JPS6421082A - Production of powdery plated material - Google Patents
Production of powdery plated materialInfo
- Publication number
- JPS6421082A JPS6421082A JP62174919A JP17491987A JPS6421082A JP S6421082 A JPS6421082 A JP S6421082A JP 62174919 A JP62174919 A JP 62174919A JP 17491987 A JP17491987 A JP 17491987A JP S6421082 A JPS6421082 A JP S6421082A
- Authority
- JP
- Japan
- Prior art keywords
- plating
- solution
- suspension
- reaction
- core material
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【発明の詳細な説明】
〈産業上の利用分野〉
本発明は、めっき材料の製造法に関し、更に言えば、明
度の高いめっき材料の製造法に関する。[Detailed Description of the Invention] <Industrial Field of Application> The present invention relates to a method for manufacturing plating materials, and more specifically, to a method for manufacturing high-brightness plating materials.
〈従来の技術〉
一般に、無電解めっきはその技術の進歩と用途の開発に
よって、今日では有機または無機の材料を問わないのは
勿論、その形状や大きさに間係なく適用されている。と
は言え多くの場合、基材は板状又は成型体が多く、粉末
又は粒状のごとき微細なめつき基材についてはその用途
開発が新しいだけに最近のことであって、確立された製
造方法はなく、僅かに従来の一般的方法に従って処理さ
れているのが現状である。<Conventional Technology> Generally, due to advancements in technology and the development of applications, electroless plating can now be applied to organic or inorganic materials, regardless of their shape or size. However, in most cases, the substrates are in the form of plates or molded bodies, and the development of applications for finely plated substrates such as powders or granules is relatively recent, and there are no established manufacturing methods. Currently, they are mostly processed according to conventional general methods.
そこで、本発明者は、先に粉末、粉粒状基材に無電解め
っきをする方法として、基材を水性懸濁体にして、これ
に無電解めっき液を添加することによりめっき皮膜を形
成させる方法(特開昭60−59090@公報)を開発
している。Therefore, the inventors have previously developed a method for electroless plating powder or granular substrates, in which the substrate is made into an aqueous suspension and an electroless plating solution is added to form a plating film (Japanese Patent Publication No. 60-59090).
〈発明が解決しようとする問題点〉
一般に、金属粉体は粒径が小さくなると黒色となるので
、これらを混練して得られる塗料、JJ’l脂成型品等
は色調を暗くしたり、あるいは着色顔料を同時に使用す
る場合に彩度を低下させたりするが、無電解めっきによ
り臂られるめつき材料も例外ではないので、用途が限ら
れてしまう問題があった。<Problems the invention aims to solve> Generally, metal powders turn black as their particle size decreases, so paints and resin molded products obtained by mixing them tend to have a darker color tone, or the saturation is reduced when colored pigments are used at the same time. However, plated materials obtained by electroless plating are no exception, which limits their applications.
そこで、本発明者はシリカ又は/及びアルミナを含有す
るめつき皮膜を有する粉末めっき材料が、上記の問題点
を解決することを知見し本発明を得た。Therefore, the inventors discovered that a powder plating material having a plated film containing silica and/or alumina solves the above problems, and thus obtained the present invention.
く問題点を解決するための手段〉
即ち、被めつき基材粉末の水性懸濁体に無電解めっき液
を添加しながら、該粉末粒子表面に無電解めっき反応を
行わせるに際し、シリカゾル又は/及びアルミナゾルを
添加することを特徴とする粉末めっき材料のHR法であ
る。<Means for solving the problem> That is, an HR method for powder plating materials characterized by adding silica sol and/or alumina sol when performing an electroless plating reaction on the surface of the powder particles while adding an electroless plating solution to an aqueous suspension of the substrate powder to be coated.
まず、めっき材料におけるめつき基材(以下、単に「芯
材」と記載する)について説明する。First, let's explain the plating substrate (hereinafter simply referred to as "core material") in plating materials.
本発明の芯材は、その粒子径を特に限定するものではな
い。又、水に懸濁するものであればその形状は球状、棒
状、針状、中空状又は41維状いずれであってもよい。The core material of the present invention is not particularly limited in terms of particle size. Furthermore, as long as it is suspended in water, its shape may be spherical, rod-shaped, needle-shaped, hollow, or fibrous.
水に懸濁し得るものであるから、水に実質的に不溶性の
もの、好ましくは酸やアルカリに対しても溶解又は変質
しない安定なものである。Since it can be suspended in water, it is substantially insoluble in water, and preferably stable and does not dissolve or deteriorate in acids or alkalis.
