JPS6468480A - Surface treatment of product combined with aluminum molding and iron molding - Google Patents

Surface treatment of product combined with aluminum molding and iron molding

Info

Publication number
JPS6468480A
JPS6468480A JP22703987A JP22703987A JPS6468480A JP S6468480 A JPS6468480 A JP S6468480A JP 22703987 A JP22703987 A JP 22703987A JP 22703987 A JP22703987 A JP 22703987A JP S6468480 A JPS6468480 A JP S6468480A
Authority
JP
Japan
Prior art keywords
zinc phosphate
molded body
aluminum
iron
sheets
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP22703987A
Other languages
Japanese (ja)
Inventor
羽田野 渡
章 山下
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nissan Shatai Co Ltd
Original Assignee
Nissan Shatai Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nissan Shatai Co Ltd filed Critical Nissan Shatai Co Ltd
Priority to JP22703987A priority Critical patent/JPS6468480A/en
Publication of JPS6468480A publication Critical patent/JPS6468480A/en
Pending legal-status Critical Current

Abstract

PURPOSE:To improve the rust inhibitive effect, etc., of coated films by subjecting the moldings of Al sheets to a chemical conversion treatment to form zinc phosphate films thereon and combining the moldings with steel sheet moldings and further, forming the zinc phosphate films on the surface of the assembly, then painting the assembly at the time of producing the combined members of the steel sheets and Al sheets of automobile bodies, etc. CONSTITUTION:An engine hood 11 and fender panel 12 of the automobile body 10 are formed by pressing 2 of the Al sheets A and the zinc phosphate films are formed on the surface in a 1st chemical conversion treatment stage 3. On the other hand, the steel sheets S are pressed 1 to form a body 13 and hood hinges 14. These Al sheet parts 11, 12 and the steel sheet parts 13, 14 are combined and coupled in an assembling stage 4 and thereafter, the zinc phosphate films are formed thereon in the 2nd chemical conversion treatment stage 5. The Al sheet parts are previously subjected to not the chromate treatment but the zinc phosphate pretreatment and, therefore, the degradation in the capacity of the treating liquid by elution of Cr acid is obviated and the deterioration in the adhesiveness of the coated films in the subsequent painting stage 6 is obviated.

Description

【発明の詳細な説明】 産業上の利用分野 本発明は、アルミ材からなる成形体と鉄材からなる成形
体とを組合わせて構成された製品の表面処理方法に関す
る。
[Detailed Description of the Invention] Industrial Application Field The present invention relates to a surface treatment method for a product composed of a molded body made of aluminum and a molded body made of iron.

従来の技術 従来、例えば自動車の車体には、アルミ材と鉄材とを各
々所定形状の成形体に加工し、これらアルミ成形体と鉄
成形体とを組合わ仕てなるものがあり、かかる車体の表
面処理方法としては第6図に示したものが提案されてい
る(特開昭61−96074号公報参照)。すなわち、
この方法においては、鉄材である鋼板を第1プレス工程
Uで所定形の鉄成形体にプレス加工する一方、アルミ板
を第2プレス加工Vで所定形状の成形体にプレス加工し
、このアルミ成形体をクロメート処理工程Wでクローム
酸を含む処理液にて表面処理する。
Conventional Technology Conventionally, for example, the body of an automobile is made by processing aluminum and iron materials into molded bodies of predetermined shapes, and then combining these aluminum and iron molded bodies. As a surface treatment method for such a body, the method shown in Figure 6 has been proposed (see Japanese Patent Publication No. 61-96074). That is,
In this method, a steel sheet is press-formed into a predetermined shape in a first pressing step U, while an aluminum sheet is press-formed into a predetermined shape in a second pressing step V, and this aluminum molded body is surface-treated with a treatment solution containing chromic acid in a chromate treatment step W.

しかる後に前記鉄成形体とクロメート処理されたアルミ
成形体とを組付工程Xで組合わ仕て製品としての車体を
完成させ、さらに化成処理工程Yで車体の鉄成形体にリ
ン酸亜鉛被膜を形成する。さらに塗装工程Zにて、クロ
メート処理されたアルミ成形体と、リン酸亜鉛被膜が形
成された鉄成形体とからなる車体の塗装を行うものであ
る。
Subsequently, the iron molded body and the chromate-treated aluminum molded body are assembled in assembly process X to complete the vehicle body as a product, and then a zinc phosphate coating is formed on the iron molded body of the vehicle body in chemical conversion process Y. Furthermore, in painting process Z, the vehicle body consisting of the chromate-treated aluminum molded body and the iron molded body with the zinc phosphate coating is painted.

