JPS6445828A - Production of nylon 6 highly extensible processed yarn - Google Patents
Production of nylon 6 highly extensible processed yarnInfo
- Publication number
- JPS6445828A JPS6445828A JP20257387A JP20257387A JPS6445828A JP S6445828 A JPS6445828 A JP S6445828A JP 20257387 A JP20257387 A JP 20257387A JP 20257387 A JP20257387 A JP 20257387A JP S6445828 A JPS6445828 A JP S6445828A
- Authority
- JP
- Japan
- Prior art keywords
- yarn
- false
- heater
- nylon
- highly
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【発明の詳細な説明】
(産業上の利用分野)
本発明は、ナイロン6高伸縮性加工糸の製造方法に係り
、さらに詳しくは、ナイロン6高配向未延伸糸から2ヒ
ータ仮撚法によって、低収縮で高伸縮性の高伸縮性加工
糸を製造する方法に関するものである。[Detailed Description of the Invention] (Industrial Field of Application) The present invention relates to a method for producing highly elastic processed nylon 6 yarn, and more specifically, to a method for producing a highly elastic processed yarn with low shrinkage and high elasticity from highly oriented undrawn nylon 6 yarn by a two-heater false twist method.
(従来の技術)
従来、靴下や水着用等の用途に用いられる高伸縮性加工
糸の製法としては、イタツー法や仮撚法がある。(Conventional Technology) Conventionally, methods for producing highly elastic processed yarn used for applications such as socks and swimwear include the Itatsu method and the false twist method.
イタツー法は、熱可塑性合成繊維のマルチフィラメント
糸を用いて1強撚−熱固定−オーバー解□撚する方法で
あるため、高伸縮性力i工糸を製造するのに三工程を必
要とし、このため生産性が悪くて生産コストが高いとい
う′欠点がある。The Itatsu method uses a multifilament yarn of thermoplastic synthetic fibers and involves a process of strong twisting, heat fixing, and over-untwisting. Therefore, it requires three steps to produce a highly elastic yarn, resulting in poor productivity and high production costs.
また、仮撚法として、熱可塑性合成繊維のマルチフィラ
メント糸に仮撚加工を施した後、仮撚方向とは逆方向に
仮撚数の1/4〜1/2の範囲で追撚する方法が知られ
ているが、この方法も二工程を必要とするため、イタツ
ー法よりは生産性がよいものの2依然として生産コスト
が高いという欠点がある。Furthermore, a false twisting method is known in which a multifilament yarn of thermoplastic synthetic fiber is false-twisted, and then further twisted in the opposite direction to the false twist by a range of 1/4 to 1/2 of the false twist number. However, this method also requires two steps, and although it is more productive than the Itatsu method, it still has the disadvantage of high production costs.
また、仮撚法の別法として、高速紡糸した熱可塑性合成
繊維のマルチフィラメント糸を用いて。Alternatively, as a false twist method, multifilament yarn of thermoplastic synthetic fibers spun at high speed is used.
仮撚加工する際の仮撚数を通常より多くして2重撚仮撚
を施し、−工程で高伸縮性加工糸を製造する方法も特公
昭57−17093号公報等で知られているが、この方
法で得られる高伸縮加工糸は、イタソー法で得られるも
のに比較して伸縮弾性率が低く9回復性が劣るという欠
点があり、また熱収縮率が高いので布帛の寸法安定性が
悪いという欠点もある。A method for producing highly elastic processed yarn in a single step, which involves increasing the number of false twists during the false twisting process to create a double false twist, is known from Japanese Patent Publication No. 57-17093, etc. However, the highly elastic processed yarn obtained by this method has the disadvantage of having a lower elastic modulus and inferior recovery properties compared to that obtained by the Itaso method, and also has the disadvantage of poor dimensional stability of the fabric due to its high thermal shrinkage rate.