又、芯材の材質は、有機質又は無機質を問わず無電解め
っき可能な材質を全て包含する。これらは、天然物又は
合成物のい゛ずれであってもよい。又、芯材は化学的に
均一な絹qで弱ることを要しないのはもちろんでおるが
、それが結晶質または非晶質(ガラスを含む)のいずれ
であってもよい。重要なことは、芯の表面が化学的にめ
っき液と反応して皮膜の形成能を有J“ることであり、
分散可能な材質ということである。Furthermore, the core material encompasses all materials that can be electrolessly plated, regardless of whether they are organic or inorganic. These may be natural or synthetic. The core material does not need to be chemically uniform, and it may be crystalline or amorphous (including glass). The important thing is that the surface of the core has the ability to chemically react with the plating solution to form a film.
It is a material that can be dispersed.
かかる芯材を例示的に列挙すれば、無機質芯材としては
、金属粉末(合金も含む)、金属又は非金属の酸化物(
含水物も含む)、アルミノ珪酸塩を含む金属珪酸塩、金
属炭化力、金属窒化物、金属炭酸塩、金属硫酸塩、金属
:模酸温、金属硫化物、金a酸塩、金属ハロゲン化物ま
たは炭素などであり、有機芯材としては天然繊維、天然
樹脂、ポリエチレン、ポリプロピレン、ポリ塩化ビニル
、ポリスチレン、ポリブテン、ポリアミド、ポリアクリ
ル酸エステル、ポリアクリルニトリル、ポリアセタール
、アイオノマー、ポリエステルなどの熱可塑性樹脂、ア
ルキッド樹脂、フェノール樹脂、尿素樹脂、メラミン樹
脂、キシレン樹脂、シリコーン樹脂又はジアリルフタレ
ート樹脂のごとき熱硬化性樹脂などが挙げられる。これ
らは、1種又は2種以上の混合物であってもよい。この
混合物というのは化学的に組成が不均一のものから芯材
として混合物であるいずれの場合も含むものである。Examples of such core materials include, as inorganic core materials, metal powders (including alloys), metal or nonmetal oxides (
Examples of organic core materials include metal silicates containing aluminosilicates (including hydrated materials), metal carbides, metal nitrides, metal carbonates, metal sulfates, metal sulfides, metal acetates, metal halides, or carbon. Examples of organic core materials include natural fibers, natural resins, thermoplastic resins such as polyethylene, polypropylene, polyvinyl chloride, polystyrene, polybutene, polyamide, polyacrylic acid esters, polyacrylonitrile, polyacetal, ionomer, and polyester, as well as thermosetting resins such as alkyd resins, phenolic resins, urea resins, melamine resins, xylene resins, silicone resins, or diallyl phthalate resins. These may be used individually or as mixtures of two or more. This mixture includes all cases from those with a chemically heterogeneous composition to those that are mixtures used as core materials.
かかる芯材表面状に無電解めっきするに当り、めっき反
応が生ずるような状態にある芯材の水性懸濁体を調製す
ることである。The process involves preparing an aqueous suspension of the core material in a state where the plating reaction occurs, in order to perform electroless plating on the surface of the core material.
ここに芯材がめつき反応が生ずるような状態にあるとい
うのは芯材をめっき処理するに当り、予め洗浄、エツチ
ング、増感及び活性化等芯材の物性に応じた前処理操作
を施してめっき反応ができる状態をいい、かかる前処理
は公知の方法が全て適用できる。The statement that the core material is in a state where a plating reaction can occur means that, before plating the core material, pretreatment operations such as cleaning, etching, sensitization, and activation are performed according to the physical properties of the core material to create a state where a plating reaction can occur, and all known methods can be applied to such pretreatment.
例えば、洗浄処理は芯材をアルカリ脱脂液にて浸漬脱脂
し、FA酸、i酸あるいは燐酸に浸漬することにより行
なわれる。引き続いて行なわれる触媒処理は可溶性第1
錫塩とパラジウム塩の混合コロイド溶液にて、次いで酸
又はアルカリ性水溶液で若しくはシランカップリング剤
とパラジウム混合水溶液にて、各々芯材と接触処理する
ことにより前処理すればよい。これらは既に公知のこと
であり、本発明において格別の前処理を行なう必要はな
い。For example, the cleaning process is carried out by immersing the core material in an alkaline degreasing solution and then immersing it in FA acid, i acid, or phosphoric acid. The subsequent catalytic treatment involves soluble first
The core material can be pretreated by contacting it with a mixed colloidal solution of tin salt and palladium salt, followed by contact with an acidic or alkaline aqueous solution, or with a mixed aqueous solution of a silane coupling agent and palladium. These methods are already known, and no special pretreatment is necessary in the present invention.