発明が解決しようとする問題点 しかしながらこのような従来の方法においては、クロメ
ート処理工程Wで表面処理されたアルミ成形体は、組付
工程Xにて鉄成形体と組合わされた後、化成処理工程Y
にて鉄成形体とともに化成処理される。このため前記ク
ロメート処理工程でアルミ成形体の表面に被膜を形成し
ていたクローム酸は、化成処理工程Yで浸漬される、リ
ン酸亜鉛溶液中に一部が溶出してしまう恐れがある。
Problems that the invention aims to solve However, in such conventional methods, the aluminum molded body, which has been surface-treated in the chromate treatment step W, is combined with the iron molded body in the assembly step X, and then undergoes a chemical conversion treatment step Y
The aluminum molded body is subjected to chemical treatment together with the iron molded body. Therefore, there is a risk that some of the chromic acid that formed a film on the surface of the aluminum molded body in the chromate treatment step may dissolve into the zinc phosphate solution into which it is immersed in the chemical treatment step Y.

このためアルミ成形体は、クロメート処理工程Wでクロ
ーム酸被膜が形成されたのにもかかわらず、化成処理工
程Xにおいて前記被膜の一部が溶出することにより塗装
工程Zにおける塗膜密着性が悪化し、一方化成処理工程
で使用されるリン酸亜鉛溶液にあっては、前述したクロ
ーム酸の溶出によって不純物(スラッジ)が増加し、早
期に被膜形成効果が低下してしまう。又特に車体のよう
に各成形体が大型であって、作業スペースの都合上、ア
ルミ成形体と鉄成形体とが異なる箇所で成形される場合
には、クロメート処理されたアルミ成形体を組付工程X
に搬送する過程で、雨や作業者の汗等によってアルミ成
形体表面のクローム酸が部分的に溶出する。このため塗
装工程Zでアルミ成形体に塗装を行った際、塗膜の均一
性が害され、防錆効果及び塗膜密着性が部分的に低下す
るおそれもあった。
Therefore, although a chromic acid film is formed on the aluminum molded body in the chromate treatment process W, a portion of the film is dissolved in the chemical conversion treatment process X, resulting in poor paint adhesion in the painting process Z. On the other hand, in the zinc phosphate solution used in the chemical conversion treatment process, the aforementioned dissolution of chromic acid increases impurities (sludge), causing the film formation effect to deteriorate prematurely. Furthermore, especially when each molded body is large, such as a car body, and the aluminum molded body and the iron molded body are molded in different locations due to space constraints, the chromate-treated aluminum molded body is assembled in the assembly process X
During the transportation process, chromic acid on the surface of the aluminum molded body may partially dissolve due to rain, sweat from workers, etc. Therefore, when the aluminum molded body is painted in painting process Z, the uniformity of the paint film may be compromised, potentially leading to a partial decrease in rust prevention effect and paint adhesion.

本発明はこのような従来の問題点に鑑みてなされたもの
であり、アルミ成形体の表面被膜の溶出を防止すること
によって前記問題点を解決したアルミ成形体と鉄成形体
組合わせ製品の表面処理方法を提供するものである。
This invention has been made in view of the above-mentioned conventional problems, and provides a surface treatment method for a combined aluminum and iron molded product that solves the aforementioned problems by preventing the dissolution of the surface coating of the aluminum molded body.

問題点を解決するための手段 前記問題点を解決するために本発明にあっては、アルミ
材を例えばプレスによって車体のエンジンフートやフェ
ンダパネル等の成形体に加工し、この加工されたアルミ
成形体をその表面にリン酸被膜と形成する化成処理液に
て化成処理する一方、鉄材を同様にプレスによって、前
記エンジンフードやフェンダパネルが組付けられるボデ
ィ本体等の成形体に加工し、該加工された鉄成形体と前
記電着塗装されたアルミ成形体とを組合わせ、該組合わ
された製品を鉄成形体にリン酸亜鉛被膜を形成する化成
処理液にて処理した後、塗装を施すように構成されてい
る。
Means for solving the problems In order to solve the aforementioned problems, the present invention is configured such that aluminum material is processed into a molded body such as an engine hood or fender panel for a vehicle body by pressing, and this processed aluminum molded body is chemically treated with a chemical conversion treatment liquid that forms a phosphate coating on its surface, while iron material is similarly processed into a molded body such as a body to which the engine hood or fender panel is assembled by pressing, the processed iron molded body and the electrodeposited aluminum molded body are combined, the combined product is treated with a chemical conversion treatment liquid that forms a zinc phosphate coating on the iron molded body, and then painted.

