JPS6347322A - Method for preventing generation of dust during transfer of molten pig iron - Google Patents
Method for preventing generation of dust during transfer of molten pig ironInfo
- Publication number
- JPS6347322A JPS6347322A JP19036686A JP19036686A JPS6347322A JP S6347322 A JPS6347322 A JP S6347322A JP 19036686 A JP19036686 A JP 19036686A JP 19036686 A JP19036686 A JP 19036686A JP S6347322 A JPS6347322 A JP S6347322A
- Authority
- JP
- Japan
- Prior art keywords
- ladle
- slag
- pig iron
- molten pig
- hot metal
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【発明の詳細な説明】
[産業上の利用分野コ
本発明は、溶銑移し替え時の発塵を防止する方法に関し
、詳細には溶銑を溶銑収納容器から取鍋へ穆し替えると
きのスラグの混入をできる限り少なくする様に工夫され
た溶銑移し替え時の発塵防止方法に関するものである。[Detailed Description of the Invention] [Industrial Field of Application] The present invention relates to a method for preventing dust generation when transferring hot metal, and more specifically, to a method for preventing dust generation when transferring hot metal from a hot metal storage container to a ladle. This invention relates to a method for preventing dust generation during transfer of hot metal, which is devised to minimize contamination.
[従来の技術]
溶銑を収納している混銑車、溶銑鍋、溶銑予備処理炉等
の溶銑収納容器から取鍋へ溶銑を穆し替えるに際しては
、取鍋内への落下時の衝!や高温溶銑からの上昇気流に
よって大量の金属ダスト等が粉塵として舞い上がる。そ
の為溶銑移し替え中は視界が悪くなり、取鍋内は勿論の
こと溶銑収納容器の出湯位置さえ判り難い状況であり、
作業看視ができないばかりか作業環境保全上の問題もあ
る。また溶銑の排出が終了した頃合いを見計って溶銑収
納容器を起立しスラグカットを行なっているが、上記の
如く発塵が激しい為に溶銑の流出状況が見えずスラグカ
ットのタイミングを間違うことがある。即ちタイミング
が遅れると、多量のスラグが溶銑に伴なわれて流出し取
鍋中へ混入してしまうが、これを恐れて早めにスラグカ
ットを行なうと溶銑が収納容器内に残り歩留りを低くす
るという問題がある。その為スラグカットのタイミング
はむしろ遅れ気味になることが多く、次工程以後におい
て色々な不都合を生じている。例えば取鍋内へ予備処理
スラグ(脱燐スラグ等)が混入すると、取鍋内の溶銑を
転炉へ穆した際に転炉内で復燐を起こすという問題が生
じる。[Prior Art] When transferring hot metal from a hot metal storage container such as a mixing car, a hot metal pot, or a hot metal pre-treatment furnace, to a ladle, it is important to avoid collisions when the hot metal falls into the ladle. A large amount of metal dust is blown up as dust by the updraft from the high-temperature hot metal. As a result, visibility was poor during the transfer of hot metal, making it difficult to see not only the interior of the ladle but also the location of the hot metal outlet in the hot metal storage container.
Not only is it impossible to monitor the work, but there are also problems in preserving the work environment. In addition, the hot metal storage container is raised to cut the slag when the discharge of hot metal is finished, but as mentioned above, due to the intense dust generation, it is difficult to see how the hot metal is flowing out, making it difficult to cut the slag at the wrong time. There is. In other words, if the timing is delayed, a large amount of slag will flow out with the hot metal and mix into the ladle, but if you fear this and cut the slag early, the hot metal will remain in the storage container and reduce the yield. There is a problem. For this reason, the timing of slag cutting is often rather delayed, causing various inconveniences in subsequent processes. For example, if pretreatment slag (dephosphorization slag, etc.) gets mixed into the ladle, a problem arises in that when the hot metal in the ladle is sifted into the converter, rephosphorization occurs in the converter.
[発明が解決しようとする問題点コ
この様に溶銑移し替え時の発塵現象は作業面及び品質面
で種々の問題を引起こす要因となフており、これを抑制
することが要請されている。[Problems to be solved by the invention] As described above, the phenomenon of dust generation during transfer of hot metal is a factor that causes various problems in terms of work and quality, and there is a need to suppress this phenomenon. There is.
