JPS6374902A - Method and device for producing gas for heat treatment - Google Patents

Method and device for producing gas for heat treatment

Info

Publication number
JPS6374902A
JPS6374902A JP61220191A JP22019186A JPS6374902A JP S6374902 A JPS6374902 A JP S6374902A JP 61220191 A JP61220191 A JP 61220191A JP 22019186 A JP22019186 A JP 22019186A JP S6374902 A JPS6374902 A JP S6374902A
Authority
JP
Japan
Prior art keywords
gas
catalyst
heat treatment
hydrocarbons
air
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP61220191A
Other languages
Japanese (ja)
Inventor
Yoshiyasu Fujitani
藤谷 義保
Hideaki Muraki
村木 秀昭
Shinichi Matsunaga
真一 松永
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toyota Central R&D Labs Inc
Original Assignee
Toyota Central R&D Labs Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toyota Central R&D Labs Inc filed Critical Toyota Central R&D Labs Inc
Priority to JP61220191A priority Critical patent/JPS6374902A/en
Publication of JPS6374902A publication Critical patent/JPS6374902A/en
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
(57) [Abstract] This bulletin contains application data before electronic filing, so abstract data is not recorded.

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明は、ブタン等の炭化水素を部分酸化し〔従来技術
〕 水素と一酸化炭素とを含有する熱処理用ガスは、ガス浸
炭法の浸炭用ガスあるいは金属粉末焼結時に用いる還元
性芥囲気ガス等として開用されている。
[Detailed Description of the Invention] [Industrial Application Field] The present invention partially oxidizes hydrocarbons such as butane [Prior Art] A heat treatment gas containing hydrogen and carbon monoxide is used for carburizing using a gas carburizing method. It is used as a reducing gas for use in metal powder sintering.

この熱処理用ガスを(資)用する方法として9例えば、
ギヤー等のw4製部分の表面硬化法であるガス浸炭法が
ある。この方法は、850〜950°Cの浸炭炉中に被
処理材としての鋼製品を配置すると共に、この中へ水素
と一酸化炭素とを含有する浸炭用ガスを尋人し、鋼製部
品の表面に炭素を固溶したオーステナイトの硬い層を形
成させる方法である。
As a method of using this heat treatment gas, for example,
There is a gas carburizing method that is a surface hardening method for parts made of W4 such as gears. In this method, a steel product to be treated is placed in a carburizing furnace at a temperature of 850 to 950°C, and a carburizing gas containing hydrogen and carbon monoxide is introduced into the furnace. This method forms a hard layer of austenite with carbon dissolved in it on the surface.

上記浸炭用ガスは、一般にブタン、天然ガス等の炭化水
素と空気とを、触媒を充填した触媒層内に導入すること
により製造している。上記触媒層中の触媒としては、多
孔頁担体にニッケルやコバIレト等を担持して成るもの
を使用している。上記触媒層内では、空気中の酸素によ
る炭化水素の部分酸化が触媒により促進され、−酸化炭
素と水素とを含有する浸炭用ガスが生成する。
The carburizing gas is generally produced by introducing a hydrocarbon such as butane or natural gas and air into a catalyst bed filled with a catalyst. As the catalyst in the catalyst layer, a catalyst formed by supporting nickel, copper or the like on a porous page carrier is used. In the catalyst layer, partial oxidation of hydrocarbons by oxygen in the air is promoted by the catalyst, and a carburizing gas containing carbon oxide and hydrogen is produced.

しかしながら、この方法は、1100〜1200°Cと
いう高温下において行なうため、上記触媒層を具備した
ガス変成レトルトの操作、W##久注に問題がある。ま
た、浸炭炉の温度は上記のごとく900°C程度である
ため、上記高温下で発生した高温の浸炭用ガスはこれを
冷却して便用に供さねばならず、熱エネルギーの面で損
失があ不。
However, since this method is carried out at a high temperature of 1,100 to 1,200°C, there are problems in the operation of the gas conversion retort equipped with the catalyst layer and in the W## injection. In addition, since the temperature of the carburizing furnace is about 900°C as mentioned above, the high-temperature carburizing gas generated at the above-mentioned high temperature must be cooled and used for convenience, resulting in a loss in terms of thermal energy. It's bad.

一方、上記方法により低温で浸炭用ガスを製造しようと
すると、生成ガス中のメタン(CL14)や二酸化炭素
(CO,)の不純物が副生しやすくなる。
On the other hand, when carburizing gas is produced at low temperatures by the above method, impurities such as methane (CL14) and carbon dioxide (CO,) in the generated gas are likely to be produced as by-products.

特に浸炭用ガスには、OH4やCO!の不純物が少ない
ことが要求されており、上記従来方法には。
In particular, carburizing gases include OH4 and CO! It is required that there are few impurities in the above conventional method.

改良すべき点が残されている。There are still points to be improved.