さらに、特公昭49−8827号公報には、仮撚加工糸
を中空ヒータを用いて60%以上の弛緩状態で熱処理す
る伸縮糸の製造法が記載されているが、同公報の実施例
2にみられるごと<、75%程度の弛緩状態で熱処理を
施すため、そのままでは潜在捲縮の発現が不十分で伸縮
性が低く、引き続いて温熱処理を要するという欠点があ
る。Furthermore, Japanese Patent Publication No. 49-8827 describes a method for producing elastic yarn by heat-treating false-twisted yarn in a relaxed state of 60% or more using a hollow heater. However, as seen in Example 2 of the said publication, the heat treatment is performed in a relaxed state of about 75%, which has the drawback of resulting in insufficient latent crimp development and low elasticity, requiring subsequent heat treatment.
(発明が解決しようとする問題点)
本発明は、上記の欠点を解消し、イタソー法で得られる
高伸縮加工糸並の伸縮性と回復性を有し。(Problems the invention aims to solve) The present invention overcomes the above drawbacks and has elasticity and recovery properties comparable to highly elastic processed yarn obtained by the Itaso method.
かつ低収縮性で寸法安定性のよい布帛を得ることのでき
るナイロン6高伸縮性加工糸を2ヒータ仮撚法を利用し
て一工程で製造する方法を提供することを技術的な課題
とするものである。The technical objective is to provide a method for manufacturing a highly elastic nylon 6 processed yarn, which can produce a fabric with low shrinkage and good dimensional stability, in a single process using a two-heater false twist method.
(問題点を解決するための手段)
本発明者らは、上記課題を達成するために鋭意検討した
結果、特定の糸条を用いて仮撚加工した後、従来にない
高オーバーフィード率の弛緩状態下に再熱処理を施せば
よいことを知見して本発明に到達した。(Means for solving the problems) As a result of diligent research to achieve the above objectives, the inventors of the present invention discovered that after false twisting using a specific yarn, a reheat treatment should be performed under a relaxed state with an unprecedentedly high overfeed rate, and thus arrived at the present invention.
すなわち2本発明は、複屈折率が36 X 10− ”
〜42xio−’のナイロン6高配向未延伸糸を、撚角
度が49〜56″となる仮撚数、下記(I)式を満足す
る仮撚ヒータ温度旧(’C)で仮撚加工した後、該糸条
を引き続きオーバーフィード率100%以上の弛緩状態
下に、下記(n)式を満足する温度1’c)で再熱処理
することを特徴とするナイロン6高伸縮性加工糸の製造
方法を要旨とするものである。In other words, the present invention has a birefringence of 36 x 10 -
The gist of this invention is a method for producing highly elastic processed nylon 6 yarn, characterized by false-twisting a nylon 6 highly oriented undrawn yarn of ~42xio-' with a false-twist number that results in a twist angle of 49 to 56″, using a false-twist heater temperature ('C) that satisfies the following formula (I), and then reheating the yarn in a relaxed state with an overfeed rate of 100% or more at a temperature (1'c) that satisfies the following formula (n).
195≧H1≧170 −・・−(I)+1
.≧H2≧V’N + too 、−、−−(
IF )ただし、Dは仮撚加工後の糸条の繊度(デニー
ル)である。195≧H1≧170 −・・−(I)+1
.. ≧H2≧V'N + too, −, −−(
IF) However, D is the fineness (denier) of the yarn after false twisting.
以下1本発明の詳細な説明する。The present invention will be described in detail below.
まず1本発明における仮撚工程への供給系としては、複
屈折率が36X10−3〜42X10−’のナイロン6
高配向未延伸糸を用いることが必要である。First, as the supply system for the false twisting process in this invention, nylon 6 with a birefringence of 36X10⁻³ to 42X10⁻' is used.
It is necessary to use highly oriented undrawn yarn.
すなわち、複屈折率が36X10−3未満の糸条を用い
ると、経時安定性に欠け1品質の安定した仮撚加工糸を
得ることができず2−・方、複屈折率が42×101を
超える糸条の場合には、捲縮の固定性が悪くて伸縮性が
低下するので好ましくない。In other words, if yarn with a birefringence of less than 36 x 10⁻³ is used, it lacks stability over time, and it is not possible to obtain a stable false-twist yarn of good quality. On the other hand, if yarn with a birefringence of more than 42 x 10¹ is used, the crimping is not fixed well and the elasticity decreases, which is undesirable.
