JPS6433902A - Voltage non-linear resistance ceramic composition - Google Patents
Voltage non-linear resistance ceramic compositionInfo
- Publication number
- JPS6433902A JPS6433902A JP62188893A JP18889387A JPS6433902A JP S6433902 A JPS6433902 A JP S6433902A JP 62188893 A JP62188893 A JP 62188893A JP 18889387 A JP18889387 A JP 18889387A JP S6433902 A JPS6433902 A JP S6433902A
- Authority
- JP
- Japan
- Prior art keywords
- parts
- weight
- varistor
- voltage
- composition
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
Description
【発明の詳細な説明】
〔産業上の利用分野〕
本発明は5rTi02を主成分とする電圧非直線性抵抗
体(以下、バリスタと称する)を得る為の磁器組成物に
関する。[Detailed Description of the Invention] [Industrial Field of Application] The present invention relates to a porcelain composition for obtaining a voltage nonlinear resistor (hereinafter referred to as a varistor) mainly composed of 5rTiO2.
電子機器で発生する異常電圧、ノイズ等を吸収もしくは
除去する為に、従来種々のバリスタが使用されているが
、特公昭55−49404号公報に示されている5rT
t03を主成分とするバリスタは、バリスタ機能のみな
らずコンデンサ機能も存するので、グロー放電、アーク
放電、異常電圧、ノイズ等の吸収又はバイパスを良好に
達成することができる利点がある。
Various varistors have been conventionally used to absorb or remove abnormal voltages, noise, etc., generated in electronic equipment, but the 5rT shown in Japanese Patent Publication No. 55-49404 is a different type.
A varistor with t03 as its main component possesses not only varistor functionality but also capacitor functionality, offering the advantage of effectively absorbing or bypassing glow discharge, arc discharge, abnormal voltage, noise, and other phenomena.
しかし、最近サージ電圧及び電流の印加による特性の劣
化が更に少ないバリスタが要求されている、そこで本発
明の目的は、サージ印加の際のバリスタ電圧、非直線係
数の劣化が少ない電圧非直線性抵抗体磁器組成物を提供
することにある。
However, there is a growing demand for varistors that exhibit even less degradation of characteristics due to the application of surge voltage and current. Therefore, the object of the present invention is to provide a voltage nonlinear resistive ceramic composition that exhibits less degradation of varistor voltage and nonlinearity coefficient when surges are applied.
前記目的を達成する為の第1番目の発明はチタン酸スト
ロンチウム5rTi03 (以下、第1成分と呼ぶ)1
00重量部に対して、酸化ニオブNbzOs、酸化タン
グステンWO,l、酸化ランタンLag’s、 M化セ
リウムCeO□、酸化ネオジムNdz03.酸化プラセ
オジムPrbG++s酸化イツトリウムYtox、 f
fJ、化ユーロピウムEuzOx1M化サマリウムSm
zOsの内の少なくとも1種の金属酸化物(以下、第2
成分と呼ぶ)を0.005〜5.0重量部、酸化シリコ
ンSiO□(以下、第3成分と呼び)を0.005〜5
.0重量部及び酸化リチウムLizO+ 酸化カリウム
に20、酸化セシウムC5zO,酸化ルビジウムRh、
Oの内の少なくとも1種の金属酸化物を0.005〜2
.5重量部含むことを特徴とする電圧非直線性抵抗体磁
器組成物である。
The first invention to achieve the above objective is strontium titanate 5rTiO3 (hereinafter referred to as the first component) 1
Per 00 parts by weight: Niobium oxide (NbzOs), Tungsten oxide (WO,l), Lanthanum oxide (Lag's), Cerium oxide (CeO□), Neodymium oxide (NdzO3), Praseodymium oxide (PrbG+s), Ytztrium oxide (Ytox), f
fJ, Europium EuzoOx1M Samarium Sm
At least one metal oxide among zoos (hereinafter referred to as the second)
0.005 to 5.0 parts by weight of component (hereinafter referred to as component 3), and 0.005 to 5 parts by weight of silicon oxide SiO□ (hereinafter referred to as component 3).