また、従来の方法においては、炭化水素と空気とを加熱
するための加熱器が、炭化水素の熱分解によるススの生
成を抑制するためにガス変成レトルトのガス導入口の前
に急速加熱器として置かれている(特公昭49−112
42号)。すなわち。
In addition, in the conventional method, a heater for heating hydrocarbons and air is installed as a rapid heater in front of the gas inlet of the gas conversion retort in order to suppress the generation of soot due to thermal decomposition of hydrocarbons. (Tokuko Sho 49-112)
No. 42). Namely.

炭化水素と空気とを加熱した状態で触媒層に導入する方
法である。しかし、この加熱器中において。
This is a method in which hydrocarbons and air are introduced into a catalyst layer in a heated state. However, in this heater.

なお炭化水素の熱分解が生じており、 0f(4やCO
!の不純物が副生じてしまう。
In addition, thermal decomposition of hydrocarbons occurs, and 0f (4 and CO
! Impurities are generated as a by-product.

〔発明が解決しようとする問題点〕[Problem that the invention seeks to solve]

本発明は、従来の問題点に鑑みなされたものであり、特
に850〜1000°Cという低温下において、効率よ
く、シかも不純物の少ない熱処理用ガスを製造すること
ができる方法および装置を提供しようとするものである
。
The present invention was made in view of the conventional problems, and it is an object of the present invention to provide a method and apparatus capable of efficiently producing a heat treatment gas with few impurities, particularly at a low temperature of 850 to 1000°C. That is.

〔問題点を解決するための手段〕[Means for solving problems]

本第1発明は、炭化水素を部分酸化して一酸化炭素と水
素とを含有する熱処理用ガスを製造する方法において、
アルミナ・マグネシアスピネルと30モル%以下のアル
ミナ、マグネシアの一方または双方とから成る担体にコ
バルトを担持して成る触aを充填した触媒層を加熱する
工程と、該触媒層に炭化水素と空気とを導入して、加熱
された触媒に炭化水素と空気とを接触させることにより
、炭化水素を部分酸化して一酸化炭素と水素とを含有す
る熱処理用ガスを生成する工程とから成ることを特徴と
する熱処理用ガスの製造方法である。
The first invention provides a method for partially oxidizing hydrocarbons to produce a heat treatment gas containing carbon monoxide and hydrogen, comprising:
A step of heating a catalyst layer filled with catalyst a made of cobalt supported on a carrier consisting of alumina/magnesia spinel and 30 mol% or less of alumina and/or magnesia; introducing a heated catalyst and bringing the hydrocarbon and air into contact with each other to partially oxidize the hydrocarbon to generate a heat treatment gas containing carbon monoxide and hydrogen. This is a method for producing a heat treatment gas.

また1本7!j2発明は、炭化水素と空気を導入するた
めのガス4人口と、アルミナ・マグネシアスピネルと3
0モル%以下のアルミナ、マグネシアの一方または双方
とから成る担体にコバルトを担持して成る触媒が充填さ
れてなり、上記導入した炭化水素と空気とを反応させる
ための触媒層を具備したガス変成レトルトと、該触媒層
を加熱するための加熱器と、上記反応により生成した一
酸化炭素と水素とを含有する熱処理用ガスを取り出すた
めのガス流出口とから成ることを特徴とする熱処理用ガ
スの製造装置である。
Another 7! j2 invention has 4 gases for introducing hydrocarbon and air, and alumina magnesia spinel and 3
A gas shift converter comprising a catalyst comprising cobalt supported on a carrier comprising 0 mol% or less of alumina and/or magnesia, and equipped with a catalyst layer for reacting the introduced hydrocarbon with air. A heat treatment gas comprising a retort, a heater for heating the catalyst layer, and a gas outlet for taking out the heat treatment gas containing carbon monoxide and hydrogen generated by the above reaction. This is the manufacturing equipment.

本発明においては、従来のようにガス変成レトルトの前
に設けた加熱器により空気と炭化水素とを予め加熱して
触媒層に導入するのではなく、加熱された触媒層内に炭
化水素と空気とを導入するものである。
In the present invention, instead of heating air and hydrocarbons in advance using a heater installed in front of a gas conversion retort and introducing them into the catalyst layer as in the past, hydrocarbons and air are mixed into the heated catalyst layer. This will introduce the following.

本第2発明の装置の一例を第1図に示す。この装置は9
反応器であるガス変成レトルト1と、その周囲に設けた
加熱器2と、原料ガスである炭化水素と空気とを導入す
るためのガス導入口5と。
An example of the apparatus of the second invention is shown in FIG. This device is 9
A gas conversion retort 1 that is a reactor, a heater 2 provided around it, and a gas inlet 5 for introducing hydrocarbons and air that are raw material gases.

生成した熱処理用ガスを取り出すためのガス流出口4と
からなる。
It consists of a gas outlet 4 for taking out the generated heat treatment gas.