上記した複屈折率が36X10−”〜42X10−’の
ナイロン6高配向未延伸糸は、紡糸速度4.00軸/l
l1in以上の高速紡糸法によって得ることができる。The above-mentioned nylon 6 highly oriented undrawn yarn with a birefringence of 36 x 10⁻'' to 42 x 10⁻'' is used at a spinning speed of 4.00 axial/l.
It can be obtained by a high-speed spinning method of 1 in or more.
紡糸速度が4.000m/min未満では、得られるナ
イロン6高配向未延伸系が膨潤して捲取パッケージの捲
姿が不良になりやすく、このため仮撚加工時に解舒張力
が変動して糸切れを誘発しやすくなって、安定した操業
性を確保することができず、また得られる仮撚加工糸に
染斑等が発生しやすくなる。したがって、複屈折率が3
6X10−3〜42X10−’のナイロン6高配向未延
伸糸を得るために゛は、 4.000m/min以上、
好ましくは4,100〜5,00011/mtnの紡糸
速度を採用すればよい。If the spinning speed is less than 4,000 m/min, the resulting highly oriented undrawn nylon 6 tends to swell, resulting in poor winding of the winding package. This causes fluctuations in unwinding tension during false twisting, easily inducing yarn breakage and making it difficult to ensure stable operation. Furthermore, uneven dyeing is likely to occur in the resulting false twisted yarn. Therefore, a birefringence of 3
To obtain a highly oriented undrawn nylon 6 yarn of type 6X10-3 to 42X10-', a density of 4,000 m/min or more is required.
Preferably, a spinning speed of 4,100 to 5,000¹¹/mtn should be adopted.
本発明では、上記のナイロン6高配向未延伸糸を仮撚捲
縮加工するが、仮撚条件としては仮撚数及び仮撚ヒータ
温度が極めて重要である。In this invention, the above-mentioned nylon 6 highly oriented undrawn yarn is subjected to false twist crimping, and the false twist conditions, specifically the number of false twists and the false twist heater temperature, are extremely important.
まず、仮撚数T (T/M)としては、糸条の強力を低
下させることな(良好な捲縮性を付与するために、下記
式で算出した撚角度θが49〜56°となる範囲で行う
必要がある。First, the false twist count T (T/M) must be set within a range where the twist angle θ calculated using the following formula is 49 to 56°, in order to avoid reducing the strength of the yarn and to impart good crimpability.
撚角度が56°を超える仮撚数では、得られる加工糸の
強力が低下し、織編物用として要求される強力を満たし
得なくなり、さらに仮撚加工中に毛羽及び糸切れが発生
し、安定した操業性を確保することができない。一方、
撚角度が49°未満では捲縮性が低下し1本発明の目的
とする高伸縮性の加工糸は得られない。At false twist angles exceeding 56°, the strength of the resulting processed yarn decreases, failing to meet the strength requirements for woven and knitted fabrics. Furthermore, fuzzing and yarn breakage occur during the false twisting process, making it impossible to ensure stable operation. On the other hand,
If the twist angle is less than 49°, the crimpability decreases, and the highly elastic processed yarn that is the objective of this invention cannot be obtained.
次に、仮撚ヒータ温度H,は前記式(1)を満足する必
要があり、この範囲の仮撚ヒータ温度litを採用する
ことにより、仮撚加熱域で付与される撚が十分熱固定さ
れ、糸条に良好な捲縮を付与することができる。Next, the false twist heater temperature H must satisfy the above formula (1), and by adopting a false twist heater temperature lit within this range, the twist applied in the false twist heating region is sufficiently heat-fixed, and good crimp can be imparted to the yarn.
一方、仮撚ヒータ温度IIが170℃未満になると。On the other hand, when the false twist heater temperature II falls below 170°C...