0 parts by weight and 20 parts lithium oxide (LizO+) and potassium oxide, cesium oxide (C5ZO), rubidium oxide (Rh),
At least one metal oxide from O is 0.005 to 2
This is a voltage-nonlinear resistive ceramic composition characterized by containing 5 parts by weight of [a specific substance].
上記発明において第1成分は磁器の主成分であり、第2
成分は主に半導体化に寄与する金属酸化物であり、第3
成分は主に非直線係数の改善及びサージに対するバリス
タ電圧、非直線係数の劣化防止に寄与し、第4成分は主
にサージに対するバリスタ電圧、非直線係数の劣化防止
及び非直線係数の改善に寄与するものである。In the above invention, the first component is the main component of porcelain, and the second component is...
The components are mainly metal oxides that contribute to semiconductor formation, and the third
The components primarily contribute to improving the nonlinearity coefficient and preventing deterioration of the varistor voltage and nonlinearity coefficient against surges, while the fourth component primarily contributes to preventing deterioration of the varistor voltage and nonlinearity coefficient against surges and improving the nonlinearity coefficient.
従って、第1.第2.第3及び第4成分を含む磁器組成
物でバリスタを作成すると、非直線係数が改善されるば
かりでなくサージの印加に対するバリスタ電圧、非直線
係数の劣化が少なくなる。Therefore, when a varistor is made using a porcelain composition containing the first, second, third, and fourth components, not only is the nonlinearity improved, but the degradation of the varistor voltage and nonlinearity in response to surge application is also reduced.
次に、第2番目の発明は、前記第1番目の磁器組成に更
に酸化コバル)Cod、酸化クロムCrtOs+酸化ニ
ッケルNip、酸化鉄FezOx、酸化アンチモン5b
zOt、酸化ビスマスBizOz+酸化マンガンMnO
、酸化アルミニウム^”!(hの内の少な(とも1種の
酸化物(以下、第5成分と呼ぶ)を0.01〜5.0重
量部を付加したことを特徴とする電圧非直線性抵抗体磁
器組成物である。Next, the second invention further adds cobalt oxide (Cod), chromium oxide (CrtOs), nickel oxide (Nip), iron oxide (FeZOx), and antimony oxide (5b) to the first porcelain composition.
zOt, bismuth oxide (BizOz) + manganese oxide (MnO)
This is a voltage-nonlinear resistive ceramic composition characterized by the addition of 0.01 to 5.0 parts by weight of at least one type of oxide (hereinafter referred to as the fifth component) from among aluminum oxide.
この第5成分は主として非直線係数の改善に寄与するも
のであり、従って、これを付加することによりサージ印
加による特性劣化が少なく且つ非直線係数が更に大きな
バリスタを提供することが可能になる。This fifth component primarily contributes to improving the nonlinearity coefficient; therefore, by adding it, it becomes possible to provide a varistor with less characteristic degradation due to surge application and an even larger nonlinearity coefficient.
次に、第1番目の発明に係る実施例(1〜3)を示す。Next, embodiments (1 to 3) of the first invention are shown.
(実施例1)
原料としてSrCO3,Ti0z、 Nb*05,5i
Ot、 LizCOi。
(Example 1) Raw materials: SrCO3, Ti0z, Nb*05, 5i
Ot, LizCOi.
KxCOs、 C5zCOs+ Rb2CO5を第1表
の組成になる様(但し、5rCOsとTie、から得ら
れる5rTiOsの組成は、いずれも100重量部とし
た。以下の実施例において同じ、)にそれぞれ換算秤量
配合し、ポリエチレンポット及びin石を用いて10〜
20時間混合した後、脱水、乾燥する。その後1150
〜1250℃で仮焼成し、粗粉砕の後、再びポリエチレ
ンポット及び璃瑞石を用いて10〜20時間混合する。KxCOs, C5zCOs + Rb2CO5 were each weighed and mixed to obtain the composition shown in Table 1 (however, the composition of 5rTiOs obtained from 5rCOs and Tie was set to 100 parts by weight each. The same applies in the following examples), and then mixed using polyethylene pots and in stone for 10 to 10
After mixing for 20 hours, dehydrate and dry. Then 1150
After calcination at ~1250°C and coarse grinding, the mixture is mixed again in a polyethylene pot and rizuite for 10 to 20 hours.