作用 前記構成において、アルミ成形体は単体で化成処理され
、その表面にリン酸亜鉛からなる被膜が形成される。前
記リン酸亜鉛は、親水性がないことから、アルミ成形体
に形成された被膜は、雨や作業者の汗による溶出なく良
好な被膜状態を維持する。そしてリン酸亜鉛被膜が形成
されたアルミ成形体は、鉄成形体と組合わされて再度鉄
成形体とともにリン酸亜鉛溶液中に浸漬される。このと
きアルミ成形体に形成されているリン酸亜鉛被膜は、リ
ン酸亜鉛溶液中で成長はするものの溶出はないことから
、前記被膜はリン酸亜鉛溶液中においても良好な状態に
維持される。したがってアルミ成形体が鉄成形体の化成
処理を行う化成処理液中に溶出してしまうことらなく、
該化成処理液内へのアルミイオン等不純物混入は防止さ
れ、化成処理液の鉄成形体に対する被膜形成効果は一定
に維持される。
In the above configuration, the aluminum molded body is chemically treated individually, and a coating made of zinc phosphate is formed on its surface. Since zinc phosphate is not hydrophilic, the coating formed on the aluminum molded body maintains a good coating state without leaching due to rain or the sweat of workers. The aluminum molded body with the zinc phosphate coating is then combined with an iron molded body and immersed again in a zinc phosphate solution together with the iron molded body. At this time, the zinc phosphate coating formed on the aluminum molded body grows in the zinc phosphate solution but does not leach out, so the coating is maintained in a good state even in the zinc phosphate solution. Therefore, the aluminum molded body does not leach into the chemical treatment solution used to chemically treat the iron molded body.
The contamination of the chemical treatment solution with impurities such as aluminum ions is prevented, and the film-forming effect of the chemical treatment solution on the iron molded body is maintained at a constant level.

実施例 以下本発明の実施例について図面に従って説明する。本
実施例は第5図に示したように自動車の車体IOにおい
て、エンジンフード11とフェンダパネル12とをアル
ミ材で成形するとともに、この両部材以外のボディ本体
13及び該ボディ本体13に前記エンジンフード11を
枢支するフードヒンジ14.14を鉄材である鋼板で成
形した場合を示すものである。すなわち第1図に示した
ように鉄材である鋼板Sはプレス工程1にて所定形状の
鉄成形体たるボディ本体10に成形される。
Examples Hereinafter, embodiments of the present invention will be described with reference to the drawings. As shown in Figure 5, this embodiment shows a case in which the engine hood 11 and fender panel 12 of an automobile body IO are formed from aluminum, and the body main body 13 other than these two members and the hood hinges 14.14 that pivotally support the engine hood 11 to the body main body 13 are formed from steel plates, which are made of iron. That is, as shown in Figure 1, the steel plate S, which is made of iron, is formed into a body main body 10, which is an iron molded body of a predetermined shape, in a pressing process 1.

