JPS6470902A - Magnetic head - Google Patents

Magnetic head

Info

Publication number
JPS6470902A
JPS6470902A JP22660887A JP22660887A JPS6470902A JP S6470902 A JPS6470902 A JP S6470902A JP 22660887 A JP22660887 A JP 22660887A JP 22660887 A JP22660887 A JP 22660887A JP S6470902 A JPS6470902 A JP S6470902A
Authority
JP
Japan
Prior art keywords
magnetic
layer
oxide
glass
layers
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP22660887A
Other languages
Japanese (ja)
Inventor
三上 寛祐
稲子谷 修
猛志 鳥取
和成 中川
英夫 藤原
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Maxell Ltd
Original Assignee
Hitachi Maxell Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hitachi Maxell Ltd filed Critical Hitachi Maxell Ltd
Priority to JP22660887A priority Critical patent/JPS6470902A/en
Publication of JPS6470902A publication Critical patent/JPS6470902A/en
Pending legal-status Critical Current

Abstract

PURPOSE:To reduce a heating temperature at the time of joining and to prevent the magnetic characteristic deterioration of a magnetic substance by forming a nonmagnetic substrate with an oxide series ceramic material and using a glass soldering as a joining material. CONSTITUTION:First and second core half bodies 9 and 10 faces first and second magnetic layers 4a and 4b, are protruded to a front part (medium sliding surfaces 2a and 2b sides) and a rear part (opposite side through a recessed groove 5a for a winding window to medium sliding surfaces 2a and 2b) through a gap regulating material 11 such as, for example, SiO2 and joined by heating up to the vicinity of the melting temperature of glass soldering layers 22a, 22b and 22c. Namely, metallic magnetic layers 4a and 4b are joined in the same point as the usual soldering through a lead and a tin, which are the main component of glass soldering, and oxide series ceramic-made substrates 1a and 1b and metallic magnetic layers 4a and 4b are joined while the element having a large affinity with oxygen in the glass soldering such as Al, Ti, tin and lead is combined with the oxygen in a oxide series ceramic.

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明は、ギャップ規制材を介して2つのコア半体を接
合して成る磁気ヘッドであって、それら2つのコア半体
が、非磁性材料にて形成された基体と、この基体の磁気
ギャップ形成面側に被着された高透磁率かつ高飽和磁束
密度の磁性層とから成るものに関する。
[Detailed Description of the Invention] [Industrial Field of Application] The present invention relates to a magnetic head formed by joining two core halves via a gap restricting material, wherein the two core halves consist of a substrate made of a non-magnetic material and a magnetic layer with high permeability and high saturation magnetic flux density attached to the magnetic gap forming surface of the substrate.

〔従来の技術〕[Conventional technology]

磁気記録の高密度化に伴って、磁気記録媒体の保磁力が
高められ、この磁気記録媒体に記録可能な磁気ヘッドと
して、少なくとも磁気ギャップと対向する部分を高透磁
率及び高飽和磁束密度を有する磁性材料で構成した磁気
ヘッドの開発が進められている。
With the increasing density of magnetic recording, the coercivity of magnetic recording media is being enhanced, and development is underway to create magnetic heads capable of recording on these magnetic recording media. These heads are constructed using a magnetic material with high permeability and high saturation magnetic flux density, at least in the portion facing the magnetic gap.

一方、従来より、ヘッドコアの耐摩耗性の向上と摺動ノ
イズの低域化を図るために、媒体摺動面におけるコア基
体部を非磁性材料にて構成した磁気ヘッド(特開昭53
−116809号)や、単位インダクタンス当りのヘッ
ド出力を高めるために、巻線窓までは非磁性材料にて構
成し、バンクコアを高透磁率コアで構成した磁気ヘッド
(特開昭61−184705号)が提案されている。
On the other hand, conventionally, in order to improve the wear resistance of the head core and reduce sliding noise, a magnetic head (Japanese Patent Publication No. 53) has been constructed in which the core base portion on the media sliding surface is made of a non-magnetic material.
In order to increase the head output per unit inductance, a magnetic head has been proposed in which the winding window is made of a non-magnetic material and the bank core is made of a high-permeability core (Japanese Patent Publication No. 61-184705).

本願出願人は、先に、かかる利点を全て備えた磁気ヘッ
ドとして、第10図に示すものを提案した(特願昭61
−26393.5号)。
The applicant previously proposed the magnetic head shown in Figure 10, which possesses all of the above advantages (Japanese Patent Application No. 1986).
-26393.5).