その後、再び脱水、乾燥するやできあがった材料に10
〜15重量%のポリビニールアルコールを有機結合剤と
して混入して造粒し、成型圧約2 ton/cdで直径
10籠、厚さ1鶴の成形体を作成した。After that, the finished material is dehydrated and dried again, and then 10
The material was granulated with approximately 15% by weight of polyvinyl alcohol as an organic binder, and molded into a 10-centimeter diameter basket with a thickness of 1 tsuru (a unit of measurement) at a molding pressure of approximately 2 tons/cd.
これらの円板をN1(95容積%)−+−ox(5容積
%)の還元雰囲気中で約1350℃14時間の焼成を行
ない半導体磁器を得た。次にこれを空気中(elI化性
雰囲気中)において1000〜1300℃の温度範囲で
3時間の熱処理(再酸化処理)を行なった。These discs were fired in a reducing atmosphere of N1 (95 vol%) -+-ox (5 vol%) at approximately 1350°C for 14 hours to obtain semiconductor porcelain. Next, these were subjected to heat treatment (re-oxidation treatment) in air (elI-forming atmosphere) at a temperature range of 1000 to 1300°C for 3 hours.
次に、上記磁器の特性を調べる為に第1図に示す如く磁
器lの両生面に銀ペーストを塗布し、800℃で焼付け
ることによって銀電極2,3を形成し、バリスタ4を完
成させた。Next, in order to investigate the properties of the porcelain, silver paste was applied to both sides of the porcelain l as shown in Figure 1, and silver electrodes 2 and 3 were formed by firing at 800°C, thereby completing the varistor 4.
次に、バリスタの特性評価を行なう為に、バリスタ電圧
■1、非直線係数α、静電容量C、サージ電圧印加によ
る■1及びαの変化率Δv1.。Next, in order to evaluate the characteristics of the varistor, the varistor voltage ■1, the nonlinearity coefficient α, the capacitance C, and the rate of change Δv1 of ■1 and α due to the application of surge voltage are determined.
Δα2を測定した所、第1表(電気的特性の項)に示す
結果が得られた。When Δα² was measured, the results shown in Table 1 (Electrical Characteristics section) were obtained.
各測定方法を更に詳しく説明すると、バリスタ電圧■1
は第2図に示す回路を使用して測定した。To explain each measurement method in more detail, let's look at the varistor voltage ■1
The measurement was performed using the circuit shown in Figure 2.
即ち、直流定電流源5とバリスタ4との間に電流計6を
接続し、バリスタ4に並列に電圧計7を接続し、バリス
タ4に1w+Aの電流■、を流し、その時の電圧を測定
してバリスタ電圧v1とした。また非直線係数αは、第
2図の装置を使用しバリス夕電圧v1の他にバリスタ4
に10a+Aの電流■1・を流した時の印加電圧v1゜
を測定し、次式によって求めた。Specifically, an ammeter 6 was connected between the DC constant current source 5 and the varistor 4, a voltmeter 7 was connected in parallel with the varistor 4, and a current of 1W + A was passed through the varistor 4. The voltage at that time was measured and defined as the varistor voltage v1. In addition, the nonlinearity coefficient α was determined using the apparatus shown in Figure 2, in addition to the varistor voltage v1, by measuring the voltage of the varistor 4
The applied voltage v1° was measured when a current of 10a + A was passed through it, and was calculated using the following formula.