次に、かかる芯材の水性懸濁体というのは水または少な
くとも1種のめっき用薬剤などを添加した水溶液を媒体
とする芯材の懸濁体をいい、又めつき用薬剤というのは
金属塩、還元剤、錯化剤、反応促進剤あるいはpl−1
調整剤等めっき液を構成し得る薬剤であり、それらは1
種又は2!I以上であってもよい。Next, the aqueous suspension of the core material refers to a suspension of the core material using water or an aqueous solution to which at least one plating agent has been added as a medium, and the plating agent refers to a metal salt, reducing agent, complexing agent, reaction accelerator or pl-1
These are chemicals that can constitute a plating solution, such as adjusting agents, and they are 1
It can be one or more species.
ただ、めっき液内体を懸濁媒体とする場合には芯材の懸
濁体の調製の際に予めめっき反応が生じない程度の薄い
状態で用いることが必要である。通常は単なるpHを調
整した水性懸濁体で充分であるが、多くの場合芯材によ
っては錯化剤を添加した水性懸濁体が好適である。However, when using a suspension medium in the plating solution, it is necessary to prepare the suspension of the core material in a dilute state beforehand so that the plating reaction does not occur. Usually, a simple pH-adjusted aqueous suspension is sufficient, but in many cases, depending on the core material, an aqueous suspension with a complexing agent added is preferable.
錯化剤というのはめつぎ金属のイオンに対して錯化作用
のある化合物であり、例えば、クエン酸、酒石酸、リン
ゴ酸、乳酸、グルコン酸又はそのアルカリ金属塩やアン
モニウム塩等のカルボン酸く塩)、グリシン等のアミノ
酸、エチレンジアミン、アルキルアミン等のアミン類、
その他のアンモニウム、EDTA、ビロリン酸く塩)等
が挙げられ、それらは1種または2種以上であってもよ
い。A complexing agent is a compound that has a complexing effect on metal ions, such as citric acid, tartaric acid, malic acid, lactic acid, gluconic acid or its alkali metal salts or ammonium salts (carboxylates), amino acids such as glycine, amines such as ethylenediamine and alkylamine.
Other examples include ammonium compounds, EDTA, pyrophosphates, etc., and these may be present in one or more types.
かかる錯化剤を懸濁体に予め溶解させる場合の含有量は
最大10(1/1、望ましくは5〜5(1/jの範囲に
ある。When such a complexing agent is pre-dissolved in a suspension, the content is in the range of a maximum of 10 (1/1), preferably 5 to 5 (1/j).
又、L!濁体のpHはシリカゾルを添加する場合には4
〜10の範囲に調整し、アルミナゾル又はシリカゾルと
アルミナゾルの混合物を添加する場合には8〜10の範
囲に調製するのがよい。Also, the pH of the turbid substance is 4 when silica sol is added.
It is preferable to adjust the concentration to a range of ~10, and if alumina sol or a mixture of silica sol and alumina sol is added, it is preferable to adjust it to a range of 8 to 10.
水性懸濁体における芯材の分散性は物性によって異なる
ので、分散方法は適宜所望の手段、例えば、通常撹拌か
ら高速撹拌、あるいはコロイドミルまたはホモジナイザ
ーのごとき剪断分散装置等を用い、芯材のアグロメレー
トを出来るだけ除去した一次粒子に近い分散状態の懸濁
体を調製することが望ましい。なお、芯材を分散させる
に際し、例えば、界面活性剤等の分散剤を上記したよう
に必要に応じて用いることかできる。懸濁体の濃度は、
特に限定する理由はないが、スラリー濃度が低いとめつ
き濃度が低下するので処理容量が大となるから経済的で
なく、又、逆にその濃度が高くなると芯材の分散性が悪
くなるので芯材の物性に応じ適宜所望のスラリー濃度に
設定すればよい。多くの場合50〜700g/J、好ま
しくは100〜500g/Jの範囲にある。また、この
懸濁体中に芯材をめっきするに当り、めっきが効果的に
実施されるべく懸濁体の温度をめっき可能温度に予め調
節しておくことが、望ましい。Since the dispersibility of the core material in an aqueous suspension varies depending on its physical properties, it is desirable to prepare a suspension in a dispersion state close to primary particles by using appropriate means, such as normal stirring to high-speed stirring, or a shear dispersion device such as a colloid mill or homogenizer, to remove as much agglomerate of the core material as possible. Furthermore, when dispersing the core material, dispersants such as surfactants may be used as needed, as described above. The concentration of the suspension is:
There is no particular reason to limit it, but if the slurry concentration is low, the plating concentration decreases, resulting in a large processing capacity, which is not economical. Conversely, if the concentration is high, the dispersibility of the core material deteriorates, so the slurry concentration should be set appropriately according to the physical properties of the core material. In most cases, it is in the range of 50 to 700 g/J, preferably 100 to 500 g/J. Furthermore, when plating the core material in this suspension, it is desirable to pre-adjust the temperature of the suspension to the plating temperature in order to carry out the plating effectively.