撚の熱固定が不十分で捲縮堅牢度が悪く、高伸縮性の加
工糸は得られない。また、仮撚ヒータ温度H,が195
℃を超えると、仮撚時に毛羽が発生しやすく、そのため
加工糸の強力低下が著しくなり、しかもくびれ等が発生
するので好ましくない。The heat setting of the twist is insufficient, resulting in poor crimp fastness, and a highly elastic processed yarn cannot be obtained. Also, the false twist heater temperature H is 195
When the temperature exceeds ℃, fluffing is likely to occur during false twisting, which significantly reduces the strength of the processed yarn and can also cause constriction, so it is undesirable.
また、仮撚加工時の糸条供給率は、加工速度や銘柄等に
よって異なるが、延伸倍率が1.2〜1.3程度となる
糸条供給率が好ましい。Furthermore, while the yarn supply rate during false twisting varies depending on the processing speed and brand, a yarn supply rate that results in a draw ratio of approximately 1.2 to 1.3 is preferable.
本発明では、上記の仮撚加工で得られた捲縮糸を引き続
き弛緩状態で再熱処理して捲縮の固定を行い、高伸縮性
で回復性もよく、かつ低収縮性で寸法安定性のよい布帛
を得ることのできるポリアミド系高伸縮性加工糸とする
。In this invention, the crimped yarn obtained by the above false twisting process is subsequently reheat-treated in a relaxed state to fix the crimp, thereby obtaining a polyamide-based highly elastic processed yarn that has high elasticity, good recovery properties, low shrinkage, and good dimensional stability.
この熱処理は捲縮糸の熱収縮と捲縮の固定が十分行なえ
るように100%以上のオーバーフィード率で行う必要
があるが1通常の仮撚機のヒータでは、かかる高オーバ
ーフィード率での再熱処理は実質上不可能である。This heat treatment needs to be performed with an overfeed rate of 100% or more to ensure sufficient thermal shrinkage and crimping of the crimped yarn, but it is practically impossible to perform such a high overfeed rate of reheating with the heater of a typical false twisting machine.
すなわち1通常の2ヒ一タ仮撚機の加熱方式としては、
ヒータの加熱板に走行糸条が接触する方式(接触式)と
接触しない方式(非接触式)とがあるが1本発明のよう
に100%以上のオーバーフィード率で弛緩熱処理を施
す場合、接触式ヒータでは走行糸条の弛みが、また非接
触式ヒータでは走行糸条の糸振れや弛みが発生し、何れ
のヒータの場合も糸切れや染色斑を誘発する。In other words, the heating method for a typical two-heater false twisting machine is as follows:
There are two types of heaters: one in which the running yarn comes into contact with the heating plate (contact type) and one in which it does not come into contact (non-contact type). However, when performing relaxation heat treatment with an overfeed rate of 100% or more, as in the present invention, a contact type heater causes the running yarn to slacken, and a non-contact heater causes the running yarn to vibrate or slacken. In either case, this can induce yarn breakage or uneven dyeing.
しかるに9本発明のように2点接触ヒータで再熱処理す
れば、走行糸条と加熱板との抵抗が少なく、このため糸
振れや糸の弛みの発生が少なくなり、走行状態が安定す
るので、100%以上のオーバーフィード率で弛緩熱処
理を施しても、接触式や非接触式ヒータ使用時に見られ
るような糸切れや染色斑の発生がなく、良好な高伸縮糸
が得られる。However, if reheat treatment is performed with a two-point contact heater as in the present invention, the resistance between the running yarn and the heating plate is reduced, which reduces yarn vibration and slack, and stabilizes the running state. Therefore, even if relaxation heat treatment is performed with an overfeed rate of 100% or more, yarn breakage and uneven dyeing, which are seen when using contact-type or non-contact-type heaters, do not occur, and a good high-elasticity yarn can be obtained.
し7
本発明でいう点接触ヒータとは9例えば第2図△
で示したように、糸条12が加熱板13に直接接触する
ことなく少々の曲率をもって走行するように0字型ガイ
ド11を加熱板13に沿って10〜15cm間隔で設置
したものがあり、またU字型ガイドの材質としては、金
属製でかつ表面研磨の良いものが好ましい。7. In the present invention, a point contact heater is, for example, as shown in Figure 2△, one in which a U-shaped guide 11 is installed along the heating plate 13 at intervals of 10 to 15 cm so that the thread 12 does not directly contact the heating plate 13 but travels with a slight curvature. Furthermore, the material of the U-shaped guide is preferably metal with a good surface polish.