tog(v+a/v+) log(v+++/v+
)次に、過電圧の鋭いパルス即ちサージ電圧が印加され
た時にバリスタ4の各特性がどの様に変化するかを模擬
的に調べる為に、第3図に示す様に2kVの直流定電圧
電源8に並列に電圧計9を接続し、電源8に5Ωの抵抗
10と単極双投スイッチIIの接点11aとを介して2
.5μFのコンデンサ12を接続し、かつスイッチ11
の接点11bにバリスタ4を接続し、5秒間隔でコンデ
ンサ12の充電エネルギーをバリスタ4に印加すること
を5回繰り返し、その後のバリスタ電圧v4及び非直線
係数α7を第2図の回路で測定し、次式でバリスタ電圧
の変化率ΔVIF(%)及びαの変化率ΔαP(%)を
求めた。tog(v+a/v+) log(v+++/v+
Next, in order to simulate how the characteristics of the varistor 4 change when a sharp pulse of overvoltage, i.e., a surge voltage, is applied, a voltmeter 9 is connected in parallel to a 2kV DC constant voltage power supply 8 as shown in Figure 3, and a 5Ω resistor 10 and the contact 11a of a single-pole double-throw switch II are connected to the power supply 8.
Connect the 5μF capacitor 12 and switch 11
A varistor 4 was connected to contact 11b, and the charging energy of the capacitor 12 was applied to the varistor 4 at 5-second intervals. This process was repeated 5 times, and the varistor voltage v4 and the nonlinearity coefficient α7 were measured using the circuit shown in Figure 2. The rate of change of the varistor voltage ΔVIF (%) and the rate of change of α ΔαP (%) were then calculated using the following formulas.
VIP Vl
ΔVIF−X100 (%)
α
また、各試料の静電容IC(nF)は1 kllz、
IVol tr+wsで測定した。VIP Vl ΔVIF-X100 (%) α Also, the electrostatic capacitance IC (nF) of each sample is 1 kl tz.
Measurements were taken using IVol tr+ws.
第1表において試料丸1. 9. 10. 18.19
及び27は、αが5.0未満か、ΔVIFが一5%を超
えるか、またはΔα、が一5%を超えるため本発明の範
囲外のものである。Table 1 shows the sample numbers 1, 9, 10, 18, and 19.
And 27 are outside the scope of the present invention because α is less than 5.0, ΔVIF is greater than -5%, or Δα is greater than -5%.
すなわち 第1表において、(SrTi0.100 M
置部に対し’) Nbzosの含有量が0.005 f
fli部未満であるか、または0.5重量部を超えると
αが5.0未満となり、ΔVIFが一5%を超え、Δα
、も−5,0%を超える。また、SiO2の含有量が0
.005重量部未満であるとΔVIF及びΔα2が−5
,0%を超え、5.0重量部を超えるとαが5.0未満
となり、ΔV□及びΔα、が−5,0%を超える。さら
に、K、0等の含有量が0.005重量部未満であるか
、または2.5重量部を超えるとΔVIF及びΔαPが
−5,0%を超える。That is, in Table 1, (SrTi 0.100 M
The Nbzos content relative to the base is 0.005 f
If the amount is less than fli parts or more than 0.5 parts by weight, then α will be less than 5.0, ΔVIF will be more than -5%, and Δα
, also exceeds -5.0%. Also, the SiO2 content is 0
If the amount is less than 0.005 parts by weight, then ΔVIF and Δα2 are -5
If the content exceeds 0% and exceeds 5.0 parts by weight, α becomes less than 5.0%, and ΔV□ and Δα exceed -5.0%. Furthermore, if the content of K, 0, etc. is less than 0.005 parts by weight or exceeds 2.5 parts by weight, ΔVIF and ΔαP exceed -5.0%.
したがって第1表に示される如く、第1成分(SrTi
Os) 100重量部と半導体化に寄与する第2成分
0.005〜5.0重量部と第3成分(SiO□)0.
005〜5.0重量部と第4成分0.005〜2.5重
量部とから成る磁器組成物でバリスタを形成すれば、サ
ージ印加によるバリスタ電圧の変化率ΔVIFの絶対値
が5%以下となり、サージ電圧印加による非直線係数α
の変化率Δα、の絶対値も5%以下になる。また、非直
線係数αは5以上となる。Therefore, as shown in Table 1, the first component (SrTi
Os) 100 parts by weight, a second component contributing to semiconductor formation 0.005 to 5.0 parts by weight, and a third component (SiO□) 0.