この図に示すように、本願出願人が先に提案した磁気ヘ
ッドは、非磁性基体1a、lbの一側面に、媒体摺動面
2a)2bまで貫通するトラック幅規制溝3a、3bを
凹設し、このトラック幅規制1113a、3b内に磁性
層4a、4bが充填されている。そして、非磁性基体1
a、lbの前記トラック幅規制溝3a、3b影形成に凹
設された巻線窓用凹溝5a、5b内に露出した前記磁性
層4a、4bの表面、及び巻線窓用凹溝4a、4bと平
行に凹設された接合用′a6に、接合用ガラス層7a+
7b*7cが形成されている。さらに、非磁性基体1a
と接合用ガラス層7aの間、及び非磁性基体1aと接合
用ガラス層7cの間には、ガラス中の有害成分から磁性
層4a、4bを保護するための保護膜8が介設されてい
る。
As shown in this figure, the magnetic head previously proposed by the applicant has track width regulating grooves 3a and 3b recessed on one side surface of the non-magnetic substrate 1a and lb, penetrating to the media sliding surface 2a and 2b, and magnetic layers 4a and 4b are filled within these track width regulating grooves 1a and 3a and 3b.
The surfaces of the magnetic layers 4a and 4b exposed within the winding window grooves 5a and 5b recessed in the track width regulating grooves 3a and 3b of a and lb, and the bonding glass layer 7a+ in the bonding 'a6 recessed parallel to the winding window grooves 4a and 4b
7b*7c is formed. Furthermore, a non-magnetic substrate 1a
A protective film 8 is interposed between the bonding glass layer 7a and the non-magnetic substrate 1a and the bonding glass layer 7c to protect the magnetic layers 4a and 4b from harmful components in the glass.

前記トラック幅規制溝3a、3bの両側は、非磁性基体
1aと磁性層4aと接合材層7aと保護膜8とから成る
第1のコア半体9と、非磁性基体1bと磁性層4bと接
合材層7bとから成る第2のコア半体10との突き合せ
面となる面であって。
Both sides of the track width regulating grooves 3a and 3b are surfaces that abut against a first core half 9, which consists of a non-magnetic substrate 1a, a magnetic layer 4a, a bonding material layer 7a, and a protective film 8, and a second core half 10, which consists of a non-magnetic substrate 1b, a magnetic layer 4b, and a bonding material layer 7b.

相手コア半体と突き合わされたときに互いに平行になる
ように形成されている。
They are formed so that they are parallel to each other when they come into contact with the other core half.

前記磁気ヘッドの製造は、別体に形成された第1のコア
半体9と第2のコア半体lOとをギャップ規制材11を
介して突き合せ、この結合体を加熱して接合用ガラス層
7a、7bを溶融一体化すると共に、接合用ガラス層7
cを磁性層4bに接合することによって行われる。
The manufacturing of the magnetic head involves butting together a first core half 9 and a second core half 10, which are formed separately, via a gap restricting material 11, and heating this joint to melt and integrate the bonding glass layers 7a and 7b, and the bonding glass layer 7
This is done by joining c to the magnetic layer 4b.

この磁気ヘッドは、コア半体9.10の突き合せ面の一
部に接合用ガラス層7 a s 7 b y 7 cを
形成したので、山形に形成された突き合せ面の両側に接
合材を充填する従来の磁気ヘッドに比べてガラスの使用
量を大幅に減少することができる。
This magnetic head has bonding glass layers 7 a s 7 by y 7 c formed on a portion of the abutting surface of the core halves 9 and 10. Compared to conventional magnetic heads that fill both sides of the V-shaped abutting surface with bonding material, the amount of glass used can be significantly reduced.

よって、コア半体9,10を接合する際の熱応力が;減
少され、接合用ガラス層にクラックを生じたり、コア半
体9.lOが剥離するといった問題を防止することがで
きる。また、媒体摺動面2 a H2bにガラスが露出
しないので、磁気記録媒体によって接合用ガラス層が摩
耗されるということがな(、コア半体9,10の接合部
に段差を生じて磁気記録媒体が損傷するという問題を生
じることがない。
Therefore, the thermal stress when joining the core halves 9 and 10 is reduced, preventing problems such as cracks in the joining glass layer or delamination of the core halves 9 and 10. Furthermore, since the glass is not exposed on the media sliding surface 2a H2b, the joining glass layer is not worn down by the magnetic recording medium, and the problem of damage to the magnetic recording medium due to a step at the joint of the core halves 9 and 10 is not caused.

〔発明が解決しようとする問題点〕[Problems that the invention aims to solve]

ところで、前記磁性層4a、4bとしてはコバルト系の
非晶質合金が優れるが、この磁性材料は500°C〜5
50℃で結晶化し、飽和磁束密度などの磁気特性が劣化
する。一方、接合用ガラス層として用いられる低融点ガ
ラスは、市場に提供さ九でいるもののうち最も融点の低
いものを用いたとしても、2つのコア半体9,10を接
合するのに、その結合体を500℃近い温度に数分ない
し数10分保持しなくてはならない。このため、コア半
体9.10の接合工程にむいて、磁性層4a+4bが部
分的に結晶化し、磁気特性が劣化するという問題がある
。
Incidentally, a cobalt-based amorphous alloy is preferable for the magnetic layers 4a and 4b, but this magnetic material is suitable for temperatures between 500°C and 5°C.
Crystallization occurs at 50°C, degrading magnetic properties such as saturation magnetic flux density. On the other hand, even if the lowest melting point glass available on the market is used as the bonding glass layer, the bonded structure must be held at a temperature of nearly 500°C for several minutes to several tens of minutes to bond the two core halves 9 and 10. Therefore, during the bonding process of the core halves 9 and 10, the magnetic layer 4a + 4b partially crystallizes, leading to a degradation of its magnetic properties.

