resistance and is inexpensive, as a component of the laminated material, but the adhesion of aluminum vapor-deposited film to the base plastic film deteriorates due to heating such as boiling. This was a drawback and was considered unsuitable as a laminated material for retort sterilization.

〔発明の目的〕[Purpose of the invention]

アルミニウム箔介在の積層材料と性能的にはほぼ同等の
ガスバリア性、光遮断性があり、積層材料の製造方法、
製造価格の点で非常に優れるアルミニウム等の金属蒸着
フィルムを介在させた、ボイル及びレトルト適性を有す
る包装材料を提供することにある。
It has gas barrier properties and light shielding properties that are almost the same as laminated materials with aluminum foil interposed, and the method for manufacturing laminated materials.
It is an object of the present invention to provide a packaging material which is suitable for boiling and retorting and has a metal vapor-deposited film such as aluminum interposed therebetween, which is very superior in terms of production cost.

(発明の構成〕 本発明は、ポリアミドフィルム又は二輪延伸ポリエチレ
ンテレフタレートフィルム等のプラスチックフィルムの
片面を窒素又は窒素を含む混合ガスの低温プラズマ雰囲
気中で処理した被処理面に金属蒸着層を設けた基材、こ
の基材の金属蒸着層側に接着層を介して熱接着性フィル
ムを積層することにより解決した。
(Structure of the Invention) The present invention provides a base material in which one side of a plastic film such as a polyamide film or a two-wheel stretched polyethylene terephthalate film is treated in a low-temperature plasma atmosphere of nitrogen or a mixed gas containing nitrogen, and a metal vapor-deposited layer is provided on the treated surface. The problem was solved by laminating a thermal adhesive film on the metal vapor-deposited layer side of the base material via an adhesive layer.

一般的に、低温プラズマ処理に使用されるガスとしては
、酸素、窒素、酸素と窒素の混合ガス、ヘリウムガス、
アルゴンガス等があるが、本発明者らは、上述のプラス
チックフィルムにアルミニウム等の金属を蒸着する場合
の蒸着強度の向上(蒸着被膜の密着性の向上)には、窒
素及び窒素を含む混合ガスによる低温プラズマ処理が非
常に効果的であり、アルミニウム等の金属をプラズマ被
処理面に蒸着する。蒸着膜厚は、所望のガスバリヤ性、
水蒸気バリア性の点から、数百オングストロームから1
000オングストロームの範囲が適当であるが、最適な
膜厚は700オングストロ一ム程度が好適である。
Generally, gases used for low-temperature plasma processing include oxygen, nitrogen, mixed gas of oxygen and nitrogen, helium gas,
Argon gas, etc., but the present inventors believe that nitrogen and a mixture containing nitrogen can be used to improve the vapor deposition strength (improve the adhesion of the vapor-deposited film) when vapor-depositing metals such as aluminum onto the above-mentioned plastic film. Low-temperature plasma treatment is very effective, and metals such as aluminum are deposited on the plasma-treated surface. The thickness of the deposited film is determined by the desired gas barrier property,
In terms of water vapor barrier properties, the thickness ranges from several hundred angstroms to 1
The optimum film thickness is approximately 700 angstroms.

〔作   用〕[For production]

以上述べたようにアルミニウム等の蒸着を施こしたポリ
アミド樹脂フィルム、及び二輪延伸ポリエチレンテレフ
タレート樹脂フィルム等のプラスチックフィルムの被処
理面と蒸着層との接着強度は、セロハンテープ’AMテ
ストで脱落することがない。
As mentioned above, the adhesive strength between the treated surface and the vapor-deposited layer of polyamide resin films coated with aluminum, etc., and plastic films such as two-wheel stretched polyethylene terephthalate resin films is such that the adhesive strength between the treated surface and the vapor-deposited layer is such that the cellophane tape will fall off in the AM test. There is no.

なお、レトルト殺気包装材料となすには、ポリエチレン
、ポリプロピレン等の熱tl、fF性フィルムを、ドラ
イラミネート又は、エキストルージ四ンラミネート等の
積層化手段により積層すれば良く、特に限定されるもの
ではない。
In order to make the retort air-killing packaging material, it is sufficient to laminate heat tl and ff films of polyethylene, polypropylene, etc. by dry lamination, extrusion lamination, etc., and there are no particular limitations. do not have.

以下、実施例にて説明する。Examples will be described below.

〔実  施  例〕〔Example〕

1)厚さ15μのポリアミド樹脂製フィルム(以下、ナ
イロンフィルム(Ny)と称す、ユニチカ側製エンブレ
ム)及び、厚さ12μの二輪延伸ポリエチレンテレフタ
レートフィルム(以下、ポリエステルフィルムCPET
)と称す、東し■製ルミラーF−65)の片面に、下記
条件による低温プラズマ処理を行なった。
1) 15μ thick polyamide resin film (hereinafter referred to as nylon film (Ny), emblem made by Unitika) and 12μ thick two-wheel stretched polyethylene terephthalate film (hereinafter referred to as polyester film CPET)
), one side of Lumirror F-65) manufactured by Toshi Corporation was subjected to low-temperature plasma treatment under the following conditions.