しかるに現状の抑制手段としてはせいぜい集塵機の能力
を大きくして視界の回復を図ろうとする程度のものであ
り、集a機の電力費が高くなるばかりで有効な解決手段
とはなり得ていない。However, the current control measures are at best intended to restore visibility by increasing the capacity of the dust collector, which is not an effective solution as it only increases the electricity costs of the dust collector.
本発明はこうした事情に着目してなされたものであって
、発生するにまかせた粉塵を集塵機によって収集すると
いった事後対策的なものではなく、粉塵の発生自体を抑
制することにより作業環境を改善し、取鍋へのスラグ混
入を可及的少量に抑制しようとするものである。The present invention has been made with attention to these circumstances, and is not a reactive measure such as collecting dust that has been allowed to occur with a dust collector, but rather improves the working environment by suppressing the generation of dust itself. The aim is to suppress the amount of slag mixed into the ladle as small as possible.
[問題点を解決する為の手段]
しかして上記目的を達成した本発明方法は、溶銑収納容
器から取鍋への溶銑移し替えに際し、次工程で使用され
る予定の造滓剤を、溶銑1トン当たり0.5 kg以上
カバースラグとして溶銑受入れに先立って取鍋内へ投入
しておく点に要旨を有するものである。[Means for Solving the Problems] According to the method of the present invention which has achieved the above object, when transferring the hot metal from the hot metal storage container to the ladle, the slag forming agent to be used in the next process is added to the hot metal 1. The gist is that 0.5 kg or more per ton of cover slag is charged into the ladle before receiving hot metal.
[作用]
前記発塵現象が生じる原因については、取鍋内へ落下し
た溶銑が落下時の衝撃によって多量の微細な飛沫(金属
ダスト等)を生成し、これが高温溶銑からの上昇気流に
乗って舞い上がる為に起こると考えられる。そこで本発
明では取鍋内に予めカバースラグを投入しておき、該カ
バースラグ層によって溶銑飛沫の生成を抑制するという
構成を採用したのである。即ち取鍋の底部に予めカバー
スラグ層を形成しておくと、取鍋内へ投入された溶銑は
カバースラグ層を突きやぶって下層へもぐり込むので溶
銑の跳ね上がりはカバースラグ層に抑えられ飛沫の生成
ひいては発塵が防止される。[Function] The reason why the dust generation phenomenon occurs is that the molten metal that falls into the ladle generates a large amount of fine droplets (metal dust, etc.) due to the impact of the fall, and these droplets are carried by the rising air from the high-temperature molten metal. It is thought that this happens because it soars. Therefore, in the present invention, a cover slag is placed in the ladle in advance, and the cover slag layer suppresses the generation of hot metal splashes. In other words, if a cover slag layer is formed at the bottom of the ladle in advance, the hot metal poured into the ladle will break through the cover slag layer and sink into the lower layer, so the splashing of the hot metal will be suppressed by the cover slag layer and the generation of splashes. As a result, dust generation is prevented.
前述の如く本発明においてはカバースラグ層形成の為の
造滓剤を取鍋内へ投入しておくのであるが、該造滓剤と
しては溶銑と積極的に反応したり、高温に暖められてガ
スを発生する様な生成であってはならず、また取鍋役人
後の溶銑は取鍋精練や予備処理に付すか、或はさらに次
工程(転炉等)へ移し替えられていくのでこれら各f!
!lIA理の実施に悪影響を及ぼすものであ−りではな
らないということも必要条件となる。As mentioned above, in the present invention, a slag-forming agent is charged into the ladle for forming the cover slag layer. The production must not generate gas, and the hot metal after ladle processing is either subjected to ladle smelting or preliminary treatment, or transferred to the next process (converter, etc.). Each f!
! It is also a necessary condition that it must not have a negative impact on the implementation of the IIA process.
こうした条件を満足する造滓剤は当該移し替え操作に続
いて行なわれる次工程の種類によって異なフてくるが、
次工程で使用される造滓剤を使用するのがもっとも安全
である。例えば次工程が転炉の場合にはCab、軽焼ド
ロマイト、珪石等の転炉造滓剤をカバースラグ形成用造
滓剤とすればよい。尚次工程においては格別の処理が行
なわれず、車に保温や酸化防止等の為のスラグが必要で
あるに止まり、用済み後は排滓される様な場合には安価
な高炉滓を使うことも可能である。即ち本発明における
「次工程」とはこの様に広い意味で理解されるべきであ
る。尚取鍋への造滓剤投入量は、溶銑1トン当たり0.