上記ガス変成レトルト1の一端面に導入管6全固着して
ガス導入口3が形成されて、ガス変成レト7レト1内部
の触媒層11と連絡している。ガス変成レトルト1の内
部には、原料ガスを反応させるための触媒層11を有す
る。また、ガス変成レトルトの他端面に流出管7を固着
してガス流出口4が形成されて、上記触媒層11と連絡
している。
A gas introduction port 3 is formed by completely fixing an introduction pipe 6 to one end surface of the gas shift retort 1, and the gas shift retort 7 communicates with a catalyst layer 11 inside the retort 1. Inside the gas shift retort 1, there is a catalyst layer 11 for reacting raw material gas. Further, an outflow pipe 7 is fixed to the other end surface of the gas conversion retort to form a gas outflow port 4, which communicates with the catalyst layer 11.

マタ、ガス変成レトルト1のガス導入口3付近およびガ
ス流出口4付近には断熱れんが層12が設けられており
、ガス変成し)A/)1から熱が逃げないようにしであ
る。
Insulating brick layers 12 are provided near the gas inlet 3 and gas outlet 4 of the gas conversion retort 1 to prevent heat from escaping from the gas conversion retort (A/) 1.

上記加熱II2は、複数個の円筒状加熱体21からなる
。
The heating II2 is composed of a plurality of cylindrical heating bodies 21.

また、ガス変成レトルト1と加熱器2との間にはそれぞ
れ独立した熱電対5が複数個設けられ。
Furthermore, a plurality of independent thermocouples 5 are provided between the gas conversion retort 1 and the heater 2.

ガス変成レトルト1の加熱温度を測定するようになって
いる。
The heating temperature of the gas conversion retort 1 is measured.

この装置を用いて、欠のようにして熱処理用ガスを製造
する。まず導入管6を通って炭化水素と空気とが送られ
、ガス導入口5を経てガス変成レトlレト1中の触媒層
11に導入される。該触媒層11は、外部の加熱器2に
より加熱されており。
Using this apparatus, a heat treatment gas is produced in a similar manner. First, hydrocarbons and air are sent through the introduction pipe 6, and introduced into the catalyst bed 11 in the gas conversion reactor 1 through the gas introduction port 5. The catalyst layer 11 is heated by an external heater 2.

上記導入された炭化水素と空気とは触媒層11内で加熱
された触媒と接触して反応を起とし、水素と一酸化炭素
とを含有する熱処理用ガスを生成する。この生成したガ
スはガス流出口4を経て排出管7を通って取り出される
。
The introduced hydrocarbon and air come into contact with the heated catalyst in the catalyst layer 11 to cause a reaction, producing a heat treatment gas containing hydrogen and carbon monoxide. The generated gas is taken out through the gas outlet 4 and the exhaust pipe 7.

本発明において、触媒層に充填する触媒は、空気と炭化
水素との反応を促辿するものでおり、該触媒としては、
ア?シミナ・マグネシアスピネルとアルミナ、マグネシ
アの一方または双方とから成る担体にコバルトを担持し
て成るもの1に使用する。
In the present invention, the catalyst packed in the catalyst layer promotes the reaction between air and hydrocarbons, and the catalyst includes:
a? Cobalt is supported on a carrier consisting of simina/magnesia spinel and one or both of alumina and magnesia.

なお、上記担体は、アルミナ・マグネシア(MpAJx
Oa)スピネルが70モル%以上を占め、一方7&ミナ
(Aex03)、マグ*シフ(MgO)(’)一方また
は双方が30モル%以下において存在するものである。
Note that the above carrier is alumina magnesia (MpAJx
Oa) Spinel accounts for 70 mol% or more, while one or both of 7 & Mina (Aex03) and Mag*Schiff (MgO) (') is present in 30 mol% or less.

上記構成の触媒は、1000°C以下という低温におい
て、非常に高い活性と耐久性を有しており。
The catalyst with the above structure has extremely high activity and durability at a low temperature of 1000°C or less.

しかもその機械的強度も高い。なお、上記触媒の担体中
にムl*osおよびMpOがほとんど存在しない場合で
あっても、上記の特性を有している。
Furthermore, its mechanical strength is high. Note that even if the catalyst carrier contains almost no Mul*os and MpO, it has the above characteristics.

また、上記担体は、その平均細孔径が101〜2μmの
多孔質体であることが好ましい。かかる範囲の多孔質体
は、触媒の活性をより一層向上させることができる。ま
た、上記触媒成分であるコバlシトの担持量は、上記担
体に対して2〜12重量%(以下W(%とする)の範囲
とすることが好ましい1.該担持量が2wt%より少な
い場合触媒活性が低くなり、また12wt%を越える場
合その担持量に見会うだけの活性の向上が見られない、
。
Further, the carrier is preferably a porous material having an average pore diameter of 101 to 2 μm. A porous body within this range can further improve the activity of the catalyst. Further, the supported amount of the above-mentioned catalytic component is preferably in the range of 2 to 12% by weight (hereinafter referred to as W (%)). 1. The supported amount is less than 2% by weight. If the amount is more than 12 wt%, the catalyst activity will not be improved commensurate with the amount supported.
.