一方アルミ板Aは別のプレス工程2にて、アルミ成形体
たるエンジンフード11及びフェンダパネル12にプレ
ス加工された後、第1化成処理工程3に移送される。該
第1化成処理工程3においては、第2図に示したように
、アルカリ水溶液を用いた予備脱脂3a及び脱脂3bに
てプレス工程■でエンジンフード11及びフェンダパネ
ル12の表面に付着した油脂成分が除去され、第1水洗
3cが行われた後、表面調整3dにてデオキシジンによ
る中和がなされる。しかる後に、ノンフッソ系のリン酸
亜鉛溶液に浸漬されるリン酸亜鉛処理6eがなされ、こ
れによってエンジンフード11及びフェンダパネル12
の表面にはリン酸亜鉛被膜が形成される。そしてこのよ
うにリン酸亜鉛被膜が形成されたエンジンフード11及
びフェンダパネルI2は、第2水洗3f、第3水洗3g
、第4水洗6h純水洗61がなされた後、乾燥6jがな
される。次にエンジンフード11お及びフェンダパネル
12は、ボディ本体13が成形されている場所に設定さ
れた組付工程4に搬送される。このとき前記リン酸亜鉛
被膜は、親水性がないことから、ボディ本体13が成形
されている場所に搬送する過程で雨や作業者の汗等が付
着しても、リン酸亜鉛被膜が溶出するようなことはなく
、良好な被膜状態を維持し得る。
Meanwhile, aluminum plate A is pressed into aluminum molded bodies, the engine hood 11 and fender panel 12, in a separate pressing process 2, and then transferred to the first chemical treatment process 3. In the first chemical treatment process 3, as shown in Figure 2, oil and grease components adhering to the surface of the engine hood 11 and fender panel 12 in the pressing process are removed by preliminary degreasing 3a and degreasing 3b using an alkaline aqueous solution, followed by a first rinse 3c, and then neutralization with deoxyzine in surface adjustment 3d. After that, a zinc phosphate treatment 6e is performed, in which the engine hood 11 and fender panel 12 are immersed in a non-fluorine zinc phosphate solution.
A zinc phosphate coating is formed on the surface. The engine hood 11 and fender panel I2, which have this zinc phosphate coating formed on them, are then subjected to a second rinse 3f and a third rinse 3g.
After the fourth rinse 6h (pure water rinse 61) is performed, drying 6j is carried out. Next, the engine hood 11 and fender panel 12 are transported to the assembly process 4, which is set up in the location where the body 13 is being molded. At this time, since the zinc phosphate coating is not hydrophilic, even if rain or sweat from workers adheres to it during the transport process to the location where the body 13 is being molded, the zinc phosphate coating will not dissolve, and a good coating condition can be maintained.

前記組付工程4では第5図に示し大ようにエンジンフー
ド11は、予め電着塗装が施されているフードヒンジ1
4.14を介してボディ本体13に枢支されるとともに
、フェンダパネル12は直接ボディ本体13に装着され
て製品たる車体lOの組合わせ結合が完了し、しかる後
に第2化成処理工程5に移送される。該第2化成処理工
程5では、第2図に示した第1化成処理と工程として同
一であってフッソ系のリン酸亜鉛溶液を用いた処理がな
され、したがってエンジンフード11及びフェンダパネ
ル12は、ボディ本体13とともに、リン酸亜鉛処理3
eにて再度リン酸亜鉛溶液中に浸漬される。しかしエン
ジンフード11及びフェンダパネル12両部材が浸漬さ
れるリン酸亜鉛溶液は、前記両部材の被膜を成形する素
性と同質であるから、該被膜すなわちリン酸亜鉛被膜は
、リン酸亜鉛液中において成長はするものの溶出するこ
とはない。したがってエンジンフード11及びフェンダ
パネル12に形成されたリン酸亜鉛被膜は第2化成処理
工程5においても良好な状態に維持され、エンジンフー
ド11及びフェンダパネル12の、アルミ表面が露出す
ることはない。したがって第2化成感理工程5において
、リン酸亜鉛溶液中にアルミイオン等の不純物混入が生
ずることもなく、リン酸亜鉛溶液のボディ本体13に対
する被膜形成効果は一定維持され、ボディ本体13にも
良好なリン酸亜鉛被膜を形成することが可能となる。そ
してこのようにボディ本体13にリン酸亜鉛被膜が形成
されると、車体10は塗装工程6に移送され、該塗装工
程6において、第3図に示した電着6a、メラミンアル
キド樹脂系塗料が塗装される中塗6b、及び上塗6cが
行われることにより、車体IOの表面処理全般は完了す
る。
In the assembly process 4, as shown in Figure 5, the engine hood 11 is attached to the hood hinge 1 which has been pre-coated with electrodeposition paint.
4.14 The fender panel 12 is pivotally supported to the body 13, and is directly attached to the body 13, completing the assembly and bonding of the finished vehicle body 10, after which it is transferred to the second chemical treatment process 5. In the second chemical treatment process 5, the process is the same as the first chemical treatment shown in Figure 2, and a fluorine-based zinc phosphate solution is used for treatment. Therefore, the engine hood 11 and fender panel 12, together with the body 13, undergo zinc phosphate treatment 3.
In step e, the parts are immersed again in the zinc phosphate solution. However, since the zinc phosphate solution into which both the engine hood 11 and the fender panel 12 are immersed has the same properties as the solution that forms the coating on both parts, the coating, i.e., the zinc phosphate coating, grows in the zinc phosphate solution but does not dissolve. Therefore, the zinc phosphate coating formed on the engine hood 11 and the fender panel 12 is maintained in good condition even in the second chemical treatment step 5, and the aluminum surface of the engine hood 11 and the fender panel 12 is not exposed. Therefore, in the second chemical treatment step 5, no impurities such as aluminum ions are introduced into the zinc phosphate solution, the coating-forming effect of the zinc phosphate solution on the body 13 is maintained at a constant level, and a good zinc phosphate coating can be formed on the body 13 as well. Once the zinc phosphate coating is formed on the body 13 in this manner, the vehicle body 10 is transferred to the painting process 6, where the electrodeposition 6a shown in Figure 3, the intermediate coating 6b with melamine alkyd resin paint, and the topcoat 6c are applied, thereby completing the overall surface treatment of the vehicle body IO.

