JPS6420249A - Polyolefin composition of improved stability - Google Patents

Polyolefin composition of improved stability

Info

Publication number
JPS6420249A
JPS6420249A JP17384787A JP17384787A JPS6420249A JP S6420249 A JPS6420249 A JP S6420249A JP 17384787 A JP17384787 A JP 17384787A JP 17384787 A JP17384787 A JP 17384787A JP S6420249 A JPS6420249 A JP S6420249A
Authority
JP
Japan
Prior art keywords
tert
polyolefin
butyl
composition
improved stability
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP17384787A
Other languages
Japanese (ja)
Other versions
JPH07107111B2 (en
Inventor
徳竹 ▲あつ▼夫
日向 伸
二杉 俊治
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Eneos Corp
Original Assignee
Nippon Petrochemicals Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Petrochemicals Co Ltd filed Critical Nippon Petrochemicals Co Ltd
Priority to JP62173847A priority Critical patent/JPH07107111B2/en
Publication of JPS6420249A publication Critical patent/JPS6420249A/en
Publication of JPH07107111B2 publication Critical patent/JPH07107111B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PURPOSE:To obtain the title polyolefin composition remarkably improved in yellowing during a long-term storage, degradation upon heating or melting and stability or resistance to corrosion of metal, etc., by adding five specified additives to a polyolefin. CONSTITUTION:The title composition is formed by adding pentaerythritol diphosphite (A) of the formula (wherein R1 and R2 are each an aryl), tetrakis(2,4- di-tert-butylphenyl)4,4'-biphenylene diphosphite (B), an ester (C) of 3-(3',5'-di-tert- butyl-4'-hydroxyphenyl)propionic acid, a metal salt (D) of a fatty acid and a hydrotalcite (E) to a polyolefin. This composition is remarkably improved in color stability, heat stability and noncorrosiveness and its improving effect is marked when applied to, especially, a polyolefin produced by a process without deashing.

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は安定性の改善された新規なポリオレフィン組成
物に関し、詳しくはポリオレフィンに各特定のホスファ
イト系、ホスホナイト系およびフェノール系化合物、脂
肪酸金属塩ならびにハイドロタルサイトを添加して得ら
れる色安定性、熱安定性および耐腐食性の改善されたポ
リオレフィン組成物に関する。
[Detailed Description of the Invention] (Industrial Field of Application) The present invention relates to a novel polyolefin composition with improved stability, and more particularly to a polyolefin composition with improved color stability, thermal stability, and corrosion resistance obtained by adding specific phosphite-based, phosphonite-based, and phenol-based compounds, fatty acid metal salts, and hydrotalcite to a polyolefin.

(従来の技術) ポリオレフィンからなるペレットまたは成形品の安定性
としては、まず長期保管する際の黄変および加熱時の劣
化を考慮しなければならない。両者を同時に解決するた
めの対策は必ずしも容易でな(、加熱時の劣化を防止す
るためにフェノール系の酸化防止剤たとえば3,5−ジ
−tert−ブチル−4−ヒドロキシトルエン(BIT
)を添加すると、長期保管中に黄変を示すことはよく知
られた事実である。
(Conventional Technology) When considering the stability of pellets or molded products made of polyolefins, first, yellowing during long-term storage and degradation during heating must be considered. Addressing both simultaneously is not always easy (to prevent degradation during heating, phenolic antioxidants such as 3,5-di-tert-butyl-4-hydroxytoluene (BIT) are used).
It is a well-known fact that adding ) causes yellowing during long-term storage.

近年、高活性触媒の利用により触媒除去工程の省略され
た、いわゆる無脱灰プロセスによりポリオレフィンが製
造されろようになったが、ポリマー中に残る触媒残さと
くにチタンが各種の劣化を促進するといわれている。
In recent years, polyolefins have been manufactured using so-called no-decalcification processes, which omit the catalyst removal step by utilizing highly active catalysts. However, it is said that catalyst residues, particularly titanium, remaining in the polymer accelerate various types of degradation.

さらに無脱灰プロセスにより製造されたポリオレフィン
には、触媒残さとして塩素化合物も残存しており、この
塩素化合物がポリオレフィンの溶融加工を行う際に成形
機などの金属を腐食させろ問題が指摘されている。塩素
化合物による腐食を防止するためには通常脂肪酸金属塩
が添加されるが、同金属塩は酸化防止剤としてリン化合
物とくにホスファイト系のものが共存するとその防食効
果が失われろ欠点がある。このように酸化防止剤の選択
にあたっては防食効果に対する影Oも考慮しなければな
らない。
Furthermore, polyolefins produced by a non-decalcification process retain chlorine compounds as catalyst residues, and it has been pointed out that these chlorine compounds corrode metals such as molding machines during the melting process of polyolefins. To prevent corrosion by chlorine compounds, fatty acid metal salts are usually added, but these metal salts have the drawback that their corrosion-preventive effect is lost when phosphorus compounds, especially phosphite-type antioxidants, are present. Thus, when selecting antioxidants, the impact on corrosion prevention must also be considered.