本発明において(資)用する触媒の形状は、熱膨張(ひ
ずみ)による触媒の崩壊をさけるため粒状体とするのが
よい。また9粒状体の@媒を使用する場合、触媒の粒径
は、以下の範囲内とするのが望ましい。ガス変成レトル
トが円筒状の場合、ガス変成し?/レトの内径(M謀層
の外径)と触媒の粒径との比(レトルトの内径/触媒の
粒径)が6〜60の範囲となるようにするのがよい。ま
た、ガス変成し)/レトが角筒状の場合、レトルトの内
壁間距離/触媒の粒径が6〜60の範囲となるようにす
るのがよい。かかる比が上記範囲より小さい場合には、
炭化水素と空気とのガスのすぬけが多くなり2反応が進
行しにくい。また、かかる比がh+fa範囲を越える場
合には、レトルト内の圧力損失が大きくなり、操作上好
ましくない。
The shape of the catalyst used in the present invention is preferably granular in order to avoid collapse of the catalyst due to thermal expansion (strain). Further, when using a 9-part catalyst, the particle size of the catalyst is preferably within the following range. If the gas conversion retort is cylindrical, will it convert to gas? The ratio of the inner diameter of the retort (outer diameter of the M layer) to the particle diameter of the catalyst (inner diameter of the retort/particle diameter of the catalyst) is preferably in the range of 6 to 60. Further, when the retort is in the shape of a rectangular tube, the distance between the inner walls of the retort/the particle size of the catalyst is preferably in the range of 6 to 60. If such ratio is less than the above range,
There is a large amount of gas leaking between the hydrocarbon and air, making it difficult for the two reactions to proceed. Furthermore, if this ratio exceeds the range of h+fa, the pressure loss within the retort will increase, which is unfavorable for operation.

欠VC、上記の触媒f調製する方法についてその例を説
明する。
An example of a method for preparing the above catalyst f lacking VC will be explained.

まず、担体の調製としては、A/、03粉末とMgO粉
末との混合粉末の成形体を加熱焼成して9両者を反応さ
せる方法がある。なお1粒状体の触媒とする場合、上記
混廿粉末の成形体を粒状体としておくのが望ましい。上
記の加熱焼成により、 M9Ae!0゜スピネルが生成
する。しかして、該スピネルは。
First, to prepare the carrier, there is a method in which a molded body of a mixed powder of A/, 03 powder and MgO powder is heated and fired to cause the two to react. In addition, in the case of preparing a single granular catalyst, it is preferable that the molded body of the above-mentioned mixed powder is made into a granular body. By heating and baking as described above, M9Ae! 0° spinel is generated. However, the spinel...

A/、03とMgOとが等そル址反応して生成するので
あるから、前記混合粉末中にhg、 o、おるいはbt
yoを等モル1より過剰に配合しておくことにより、k
l、0.あるいはMgOを加熱焼結後の担体中に残存さ
せることができる。また、A[,03およびMgOを未
反応のまま残存させることにより、担体中にAfi、0
3およびMgOの双方を含有させることができる。なお
、Afi!03とMfOとの等モル量は。
Since A/, 03 and MgO are produced by an isostatic reaction, hg, o, or bt is present in the mixed powder.
By blending yo in excess of 1 molar equivalent, k
l, 0. Alternatively, MgO can be left in the carrier after heating and sintering. In addition, by leaving A[,03 and MgO unreacted, Afi,0
3 and MgO can be included. In addition, Afi! What is the equimolar amount of 03 and MfO?

重量比で示すとH90に対するAl t Os (Al
x Os7H90)の量がz5重量倍の場合に相当する
。
In terms of weight ratio, Al t Os (Al
xOs7H90) is z5 times the weight.

上記に関して具体例を示せば、実施例1に示すようIc
 、 f −Alx Us粉末55モル%とMIO粉末
45モル%の混合粉末を焼結することにより、MgOは
r−A/、Osと完全に反応し、過剰のr−A5,0゜
は焼結中にa −his Osに変化し、担体中に残存
する。従って、担体中にはMyA/、04スピネル82
モル%、 a −AlxOs 18モル%を占めるよう
だなる。
To give a specific example regarding the above, as shown in Example 1, Ic
By sintering a mixed powder of 55 mol% of f-Alx Us powder and 45 mol% of MIO powder, MgO completely reacts with r-A/, Os, and the excess r-A of 5,0° is sintered. It is converted into a-hisOs during the reaction and remains in the carrier. Therefore, MyA/, 04 spinel 82
It appears that a-AlxOs accounts for 18 mol%.