かくしてwI製した芯材の水性懸濁体に、シリカゾル又
は/及びアルミナゾルと無電解めっき液を添加しながら
、被めりき基材の表面にめっき反応で行わせる際にシリ
カ又は/及びアルミナのゾルを添加してめっき皮膜を形
成させることが本発明において重要である。Thus, in the present invention, it is important to add silica sol and/or alumina sol and electroless plating solution to the aqueous suspension of the core material manufactured by wI, and to add silica and/or alumina sol during the plating reaction on the surface of the substrate to be plated to form a plating film.
本発明において用いる無電解めっき液は基本的には金属
塩、還元剤、錯を剤及びpH調整剤の各薬剤を所望の配
合割合により組成される水溶液でおる。The electroless plating solution used in this invention is basically an aqueous solution composed of a metal salt, a reducing agent, a complexing agent, and a pH adjusting agent in a desired mixing ratio.
本発明にかかる方法に6いて適用されるめっき皮膜は特
に限定はなく、従来知られている無電解めっきは全て適
用でき、例えば、代表的にはニッケルめっき、コバルト
めっき、銅めっき、金めつき、銀めっき等が挙げられる
ので、金属塩としては上記金属の可溶性塩の1種又は2
種以上があげられる。The plating film to be applied to the method of the present invention is not particularly limited, and all conventionally known electroless plating can be applied. For example, typical examples include nickel plating, cobalt plating, copper plating, gold plating, silver plating, etc. Therefore, as the metal salt, one or two of the soluble salts of the above metals can be used.
There are more than a few species.
還元剤としては、例えば、次亜りん酸ソーダ、水素化硼
素アルカリ、ヒドラジン等であり、錯化剤は前記したと
通りのものであり、また、pH調整剤としては酸又は苛
性アルカリ等が代表例である。Examples of reducing agents include sodium hypophosphite, boron hydride alkali, and hydrazine, while complexing agents are as described above. Typical pH adjusting agents include acids or caustic alkalis.
上記めっき液において、金属塩と還元剤の配合割合は、
使用する還元剤により異なるが、例えば、還元剤に次亜
′II4酸ソーダを使用し、金属塩としてニッケル塩を
使用する場合、ニッケル塩1モルに対し次亜燐酸ソーダ
2.0〜3.0モルが適当でおり、還元剤に水素化硼素
アルカリを使用する場合には、ニッケル塩1モルに対し
て水素化lI素アルカリが1.5〜2.5モルが適当で
ある。In the above plating solution, the mixing ratio of the metal salt and the reducing agent is:
The appropriate amount varies depending on the reducing agent used. For example, when sodium hypophosphate is used as the reducing agent and nickel salt is used as the metal salt, 2.0 to 3.0 moles of sodium hypophosphate is appropriate per mole of nickel salt. When using alkali borohydride as the reducing agent, 1.5 to 2.5 moles of alkali 1.0 nickel salt is appropriate.
添加する金属及び還元剤の水溶液濃度は高い程経済的で
あるが特に限定はない。While higher concentrations of the aqueous solutions containing the added metal and reducing agent are more economical, there are no particular limitations.
通常めっき液を建浴し、該浴に基材を浸漬処理してめっ
き操作を行なうのと異なり、本発明では無電解めっき液
を、水性懸濁体に添加してめっき反応を行わせるために
、その容量の大小に応じて希釈されることと相俟つて、
通常建浴めっき液の濃度よりも濃くすることができる。Unlike conventional methods where a plating solution is prepared as a bath and the substrate is immersed in it to perform the plating operation, in this invention, the electroless plating solution is added to an aqueous suspension to carry out the plating reaction. Combined with the fact that it is diluted according to the volume,
The concentration of the plating solution can be made higher than that of a typical plating bath.