加熱劣化を防止するためにフェノール系およびホスファ
イト系の酸化防止剤を併用することは公知であり、たと
えば特公昭56−5417号公報にはトリスアリール・
ホスファイトとフェノール系酸化防止剤との組合せが記
載されている。しかしこれらの組合せでは長期保管中の
黄変および高温成形時の熱劣化を防止することができな
い。
It is well known that phenolic and phosphite-based antioxidants are used in combination to prevent heat degradation; for example, Japanese Patent Publication No. 56-5417 describes trisaryl...
The text describes combinations of phosphites and phenolic antioxidants. However, these combinations cannot prevent yellowing during long-term storage or thermal degradation during high-temperature molding.

また長期保管中の黄変を解決するため、アルキル置換フ
ェノール系安定剤とともに特定の有機ホスファイト化合
物を併用する方法が報告されているが(特公昭56−2
5935号公報)、その防止効果もまだ十分とはいい難
く、かつ無脱灰プロセスによるポリオレフィンにこれを
適用した場合には腐食の問題が避けられない。
Furthermore, to address yellowing during long-term storage, a method has been reported in which a specific organic phosphite compound is used in combination with an alkyl-substituted phenol-based stabilizer (Japanese Patent Publication No. 56-2).
(Publication No. 5935) However, its preventative effect is still not entirely sufficient, and when applied to polyolefins produced by a non-decalcification process, corrosion problems are unavoidable.

さらに特開昭61−14240号公報には、直鎖低密度
ポリエチレンにホスファイト、ホスホナイトおよびホス
ホン酸誘導体から選ばれた少なくとも18にのリン化合
物ならびに分子量が400以上のフェノール系酸化防止
剤を配合する方法が記載されているが、これらの組合せ
でも長期保管中の黄変を防止するには必ずしも十分でな
く、かつ腐食対策の点で問題がある。
Furthermore, Japanese Patent Publication No. 61-14240 describes a method of compounding linear low-density polyethylene with at least 18 phosphorus compounds selected from phosphite, phosphonite, and phosphonic acid derivatives, as well as a phenolic antioxidant with a molecular weight of 400 or more. However, even these combinations are not necessarily sufficient to prevent yellowing during long-term storage and present problems in terms of corrosion prevention.

特開昭61−133251号公報には、フェノール系酸
化防止剤、ジ(アルキルまたはアリール)ペンタエリス
リトール・ジホスファイトおよびハイドロタルサイトを
組み合わせた組成物が記載されている。ハイドロタルサ
イトを混合することにより塩素化合物による腐食は防止
できるものの、上記の組合せでは長期保管中および高温
条件下で黄変防止効果が低下し、とくに溶融時には樹脂
が褐色に着色しやすくなる。
Japanese Patent Publication No. 61-133251 describes a composition combining a phenolic antioxidant, di(alkyl or aryl)pentaerythritol diphosphite, and hydrotalcite. Although corrosion by chlorine compounds can be prevented by mixing in hydrotalcite, the above combination has a reduced anti-yellowing effect during long-term storage and under high-temperature conditions, and the resin is particularly prone to brown discoloration when melted.

(発明が解決しようとする問題点) 本発明は、ポリオレフィンとくに無脱灰プロセスにより
製造したポリオレフィンに適する添加剤の組合せを選択
し、それらを用いて長期保管中の黄変および加熱時の劣
化を防止し、かつ金属腐食性を低減したポリオレフィン
組成物を提供することを目的とする。
(Problems to be solved by the invention) The present invention aims to provide a polyolefin composition that prevents yellowing during long-term storage and deterioration during heating, and reduces metal corrosivity, by selecting a combination of additives suitable for polyolefins, particularly polyolefins produced by a non-decalcification process.

(問題を解決しようとする手段) 本発明者らは、上記目的に沿って鋭意検討した結果、特
定の添加剤5mを用いろことにより上記の目的を満足す
るポリオレフィン組成物が得られろことを見いだした。
(Means for attempting to solve the problem) As a result of diligent research in line with the above objective, the present inventors have found that a polyolefin composition satisfying the above objective can be obtained by using a specific additive 5m.

すなわち本発明は、ポリオレフィンが下記の添加剤を含
むことからなる安定性の改善されたポリオレフィン組成
物を提供するものである。
In other words, the present invention provides a polyolefin composition with improved stability, comprising a polyolefin containing the following additives.