また、平均細孔径が(101〜2μmの多孔質体から成
る担体を得るためには、A[、0,粉末として1101
〜2μmの平均粒径を有するものを用いる。また、 M
yo粉末は、焼結多孔質体中においてA/、03粉末の
最適な接合剤とも言うべきもので、その粒径は特に限定
するものではないが、担体の孔径をほぼ均一なものとす
るためには、α1〜500μmの平均粒径を有するもの
を使用するのが望ましい。ここに「平均粒径」とは重量
平均粒径を意味する。なお、 Al、 03は、α−A
l、03゜γ−Ad、 O,等いかなる種類のAljO
,を使用してもよい。
In addition, in order to obtain a carrier made of a porous material with an average pore diameter of (101 to 2 μm), A[,0, 1101 as a powder
Those having an average particle size of ~2 μm are used. Also, M
The yo powder can be said to be the optimal bonding agent for the A/, 03 powder in the sintered porous body, and its particle size is not particularly limited, but in order to make the pore size of the carrier almost uniform. It is desirable to use particles having an average particle size of α1 to 500 μm. The "average particle size" herein means the weight average particle size. In addition, Al, 03 is α-A
l, 03°γ-Ad, O, etc. Any kind of AljO
, may be used.

また、前記混合粉末の成形体の加熱焼成は1000〜1
600°Cの範囲において行なうのがよい。上記範囲内
であれば、I&れた耐熱性1強度を有する担体を得るこ
とができる。
Further, the heating and firing of the molded body of the mixed powder is 1000 to 1
It is preferable to carry out the process at a temperature of 600°C. Within the above range, it is possible to obtain a carrier having a heat resistance of 1 and a strength of 1.

次に、上記担体に触媒成分たるコバルトを担持させるに
当っては9通常の触媒成分の担持の場合と同様に行ない
9例えば、硝酸コバルト、硫酸コバルト、塩化コバルト
等の触媒成分を形成するための原料の溶液中に、上記担
体を浸漬し、乾燥。
Next, in order to support cobalt as a catalyst component on the above-mentioned carrier, it is carried out in the same manner as in the case of supporting a normal catalyst component. The above carrier is immersed in the raw material solution and dried.

焼成する。Fire.

上記触媒が充填して成る触g層に空気と炭化水素との導
入ガスを導入する際、触媒層内のl温度は850〜10
00℃の範囲にするのが望ましい。
When introducing the introduction gas of air and hydrocarbon into the catalytic layer filled with the above-mentioned catalyst, the l temperature in the catalyst layer is 850-10
It is desirable that the temperature be within the range of 00°C.

1000°Cより高温になると、その後の浸炭処理等の
熱処理用ガスを利用する場合に該ガスを冷却する必要が
あり、エネルギー的に効率が悪い。また、850°Cよ
り低温では、空気中の酸素と炭化水素との反応が進行し
にくい。
When the temperature is higher than 1000°C, it is necessary to cool the gas for subsequent heat treatment such as carburizing treatment, which is inefficient in terms of energy. Further, at a temperature lower than 850°C, the reaction between oxygen in the air and hydrocarbons is difficult to proceed.

また、空気と炭化水素とから成る導入ガスの空気過剰率
は、 1.01〜1,10とするのが望ましい。
Further, it is desirable that the excess air ratio of the introduced gas consisting of air and hydrocarbons is 1.01 to 1.10.

ここで、空気過剰率とは、空気中の酸素と炭化水素とが
反応して、完全に水素と一酸化炭素とに変化するために
要する空気量(理論空気it)に対する供給空気量の割
合(供給空気墓/理論空気量の比)である。本発明にお
いては、空気過剰率が1゜01禾満では熱処理ガス中の
副生ずるメタン(CH4)ガスの量が増加し、逆に1.
10を越える場合には、副生ずる二酸化炭素(CO,)
ガスの量が増加する。
Here, the excess air ratio is the ratio of the amount of air supplied to the amount of air (theoretical air it) required for oxygen and hydrocarbons in the air to react and completely change into hydrogen and carbon monoxide ( supply air capacity/theoretical air volume ratio). In the present invention, when the excess air ratio is less than 1°01, the amount of by-product methane (CH4) gas in the heat treatment gas increases;
If it exceeds 10, the by-product carbon dioxide (CO,)
The amount of gas increases.

史に、触媒層内に空気と炭化水素との導入ガスを導入す
る空間速度(8■)は、1000〜20000 hr”
の範囲とするのが望ましい、SVが1ooohr−’未
満では1反応により生成した生成物の触媒層中に滞在す
る時間が長ずごて、触媒とに炭素析出をきたしやすい。
Historically, the space velocity (8) for introducing gases of air and hydrocarbon into the catalyst layer is 1,000 to 20,000 hr.
If the SV is less than 1 ooohr-', the product produced by one reaction will stay in the catalyst layer for a long time, and carbon will easily be deposited on the catalyst.