また、低融点ガラスの融点、ひいてはコア半体9.10
を接合するに必要な作業温度が高いために、非磁性基体
1a、lb、磁性層4a、4b。
Furthermore, the melting point of low-melting-point glass, and consequently the core half, 9.10
Because the working temperature required to bond them is high, the non-magnetic substrate 1a, lb and magnetic layers 4a, 4b are used.

接合用ガラス層?a、7b、7cの熱膨張率の差に起因
する熱応力が大きくなり、磁性層4a、4bに大きな熱
応力が残留する。このため、磁性層4a、4bの磁化容
易軸にゆがみを生じ、やはり磁気特性が劣化するという
問題がある。
Bonding glass layer? The difference in thermal expansion coefficients between a, 7b, and 7c causes significant thermal stress, resulting in large residual thermal stress in magnetic layers 4a and 4b. This causes distortion in the easy magnetization axis of magnetic layers 4a and 4b, leading to a deterioration of magnetic properties.

尚、この残留熱応力の影響による磁性層4a。Furthermore, this magnetic layer 4a is affected by residual thermal stress.

4bの磁気特性の劣化という問題は、磁性層4a。The problem of degradation of the magnetic properties of 4b is related to the magnetic layer 4a.

4bとして結晶質の磁性材料を用いた場合にも同様に発
生する。
The same phenomenon occurs when a crystalline magnetic material is used as 4b.

本発明は、前記した従来技術の問題点を解決するために
なされたものであって、コア半体を接合する際の熱の影
響による磁性層の特性劣化を防止し、記録、再生特性に
優れた磁気ヘッドを提供することを目的とするものであ
る。
The present invention was made to solve the problems of the prior art described above, and aims to prevent deterioration of the magnetic layer's properties due to the effects of heat when joining the core halves, thereby providing a magnetic head with excellent recording and playback characteristics.

【問題点を解決するための手段〕[Means for addressing the problem]

本発明は、叙上の目的を達成するため、非磁性基体の一
側面に高透磁率磁性材料から成る磁性層が設けられた2
つのコア半体を、ギャップ規制材及び接合材を介して接
合して成る磁気ヘッドにおいで、前記非磁性基体を酸化
物系セラミックス材料にて形成すると共に、前記接合材
としてガラスはんだを用いたことを特徴とするものであ
る。
To achieve the above objective, the present invention provides a magnetic layer made of a high-permeability magnetic material on one side surface of a non-magnetic substrate.
In a magnetic head formed by joining two core halves via a gap restricting material and a bonding material, the non-magnetic substrate is formed from an oxide-based ceramic material, and glass solder is used as the bonding material.

[作用〕 ガラスはんだは、100℃〜400℃で溶融する。従っ
て、磁性層を構成する磁性材料としてコバルト系の非晶
質合金を用いた場合にも、その結晶化温度よりも充分に
低温でコア半体を接合することができる。また、コア半
体を接合する際の作業温度が低いので、磁性層に大きな
熱応力が残留することがない、これらのことから、磁性
層の磁気特性の劣化を防止することができる。また、コ
ア基体を酸化物系セラミックス材料にて形成すると、ガ
ラスはんだとの接合性が良く、充分な接合力を得ること
ができる。
[Function] Glass solder melts at 100°C to 400°C. Therefore, even when a cobalt-based amorphous alloy is used as the magnetic material constituting the magnetic layer, the core halves can be joined at a temperature sufficiently lower than its crystallization temperature. Furthermore, because the working temperature when joining the core halves is low, large thermal stresses do not remain in the magnetic layer, thus preventing deterioration of the magnetic properties of the magnetic layer. In addition, if the core substrate is formed from an oxide-based ceramic material, it exhibits good bonding properties with glass solder, and sufficient bonding strength can be obtained.

〔実施例〕[Examples]

以下、本発明に係る磁気ヘッドの一実施例を第1図及び
第2図に基づいて説明する。
Hereinafter, an embodiment of the magnetic head according to the present invention will be described with reference to Figures 1 and 2.