(i)  下式で示されるペンタエリスリトール・ジホ
スファイト (R8,R2ニアリール基) (1))  テトラキス(2,4−ジ−tert−ブチ
ルフェニル)4.4′−ビフェニレン・ジホスホナイト
GiD3− (3’、S’−ジ−tert−ブチル−4
’−ヒドロキシフェニル)プロピオン酸のエステル (lψ 脂肪酸の金属塩 [v)  ハイドロタルサイト類 本発明に使用するポリオレフィンは中・低密度ポリエチ
レン、高密度ポリエチレン、ポリプロピレン、ポリ1−
ブテンなどのホモポリマーのほか、エチレン、フロピレ
ン、1−ブテン、1−ヘキセン、4−メチル−1−ペン
テンなとのa−オレフィンの交互共重合体およびエチレ
ン−酢酸ビニル共重合体、エチレン−アクリル酸エチル
共重合体などが挙げられる。とくに高活性チーグラー系
触媒で重合され、かつ触媒除去工程いわゆる脱灰工程を
経ていない上記各重合体を使用した場合に著しい効果を
示す。
(i) Pentaerythritol diphosphite (R8, R2 niaryl group) represented by the following formula (1) Tetrakis(2,4-di-tert-butylphenyl)4,4'-biphenylene diphosphonite GiD3- (3',S'-di-tert-butyl-4
'-hydroxyphenyl)propionic acid ester (1ψ fatty acid metal salt [v] Hydrotalcites The polyolefins used in this invention are medium- and low-density polyethylene, high-density polyethylene, polypropylene, poly-1-
Examples include homopolymers such as butene, as well as alternating copolymers of α-olefins such as ethylene, fluoropolymer, 1-butene, 1-hexene, and 4-methyl-1-pentene, and ethylene-vinyl acetate copolymers and ethylene-ethyl acrylate copolymers. Particularly remarkable effects are observed when these polymers are polymerized with a highly active Ziegler catalyst and have not undergone a catalyst removal process, also known as a demineralization process.

本発明に使用する添加剤のうち(i)ペンクエリスリト
ール・ジホスファイトの具体例としては、ジベンジル・
ペンタエリスリトール・ジホスファイト、ビス(2,4
−ジ−tert−ブチルフェニル)ペンタエリスリトー
ル・ジホスファイト、ビス(2−tert−ブチル−4
−メチルフェニル)ペンタエリスリトール°ジホスファ
イト、ビス(2,6−ジ−tert−ブチル−4−メチ
ルフェニル)ペンタエリスリトール・ジホスファイト、
ビス(2−シクロヘキシルフェニル)ペンタエリスリト
ール・ジホスファイトなどが挙げられるが、とくにビス
(2,4−ジ−tert−ブチルフェニル)ペンタエリ
スリトール・ジホスファイトおよびビス(2,6−ジ−
tert−ブチル−4−メチルフェニル)ペンタエリス
リトール・ジホスファイトが好ましい。
Among the additives used in the present invention, (i) specific examples of penquerythritol diphosphite include dibenzyl
Pentaerythritol diphosphite, bis(2,4
(-di-tert-butylphenyl) pentaerythritol diphosphite, bis(2-tert-butyl-4)
(-methylphenyl) pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl) pentaerythritol diphosphite,
Examples include bis(2-cyclohexylphenyl)pentaerythritol diphosphite, but especially bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite and bis(2,6-di-
tert-butyl-4-methylphenyl)pentaerythritol diphosphite is preferred.

本発明に使用する添加剤のうち(ii)テトラキス(2
,4−ジ−tert−ブチルフェニル)4.4−ビフェ
ニレン・ジホスホナイトは、単独では上記(i)の各種
ホスファイトと同等の黄変防止効果を示すにすぎないが
、同ホスホナイトと併用する場合には相乗効果により抜
群の黄変防止効果を発現することが見いだされたもので
ある。
Among the additives used in the present invention, (ii) tetrakis (2
4,4-biphenylene diphosphonite (4-di-tert-butylphenyl) exhibits only the same anti-yellowing effect as the various phosphates listed in (i) above when used alone. However, it has been found that when used in combination with the phosphonite, it exhibits an outstanding anti-yellowing effect due to a synergistic effect.

本発明に使用する添加剤のうち(iii13−(3″、
5′−ジ−tert−ブチル−4′−ヒドロキシフェニ
ル)プロピオン酸のエステルとしては、たとえばペンタ
エリスリトール・テトラキス[3−(3″、5′−ジ−
tert−ブチル−4′−ヒドロキシフ二ニル)プロピ
オネート]およびオクタデシル・3− (3’、 5’
−ジ−tert−ブチル−4′−ヒドロキシフェニル)
プロピオネートなどが挙げられる。
Among the additives used in the present invention (iii13-(3″,
Examples of esters of 5'-di-tert-butyl-4'-hydroxyphenyl)propionic acid include pentaerythritol tetrakis[3-(3'',5'-di-
[tert-butyl-4'-hydroxyphenyl)propionate] and octadecyl 3-(3',5'
(di-tert-butyl-4'-hydroxyphenyl)
Examples include propionate.