5 kg以上とする必要があり、投入量がこれより少な
いと発塵低減効果を有効に発揮させることができない。The sludge-forming agent that satisfies these conditions varies depending on the type of the next process that follows the transfer operation, but
It is safest to use the slag forming agent used in the next process. For example, when the next step is a converter, a converter slag forming agent such as Cab, light calcined dolomite, or silica stone may be used as the sludge forming agent for forming the cover slag. In addition, if no special treatment is performed in the next process, slag is only needed for heat insulation or oxidation prevention in the car, and the slag is discarded after use, cheap blast furnace slag can be used. is also possible. That is, the "next step" in the present invention should be understood in this broad sense. The amount of slag forming agent added to the ladle is 0.00 slag per ton of hot metal.
It is necessary to set the amount to be 5 kg or more, and if the input amount is less than this, the dust reduction effect cannot be effectively exhibited.
但しあまりに多く造滓剤を投入すると造滓剤への吸熱に
よって地金つき、皮はり等の操業トラブルが発生するの
で投入量は溶銑1トン当たり6kg以下に抑えることが
望ましい。However, if too much slag-forming agent is added, heat absorption by the slag-forming agent will cause operational troubles such as metal sticking and peeling, so it is desirable to keep the amount of slag-forming agent to 6 kg or less per ton of hot metal.
[実施例]
第1表に示す成分組成の予備処理溶銑を取鍋へ移し替え
るに当たり、造滓剤を添加した場合と添加しなかった場
合の発車状況及び取鍋内への流出スラグ量を調べたとこ
ろ第1表に併記する結果が得られた。[Example] When pre-treated hot metal having the composition shown in Table 1 was transferred to a ladle, the starting situation and the amount of slag flowing into the ladle were investigated with and without adding a slag-forming agent. As a result, the results shown in Table 1 were obtained.
第1表に示す様に本発明例においては発塵が少なく取鍋
内への流出スラグ量も低減することができた。As shown in Table 1, in the examples of the present invention, there was little dust generation and the amount of slag flowing into the ladle could be reduced.
[発明の効果]
本発明は以上の様に構成されており、以下要約する効果
を得ることができる。[Effects of the Invention] The present invention is configured as described above, and can obtain the effects summarized below.
(1)溶銑穆し替えに先立って取鍋内にカバースラグ層
を形成しておくので、取鍋内へ溶銑を投入しても発塵が
少なくて済み穆し替え作業性が改善されると共に、作業
環境が向上した。又集塵機への負担が大幅に軽減され電
力費を低減することができた。(1) Since a cover slag layer is formed in the ladle before the molten pig iron is replaced, less dust is generated even when the molten pig iron is poured into the ladle, improving the workability of resizing. , the working environment has improved. In addition, the burden on the dust collector was significantly reduced, making it possible to reduce electricity costs.
(2)発塵抑制によりスラグ流出状況の把握が容易とな
り、スラグカットを正確に行なうことができ取鍋内へ流
出スラグ量を低減することができた。(2) Suppression of dust generation made it easier to grasp the slag outflow situation, allowing accurate slag cutting and reducing the amount of slag flowing into the ladle.
(3)カバースラグとして次工程で使用される造滓剤を
使用したので次工程において復燐等の現象を起こす恐れ
もなく、また造滓剤に余分のコストを費すこともない。(3) Since the slag forming agent used in the next process is used as the cover slag, there is no risk of phenomena such as rephosphorization occurring in the next process, and there is no need to spend extra cost on the sludge forming agent.
Claims (1)
で使用される予定の造滓剤を、溶銑1トン当たり0.5
kg以上カバースラグとして溶銑受入れに先立って取鍋
内へ投入しておくことを特徴とする溶銑移し替え時の発
塵防止方法。When transferring hot metal from the hot metal storage container to the ladle, the slag-forming agent that will be used in the next process is added at a rate of 0.5 per ton of hot metal.
A method for preventing dust generation during transfer of hot metal, characterized in that cover slag of kg or more is placed in a ladle before receiving hot metal.