第1図にむいて、21a、21bは酸化物系セラミック
ス基体* 22a、 22b、22cはガラスはんだ層
を示し、その他力1O図に示したと同様の部材や部分に
ついては、そ九と同様の符号をもって表示しである。
Referring to Figure 1, 21a and 21b represent oxide ceramic substrates, 22a, 22b, and 22c represent glass solder layers, and other components and parts similar to those shown in Figure 10 are indicated with the same reference numerals.

この図に示すように、本発明の磁気ヘッドも基本的な構
成については前記した従来例のものと全く同様であり、
基体21a、21bを酸化物系のセラミックス材料にて
形成すると共に、接合材としてガラスはんだを用いた点
において相違する。
As shown in this figure, the magnetic head of the present invention has the same basic configuration as the conventional example described above.
The difference lies in the fact that the substrates 21a and 21b are formed from oxide-based ceramic materials, and glass solder is used as the bonding material.

前記基体21a、21bを形成する酸化物系のセラミッ
クス材料としては、例えば非磁性フェライトや結晶化ガ
ラスなど、公知に属する任意の酸化物系セラミックスを
用いることができる。
As the oxide-based ceramic material forming the substrates 21a and 21b, any known oxide-based ceramic material can be used, such as nonmagnetic ferrite or crystallized glass.

ガラスはんだは、鉛と錫を主成分とし、これにアルミニ
ウム、亜鉛、チタン、アンチモン等の添加剤を最大で敬
重量%添加したものであって、金属同士、酸化物系セラ
ミックス材料、あるいは金属と酸化物系セタミックスと
を接合する接合材である。溶融温度は、それに含まれる
成分の組成を変えることによって調節され、100℃〜
400℃のものが市場に提供されている。
Glass solder is primarily composed of lead and tin, with additives such as aluminum, zinc, titanium, and antimony added in up to 100°C by weight. It is a bonding material used to join metals together, oxide-based ceramic materials, or metals with oxide-based Cetamix. The melting temperature is adjusted by changing the composition of the components it contains, ranging from 100°C to
Products heated to 400°C are being offered on the market.

また、第1の磁性層4a及び第2の磁性層4bは、高飽
和磁束密度で、かつ高透磁率の結晶質合金や非晶質合金
によって形成される。前記結晶質合金としては、鉄−ア
ルミニウム−ケイ素合金、鉄−ケイ素合金、ならびに鉄
−ニッケル合金などがある。また、非晶質合金としては
、鉄、ニッケル、コバルトのグループから選択された1
種以上の元素と、リン、炭素、ホウ素、ケイ素のグルー
プから選択された1種以上の元素とからなる合金、また
はこれらを主成分として、アルミニウム、ゲルマニウム
、ベリリウム、スズ、モリブデン、インジウム、タング
ステン、チタン、マンガン、クロム、ジルコニウム、ハ
フニウム、ニオブなどの元素を添加した合金、あるいは
コバルト、ジルコニウムを主成分として前記の各添加元
素を含んだ合金などがある。
Furthermore, the first magnetic layer 4a and the second magnetic layer 4b are formed from a crystalline alloy or amorphous alloy with high saturation magnetic flux density and high permeability. Examples of crystalline alloys include iron-aluminum-silicon alloy, iron-silicon alloy, and iron-nickel alloy. As for amorphous alloys, one selected from the group of iron, nickel, and cobalt is used.
Examples include alloys composed of 10 or more elements and one or more elements selected from the group of phosphorus, carbon, boron, and silicon; alloys in which these are the main components and elements such as aluminum, germanium, beryllium, tin, molybdenum, indium, tungsten, titanium, manganese, chromium, zirconium, hafnium, and niobium are added; and alloys in which cobalt and zirconium are the main components and each of the aforementioned additive elements is included.

前記保護膜8は、第2図に詳細に示すように。The protective film 8 is shown in detail in Figure 2.

前記磁性層4aを被覆する酸化物系セラミックス層8a
と、この酸化物系セラミックス層8aを被覆するクロム
層8bとから成る。クロム層8bは。
Oxide-based ceramic layer 8a covering the magnetic layer 4a
It consists of this oxide ceramic layer 8a and a chromium layer 8b that covers it. The chromium layer 8b is...

ガラスはんだ中の鉛元素が磁性層4a中に拡散するのを
防止するために設けられ、また、酸化物系セラミックス
層8aは、クロム層8bのクロム元素が磁性層4a中に
拡散するのを防止するために設けられる。この酸化物系
セラミックスP:j8aは、例えば5iOzやAlzO
aなどによって形成される。なお、酸化物系セラミック
ス層8aは最大2μmの厚さに形成すれば充分であり、
また、クロム層8bは最大1μmの厚さに形成すれば充
分である。
The lead element in the glass solder is provided to prevent diffusion into the magnetic layer 4a, and the oxide ceramic layer 8a is provided to prevent the chromium element in the chromium layer 8b from diffusing into the magnetic layer 4a. This oxide ceramic P:j8a is, for example, 5 0 oz or AlzO
It is formed by a, etc. Note that it is sufficient to form the oxide ceramic layer 8a to a maximum thickness of 2 μm.
Furthermore, it is sufficient to form the chromium layer 8b to a maximum thickness of 1 μm.