本発明に使用する添加剤のうち0ψ脂肪酸の金属塩とし
ては、ラウリン酸、ミリスチン酸、パルミチン酸、ステ
アリン酸、オレイン酸、リノール酸、リルン酸などの脂
肪酸とリチウム、ナトリウム、マグネシウム、カルシウ
ム、亜鉛などの金属との塩が挙げられるが、とくにステ
アリン酸カルシウムが好ましい。
Among the additives used in the present invention, examples of metal salts of 0ψ fatty acids include salts of fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, oleic acid, linoleic acid, and lyuronic acid with metals such as lithium, sodium, magnesium, calcium, and zinc, but calcium stearate is particularly preferred.

本発明に使用する添加剤のうちMハイドロタルサイト類
は次式で示される複塩化合物である。
Among the additives used in this invention, M hydrotalcites are double salt compounds represented by the following formula.

(M”)、、A I 、 (OH)2(A’−)、、、
、・mH20(ここで0 < x≦0.5.  m:実
数。
(M”),,A I, (OH)2(A'-),,,
,・mH20 (where 0 < x ≤ 0.5, m: real number).

M”: Mg、CaまたはZn。M”: Mg, Ca, or Zn.

A : n価の陰イオン) この化合物としては天然品および合成品のいずれも用い
られるが、とくにVがMg、 A’−がCO;−である
合成品が好ましい。
A: n-valent anion) Both natural and synthetic compounds can be used for this compound, but synthetic compounds in which V is Mg and A'- is CO- are particularly preferred.

本発明に使用する上記成分の配合組成は、ポリオレフィ
ン100重量部に対しで、添加剤(i)および(■)は
いずれもo、 oos〜0.2重量部、好ましくは0.
01〜0.15重量部、添加剤−はo、 oos〜0.
15重量部、好ましくは0.01〜0.08重量部、添
加剤Gψは0.O1〜0、25重量部、好ましくは0.
02〜0.15重1部、添加剤Mは0.01〜0.1重
量部、好ましくは0.02〜0.08重量部である。
The composition of the above components used in the present invention is such that, per 100 parts by weight of polyolefin, additives (i) and (■) are both 0, oos to 0.2 parts by weight, preferably 0.
0.1 to 0.15 parts by weight, additive - is 0, oos to 0.
15 parts by weight, preferably 0.01 to 0.08 parts by weight, additive Gψ is 0.01 to 0.25 parts by weight, preferably 0.
The amount of additive M is 0.01 to 0.1 parts by weight, preferably 0.02 to 0.08 parts by weight.

添加剤(i)の量が0.005重量部未満のときは長期
保管中の黄変が避けられず、一方0.2重量部を超えて
添加するとさびの発生が増大する。添加剤(iilの量
が0.005重景1未満のときも長期保管中の黄変が避
けられず、他方0.2重量部を超えて添加しても効果の
向上は認められない。添加剤口の量が0.005!!1
量部未満のときは加熱時の劣化が抑制されず、一方01
5重量部を超えて添加すると長期保管中の黄変が促進さ
れる。添加剤Gvlおよび(v)の量は相互に密接な関
係を有しており、添加剤0ψの量が001重量部未満の
ときは防食効果の上から添加剤(■)の量が01重量部
超えることとなり、このため高温条件下における着色が
進行する結果となって好ましくない。また添加剤(v)
の量が0.01重量部未満のときは、添加剤(ivlの
みを増量してもリン系の酸化防止剤とくにホスファイト
系のものと併用する場合に防食効果は逆に低下し、02
重量部を超えろとこの傾向が著しい。
When the amount of additive (i) is less than 0.005 parts by weight, yellowing during long-term storage is unavoidable, while adding more than 0.2 parts by weight increases the occurrence of rust. Similarly, when the amount of additive (i) is less than 0.005 parts by weight, yellowing during long-term storage is unavoidable, while adding more than 0.2 parts by weight does not improve the effect.
When the amount is less than a certain volume, deterioration during heating is not suppressed, on the other hand 01
Adding more than 5 parts by weight will accelerate yellowing during long-term storage. The amounts of additives Gvl and (v) are closely related, and when the amount of additive 0ψ is less than 0.01 parts by weight, the amount of additive (■) will exceed 0.01 parts by weight for corrosion protection purposes, which is undesirable as it results in discoloration under high-temperature conditions. Also, additive (v)
When the amount is less than 0.01 parts by weight, even if only the amount of additive (ivl) is increased, the corrosion protection effect will actually decrease when used in combination with phosphorus-based antioxidants, especially phosphite-based ones, and 02
This tendency is particularly pronounced when the weight exceeds a certain limit.

本発明による組成物を製造する方法としては任意の公知
技術が使用できろ。代表的な例は上記5成分を乾燥混合
した後、配合物を機械的に溶融混練する方法であり、混
練には一軸および二軸押出機、各種ニーダ−などを用い
ることができる。
Any known technique can be used to produce the composition according to the present invention. A typical example is a method in which the five components are dried and mixed, and then the mixture is mechanically melt-kneaded. For kneading, single-screw and twin-screw extruders, various kneaders, etc., can be used.