If a varistor is formed using a porcelain composition consisting of 0.05 to 5.0 parts by weight of a fourth component and 0.005 to 2.5 parts by weight of a fourth component, the absolute value of the rate of change ΔVIF of the varistor voltage due to surge application will be 5% or less, and the nonlinear coefficient α due to surge voltage application will be reduced.
The absolute value of the rate of change Δα is also 5% or less. Furthermore, the nonlinear coefficient α is 5 or greater.
(実施例2) 第2成分をNbzOs以外のもの、すなわち−〇、。(Example 2) The second component is something other than NbzOs, i.e., -O.
La意Os+ Cent、 NdzOs+ Pr1O+
+、 YzOs、 EutOs、SmzOsの内の少な
くとも1種の金属酸化物に代えても上記同様の良好な結
果が得られることを確かめるために、原料として5rC
Oz、 Ti1t、 WOi+ La2O2,Cent
。LaOs+ Cent, NdzOs+ Pr1O+
To confirm that the same good results as above can be obtained by substituting at least one metal oxide from +, YzOs, EutOs, and SmzOs, 5rC was used as the raw material.
Oz, Ti1t, WOi+ La2O2, Cent
.
NdtOs+ Pr1Ot+、 YtOz、 Eu
103. S+wtOs とStagと、LizC(h
、にzcOs、 C5gCO3,pb、co、を第2表
の組成になる様にそれぞれ換算秤量配合し、実施例1と
同じ方法でバリスタを作り、同一方法で特性を測定した
。その結果を第2表(電気的特性の項)に示す。NdtOs+ Pr1Ot+, YtOz, Eu
103. S + wtOs, Stag, and LizC(h
zcOs, C5gCO3,pb, and co were each weighed and blended to achieve the composition shown in Table 2, and a varistor was prepared using the same method as in Example 1, and its characteristics were measured using the same method. The results are shown in Table 2 (Electrical Characteristics section).
第2表から、第2成分をNb!O5以外の一0sla1
02゜Ce0tlNdtOx+ Pr60++、 Yg
Os、 EuzO3+ 5IlxOtの少な(とも1種
の金属酸化物に代えても、ΔVIFの絶対値が5%以下
となること、Δα2の絶対価が5%以下になること、ま
た非直線係数αが5.0以上になることがわかる。さら
に、第4成分をに茸0以外のLi、O,Rb1O,Cs
、Oの少なくとも1種の金属酸化物に代えても、その添
加量が前記限定範囲内であれば上記同様の良好な結果が
得られることが確認できた。From Table 2, the second component is Nb₂O₅ - 0sla₁
02゜Ce0tlNdtOx+ Pr60++, Yg
It can be seen that even if Os, EuzO3 + 5IlxOt are replaced with a small amount of one type of metal oxide, the absolute value of ΔVIF will be 5% or less, the absolute value of Δα2 will be 5% or less, and the nonlinearity coefficient α will be 5.0 or more. Furthermore, the fourth component is Li, O, Rb1O, Cs other than O.
It was confirmed that even if at least one metal oxide of O is substituted, the same good results as described above can be obtained as long as the amount added is within the aforementioned limiting range.
次に、第2番目の発明に係る実施例(3及び4)を示す
。Next, embodiments (3 and 4) relating to the second invention are shown.
(実施例3)
原料として5rCOs、 Ti0z、Nb1OsJOs
+YzOz、PrJ+ 1+1、azOs、 Stow
、 K!cOx、 Li2CO3,C5tO,CoO+
MnO+Aj!go!+ NiO+ FezO3+
Bit’s、 5l)zos+ Cr2O2(Co。(Example 3) Raw materials: 5rCOs, Ti0z, Nb1OsJOs
+YzOz, PrJ+ 1+1, azOs, Stow
, K! cOx, Li2CO3, C5tO, CoO+
MnO+Aj! Go! + NiO+ FezO3+
Bit's, 5l) zos+ Cr2O2(Co.