また、MVが20o o o hr”を越える場合には
、炭化水素を完全に部分酸化できない。
Furthermore, if the MV exceeds 20 o o o hr'', hydrocarbons cannot be completely partially oxidized.

前記第1図に示した例では、加熱器が触媒層の外部に設
けられていたが、加熱器は触V&層内に設けるなど、触
媒層を加熱することができれば、どのような位置に配置
してもよい。
In the example shown in FIG. 1, the heater was installed outside the catalyst layer, but the heater could be placed in any position if it could heat the catalyst layer, such as inside the contact layer. You may.

以上のように9本発明により製造した熱処理用ガスは、
浸炭用ガス、金属粉末焼結時に用いる還元性雰囲気ガス
等として用いることができる。特に、 cli、やCO
2の不純物の少ないガスを必要とする浸炭処理用として
使用する場合には有効に働くことができる。
As described above, the heat treatment gas produced according to the present invention is as follows:
It can be used as carburizing gas, reducing atmosphere gas used during metal powder sintering, etc. In particular, cli, CO
It can work effectively when used for carburizing treatment which requires a gas with few impurities.

例えば1本発明により製造した熱処理用ガスをガス浸炭
法における浸炭用ガスとして(資)用する場会、該熱処
理用ガス1に温度850〜950°C95V2000〜
12000 hr−1にオイて浸炭炉中へ導入するのが
望しい。
For example, when the heat treatment gas produced according to the present invention is used as a carburizing gas in a gas carburizing method, the heat treatment gas 1 is heated to a temperature of 850 to 950°C, 95V, 2000 to
It is preferable to introduce the carburizing furnace into the carburizing furnace at 12,000 hr-1.

〔発明の効果〕〔Effect of the invention〕

本発明によれば、850〜1000°Cという低温でも
、水素と一酸化炭素とから成る熱処理用ガス’kW造す
ることができる。従って1本発明により製造された熱処
理用ガスを浸炭用ガスとじて(資)用する場合、冷却し
て使用する必要はない。
According to the present invention, it is possible to produce a heat treatment gas of 1 kW consisting of hydrogen and carbon monoxide even at a low temperature of 850 to 1000°C. Therefore, when the heat treatment gas produced according to the present invention is used as a carburizing gas, there is no need to cool it before use.

また1本発明によれば、空気と炭化水素とを触媒層に導
入する前に予め加熱する場合に比べて。
Also, according to the present invention, compared to the case where air and hydrocarbons are preheated before being introduced into the catalyst layer.

メタンや二酸化炭素の副生量の少ない熱処理用ガスを製
造することができる。従って、不純物の少ないことが要
求される浸度用ガスとして9本発明により製造した熱処
理用ガスは、特に優れたものでおる。。
It is possible to produce a gas for heat treatment with a small amount of by-products of methane and carbon dioxide. Therefore, the heat treatment gas produced according to the present invention is particularly excellent as an immersion gas that is required to contain few impurities. .

これは、従来のように空気と炭化水素とをガス変成レト
ルトに導入する前に加熱する場会、加熱中に炭化水素が
熱分解を起こして、メタンや二酸化炭素が副生じやすい
のに対して1本発明では。
This is because when air and hydrocarbons are conventionally heated before being introduced into a gas conversion retort, the hydrocarbons tend to undergo thermal decomposition during heating, producing methane and carbon dioxide as by-products. 1 In the present invention.

加熱された触媒に炭化水素と空気とを接触させるため、
熱処理用ガスの生成反応は促進するが、炭化水素の熱分
解は生じないためであり、しかも本発明に用いる触媒の
活性が高いためである。
To bring the hydrocarbon and air into contact with the heated catalyst,
This is because although the production reaction of heat treatment gas is promoted, thermal decomposition of hydrocarbons does not occur, and furthermore, the activity of the catalyst used in the present invention is high.

更に9本発明によれば、触媒層内へ空気と炭化水素とを
、高い空間速度で導入することができ。
Furthermore, according to the present invention, air and hydrocarbons can be introduced into the catalyst layer at a high space velocity.

少ない触媒量で多量の熱処理用ガスを製造することがで
きる。
A large amount of heat treatment gas can be produced with a small amount of catalyst.

〔実施例〕〔Example〕

以F9本発明の詳細な説明する。 Hereinafter, the present invention will be explained in detail.

V奏 平均粒形1μinのγ−アルミナ(A′ez Os )
粉末と、平均粒径5μmのマグネシア(MfO)粉末と
を55:45の割合(モル%)で混合し、これを粒径約
4Hφの球状ベレットに成形した5、欠に。
γ-Alumina (A'ez Os) with a V average grain size of 1 μin
The powder and magnesia (MfO) powder with an average particle size of 5 μm were mixed at a ratio of 55:45 (mol%), and this was formed into a spherical pellet with a particle size of about 4Hφ.