なお本発明においては上記5成分のほかに、必要に応じ
て帯電防止剤、滑剤、紫外線吸収剤、光安定剤、造核剤
、難燃剤、抗ブロツキング剤、発泡剤、充てん剤、顔料
その他の添加剤を配合してもよい。
In addition to the five components mentioned above, the present invention may also include, as needed, an antistatic agent, a lubricant, an ultraviolet absorber, a light stabilizer, a nucleating agent, a flame retardant, an antiblocking agent, a foaming agent, a filler, a pigment, and other additives.

(発明の効果) 本発明によって得られろポリオレフィン組成物は、色安
定性、熱安定性および#4腐食性が著しく向上したもの
であり、とくに無脱灰プロセスにより製造されたポリオ
レフィンに適用した場合にその改良効果が大きく、これ
により従来に比べて長期保管中の黄変、加熱時または溶
融時の劣化および金属腐食などに対する安定性もしくは
抵抗性の大きく改善された組成物を提供することが可能
となった。
(Effects of the Invention) The polyolefin composition obtained by the present invention exhibits significantly improved color stability, thermal stability, and #4 corrosion resistance. The improvement effect is particularly pronounced when applied to polyolefins produced by a non-decalcification process. This makes it possible to provide a composition with significantly improved stability or resistance to yellowing during long-term storage, deterioration during heating or melting, and metal corrosion compared to conventional compositions.

(実施例および比較例) 以下、本発明を実施例および比較例に基づいて具体的に
説明するが、本発明はこれらによって限定されるもので
はない。なお実施例および比較例における性状の測定は
下記の方法によった。
(Examples and Comparative Examples) The present invention will be described in detail below based on examples and comparative examples, but the present invention is not limited thereto. The properties in the examples and comparative examples were measured by the following methods.

(色安定性) ペレットまたは成形品について、長期保管中の黄変の程
度を推定するための加速試験を行った。
(Color Stability) Accelerated testing was conducted on pellets or molded products to estimate the degree of yellowing during long-term storage.

すなわちm!!!l、た組成物で作製した厚さ21のプ
レスシートを温度80℃、相対湿度90%の恒温恒湿槽
内に2週間thn t、、 タe、黄色度(JIS K
7103ニヨる)を測定した。
In other words, a press sheet with a thickness of 21 made from the composition was placed in a constant temperature and humidity chamber at 80°C and 90% relative humidity for two weeks.
(Measured according to 7103)

(熱安定性) 成形品の熱安定性の目安として、同上のシートを120
℃のオーブン中に10日間J[した後の黄色度を測定し
た。これを加熱黄色度とする。
(Thermal Stability) As a guideline for the thermal stability of molded products, the same sheet as above is used at 120°C.
The degree of yellowness was measured after being placed in an oven at °C for 10 days. This is defined as the heated yellowness.

また組成物を溶融混練する際の熱安定性の目安として、
混線中の粘度変化に対応するトルクの変化を測定した。
Furthermore, as a guideline for thermal stability when melting and kneading the composition,
We measured the change in torque corresponding to the change in viscosity during wire interference.

すなわちTA製した組成物を東洋精機■製のラボプラス
トミルを用いて210℃、 4Qrpmで混練を行い、
ポリエチレンについてはトルクの変化が認められるに至
るまでの時@(IIIin)を測定し、ポリプロピレン
については201n混味後のトルクの低下率(%)を測
定した。これらを熱劣比変とする。
In other words, the TA-processed composition was kneaded at 210°C and 4Qrpm using a Laboplast mill manufactured by Toyo Seiki Co., Ltd.
For polyethylene, the time (III in) until a change in torque was observed was measured, and for polypropylene, the percentage decrease in torque after mixing with 201n was measured. These were defined as the thermal inferiority ratios.

(耐腐食性) 調製した組成物を250℃に加熱して溶融させ、その中
に軟鉄板を2hr浸せきし、取り出した後付着した組成
物を除去して、さらに温度80℃、相対湿度100%の
雰囲気中に20hrIk露した後のさびの発生量を重量
増加率で求めた。1%以下を014%以上を×1両者の
中間をΔとして表わした。
(Corrosion Resistance) The prepared composition was heated to 250°C and melted. A soft iron plate was immersed in it for 2 hours. After removing the plate, the adhering composition was removed, and the plate was further exposed to an atmosphere of 80°C and 100% relative humidity for 20 hours. The amount of rust generated was determined by the weight increase rate. Less than 1% was represented as 0, 4% or more as ×1, and the intermediate value between the two was represented as Δ.