以下のものは第5成分)を第3表の組成になる様にそれ
ぞれ換算秤量配合し、実施例1と同じ方法でバリスタを
作り、同一方法で特性を測定した。The following components (the fifth component) were each weighed and blended to achieve the composition shown in Table 3. A varistor was prepared using the same method as in Example 1, and its characteristics were measured using the same method.
その結果を第3表に示す。The results are shown in Table 3.
試料Na 48 (CoOは0.01重量部未満)では
第5成分を添加した効果が認められず、試料11h55
(CoOは5.0重世部を超える)ではαが5.0未満
、Δv14.Δα、の絶対値がともに5.0%を超える
ため、本発明の範囲外である。In sample Na 48 (CoO less than 0.01 parts by weight), no effect was observed from adding the fifth component, and in sample 11h55
In cases where CoO exceeds 5.0, α is less than 5.0, and the absolute values of Δv14 and Δα both exceed 5.0%, thus falling outside the scope of the present invention.
したがって第3表に示される如く、第5成分を前記限定
範囲内の添加量で加えればΔVIFの絶対値が5%以下
、Δα、の絶対値が5%以下になる。Therefore, as shown in Table 3, if the fifth component is added in an amount within the aforementioned limited range, the absolute value of ΔVIF will be 5% or less, and the absolute value of Δα will be 5% or less.
またαは10.0より大で、第1番目の発明よりも優れ
たαを有する磁器組成物が得られることがわかる。Furthermore, it can be seen that a porcelain composition with α greater than 10.0 can be obtained, which is superior to that of the first invention.
(実施例4)
第4成分の添加を出発原料に対して行わず焼成後に行っ
ても差支えないことを確めるため5rCOs。(Example 4) To confirm that the fourth component can be added after calcination rather than to the starting material, 5rCOs was added.
Ti0z、 NbzOs、 5i02. Cooを第4
表の組成になる様に換算秤量配合し、実施例1と同じ方
法で磁器組成物を製作した。Ti0z, NbzOs, 5i02. Coo is the 4th
The porcelain compositions were prepared by converting and weighing the materials to match the composition shown in the table, using the same method as in Example 1.
次に実施例1における空気中の熱処理の工程の代りに上
記磁器円板の一方の主面に第4表に示す第4成分のペー
ストを塗布し、大気中で1000〜1300℃で3時間
の熱処理を施して第4成分を磁器円板中に熱拡散させた
後、実施例1と同じ方法でバリスタを作り、同一方法で
特性を測定した。その結果を第4表に示す。Next, instead of the heat treatment step in air in Example 1, a paste of the fourth component shown in Table 4 was applied to one main surface of the porcelain disc, and the fourth component was thermally diffused into the porcelain disc by heat treatment at 1000 to 1300°C in air for 3 hours. Then, a varistor was made in the same manner as in Example 1, and its characteristics were measured in the same manner. The results are shown in Table 4.
(以下、余白)
この結果から、第4成分を磁器組成物に熱拡散しても、
ΔVIFの絶対値が5%以下となること、Δα、の絶対
値も5%以下になること、またαが10.0より大とな
ることがわかる。(The rest is blank space) From these results, even if the fourth component is thermally diffused into the porcelain composition,
It can be seen that the absolute value of ΔVIF is 5% or less, the absolute value of Δα is also 5% or less, and α is greater than 10.0.
以上述べたように本発明の組成物は、バリスタとして使
用することが可能な非直線係数ぼを有すると共に、大き
な静電容量を有し、さらにはサージの印加による特性の
変化率が小さく、広範囲にわたって所望のバリスタ電圧
を有するものが得られ、安価で製造ができるうえ、バリ
スタ素子用として極めて優れた磁器組成物となりうるち
のである。
As described above, the composition of the present invention has a nonlinear coefficient that makes it usable as a varistor, has a large capacitance, and furthermore, the rate of change in characteristics due to the application of surges is small, and a desired varistor voltage can be obtained over a wide range, and it can be manufactured at low cost, making it an extremely excellent porcelain composition for varistor elements.