前記第1のコア半体9及び第2のコア半体10は、第1
の磁性層4a及び第2の磁性層4bを対向にし、そのフ
ロント部(媒体摺動面2a、2b側)及びリア部(巻線
窓用凹溝5aを介して媒体摺動面2a、2bと反対側)
に、例えば5iOzなどのギャップ規制材11を介して
突き合わされ、ガラスはんだ層22 a+ 22 bg
 22 Cの溶融温度近傍まで加熱することによって接
合される。即ち、金属製の磁性層4a、4bが、ガラス
はんだの主成分である鉛と錫を介して通常のはんだと同
様の要領で接合され、また、酸化物系セラミックス製の
基体1a、lb及び金属製の磁性層4a。
The first core half 9 and the second core half 10 are the first
The magnetic layer 4a and the second magnetic layer 4b are facing each other, and the front portion (the side facing the media sliding surfaces 2a and 2b) and the rear portion (the side opposite to the media sliding surfaces 2a and 2b via the winding window groove 5a)
They are then butted together via a gap-limiting material 11, such as 5 oz, and the glass solder layers 22 a + 22 b g
The materials are joined by heating to near the melting point of 22°C. That is, the metallic magnetic layers 4a and 4b are joined in the same manner as ordinary soldering via lead and tin, which are the main components of glass solder, and the oxide ceramic substrates 1a and lb and the metallic magnetic layer 4a.

4bが、アルミニウム、チタン、ti!!、亜鉛といっ
たガラスはんだ中の酸素との親和力の大きな元素が酸化
物系セラミックス中の酸素と結合することによって1妾
合される。
4b is formed when elements with a high affinity for oxygen in the glass solder, such as aluminum, titanium, ti, and zinc, combine with oxygen in the oxide ceramics.

このようにすると、第1の磁性層4a及び第2の磁性M
4bの中央部が、巻線窓用凹溝5aと第2のコア半体1
0によって形成される巻線窓23にて離隔されると共に
、フロント部及びリア部で近接し、フロント部ではギャ
ップ規制材11を介して磁気ギャップが構成され、これ
によって所望の磁路が形成される。
In this way, the first magnetic layer 4a and the second magnetic layer M
The central part of 4b is the winding window groove 5a and the second core half 1
The winding window 23 formed by the zeros is separated, and the front and rear sections are close together, with a magnetic gap being formed in the front section via the gap restricting material 11, thereby forming the desired magnetic path.

前記実施例の磁気ヘッドは、コア半体9.10の接合材
として融点がlOO℃〜400℃程度のガラスはんだを
用いたので、磁性層4a、4bを非晶質合金にて形成し
た場合にも、コア半体9゜IOを接合する際の熱によっ
て磁性層4a、4bが結晶化することがなく、磁気特性
が劣化することがない、また、100℃〜400℃程度
の低温でコア半体9,10を接合するようにしたので。
In the above embodiment, since glass solder with a melting point of about 100°C to 400°C was used as the joining material for the core halves 9 and 10, even when the magnetic layers 4a and 4b were formed from an amorphous alloy, the magnetic layers 4a and 4b did not crystallize due to the heat generated when joining the core halves 9 and 10, and the magnetic properties did not deteriorate. Furthermore, the core halves 9 and 10 were joined at a low temperature of about 100°C to 400°C.

磁性層4a、4bに大きな熱応力が残留することがなく
、この点からも磁性層4a14bの磁気特性の劣化を防
止することができる。
Since no significant thermal stress remains in the magnetic layers 4a and 4b, the deterioration of the magnetic properties of the magnetic layers 4a and 4b can be prevented.

さらに、2つのコア基体1a、lbに間に弾性に優れた
ガラスはんだ層22 a H22b H22Cを介設し
たので、熱応力がこのガラスはんだ層22as 22b
、22cにて吸収され、磁気ヘッドが経時変形すること
がない。
Furthermore, since a highly elastic glass solder layer 22a H22b H22C is interposed between the two core substrates 1a and lb, thermal stress is absorbed by this glass solder layer 22as 22b
The magnetic field is absorbed at 22c, preventing deformation of the magnetic head over time.

また、磁性層4aとガラスはんだ層22a、2222c
との間に保護膜8を形成したので、磁性層4aが接合材
によって侵されることがなく、耐久性に優れる。
Furthermore, the magnetic layer 4a and the glass solder layers 22a, 2222c
Since a protective film 8 is formed between the magnetic layer 4a and the bonding material, the magnetic layer 4a is not damaged by the bonding material, resulting in excellent durability.