したがって有害なりローム酸化物を用いることなく車体
11の表面処理全般を行うことができ、クローム酸化物
に対する公害防止設備を不要にして設備コストの低減を
図ることができるものである。
Therefore, the entire surface treatment of the vehicle body 11 can be performed without using harmful chromium oxides, eliminating the need for pollution control equipment for chromium oxides and thus reducing equipment costs.

なお第5図に示したように前記実施例における第1化成
処理工程3に代えて、タンニング酸ジルコン(商品名:
CT3756  パルコート)を用いたノンクローム処
理工程7を設定し、前記タンニング酸ジルコンによりア
ルミ成形体であるエンジンフード11及びフェンダパネ
ル12の表面に被膜を形成するような構成であっても前
記実施例と同様の作用効果を得ることができる。
As shown in Figure 5, instead of the first chemical treatment step 3 in the above example, tanning acid zircon (product name:
Even if a non-chrome treatment step 7 using CT3756 Palcoat is set up, and a coating is formed on the surface of the aluminum molded body, the engine hood 11 and fender panel 12, using the zircon tanning acid, the same effects as in the above embodiment can be obtained.

発明の詳細 な説明したように本発明は、アルミ材を所定形状に加工
したアルミ成形体をその表面にリン酸亜鉛被膜を形成す
る化成処理液にて化成処理する一方、鉄材を所定形状に
加工し鉄成形体を前記アルミ成形体と組合わせ、該組合
わされた製品を化成処理した後塗装を施すようにしたこ
とから以下のような効果を得ることができる。
As described in detail in the invention, the present invention provides the following effects by chemically treating an aluminum molded body, which is processed from aluminum material into a predetermined shape, with a chemical treatment solution that forms a zinc phosphate coating on its surface, while processing iron material into a predetermined shape to form an iron molded body and combining it with the aluminum molded body, then chemically treating the combined product and applying paint.

(1)アルミ成形体に被膜を形成するリン酸亜鉛は、親
水性がないことがら化成処理した後アルミ成形体を鉄成
形体に組合わせるべく屋外に搬送した際の雨や、作業者
の汗によってリン酸亜鉛被膜が部分的に溶出してしまう
ようなことはなく、良好な被膜状態を維持し、前記溶出
に起因するアルミ成形体の外観品質及び防錆効果の低下
を解消することができる。
(1) Since zinc phosphate, which forms a coating on aluminum molded bodies, is not hydrophilic, the zinc phosphate coating will not be partially dissolved by rain or sweat from workers when the aluminum molded bodies are transported outdoors to be combined with iron molded bodies after chemical treatment, thus maintaining a good coating state and eliminating the deterioration of the appearance quality and rust prevention effect of the aluminum molded bodies caused by such dissolution.

(2)リン酸亜鉛被膜が形成されたアルミ成形体は、鉄
成形体と組合わされた後接鉄成形体とともに化成処理さ
れるが、該化成処理に用いられるリン酸亜鉛溶液中にお
いてリン酸亜鉛被膜は成長はするものの溶出することは
ない。したがって、鉄成形体を化成処理する際にもアル
ミ成形体に形成された被膜を良好な状態に維持すること
可能となる。
(2) When an aluminum molded body with a zinc phosphate coating is combined with an iron molded body and then subjected to chemical conversion treatment together with the iron molded body, the zinc phosphate coating grows in the zinc phosphate solution used in the chemical conversion treatment but does not dissolve. Therefore, it is possible to maintain the coating formed on the aluminum molded body in good condition even when the iron molded body is subjected to chemical conversion treatment.