第1図は、本発明の実施例に係わるバリスタを概略的に
示す断面図である。
第2図は■1.α、ΔVIF+ Δα、を測定する装
置の回路図である。
第3図はサージ印加装置の回路図である。
1・・・磁器、2.3・・・銀電極、4・・・バリスタ
、5・・・直流定電流源、6・・・電流計、7・・・電
圧計、8・・・直流定電圧電源、9・・・電圧計、10
・・・抵抗、11・・・単極双投スイッチ、lla、I
lb・・・接点、12・・・コンデンサ。
Figure 1 is a schematic cross-sectional view showing a varistor according to an embodiment of the present invention. Figure 2 is a circuit diagram of a device for measuring α, ΔVIF + Δα. Figure 3 is a circuit diagram of a surge application device. 1...Porcelain, 2.3...Silver electrode, 4...Varistor, 5...DC constant current source, 6...Ammeter, 7...Voltmeter, 8...DC constant voltage power supply, 9...Voltmeter, 10
...Resistor, 11...Single-pole double-throw switch, lla, I
lb...contact, 12...capacitor.
Claims (2)
_5,WO_3,La_2O_3CeO_2,Nd_2
O_3,Pr_6O_1_1,Y_2O_3,Eu_2
O_3及びSm,O_3からなる群から選択された少な
くとも1種の金属酸化物0.005〜5.0重量部と、
SiO_20.005〜5.0重量部と、Li_2O,
K_2O,Cs_2O及びRb_2Oからなる群から選
択された少なくとも1種の金属酸化物0.005〜2.
5重量部とを含んでいることを特徴とする電圧非直線性
抵抗体磁器組成物。(1) Nb₂O to 3100 parts by weight of SrTiO
_5, WO_3, La_2O_3CeO_2, Nd_2
O_3, Pr_6O_1_1, Y_2O_3, Eu_2
0.005 to 5.0 parts by weight of at least one metal oxide selected from the group consisting of O_3 and Sm,O_3,
SiO₂ 0.005 to 5.0 parts by weight, and Li₂O,
0.005 to 2.005 of at least one metal oxide selected from the group consisting of K₂O, Cs₂O, and Rb₂O.
A voltage nonlinear resistive porcelain composition characterized by containing 5 parts by weight of [the specified substance].
_5,WO_3,La_2O_3,CeO_3,Nd_
2O_3,Pr_6O_1_1,Y_2O_3,Eu_
2O_3及びSm_2O_3からなる群から選択された
少なくとも1種の金属酸化物0.005〜5.0重量部
と、SiO_20.005〜5.0重量部と、Li_2
O,K_2O,Cs_2O及びRb_2Oからなる群か
ら選択された少なくとも1種の金属酸化物0.005〜
2.5重量部と、CoO,Cr_2O_3,NiO,F
e_2O_3Sb_2O_3,Bi_2O_3,MnO
及びAl_2O_3からなる群から選択された少なくと
も1種の金属酸化物を0.01〜5.0重量部とを含ん
でいることを特徴とする電圧非直線性抵抗体磁器組成物
。(2) Nb₂O
_5, WO_3, La_2O_3, CeO_3, Nd_
2O_3, Pr_6O_1_1, Y_2O_3, Eu_
0.005 to 5.0 parts by weight of at least one metal oxide selected from the group consisting of 2O3 and Sm2O3, 0.005 to 5.0 parts by weight of SiO2, and Li2
0.005 to 0.005 of at least one metal oxide selected from the group consisting of O, K₂O, Cs₂O and Rb₂O
2.5 parts by weight, CoO, Cr₂O₃, NiO, F
e_2O_3Sb_2O_3, Bi_2O_3, MnO
A voltage nonlinear resistive ceramic composition characterized by containing 0.01 to 5.0 parts by weight of at least one metal oxide selected from the group consisting of Al₂O₃ and Al₂O₃.