点接触ヒータ内での糸条走行方向としては、上から下、
下から上のいずれでもよいが、加工の安定性を計るには
、上から下方向に走行させる方が好ましい。The direction of thread movement within the point-contact heater is from top to bottom.
It can be done from bottom to top, but to ensure processing stability, it is preferable to run it from top to bottom.
仮撚後の糸条を弛緩状態で再熱処理するのは。Why re-heat-treat false-twisted yarn in a relaxed state?
仮撚加工糸の潜在捲縮を十分に発現させて熱固定するこ
とにより、糸1条に高捲縮性を付与して伸縮性と伸縮弾
性率を向上させるとともに、低収縮性にするためであり
、そのためには再熱処理域における糸条のオーバーフィ
ード率は100%以上8好ましくは150%以上にする
必要がある。The purpose of this process is to fully develop the latent crimp of the false-twisted yarn and then heat-set it to impart high crimpability to each strand of yarn, thereby improving its elasticity and elastic modulus, while also reducing shrinkage. To achieve this, the yarn overfeed rate in the reheat treatment area must be 100% or more, preferably 150% or more.
一方、オーバーフィード率を100%未満にすると、糸
条は潜在捲縮の発現が不十分な状態で再熱処理されるこ
とになるため捲縮性が低く、このため伸縮性とボリュー
ム感に欠けるものとなる。On the other hand, if the overfeed rate is less than 100%, the yarn will be reheat-treated before the latent crimp has fully developed, resulting in low crimpability and a lack of elasticity and volume.
上記再熱処理時の点接触ヒータ温度は、前記(n)式を
満足する温度1’c)に設定し、捲縮の固定と熱収縮を
施す必要がある。The point contact heater temperature during the above reheat treatment should be set to a temperature 1'c) that satisfies equation (n) above, and the crimp should be fixed and thermally shrunk.
この温度が仮撚ヒータ温度H,より高くなると。When this temperature becomes higher than the false twist heater temperature H,
合成繊維の特性である熱可塑性により糸条の潜在捲縮性
が小さくなり、糸条の伸縮性が低下するので好ましくな
く、一方(V′5′″+100) ℃より低い温度では
糸条の熱収縮と捲縮の固定が十分節されないうちに熱処
理が終わるため、捲縮堅牢度が悪く不適当である。Due to the thermoplastic properties of synthetic fibers, the latent crimpability of the yarn decreases, reducing its elasticity, which is undesirable. On the other hand, at temperatures lower than (V'5' + 100) °C, the heat treatment is completed before sufficient thermal shrinkage and crimp fixation of the yarn occurs, resulting in poor crimp fastness and making it unsuitable.
(作用)
上述したように1本発明では、複屈折率が36×10−
3〜42X10−’のナイロン6高配向未延伸糸を。(Effect) As described above, in this invention, the birefringence is 36 × 10⁻⁶.
3-42X10-' highly oriented undrawn nylon 6 yarn.
撚り角度が49〜56°となる仮撚数、前記(1)式を
満足する仮撚ヒータ温度+1.(”C)で仮撚加工した
後。The number of false twists that results in a twist angle of 49 to 56°, and the false twist heater temperature that satisfies equation (1) above + 1. After false twisting at ("C).
該糸条を引き続きオーバーフィード率100%以上の弛
緩状態下に、前記(n)式を満足する温度11□(”C
)で再熱処理することにより、糸条の潜在1を縮性が損
なわれることなく良好な捲縮として発現し、このため加
工糸は高伸縮性、かつ伸縮弾性率が高くて回復性がよく
、さらに低収縮性で布帛の寸法安定性がよいナイロン6
高伸縮性性加工糸を2ヒータ仮撚法という簡単な工程で
効率的に製造することができる。The yarn is then subjected to a relaxed state with an overfeed rate of 100% or more, at a temperature 11□("C" that satisfies equation (n) above.
By reheating the yarn, the latent properties of the yarn are expressed as good crimp without compromising its shrinkability. As a result, the processed yarn has high elasticity, a high modulus of elasticity and good recovery, and low shrinkage, resulting in good dimensional stability of the fabric.