また、トラック規制用溝3a、3bの底面を1字状に形
成したので、媒体摺動面における磁気ギャップに対向し
た磁性層4a、4bと基体La。
Furthermore, since the bottom surfaces of the track control grooves 3a and 3b are formed in a straight line shape, the magnetic layers 4a and 4b and the substrate La face the magnetic gap on the media sliding surface.

1bとの境界が磁気ギャップと非平行になり、この境界
での疑似ギャップの発生が防止できる。
The boundary with 1b becomes non-parallel to the magnetic gap, preventing the generation of a pseudo-gap at this boundary.

以下1本実施例に係る磁気ヘッドの製造方法について説
明する。
The method for manufacturing a magnetic head according to this embodiment will be described below.

初めに、第1のコア半体9の製造方法を、第3図乃至第
5図に基づいて説明する。
First, the manufacturing method of the first core half 9 will be explained based on Figures 3 to 5.

まず、第3図に示すように、第1の基体1aのもとにな
る酸化物系セラミックスブロック31に。
First, as shown in Figure 3, the oxide-based ceramic block 31 that forms the basis of the first substrate 1a is formed.

所望のトラック幅(10〜200μm)に相当する幅の
第1のトラック幅規制溝3aを複数個等間隔に加工する
。
Multiple first track width regulating grooves 3a, with a width corresponding to the desired track width (10 to 200 μm), are machined at equal intervals.

これと同時に、この第1トラック幅規制溝3aと直角の
方向に、巻線窓用凹溝5a及び接合用凹溝6を加工する
。これら巻線窓用凹溝58及び接合用凹溝6は、前記第
1のトラック幅規制溝3aよりも充分に深く形成される
。
Simultaneously, a winding window groove 5a and a joining groove 6 are machined perpendicular to the first track width regulating groove 3a. These winding window grooves 58 and joining grooves 6 are formed to be sufficiently deeper than the first track width regulating groove 3a.

さらに、第1のトラック幅規制溝3aと媒体摺動面2a
との間に、第1のトラック幅規制溝3aよりも深く、巻
線窓用凹溝5aよりも浅い段部32を形成する。この段
部32と媒体摺動面2aとの間に形成される面33は、
加工後ギャップデイプスを構成する部分であって、所望
のギャップデイブスに加工しろを加えた寸法に設定され
る。
Furthermore, the first track width regulating groove 3a and the media sliding surface 2a
Between them, a stepped portion 32 is formed that is deeper than the first track width regulating groove 3a and shallower than the winding window recess groove 5a. The surface 33 formed between this stepped portion 32 and the media sliding surface 2a is
This is the part that constitutes the gap depth after machining, and is set to a dimension that adds a machining allowance to the desired gap depth.

次いで、第4図に示すように、前記のように加工された
酸化物系セラミックスブロック31の加工面に、例えば
スパッタリングなどの薄膜形成手段によって、第1の磁
性層4aのもとになる磁性材料34と、保護118とな
る酸化物系セラミックス層8a及びクロム層8bと、ガ
ラスはんだ層22a922b* 22cのもとになるガ
ラスはんだ35とを順次積層する。
Next, as shown in Figure 4, on the processed surface of the oxide ceramic block 31 processed as described above, a magnetic material 34 which will form the first magnetic layer 4a, an oxide ceramic layer 8a and a chromium layer 8b which will form the protective layer 118, and glass solder 35 which will form the glass solder layer 22a922b*22c are sequentially laminated by a thin film forming means such as sputtering.

最後に、第4図に示すように、酸化物系セラミックスブ
ロック31を媒体摺動面2a側から見たとき、媒体摺動
面2aに酸化物系セラミックスブロック31が露出し、
また、第5図に示すように。
Finally, as shown in Figure 4, when the oxide ceramic block 31 is viewed from the media sliding surface 2a side, the oxide ceramic block 31 is exposed on the media sliding surface 2a.
Also, as shown in Figure 5.

酸化物系セラミックスブロック31を正面から見たとき
、ギャップ突き合せ面に磁性材料34が露出する位置(
A−A位置)まで研摩する。
When the oxide ceramic block 31 is viewed from the front, the position where the magnetic material 34 is exposed on the gap abutting surface (
Polish down to position A-A.

次に、第2のコア半体10の製造方法を、第6図及び第
7図に基づいて説明する。
Next, the manufacturing method for the second core half 10 will be explained based on Figures 6 and 7.

まず、第6図に示すように、第2の基体1bのもとにな
る酸化物系セラミックスブロック41に、前記第1の酸
化物系セラミックスブロック31に加工された第1のト
ラック幅規制溝3aと同様の第2のトラック幅規制溝3
bを複数個等間隔に加工する。
First, as shown in Figure 6, the oxide ceramic block 41 that forms the basis of the second substrate 1b is processed with a second track width regulating groove 3 similar to the first track width regulating groove 3a processed on the first oxide ceramic block 31.
Process multiple pieces of b at equal intervals.