次に、めっき反応において添加するゾルとしてはシリカ
ゾル、例えば、珪酸ソーダ水溶液を陽イオン交換樹脂に
より処理して又は鉱酸類で中和して僻られるもの、アル
ミナゾルとしては、例えば、塩基性硫酸アルミニウムを
含窒素塩基で中和することによって得られるものなどが
挙げられるが、特に限定するものではない。又、ゾルの
粒子の大きさや濃度についても芯材やめつき条件に応じ
て適宜選択することができる。Next, examples of sols added in the plating reaction include silica sol, for example, obtained by treating an aqueous sodium silicate solution with a cation exchange resin or neutralizing it with mineral acids, and alumina sol, for example, obtained by neutralizing basic aluminum sulfate with a nitrogen-containing base, but these are not particularly limited. Furthermore, the particle size and concentration of the sol can be appropriately selected according to the core material and plating conditions.
めっき反応において懸濁体は分散状態が保たれるよう、
必要に応じた、撹拌、超音波分散処理などを与えておく
ことが望ましく、また温度も制御できるように設定して
おくことが望ましい。ここで、制御しながら添加すると
いうのは液濃度と共に添加速度がめつき反応に直接的に
影響し、また、この要素は芯材の物性、特に表面特性に
も著しく関係するのでこれらの要素を充分に考慮した上
で、めつきむらの生じないよう均−且つ強固なめつき皮
膜を形成させるためにめっき液の添加速度を設定すると
いうことであり、多くの場合徐々に添加する方がよい。In the plating reaction, the suspension is kept in a dispersed state.
It is desirable to provide stirring, ultrasonic dispersion treatment, etc., as needed, and it is also desirable to set the temperature so that it can be controlled. Here, adding while controlling the rate directly affects the plating reaction along with the liquid concentration, and this element is also significantly related to the physical properties of the core material, especially the surface properties, so the rate of addition of the plating solution should be set after taking these elements into full consideration in order to form a uniform and strong plated film without uneven plating, and in most cases it is better to add it gradually.
従って、本発明ではめつき液を水性懸濁液に添加すると
は、その組成液全部を添加する場合は勿論であるが、前
記の通り、例えば、錯化剤を予め水性@温体の調製に使
用している場合には残りの薬液を言うものであって、要
するにめっき反応を生ぜしめる#液を添加することをい
う。Therefore, in this invention, adding a plating solution to an aqueous suspension means not only adding the entire composition of the solution, but also, as mentioned above, if, for example, a complexing agent has been used in advance to prepare the aqueous solution, it refers to the remaining chemical solution, and in short, it means adding the solution that causes the plating reaction.
次に、本発明において、めっき反応の際にシリカゾル等
を添加するというのは、めっき液と同時に添加させる場
合、めっき液を添加してめっき反応をスタートさせた後
のいずれかであってもよいが、多くの場合、後者の方が
望ましい。Next, in the present invention, the addition of silica sol or the like during the plating reaction may be done either simultaneously with the plating solution or after the plating solution has been added and the plating reaction has started, but in most cases the latter is preferable.
尤も必要に応じ、その一部を懸濁体に分散させておいた
り、あるいは、めっき終了後、添加してコーティング処
理を行うこともできる。However, if necessary, a portion of it can be dispersed in a suspension, or it can be added after the plating process to perform a coating treatment.
このシリカゾル又は/及びアルミナゾルとの添加におい
てはめつき液の添加との関係において、いくつかの態様
が適宜選択されるが多くの場合、要すれば、水性@温体
のpH調整の為アルカリ剤を個別的且つ同時に添加する
ことが望ましい。この理由はめっき液の添加によってめ
っき反応が進行し、液中の次亜燐酸ソーダのごとき還元
剤が酸化されるに従って水素イオン濃度が増加し、次第
に水性懸濁体のpHが低下することによる。それ故、当
初に設定したpHを一定に保持するためにめっき液とD
H調整剤とを上記の如く並行して添加するのがよい。添
加方法はpHをコントロールしながら、添加する方法も
よいが、還元剤の酸化還元反応に見合った是のアルカリ
堡を所定の濃度にして添加することでもよい。シリカゾ
ル又はアルミナゾル添加量が相対的に増加すると、めっ
き材料の明度は高くなるが、導電性は逆に低下するので
、用途に応じて、適宜シリカゾル、アルミナゾルの添加
量を設定する必要がある。In the addition of silica sol and/or alumina sol, several methods can be appropriately selected in relation to the addition of the plating solution, but in many cases, it is desirable to add an alkaline agent individually and simultaneously to adjust the pH of the aqueous solution, if necessary. This is because, upon addition of the plating solution, the plating reaction proceeds, and as reducing agents such as sodium hypophosphite in the solution are oxidized, the hydrogen ion concentration increases, and the pH of the aqueous suspension gradually decreases. Therefore, in order to maintain the initially set pH constant, the plating solution and D
It is best to add the pH adjusting agent in parallel as described above. While it is possible to add the agent while controlling the pH, it is also acceptable to add an alkali solution at a predetermined concentration that matches the oxidation-reduction reaction of the reducing agent. As the amount of silica sol or alumina sol added increases relatively, the brightness of the plated material increases, but the conductivity decreases. Therefore, it is necessary to appropriately set the amount of silica sol or alumina sol added depending on the application.