Highly elastic processed yarn can be efficiently manufactured using a simple process called the two-heater false twist method.
次に9本発明の一実施態様を第1図により説明する。Next, an embodiment of the present invention will be described with reference to Figure 1.
パッケージ2から供給されたナイロン6高配向未延伸糸
糸1はガイド3を経て供給ローラ4に至り、供給ローラ
4と第1デリベリローラ7との間で延伸されると同時に
仮撚付与装置6で施撚され。The nylon 6 highly oriented undrawn yarn 1 supplied from package 2 passes through guide 3 to supply roller 4, where it is stretched between supply roller 4 and first delivery roller 7 and simultaneously twisted by false twisting device 6.
前記(I)式を満足する温度の仮撚ヒータ5で加熱され
て捲縮を付与される。The material is heated by a false twist heater 5 at a temperature that satisfies equation (I) above to impart crimp.
この捲縮糸は、引き続き第1デリベリローラ7と第2デ
リベリローラ9との間でオーバーフィード率100%以
上で一定の弛緩を与えられながら、前記(n)式を満足
する温度の点接触ヒータ8で十分な熱収縮と捲縮の固定
が施され、捲取装置10によりチーズ状パッケージに捲
取られ2本発明のナイ1コンロ高伸縮性加工糸が得られ
る。This crimped yarn is then subjected to sufficient thermal shrinkage and crimping fixation by a point contact heater 8 at a temperature satisfying equation (n) while being given a constant slack with an overfeed rate of 100% or more between the first delivery roller 7 and the second delivery roller 9, and is wound into a cheese-shaped package by the winding device 10 to obtain the 100% highly elastic processed yarn of the present invention.
なお9本発明でいうオーバーフィード率は1次式で定義
されるものである。Note that the overfeed rate referred to in this invention is defined by a linear equation.
ただし、A:供給側ローラの表面速度(m/m1n)B
:引取り側ローラの表面速度(m/ll1in)また、
加工糸の伸縮伸長率と伸縮弾性率の測定は、 JIS−
L1090(B法)に基づいて行った。However, A: Surface speed of the supply roller (m/m¹n) B
: Surface speed of the take-back roller (m/ll 1in) Also,
The measurement of the stretch elongation rate and elastic modulus of processed yarn is according to JIS-
The procedure was performed according to L1090 (Method B).
(実施例) 以下2本発明を実施例によりさらに具体的に説明する。(Examples) The present invention will be further described in detail below with reference to two examples.
実施例1
第1表に示した紡糸速度で得られた。第1表に示した複
屈折率を有するナイロン6高配向未延伸糸56d/12
fを供給系として、三菱重工■製LS−6型改造仮撚機
を用いて第1図に示す工程により仮撚捲縮加工を行い、
チーズ状パッケージに捲取った。Example 1 Obtained at the spinning speed shown in Table 1. Highly oriented undrawn nylon 6 yarn 56d/12 having the birefringence shown in Table 1.
Using f as the supply system, a modified LS-6 false twisting machine manufactured by Mitsubishi Heavy Industries is used to perform false twisting and crimping in the process shown in Figure 1.
It was rolled up in a cheese-like package.
仮撚加工条件と、得られた加工糸の物性値を第1表に示
す。Table 1 shows the conditions for false twisting and the physical properties of the resulting processed yarn.
第1表 比較のために、上記実施例1の加工条件のうち。Table 1 For comparison, among the processing conditions of Example 1 above:
複屈折率、仮撚数1点接触ヒータ温度または再熱処理時
のオーバーフィード率の何れかを変える他は同一の条件
で加工した加工糸の物性値を併せて第1表に示す。The physical properties of processed yarns processed under identical conditions, except for changes in the birefringence, false twist count, single-point contact heater temperature, or overfeed rate during reheat treatment, are shown in Table 1.
第1表から明らかなように5本発明の実施例1で得られ
た加工糸は、高伸縮性でその回復性もよく、また低収縮
性であった。As is clear from Table 1, the processed yarn obtained in Example 1 of the present invention had high elasticity, good recovery properties, and low shrinkage.