及施1−ユニ1 使用した成分は次のとおりである。The ingredients used are as follows:

ポリオレフィン: (八)エチレン・1−ブテン共ffi合体(粉末状、 
 VFR18,密度0.942g/ crd 。
Polyolefins: (v) Ethylene-1-butene coffi compound (powdered,
VFR18, density 0.942g/crd.

Ti残留量9pp諺) 添加剤(i): (D)  ビス(2,4−ジ−tert−ブチルフェニ
ル)ペンタエリスリトール・ジホスファイト (商品名:ウルトラノツクス626.ボルグワーナー社
製) (E)  ビス(2,6−ジ−tert−ブチル−4−
)チk フz ニル)ペンタエリスリトール・ジホスフ
ァイト(商品名: マークPEP36.アデヵ・アーガ
ス化学■社PjB) 添加剤(ii! : (It)テトラキス(2,4−ジ−tert−ブチル7
 x 二、+I−)4.4゛−ビア1ニレン・ジホスフ
ァイト(商品名: イルガホスP−EPQ、チバガイギ
ー社製) 添加剤(l!θ: (1)ペンタエリスリトール・テトラキス[3−(3’
、5′−ジ−tert−ブチル−4′−ヒドロキシフェ
ニル)プロピオネート] (商品名ニイルガノックス1010.チバガイギー社製
) 添加剤(Iψ: (L)ステアリン酸カルシウム 添加剤(V): (M)ハイドロタルサイト (商品名: DHT−4人、協和化学工業■製)Mg0
.7AI0.3(OH) 2(CO3)。、 、SO,
5t120上記°5上記全5成に示す配合組成でトライ
ブレンドした後、40+m++φ押出機を用いて樹脂温
度150℃で組成物として造粒し、これを用いて試料を
調製し各種の性状試験を行った。その結果を表1に示す
。
Ti residue amount 9 pp (proverb) Additives (i): (D) Bis(2,4-di-tert-butylphenyl) pentaerythritol diphosphite (trade name: Ultranox 626, manufactured by BorgWarner) (E) Bis(2,6-di-tert-butyl-4-
) Chik Fz Nyl) Pentaerythritol Diphosphite (Product name: Mark PEP36. Adecca Argus Chemicals, Inc. PjB) Additive (ii! : (It) Tetrakis(2,4-di-tert-butyl 7)
x 2, +I-)4.4''-Via-1 Nylene Diphosphite (Trade name: Irgaphos P-EPQ, manufactured by Ciba-Geigy) Additive (l!θ: (1) Pentaerythritol Tetrakis[3-(3'
[5'-di-tert-butyl-4'-hydroxyphenyl)propionate] (Trade name: Nielganox 1010, manufactured by Ciba-Geigy) Additives (Iψ: (L) Calcium stearate Additives (V): (M) Hydrotalcite (Trade name: DHT-4, manufactured by Kyowa Chemical Industry Co., Ltd.) Mg0
.. 7AI0.3(OH)2(CO3). , ,SO,
Triblending was performed using the above-mentioned composition, and then the mixture was granulated as a composition at a resin temperature of 150°C using a 40+m++φ extruder. Samples were prepared using this granulated mixture and various property tests were conducted. The results are shown in Table 1.

Yζ較;1ご」−Σ 添加剤(1)として(D)ビア、(2,4−ジ−ter
t−ブチルフェニル)ペンタエリスリトール・ジホスフ
ァイトのほかに、次のホスファイト系化合物も使用した
以外は実施例1〜3と同じ成分を用い、表1に示す配合
組成で同上実施例と同様の処理を行って組成物を得た。
Yζ comparison; 1" - Σ additive (1) as (D) via, (2, 4-di-ter
The same components as in Examples 1 to 3 were used, except that the following phosphite compounds were also used in addition to t-butylphenyl)pentaerythritol diphosphite, and the compositions were obtained by performing the same treatment as in the above examples with the formulations shown in Table 1.

これを用いて性状試験を行った結果を表1に示す。Table 1 shows the results of the property test conducted using this method.

添加剤(i): (F)トリス(2,4−ジ−tart−ブチルフェニル
)ホスファイト (商品名:イルガホス168.チバガイギー社製)(G
)ジステアリル・ペンタエリスリトール・ジホスファイ
ト (商品名:つニストンB18.ボルグワーナー社製) 実施例 5,6.   例 16〜19ポリオレフイン
および添加剤側として、(A)エチレン・1−ブテン共
重合体および(1)ペンタエリスリトール・テトラキス
[3−(3’、5’−ジ−tert−ブチル−4′−ヒ
ドロキシフェニル)プロピオネート]の代わりに、それ
ぞれ次のものを用いた以外は実施例1〜3と同じ成分を
用い、表2に示す配合組成で同上実施例と同様の処理を
行って組成物を得た。これを用いて性状試験を行った結
果を表2に示す。
Additive (i): (F) Tris(2,4-di-tart-butylphenyl) phosphite (trade name: Irgaphos 168, manufactured by Ciba-Geigy) (G
) Distearyl pentaerythritol diphosphite (trade name: Niston B18, manufactured by BorgWarner) Examples 5, 6. Examples 16-19 The same components as in Examples 1-3 were used, except that the following were used instead of (A) ethylene-1-butene copolymer and (1) pentaerythritol tetrakis[3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate] as polyolefins and additives, and compositions were obtained by performing the same treatment as in the above examples with the formulations shown in Table 2. The results of property tests using these compositions are shown in Table 2.