このようにして、無電解めっき液を水性懸濁体に制御し
て添加することにより懸濁体中で速やかなめっき反応が
生じ分散した芯材表面に均−且つ強固で、ゾル粒子を含
有した特異なめつき皮膜が形成されてゆく。従ってこれ
らの添加量に応じてめっき皮膜の膜厚を調節することが
でき、用途に応じて、添加量は設定すればよい。In this way, by controlling the addition of the electroless plating solution to the aqueous suspension, a rapid plating reaction occurs in the suspension, forming a uniform, strong, and uniquely smooth coating containing sol particles on the dispersed core material surface. Therefore, the thickness of the plating film can be adjusted according to the amount of these additives, and the amount of additives should be set according to the application.
〈実施例〉
実施例1〜6
第1表に示した各種粉末を通常の方法で脱脂し、洗浄し
て前処理をした。<Examples> Examples 1-6 The various powders shown in Table 1 were degreased and washed using conventional methods for pretreatment.
上記前処理を施した粉体20gを酒石酸ソーダの5 0
g/J水溶液1jに投入し、アグロメレートが実質的
にない様に分散処理を施し、温度を80℃に加温して水
性懸濁体を調製した。20g of the powder that has undergone the above pretreatment is mixed with 50g of sodium tartrate.
The substance was added to 1 joule of a g/J aqueous solution and dispersed until virtually no agglomerates remained. The temperature was then heated to 80°C to prepare an aqueous suspension.
次いで、1mol /j 1ii!@ニツケル水溶液及
び2、 5IRol /1次亜燐酸ソーダ水溶液を4r
d1分の速度で撹拌下の上記懸濁液に滴下し反応をスタ
ートさせた。反応開始後pH自vJ調節装置を用い水酸
化ナトリウム3no!/J水溶液でpH’=7から徐々
にpト1=9.5まで30分間で上昇させた。pH=9
.5になったところで、上記2液に加えてシリカゾルの
5%水溶液(日本化学工業(株)(製)シリカドール2
0G(商標名))を4−7分の速度で反応中の溶液に滴
下した。硫酸ニッケル及び次亜燐酸ソーダ水溶液を34
0戒、シリカゾル溶液220戴滴下したところで、滴下
を止めた。この間、水酸化ナトリウム水溶液を用いてp
H=9.5に保持した。発泡が止まったら、撹拌を止め
て反応液を濾別し、めっき製品を2回リパルプした後、
真空乾燥機で乾燥した。Next, a 1 mol/j 1ii! aqueous solution and a 2,5 IRo ol/1 sodium phosphite aqueous solution are added to 4r
The reaction was started by adding the above suspension dropwise at a rate of d1 min under stirring. After the reaction started, the pH was gradually increased from pH' = 7 to pH1 = 9.5 over 30 minutes using a pH adjustment device with a sodium hydroxide 3 no 1/J aqueous solution.
When the concentration reaches 5, add the above two liquids to a 5% aqueous solution of silica sol (Silica Doll 2, manufactured by Nippon Chemical Industrial Co., Ltd.).
0G (trademark name) was added dropwise to the reaction solution at a rate of 4-7 minutes. Nickel sulfate and sodium hypophosphite aqueous solutions were added in 34
After adding 0 drops of silica sol solution (220 ml), the addition was stopped. During this time, sodium hydroxide solution was used to p
The temperature was maintained at H = 9.5. Once the foaming stopped, the stirring was stopped and the reaction solution was filtered off. The plated product was then repulped twice.
It was dried in a vacuum dryer.
実施例7〜11
平均粒径8μm中空セラミック粒子(米国ジラント社(
製)ジオスファ#600 (商標名))を通常の方法で
脱指し、洗浄し、前処理をした。Examples 7-11 Hollow ceramic particles with an average particle size of 8 μm (Zilant Corporation, USA)
The Geospha #600 (trademark) was de-finished using the usual method, cleaned, and pre-treated.