こ九と同時に、この酸化物系セラミックスブロック41
のトラック幅規制溝3bの形成面に、前記巻線窓用凹溝
5aに対応する凹溝5bと、前記段部32に対応する段
部42とを加工する6次いで、前記のような加工がなさ
れた酸化物系セラミックスブロック41の加工面に、第
7図に示すように、第2の磁性層4bのもとになる磁性
材料43と、第2のガラスはんだ層22bのもとになる
接合材44とを積層する。
At the same time as this oxide-based ceramic block 41
On the surface where the track width regulating groove 3b is formed, a recessed groove 5b corresponding to the winding window recessed groove 5a and a stepped portion 42 corresponding to the stepped portion 32 are machined. Next, on the machined surface of the oxide ceramic block 41 that has been machined as described above, a magnetic material 43 that will become the second magnetic layer 4b and a bonding material 44 that will become the second glass solder layer 22b are laminated, as shown in Figure 7.

次いで、第7図に示すように、酸化物系セラミックスブ
ロック41を正面から見た場合、フロント側に酸化物系
セラミックスブロック41が露出し、リア側に磁性材料
43が露出する位置(B−B位置)まで研摩する。
Next, as shown in Figure 7, the oxide ceramic block 41 is polished to a position (B-B position) where, when viewed from the front, the oxide ceramic block 41 is exposed on the front side and the magnetic material 43 is exposed on the rear side.

次に、叙上のように所定の加工が施された第1の酸化物
系セラミックスブロック31及び第2の酸化物系セラミ
ックスブロック41から磁気ヘッドを作製する方法を、
第8図及び第9図に基づいて説明する。
Next, a method for manufacturing a magnetic head from the first oxide-based ceramic block 31 and the second oxide-based ceramic block 41, which have been subjected to the predetermined processing described above, is described below.
This will be explained with reference to Figures 8 and 9.

まず、第8図に示すように、前記第1の酸化物系セラミ
ックスブロック31及び第2の酸化物系セラミックスブ
ロック41のうち、少なくともいずれか一方の非磁性ブ
ロックの磁性層形成面に、ギャップ規制材11を所定の
厚さに形成する。
First, as shown in Figure 8, a gap restricting material 11 is formed to a predetermined thickness on the magnetic layer forming surface of at least one of the non-magnetic blocks, the first oxide-based ceramic block 31 and the second oxide-based ceramic block 41.

次いで、第9図に示すように、前記第1の酸化物系セラ
ミックスブロック31に形成さ九た第1のトラック規制
用溝3a及び第2の酸化物系セラミックスブロック41
に形成された第2のトラック規制用溝3bを対向にして
、これら2つの酸化物系セラミックス31.41を突き
合せる。
Next, as shown in Figure 9, the first track regulating groove 3a and the second oxide ceramic block 41 are formed in the first oxide ceramic block 31.
The two oxide ceramics 31 and 41 are butted together with their second track-regulating grooves 3b facing each other.

次いで、この酸化物系セラミックス31.41の結合体
をガラスはんだ層22a、22b、22Cの融点近傍ま
で加熱して一定時間保持し、これを一体化する。
Next, the bonded oxide ceramics 31 and 41 is heated to near the melting point of the glass solder layers 22a, 22b, and 22C and held for a certain period of time to integrate them.

前記結合体を常温まで冷却したのち、第9図に2点鎖線
にて示すように、トラック幅規制$ 3 a 。
After the composite body is cooled to room temperature, the track width restriction $3a is applied as shown by the dashed line in Figure 9.

3bの両側をスライス加工し、第1図に示した磁気ヘッ
ド本体を取り出す、最後に、巻線窓15に所定のコイル
を巻線して所望の磁気ヘッドを得る。
Both sides of 3b are sliced to remove the magnetic head body shown in Figure 1. Finally, a predetermined coil is wound in the winding window 15 to obtain the desired magnetic head.

なお、本発明の要旨は、基体1a、lbを酸化物系のセ
ラミックスで形成すると共に、接合材としてガラスはん
だを用いたことを特徴とするものであって、磁気ヘッド
を構成1する各部材の形状、構造等については、前記実
施例のものに限定されるものではない。
The gist of the present invention is that the substrates 1a and lb are formed from oxide-based ceramics, and glass solder is used as a bonding material. The shape, structure, etc., of each component constituting the magnetic head are not limited to those of the above embodiment.

例えば、耐食性に優れた磁性材料を用いることによって
、保護膜8を省略することもできる。
For example, by using a magnetic material with excellent corrosion resistance, the protective film 8 can be omitted.

また、前記実施例においては、第1の基体1aの媒体摺
動面側に段部32を形成した場合について説明したが、
この段部22は必ずしも必要ではなく、巻線窓用凹溝5
aを適宜設計することによって、これを省略することも
できる。
Furthermore, in the above embodiment, the case in which a stepped portion 32 is formed on the media sliding surface side of the first base 1a was described,
This stepped portion 22 is not necessarily required, and the recessed groove 5 for the winding window
This can also be omitted by designing 'a' appropriately.