ポリオレフィン: (B) ;!El密度ポリエチレン (粉末状、商品名:スタフレンE809 (M) 、日
本石油化学■製) 添加剤G1)l : (J)オクタデシル・3−(3’、S’−ジ−tert
−ブチル−4′−ヒドロキシフェニル)プロピオネート
(商品名ニイルガノックス107B、チバガイギー社製
) (K13.5−ジ−tert−ブチ/L、−4−1ニト
ロキシトルエン(B I T) 哀膣例 7.比較例20,21 ポリオレフィンとして(A)エチレン・1−ブテン共重
合体の代わりに次のものを用い、添加剤0ii)として
(1)ペンタエリスリトール・テトラキス[3−(3′
、5’−ジ−tert−ブチル−4−ヒドロキシフェニ
ル)プロピオネート]のほかに前記の(K)3.5−ジ
−tert−ブチル−4−ヒドロキシトルエン(BIT
)を用いた以外は実施例1〜3と同じ成分を用い、表2
に示す配合組成で同上実施例と同様の処理を行って組成
物を得た。これを用いて性状試験を行った結果を表2に
示す。
Polyolefin: (B); El high-density polyethylene (powder, product name: Staflen E809 (M), manufactured by Nippon Petrochemical Co., Ltd.) Additive G1): (J) Octadecyl-3-(3', S'-di-tert
-Butyl-4'-hydroxyphenyl)propionate (trade name Niilganox 107B, manufactured by Ciba-Geigy) (K13.5-di-tert-buty/L, -4-1 nitroxytoluene (BIT)) Example 7. Comparative Examples 20, 21 The following was used as the polyolefin instead of (A) ethylene-1-butene copolymer, and as the additive (0ii), (1) pentaerythritol tetrakis[3-(3'
In addition to the above (K) 3,5-di-tert-butyl-4-hydroxyphenyl (BIT) propionate,
Except for using ), the same components as in Examples 1 to 3 were used, as shown in Table 2.
A composition was obtained by performing the same treatment as in the above example with the formulation shown. The results of property tests performed using this composition are shown in Table 2.

ポリオレフィン: (C)ポリプロピレン (粉末状、商品名:日石ポリプロ J725N。Polyolefin: (C) Polypropylene (Powdered form, product name: Nisseki Polypro J725N)

日本石油化学■製) 尚上記実施例及び比較例で用いたポリオレフィンはいず
れも高活性チーグラー系触媒を用いて重合され、かつ脱
灰工程を経ていないものである。
(Manufactured by Nippon Petrochemical Co., Ltd.) The polyolefins used in the above examples and comparative examples were all polymerized using a highly active Ziegler catalyst and did not undergo a deashification process.

表1および表2の結果から明らかなように、本発明の範
囲である実施例1〜7のポリオレフィン組成物は色安定
性、熱安定性(加熱黄色度および熱劣化度)およびさび
抑制についてすぐれた性能を示し、安定性の改良がみら
れた。これに対し本発明の範囲外である比較例1〜21
においては、いずれも上記性状をバランスよく改善する
ことが困難であり、安定性の劣ることがわかる。
As is clear from the results in Tables 1 and 2, the polyolefin compositions of Examples 1 to 7, which fall within the scope of the present invention, showed excellent performance in terms of color stability, thermal stability (yellowing degree upon heating and degree of thermal degradation), and rust suppression, demonstrating improved stability. In contrast, Comparative Examples 1 to 21, which fall outside the scope of the present invention,
In all cases, it is difficult to improve the above properties in a balanced manner, indicating poor stability.