前処理した粉体20gを酒石酸ソーダの5g/l水溶液
1j!に投入し、アグロメレートが実質的にないように
分散処理を施し、温度を70℃に加温して水性懸濁体を
調製した。20 g of pre-treated powder was added to 1 joule of a 5 g/l aqueous solution of sodium tartrate, dispersed to virtually eliminate agglomerates, and heated to 70°C to prepare an aqueous suspension.
次いで、1110+/Jの1iAFiニツケル水溶液、
及び2.5110171次亜燐酸ソーダ水溶液を3戒/
分の速度で撹拌下の上記懸濁液に滴下し反応させスター
トさせた。反応開始後1)H自vJ調節装置を用い3n
+ol/J苛性ソーダ水溶液でpH=7から徐々にpl
−1=9.5まで30分間で上昇させた。pH=9.5
になったら上記2液に加えて第2表に示すシリカゾルの
水溶液(日本化学工業(製)シリカドール20G(商標
名))を3d/分の速度で反応中の溶液に滴下した。Next, an aqueous solution of 1 iAFi at 1110+/J,
and 2.5110171 sodium hypophosphate aqueous solution 3 times/
The reaction was started by dropping the above suspension into agitated water at a rate of 1 minute. After the reaction started, 1) the H-vJ adjustment device was used to control 3n
+ ol/J Caustic soda aqueous solution, gradually increasing the pH from 7 to pl
The pH was raised to -1 = 9.5 in 30 minutes.
Once the two solutions mentioned above were added, an aqueous solution of silica sol (Silica Doll 20G (trademark name), manufactured by Nippon Chemical Industrial Co., Ltd.) shown in Table 2 was added dropwise to the reacting solution at a rate of 3 d/min.
硫酸ニッケル及び次亜燐酸ソーダ水溶液は340d、シ
リカゾル溶液は250M1滴下したところで滴下を止め
る。この間苛性ソーダ水溶液を用いてpH=9.5に保
持した。発泡が止まったら撹拌を止め反応液を濾別し、
めっきした製品を2回リパルプした後、真空乾燥機で乾
燥した。The nickel sulfate and sodium hypophosphite aqueous solutions were added dropwise at 340d, and the silica sol solution was added dropwise at 250M, at which point the addition was stopped. During this time, the pH was maintained at 9.5 using a caustic soda aqueous solution. Once the foaming stopped, stirring was stopped and the reaction mixture was filtered off.
The plated products were repulped twice and then dried in a vacuum dryer.
実施例12
平均粒径8μm中空セラミック粒子(米国ジラント社(
製)ジオスファ#600 (商標名))を通常の方法で
脱脂し、洗浄し、前処理をした。Example 12 Hollow ceramic particles with an average particle size of 8 μm (Zilant Corporation, USA)
The Geospha #600 (trademark) was degreased, washed, and pre-treated using the usual method.
前処理した粉体20gを酒石酸ソーダの5g/l水溶液
1jに投入し、アグロメレートが実質的にないように分
散処理を施し、温度を80℃に加温して水性懸濁体を調
製した。20 g of pre-treated powder was added to 1 joule of a 5 g/l aqueous solution of sodium tartrate, dispersed to virtually eliminate agglomerates, and heated to 80°C to prepare an aqueous suspension.
次いで、ll1ol/jの硫酸ニッケル水溶液、及び2
.5nol 、1次亜燐酸ソーダ水溶液を3i/分の速
度で撹拌下の上記懸濁液に滴下し反応させスタートさせ
た。反応開始後pH自自網調節装置用い3mol/J苛
性ソーダ水溶液でpH−8から徐々にpH=9.5まで
30分間で上昇させた。pH=9.5になったら上記2
液に加えてアルミナゾルの水溶液(粒径401μ、濃度
50/J )を3d/分の速度で反応中の溶液に滴下し
た。Next, an aqueous solution of nickel sulfate in a 1 ol/j concentration, and 2
5 nol of a sodium primary phosphite aqueous solution was added dropwise to the above suspension under stirring at a rate of 3 i/min to start the reaction. After the reaction started, a pH self-adjusting device was used to gradually raise the pH from -8 to 9.5 over 30 minutes with a 3 mol/J sodium caustic soda aqueous solution. Once the pH reached 9.5, the above 2
In addition to the liquid, an aqueous solution of alumina sol (particle size 401 μm, concentration 50/J) was added dropwise to the reacting solution at a rate of 3 d/min.