〔発明の効果〕[Effects of the invention]

以上説明したように、本発明の磁気ヘッドは。As explained above, the magnetic head of the present invention is...

接合材としてガラスはんだを用いたので、コア半体を接
合する際の加熱温度を低下することができ。
Since glass solder was used as the joining material, the heating temperature when joining the core halves could be reduced.

磁性層の磁気特性の劣化が防止される。また、コア半体
を接合する際の加熱、冷却に起因する熱応力が柔軟性の
ガラスはんだに吸収され、磁気ヘッドの経時変形が防止
される。よって、記録、再生特性及び耐久性に優れた磁
気ヘッドを提供することができる。
The degradation of the magnetic properties of the magnetic layer is prevented. Furthermore, thermal stress caused by heating and cooling during the joining of the core halves is absorbed by the flexible glass solder, preventing deformation of the magnetic head over time. Therefore, a magnetic head with excellent recording and playback characteristics and durability can be provided.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図乃至第9図は本発明の実施例図であって、第1図
は第1実施例に係る磁気ヘッドの斜視図。 第2図は保護膜構造の詳細を示す要部正面図、第3図乃
至第5図は第1コア半体の製造方法を説明する説明図、
第6図及び第7図は第2コア半体の製造方法を説明する
説明図、第8図及び第9図はコア半体の接合工程を説明
する説明図である。第10図は従来の磁気ヘッドの斜視
図を示す。 21a、21b:酸化物系セラミックス基体、22a、
22bl 22c ニガラスはんだ層、23 H2b 
+媒体摺動面、3a、3bニドラック幅規制溝、’4a
、4b:磁性層、5a、5b:巻線窓用凹溝、6:接合
用凹溝、8:保護膜、9:第1のコア半体、io:第2
のコア半体、11:キャップ規制材。 第1図 第3図 第5図 第7図 第8図 第9図 第10図゛
Figures 1 to 9 are embodiments of the present invention, with Figure 1 being a perspective view of a magnetic head according to the first embodiment. Figure 2 is a front view of the main part showing the details of the protective film structure, and Figures 3 to 5 are explanatory diagrams illustrating the manufacturing method of the first core half.
Figures 6 and 7 are explanatory diagrams illustrating the manufacturing method of the second core half, and Figures 8 and 9 are explanatory diagrams illustrating the joining process of the core half. Figure 10 shows a perspective view of a conventional magnetic head. 21a, 21b: Oxide-based ceramic substrate, 22a,
22bl 22c Niglass solder layer, 23 H2b
+ Media sliding surface, 3a, 3b Nidrak width regulation groove, '4a
4b: Magnetic layer, 5a, 5b: Grooves for winding windows, 6: Grooves for bonding, 8: Protective film, 9: First core half, io: Second
The core half, 11: cap regulating material. Figures 1, 3, 5, 7, 8, 9, and 10.

Claims (3)

【特許請求の範囲】[Claims] (1)非磁性基体の一側面に高透磁率磁性材料から成る
磁性層が設けられた2つのコア半体を、ギャップ規制材
及び接合材を介して接合して成る磁気ヘッドにおいて、
前記非磁性基体を酸化物系セラミックス材料にて形成す
ると共に、前記接合材としてガラスはんだを用いたこと
を特徴とする磁気ヘッド。
(1) A magnetic head comprising two core halves, each having a magnetic layer made of a high-permeability magnetic material on one side surface of a non-magnetic substrate, joined together via a gap restricting material and a bonding material,
A magnetic head characterized in that the non-magnetic substrate is formed from an oxide-based ceramic material, and glass solder is used as the bonding material.
(2)特許請求の範囲第(1)項記載の磁気ヘッドにむ
いて、前記磁性層とガラスはんだとの間に、前記磁性層
を被覆する酸化物系セラミックス層とこの酸化物系セラ
ミックス層を被覆するクロム層とを介設したことを特徴
とする磁気ヘッド。
(2) A magnetic head as described in claim (1), characterized in that an oxide-based ceramic layer covering the magnetic layer and a chromium layer covering the oxide-based ceramic layer are interposed between the magnetic layer and the glass solder.
(3)特許請求の範囲第(2)項記載の磁気ヘッドにお
いて、前記酸化物系セラミックス層の厚さを2μm以下
、前記クロム層の厚さを1μm以下に調整したことを特
徴とする磁気ヘッド。
(3) A magnetic head according to claim (2), characterized in that the thickness of the oxide ceramic layer is adjusted to 2 μm or less and the thickness of the chromium layer is adjusted to 1 μm or less.
JP22660887A 1987-09-11 1987-09-11 Magnetic head Pending JPS6470902A (en)