(3)又このように鉄成形体を化成処理する際に、アル
ミ化成体のリン酸亜鉛被膜が溶出しない結果、アルミ成
形体の表面からアルミイオン等の不純物が溶出するよう
なこともない。よって鉄成形体の化成処理に用いられる
溶液の被膜形成効果は一定に維持され、鉄成形体の表面
に良好なリン酸亜鉛被膜を形成することが可能となると
ともに、前記溶液の管理コストを低減することができる
。
(3) Furthermore, when the iron molded body is chemically treated in this manner, the zinc phosphate coating of the aluminum chemically treated body does not dissolve, and as a result, no impurities such as aluminum ions dissolve from the surface of the aluminum molded body. Therefore, the film-forming effect of the solution used in the chemical treatment of the iron molded body is maintained at a constant level, making it possible to form a good zinc phosphate coating on the surface of the iron molded body, and reducing the management costs of the solution.

(4)有害なりローム酸化物を用いることなく、アルミ
成形体と鉄成形体とを共にリン酸亜鉛を用いて被膜形成
するようにしたことから、クローム酸化物に対する公害
防止設備を不要にして、設備コストの低減を図ることを
可能にするとともに、作業者の安全性向上をも図ること
が可能となる。
(4) By forming a coating on both the aluminum molded body and the iron molded body using zinc phosphate without using harmful chromium oxides, it becomes possible to eliminate the need for pollution control equipment for chromium oxides, thereby reducing equipment costs and improving worker safety.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図は本発明の一実施例を示す工程図、第2図は同実
施例の化成処理工程を示す詳細工程図、第3図は同実施
例の塗装工程を示す詳細工程図、第4図は、本発明の応
用例を示す工程図、第5図は本発明の実施例に用いられ
た車体の要部斜視図、第6図は従来方法の工程図である
。 1.2・・・プレス工程、3・・・第1化成処理工程、
4・・・組付工程、5・・・第2化成処理工程、6・・
・塗装工程、IO・・・車体(製品)、11・・・エン
ジンフード(アルミ成形体)、12・・・フェンダパネ
ル(アルミ成形体)、13・・・ボディ本体(鉄成形体
)。
Figure 1 is a process diagram showing one embodiment of the present invention, Figure 2 is a detailed process diagram showing the chemical treatment process of the same embodiment, Figure 3 is a detailed process diagram showing the painting process of the same embodiment, Figure 4 is a process diagram showing an application example of the present invention, Figure 5 is a perspective view of the main part of the vehicle body used in the embodiment of the present invention, and Figure 6 is a process diagram of the conventional method. 1.2... Pressing process, 3... First chemical treatment process,
4... Assembly process, 5... Second chemical treatment process, 6...
- Painting process, IO... Vehicle body (product), 11... Engine hood (aluminum molded part), 12... Fender panel (aluminum molded part), 13... Body (iron molded part).

Claims (1)

【特許請求の範囲】[Claims] (1)アルミ材を所定形状の成形体に加工し、該加工さ
れたアルミ成形体をその表面にリン酸亜鉛被膜を形成す
る化成処理液にて化成処理する一方、鉄材を所定形状の
成形体に加工し、該加工された鉄成形体と前記化成処理
されたアルミ成形体とを組合わせ、該組合わされた製品
を鉄成形体にリン酸亜鉛被膜を形成する化成処理液にて
化成処理した後、塗装を施すことを特徴とするアルミ成
形体と鉄成形体組合わせ製品の表面処理方法。
(1) A surface treatment method for a product combining an aluminum molded body and an iron molded body, characterized by processing an aluminum material into a molded body of a predetermined shape, chemically treating the processed aluminum molded body with a chemical treatment solution that forms a zinc phosphate coating on its surface, while processing an iron material into a molded body of a predetermined shape, combining the processed iron molded body with the chemically treated aluminum molded body, chemically treating the combined product with a chemical treatment solution that forms a zinc phosphate coating on the iron molded body, and then applying paint.
JP22703987A 1987-09-10 1987-09-10 Surface treatment of product combined with aluminum molding and iron molding Pending JPS6468480A (en)