得られた加工糸を用いて、ダブルシャーシー編機(福原
精機製JIL−7型)でインターロック組織にて編立し
1通常の精錬、染色仕上加工を行って得られたシャーシ
ーは、経、緯ともに今までにない程の伸縮性を有する生
地であった。Using the processed yarn obtained, the resulting chassis was knitted in an interlock structure on a double chassis knitting machine (Fukuhara Seiki JIL-7 model), and after normal scouring and dyeing finish processing, the resulting fabric had unprecedented elasticity in both the warp and weft.
一方、仮撚数が少ない比較例1.再熱処理時のオーバー
フィード率が100%未満の比較例21点接触ヒータ温
度の高い比較例3及び供給系の複屈折率が低い比較例4
で得られた加工糸は、いずれも伸縮性が本発明で得られ
た加工糸より低いものであった。On the other hand, Comparative Example 1 had a low false twist count. Comparative Example 2 had an overfeed rate of less than 100% during reheat treatment. Comparative Example 3 had a high point contact heater temperature and Comparative Example 4 had a low birefringence of the supply system.
The processed yarns obtained all had lower elasticity than the processed yarn obtained in the present invention.
(発明の効果)
本発明は、上述した構成を有するので2本発明によれば
、良好な捲縮堅牢度を有し、高伸縮性で。(Effects of the Invention) As the present invention has the above-described configuration, it has good crimp fastness and high elasticity.
かつその回復性がよく、さらに低収縮性で寸法安定性の
よい布帛とすることのできるナイロン6高伸縮性加工糸
を、2ヒータ仮撚法を利用して、低コストで容易に製造
することができる。Furthermore, a highly elastic nylon 6 processed yarn, which has good recovery properties, low shrinkage, and good dimensional stability, can be easily manufactured at low cost using a two-heater false twist method.
第1図は本発明の一実施態様を示す概略工程図であり、
第2図は点接触ヒータの一実施態様を示す縦断面図であ
る。
1:ナイロン6高配向未延伸糸
5:仮撚ヒータ
6:仮撚付与装置
8:点接触ヒータ
特許出願人 ユニチカ株式会社
γ 1 図
γ2図
Figure 1 is a schematic process diagram showing one embodiment of the present invention.
Figure 2 is a longitudinal cross-sectional view showing one embodiment of a point-contact heater. 1: Nylon 6 highly oriented undrawn yarn 5: False twist heater 6: False twist imparting device 8: Point-contact heater Patent applicant: Unitika Ltd. γ 1 γ 2
Claims (2)
^3のナイロン6高配向未延伸糸を、撚角度が49〜5
6°となる仮撚数、下記( I )式を満足する仮撚ヒー
タ温度H_1(℃)で仮撚加工した後、該糸条を引き続
きオーバーフィード率100%以上の弛緩状態下に、下
記(II)式を満足する温度H_2(℃)で再熱処理する
ことを特徴とするナイロン6高伸縮性加工糸の製造方法
。 195≧H_1≧170………( I ) H_1≧H_2≧√D+100………(II)ただし、D
は仮撚加工後の糸条の繊度(デニール)である。(1) Birefringence is 36 × 10⁻³ to 42 × 10⁻³
A 3-degree nylon 6 highly oriented undrawn yarn, with a twist angle of 49-5
A method for producing highly elastic processed nylon 6 yarn, characterized by performing false twisting at a false twist heater temperature H_1 (°C) that satisfies the false twist number of 6° and equation (I) below, and then reheating the yarn in a relaxed state with an overfeed rate of 100% or more at a temperature H_2 (°C) that satisfies equation (II) below. 195 ≥ H_1 ≥ 170 ……… (I) H_1 ≥ H_2 ≥ √D + 100 ……… (II) where D
This is the fineness (denier) of the yarn after false twisting.
とする特許請求の範囲第1項記載のナイロン6高伸縮性
加工糸の製造方法。(2) A method for producing nylon 6 highly elastic processed yarn according to claim 1, characterized in that the reheat treatment is performed with a point contact heater.