上記ベレットを1550°Cで加熱、焼結し、多孔質担
体を作製した。該担体は、Mfkl 204スピネル8
2モル%、a−アルミナ18モル%であった。
The pellet was heated and sintered at 1550°C to produce a porous carrier. The carrier is Mfkl 204 spinel 8
2 mol% and a-alumina 18 mol%.

欠に、硝酸コバルトの水溶液に上記担体を浸漬し、乾燥
後、600°C9空気中で3時間焼成し。
First, the above carrier was immersed in an aqueous solution of cobalt nitrate, dried, and then calcined at 600°C in air for 3 hours.

触媒を調製した。な賢、該触媒は9粒径511nRφの
ペレットであり、コバルトが6. Owt%担持されて
なるものである。
A catalyst was prepared. The catalyst is 9 pellets with a particle size of 511 nRφ, and the cobalt content is 6. % by weight.

欠に、上記触媒を第1図に示す装置の触媒層に充填した
。
Suddenly, the above catalyst was packed into the catalyst bed of the apparatus shown in FIG.

この装置は、ガス変成レトルト1と、その周囲に設けた
加熱器2と、ガス導入口3と、ガス流出口4とからなる
。上記ガス変成レトルト1は9円筒状の固定床触媒層式
反応器であり、その内部に触媒層11を有する。
This device consists of a gas conversion retort 1, a heater 2 provided around it, a gas inlet 3, and a gas outlet 4. The gas conversion retort 1 is a 9-cylindrical fixed bed catalyst bed type reactor, and has a catalyst bed 11 therein.

また、ガス変成レトルト1の一端面に、導入管6を固着
して、ガス導入口5が形成されており。
Furthermore, a gas introduction port 5 is formed by fixing an introduction pipe 6 to one end surface of the gas conversion retort 1.

触gX層11と連絡している。更に、ガス変成レトルト
1の他端面に、流出管7を固着して、ガス流出口4が形
成されており、触媒層11と連絡している。また、ガス
変成レトルト1のガス導入口s付近およびガス流出口4
付近において、断熱れんが層12が設けられてなる。
It is in contact with the GX layer 11. Further, an outflow pipe 7 is fixed to the other end surface of the gas conversion retort 1 to form a gas outflow port 4, which communicates with the catalyst layer 11. In addition, near the gas inlet s of the gas conversion retort 1 and the gas outlet 4
Nearby, an insulating brick layer 12 is provided.

また、上記加熱器2は、ガス変成レトルト1中の触媒層
11を加熱するための5個の円筒状加熱体21から成る
。更にガス変成レトルト1と加熱器2との間には独立し
た熱電対5が5細膜けられ。
Further, the heater 2 includes five cylindrical heating bodies 21 for heating the catalyst layer 11 in the gas conversion retort 1. Further, between the gas conversion retort 1 and the heater 2, an independent thermocouple 5 is provided with five thin films.

ガス変成レトルト1の加熱温度を測定するようになって
いる。
The heating temperature of the gas conversion retort 1 is measured.

この装置の導入管6から送られてくる原料ガスは、ガス
導入口3を通過した後、触媒′411へ導入される。m
熱器2は、5つのゾーンに分かれた制御?行うことによ
って、触媒層11内のtA度分布を最小限にすることが
できる。また、熱電対5によって触媒層11の温度は8
30〜950″Cで設定された任意の温度に制御される
1、触媒層で反応して生成したガスはガス流出口4を通
過して。
The raw material gas sent from the inlet pipe 6 of this device passes through the gas inlet 3 and is then introduced into the catalyst '411. m
Is heating device 2 controlled in five zones? By doing so, the tA degree distribution within the catalyst layer 11 can be minimized. Further, the temperature of the catalyst layer 11 is set to 8 by the thermocouple 5.
The temperature is controlled at an arbitrary temperature between 30 and 950''C. 1. The gas generated by the reaction in the catalyst layer passes through the gas outlet 4.

流出管7より取り出される。It is taken out from the outflow pipe 7.

上記ガス変成レトルト1の内径(触媒層11の外径)は
、120flφであり、該触媒層11に粒径3jlll
φの前記触媒を51充填した。なお、レトルト1の内径
/触媒の粒径−40である。また。
The inner diameter of the gas shift retort 1 (outer diameter of the catalyst layer 11) is 120flφ, and the catalyst layer 11 has a particle size of 3jllll.
Fifty-one pieces of the catalyst having a diameter of φ were packed. Note that the inner diameter of the retort 1/the particle size of the catalyst is -40. Also.

加熱器2により触媒層11を930’cに加熱した。The catalyst layer 11 was heated to 930'c by the heater 2.

そして、所定の組成比のブタンと空気との混会ガスヲS
V4000 hr−1でレトルト1内に供給した。
Then, a mixed gas of butane and air with a predetermined composition ratio is prepared.
V4000 hr-1 was supplied into the retort 1.