表中の記号説明: A:エチレン・1−ブテン共重合体エチレンB:高密度
ポリエチレンくスタフレンE809 (IJ) )C:
ポリプロピレンく日石ポリプロ J725N>D= ビ
ス(2,4−ジ−tert−ブチルフェニル)ペンタエ
リスリトール・ジホスファイトくウルトラノックス 6
26〉 E: ビス(2,6−ジ−tert−ブチに−4−/チ
k 7 x ニル)ペンタエリスリトール・ジホスファ
イトくマーク PEI’36) F: トリス(2,4−ジ−tert〜ブチルフェニル
)ホスファイトくイルガホス 168〉 G: ジステアリル・ペンタエリスリトール・ジホスフ
ァイトくウニストン 618〉 II: テトラキス(2,4−ジ−tart−ブチルフ
ェニル)4・4゛−ビフェニレン・ジホスファイトくイ
ルガホスP−EPQ) ■:ペンタエリスリトール・テトラキス[3−(3’、
 5’−ジ−tert−ブヂルー4′−ヒドロキシフェ
ニル)フロピ珂ネート]〈イルガノックス、工;オクタ
デシル・3−(3’、5’−レー乞ert−ブチル−4
′−ヒドロキシフェニル)ブ[1ビオネート〈イルガノ
ックス 1076> K:3.5−ジ−tert−ブチル−4−ヒドロキシト
ルエン<BIiT> Lニステアリン酸カルシウム
Explanation of symbols in the table: A: Ethylene-1-butene copolymer ethylene B: High-density polyethylene staflen E809 (IJ) C:
Polypropylene (Nisseki Polypropylene J725N>D = Bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite (Ultranox 6)
26) E: Bis(2,6-di-tert-butylphenyl)pentaerythritol diphosphite<mark PEI'36) F: Tris(2,4-di-tert-butylphenyl)phosphite<irgaphos 168) G: Distearyl pentaerythritol diphosphite<uniston 618) II: Tetrakis(2,4-di-tert-butylphenyl)4,4-biphenylene diphosphite<irgaphos P-EPQ) ■: Pentaerythritol tetrakis[3-(3',
[5'-di-tert-butyl-4'-hydroxyphenyl) fluorophenyl] [Irganox, octadecyl-3-(3',5'-tert-butyl-4')
'-hydroxyphenyl) b[1-bionate <Irganox 1076> K:3,5-di-tert-butyl-4-hydroxytoluene <BIiT> L calcium nystearate

Claims (4)

【特許請求の範囲】[Claims] (1)ポリオレフィンが下記の添加剤を含むことからな
る安定性の改善されたポリオレフィン組成物。 (i)下式で示されるペンタエリスリトール・ジホスフ
ァイト ▲数式、化学式、表等があります▼ (R_1、R_2:アリール基) (ii)テトラキス(2,4−ジ−tert−ブチルフ
ェニル)4,4′−ビフェニレン・ジホスホナイト(i
ii)3−(3′,5′−ジ−tert−ブチル−4′
−ヒドロキシフェニル)プロピオン酸のエステル (iv)脂肪酸の金属塩 (v)ハイドロタルサイト類
(1) A polyolefin composition with improved stability comprising the following additives: (i) Pentaerythritol diphosphite shown in the following formula ▲Formulas, chemical formulas, tables, etc. are available▼ (R_1, R_2: aryl group) (ii) Tetrakis(2,4-di-tert-butylphenyl)4,4'-biphenylene diphosphonite (i
ii) 3-(3',5'-di-tert-butyl-4'
(v) Hydroxyphenyl)propionic acid ester (iv) Metal salts of fatty acids (v) Hydrotalcites
(2)前記ポリオレフィンが高活性チーグラー系触媒を
用いて重合され、かつ脱灰工程を経ていないものである
特許請求の範囲第1項記載の安定性の改善されたポリオ
レフィン組成物。
(2) The polyolefin composition with improved stability according to claim 1, wherein the polyolefin is polymerized using a highly active Ziegler catalyst and has not undergone a decalcification step.
(3)前記(i)のペンタエリスリトール・ジホスファ
イトのR_1基およびR_2基が、いずれも2,4−ジ
−tert−ブチルフェニル基または2,6−ジ−te
rt−ブチル−4−メチルフェニル基である特許請求の
範囲第1項記載の安定性の改善されたポリオレフィン組
成物。
(3) The R_1 and R_2 groups of the pentaerythritol diphosphite in (i) above are both 2,4-di-tert-butylphenyl groups or 2,6-di-te
A polyolefin composition with improved stability as described in claim 1, wherein the group is rt-butyl-4-methylphenyl.
(4)前記(iii)のエステルがペンタエリスリトー
ル・テトラキス[3−(3′,5′−ジ−tert−ブ
チル−4′−ヒドロキシフェニル)プロピオネート]ま
たはオクタデシル・3−(3′,5′−ジ−tert−
ブチル−4′−ヒドロキシフェニル)プロピオネートで
ある特許請求の範囲第1項記載の安定性の改善されたポ
リオレフィン組成物。(5)前記(iv)の脂肪酸の金
属塩がステアリン酸カルシウムである特許請求の範囲第
1項記載の安定性の改善されたポリオレフィン組成物。
(4) The ester of (iii) above is pentaerythritol tetrakis[3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate] or octadecyl 3-(3',5'-di-tert-
(5) The improved stability polyolefin composition according to claim 1, wherein the metal salt of the fatty acid in (iv) is calcium stearate.
JP62173847A 1987-07-14 1987-07-14 Polyolefin composition with improved stability Expired - Fee Related JPH07107111B2 (en)