くプラズマ処理条件シ イ)低温プラズマ処理装置: TMZ−4072(東芝
製)口)使用ガス;窒素ガス ハ)真空度 ; 1. Otorr 二)出 力 ; 1.OOOwatt ホ)処理時間: 30sec 処理後、アルミニウム蒸着を行ない、A!’蒸着ナイロ
ンフィルム(A)、AA+蒸着ポリエステルフィルム(
B)を得た。
Plasma treatment conditions 1) Low temperature plasma processing equipment: TMZ-4072 (manufactured by Toshiba) Gas used: Nitrogen gas 3) Degree of vacuum; 1. Otorr 2) Output; 1. OOOwatt E) Processing time: 30 sec After processing, aluminum vapor deposition is performed, and A! 'Vapour-deposited nylon film (A), AA + vapor-deposited polyester film (
B) was obtained.

2)比較例として、上記フィルムに低温プラズマ処理を
行なわないでアルミニウム蒸着を施こした、Al蒸着ナ
イロンフィルム(C) 、Am!蒸着ポリエステルフィ
ルム(D)!得た。
2) As a comparative example, an Al-deposited nylon film (C), in which the above film was subjected to aluminum deposition without performing low-temperature plasma treatment, Am! Vapor-deposited polyester film (D)! Obtained.

3)レトルト用接着剤(東洋モートン側製 AC300
/CAT−10)を用い、ドライラミネート法により(
A3−(D)のフィルムのAJi着層に、無延伸ポリプ
ロピレンフィルム70μ(CPP)(東し合成フィルム
■製3931)をラミネートシ、積層材料[a)〜(d
)を得た。
3) Retort adhesive (AC300 manufactured by Toyo Morton)
/CAT-10) by dry lamination method (
Laminate an unstretched polypropylene film 70μ (CPP) (3931 manufactured by Toshi Synthetic Film ■) on the AJi adhesion layer of the film A3-(D), and laminated materials [a) to (d)
) was obtained.

(a):My/プラズマ処理/AJVM/接着剤/ C
PP(b):PE?/        同    上(
C):Ny/azvM/接着剤/CPP(d):PHT
/      同、  上4)積層材料(a) 〜(d
)を121℃−30分間のレトルト殺菌条件下において
処理後、ナイロン、あるいはポリエステルフィルムとA
l蒸着層との接着強度を測定した。その結果を表−1に
示す。
(a): My/Plasma treatment/AJVM/Adhesive/C
PP(b):PE? / Same as above (
C): Ny/azvM/adhesive/CPP(d): PHT
/ Same, above 4) Laminated materials (a) to (d
) under retort sterilization conditions at 121°C for 30 minutes, nylon or polyester film and A
The adhesive strength with the vapor deposited layer was measured. The results are shown in Table-1.

なお、レトルト殺菌前の接着強度も同表に示す。The adhesive strength before retort sterilization is also shown in the same table.

5)評価結果二表−1の通り、低温プラズマ処理による
を違差が明確である。
5) Evaluation Results As shown in Table 2-1, there are clear differences due to low-temperature plasma treatment.

表         1 なお、Al蒸着層の接着強度の測定は、蒸着層面にラミ
ネートしたCPPフィルムをl?lI Iffする事に
より、基材と蒸着層の強度を測定した。
Table 1 The adhesive strength of the Al vapor deposited layer was measured using a CPP film laminated on the surface of the vapor deposited layer. The strength of the base material and the deposited layer was measured by lIff.

〔発明の効果〕〔Effect of the invention〕

以上述べた様に、ポリアミドフィルム、ポリエチレン−
テレフタレートフィルムのプラスチックフィルムに、窒
素ガスを主体とする低温プラズマ処理を行なった後、ア
ルミニウム等の金属蒸着を施こしたフィルムの蒸着面に
熱接着性フィルムをラミネートした積層材料は、レトル
ト後(ボイル後)も、基材と蒸着層との接着強度の劣化
がなく、非常に優れたものであった。。
As mentioned above, polyamide film, polyethylene
A laminated material in which a plastic film such as a terephthalate film is subjected to low-temperature plasma treatment using mainly nitrogen gas, and then a thermally adhesive film is laminated on the vapor-deposited surface of the film is coated with a metal such as aluminum. (after) was also very excellent, with no deterioration in the adhesive strength between the base material and the vapor deposited layer. .

Claims (2)

【特許請求の範囲】[Claims] (1)プラスチックフィルムを、窒素又は窒素を含む混
合ガスの低温プラズマ雰囲気中で処理した被処理面に金
属蒸着層を設けた基材の金属蒸着層側に接着剤層を介し
て熱接着性フィルムを積層した金属蒸着層を有する包装
材料。
(1) A plastic film is treated in a low-temperature plasma atmosphere of nitrogen or a mixed gas containing nitrogen. A metal vapor-deposited layer is provided on the surface to be treated. A heat-adhesive film is attached to the metal-deposited layer side of the base material via an adhesive layer. A packaging material with a metal vapor-deposited layer.
(2)プラスチックフィルムが、ポリアミド樹脂あるい
はポリエチレンテレフタレート樹脂より成る事を特徴と
する特許請求の範囲第1項記載の金属蒸着層を有する包
装材料。
(2) The packaging material having a metal vapor-deposited layer according to claim 1, wherein the plastic film is made of polyamide resin or polyethylene terephthalate resin.
JP7733387A 1987-03-30 1987-03-30 Packaging material with metal evaporated layer Pending JPS63242534A (en)