WN酸ニッケル及び次亜燐酸ソーダ水溶液は340d、
アルミナゾル溶液は220d滴下したところで滴下を止
める。この間苛性ソーダ水溶液を用いてpH=9.5に
保持した。発泡が止まったら撹拌を止め反応液を濾別し
、めっきした製品を2回リパルプした襖、真空乾燥機で
乾燥した。Nickel WNate and sodium hypophosphite aqueous solution are 340d,
The alumina sol solution was added dropwise for 220 days, at which point the addition was stopped. During this time, the pH was maintained at 9.5 using a caustic soda solution. Once the foaming stopped, stirring was stopped, the reaction solution was filtered off, and the plated products were dried in a vacuum dryer using a repulped fusuma (paper sliding door) twice.
比較例1〜6
実施例1〜6と同じ粉体を使用し、同様のめつき条件で
、但し、シリカゾルの水溶液を滴下せず、ニッケルめつ
き粉体を製造した。Comparative Examples 1-6 Nickel-plated powder was produced using the same powder as in Examples 1-6, under the same plating conditions, except without adding an aqueous silica sol solution dropwise.
樹脂成型品の明度の比較
実施例1〜12及び比較例1〜6で作成した試料及びエ
ポキシ樹脂を第3表に示した堡を乳鉢に取り充分に混合
した後30 X 50 X 3 cmの板状に成型、固
化した後、明度をスガ試験機(株)(製)カラーメータ
ー(AUD−8CH−3型ンを用いて測定した結果を第
3表に示す。Table 3 shows the results of measuring the brightness of resin molded products. The samples and epoxy resin prepared in Examples 1 to 12 and Comparative Examples 1 to 6 were placed in a mortar and pestle as shown in Table 3, thoroughly mixed, molded into a 30 x 50 x 3 cm plate, and then solidified. The brightness was then measured using a colorimeter (AUD-8CH-3 model) manufactured by Suga Test Instruments Co., Ltd.
第 3 表
但し、表中Aは、実施例1〜11がS r O2111
2がAI203
〈発明の効果〉
かくして、本発明にかかる方法によれば粉末または粒状
の芯材について実質的に一次粒子に近い状態でシリカ又
は/及びアルミナを含有する均一なめつき皮膜を付与す
ることができ、またその膜厚は精度よく自白に設定する
ことができる。Table 3, however, in the table, A is SrO2111 for Examples 1 to 11.
2 is AI203 <Effects of the Invention> Thus, according to the method of the present invention, a uniform smooth coating containing silica and/or alumina in a state substantially close to primary particles can be applied to a powder or granular core material, and the film thickness can be precisely set to self-white.
他方、めっき操作の面からみるとめっき反応は完全に停
止するまで行なわれるのでめっき薬剤を効率よく使用で
きること、めっき雰囲気が安定しているので各成分濃度
の調節が不要であるのみならずpHの変動も実質的に回
避できその為の調製装置も特に必要としないなど従来に
比べて数々の利点が挙げられる。On the other hand, from the perspective of the plating operation, since the plating reaction is carried out until it is completely stopped, the plating agent can be used efficiently. Furthermore, because the plating atmosphere is stable, not only is it unnecessary to adjust the concentration of each component, but pH fluctuations can also be virtually avoided, and no special preparation equipment is required for that purpose. These are just some of the many advantages compared to conventional methods.
本発明により得られためつき材料は、明度が高いので、
帯電防止剤として床や壁等に適用することができる。The material obtained by the present invention has high brightness,
It can be applied to floors, walls, etc., as an antistatic agent.
又、着色顔料と併用しても彩度を低下させることが少な
いという利点がある。Furthermore, it has the advantage of not significantly reducing saturation even when used in combination with coloring pigments.
更に本発明により得られるめっき材料の用途は帯電防止
剤だけでなく導電性ゴム、4電性樹脂、導電性接着剤、
導電性ペースト等従来は、金属粉体やカーボン粉末が利
用されていた分野への利用が期待される。Furthermore, the plating material obtained by the present invention has applications not only as an antistatic agent but also as a conductive rubber, tetraelectric resin, conductive adhesive,
It is expected to be used in fields where metal powders or carbon powders were previously used, such as in conductive pastes.
Claims (1)
しながら、該粉末粒子表面に無電解めつき反応を行わせ
るに際し、シリカゾル又は/及びアルミナゾルを添加す
ることを特徴とする粉末めっき材料の製造法A method for producing a powder plating material, characterized by adding silica sol and/or alumina sol when carrying out an electroless plating reaction on the surface of powder particles while adding an electroless plating solution to an aqueous suspension of powder of a substrate to be plated.