なお、空気過剰率はブタンの流量を変えることにより調
節した。
Note that the excess air ratio was adjusted by changing the flow rate of butane.

また、比較のため、ガス変成レトルトの外側に設けた加
熱器に代えて、ガス導入口の前に急速加熱器を設置した
場合についても上記と同様な条件により熱処理用ガスを
製造した。
For comparison, a heat treatment gas was also produced under the same conditions as above when a rapid heater was installed in front of the gas inlet instead of the heater installed outside the gas conversion retort.

上記本実施例と比較例とにより生成したガス中のCO1
濃度とCH4儂度とを測定した。その結果を第2図およ
び第3図に示す。第2図は本実施例によるもの、第3図
は比較例によるものであり。
CO1 in the gas generated in the present example and comparative example above
The concentration and CH4 intensity were measured. The results are shown in FIGS. 2 and 3. FIG. 2 shows this example, and FIG. 3 shows a comparative example.

第21図、第3図とも点線は930°Cにおける平衡濃
度曲線(基準)である。
The dotted line in both FIG. 21 and FIG. 3 is the equilibrium concentration curve (reference) at 930°C.

第2図、第3図に示すごとく9本実施例によれば、比較
例によるよりも測定点が原点に近く、副生成物であるC
O2とCH4の量が少ない熱処理用ガスを製造できるこ
とがわかる。
As shown in FIGS. 2 and 3, according to this example, the measurement point is closer to the origin than in the comparative example, and the by-product C
It can be seen that a heat treatment gas containing small amounts of O2 and CH4 can be produced.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図は本発明の熱処理用ガスの製造装置の一例を示す
断面図、第2図は本実施例により製造した熱処理用ガス
中のOH,濃度とCO3濃度とを示す線図、第3図は比
較例により製造した熱処理用ガス中のCH,濃度とCO
2濃度とを示す線図である。 1・・・ガス変成レトルト、2・・・加熱器。 3・・・ガス導入0.4・・・ガス流出口。 11・・・触媒層 第7図
FIG. 1 is a sectional view showing an example of the heat treatment gas production apparatus of the present invention, FIG. 2 is a diagram showing the OH concentration and CO3 concentration in the heat treatment gas produced according to the present example, and FIG. 3 are the CH, concentration and CO in the heat treatment gas produced in the comparative example.
FIG. 2 is a diagram showing two concentrations. 1... Gas conversion retort, 2... Heater. 3...Gas introduction 0.4...Gas outlet. 11...Catalyst layer Fig. 7

Claims (2)

【特許請求の範囲】[Claims] (1)炭化水素を部分酸化して一酸化炭素と水素とを含
有する熱処理用ガスを製造する方法において、アルミナ
・マグネシアスピネルと30モル%以下のアルミナ、マ
グネシアの一方または双方とから成る担体にコバルトを
担持して成る触媒を充填した触媒層を加熱する工程と、
該触媒層内に炭化水素と空気とを導入して、加熱された
触媒に炭化水素と空気とを接触させることにより炭化水
素を部分酸化して一酸化炭素と水素とを含有する熱処理
ガスを生成する工程とから成ることを特徴とする熱処理
用ガスの製造方法。
(1) In a method for producing a heat treatment gas containing carbon monoxide and hydrogen by partially oxidizing hydrocarbons, a carrier consisting of alumina/magnesia spinel and 30 mol% or less of alumina and/or magnesia is used. heating a catalyst bed filled with a catalyst supporting cobalt;
Hydrocarbons and air are introduced into the catalyst layer, and the heated catalyst is brought into contact with the hydrocarbons to partially oxidize the hydrocarbons to produce a heat-treated gas containing carbon monoxide and hydrogen. A method for producing a heat treatment gas, comprising the steps of:
(2)炭化水素と空気とを導入するためのガス導入口と
、アルミナ・マグネシアスピネルと50モル%以下のア
ルミナ、マグネシアの一方または双方とから成る担体に
コバルトを担持して成る触媒が充填されてなり、上記導
入した炭化水素と空気とを反応させるための触媒層を具
備したガス変成レトルトと、該触媒層を加熱するための
加熱器と、上記反応により生成した一酸化炭素と水素と
を含有する熱処理用ガスを取り出すためのガス流出口と
から成ることを特徴とする熱処理用ガスの製造装置。
(2) A gas inlet for introducing hydrocarbons and air, and a catalyst comprising cobalt supported on a carrier consisting of alumina/magnesia spinel and 50 mol% or less of alumina and/or magnesia. A gas conversion retort equipped with a catalyst layer for reacting the introduced hydrocarbon and air, a heater for heating the catalyst layer, and carbon monoxide and hydrogen produced by the above reaction. 1. An apparatus for producing a heat treatment gas, comprising a gas outlet for taking out the heat treatment gas contained therein.
JP61220191A 1986-09-18 1986-09-18 Method and device for producing gas for heat treatment Pending JPS6374902A (en)