JPS6471702A - Modifier for woody material - Google Patents
Modifier for woody materialInfo
- Publication number
- JPS6471702A JPS6471702A JP15433187A JP15433187A JPS6471702A JP S6471702 A JPS6471702 A JP S6471702A JP 15433187 A JP15433187 A JP 15433187A JP 15433187 A JP15433187 A JP 15433187A JP S6471702 A JPS6471702 A JP S6471702A
- Authority
- JP
- Japan
- Prior art keywords
- bromized
- weight
- parts
- modifier
- wood
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【発明の詳細な説明】
(産業上の利用分野)
本発明は木質材料の改質剤に関し、更に詳しくは、改質
後の木質材料に防菌性、防黴性、防虫性のみならず優れ
た難燃性を付与することができ、しかもそれらの効力の
持続性にも優れ、更に合釘等の金属止め具を用いてその
木質材料から家屋等の建造物を建設した場合であっても
、用いた金属止め具の腐食を抑制することができる改質
剤に関する。[Detailed Description of the Invention] (Industrial Field of Application) The present invention relates to a wood material modifier, and more specifically, to a wood material modifier that can impart not only antibacterial, antifungal, and insecticidal properties but also excellent flame retardancy to the modified wood material, and moreover, has excellent durability of these effects, and can also suppress corrosion of metal fasteners used when constructing buildings such as houses from the wood material using metal fasteners such as nails.
(従来の技術)
木材は自然が生みだす優れた材料であり、日常生活や産
業上の利用分野で使用されている。(Conventional Technology) Wood is an excellent material produced by nature and is used in daily life and in industrial applications.
しかしながら、木材は易燃性、易腐朽性であり虫害を受
は易く、しかも容易に変形してしまうという欠点を有し
ている。However, wood has several drawbacks: it is easily flammable, easily decays, susceptible to insect damage, and easily deforms.
このような問題を解消するために、従来からは、各種の
薬剤を用いて木材を改質することが行なわれている。To address these problems, wood has traditionally been modified using various chemicals.
例えば、臭化アンモニウム、塩化亜鉛のような無機ハロ
ゲン化物、リン酸水素アンモニウム、リン酸ナトリウム
、ビニルホスホネート、アリルホスホネートのような有
機・無機のリン化合物、硫酸アンモニウム、ホウ酸及び
その塩、ペンタクロロフェノールラウレート等のハロゲ
ン化フェノール、クレオソート油、尿素等の薬剤を改質
の目的と対応させて適宜に組合わせ、それを木材に塗布
したり木材中に注入−含浸して包蔵せしめ、もって木材
に難燃性及び防腐性、防虫性等を付与している。For example, chemicals such as inorganic halides like ammonium bromide and zinc chloride, organic and inorganic phosphorus compounds like ammonium hydrogen phosphate, sodium phosphate, vinyl phosphonates, and allyl phosphonates, halogenated phenols like ammonium sulfate, boric acid and its salts, and pentachlorophenol laurate, creosote oil, and urea are appropriately combined according to the purpose of modification, and these are applied to wood or injected/impregnated into the wood to impart flame retardancy, decay resistance, insect repellency, etc.
また、木材に寸法安定性を付与するために、所定の官能
基を有する樹脂組成物を木材に注入・含浸せしめたのち
、所定の硬化処理を施して樹脂組成物を硬化せしめると
いう方法もよく知られている。この場合には、一般に防
腐性、防虫性も向上する。Furthermore, a well-known method for imparting dimensional stability to wood involves injecting or impregnating the wood with a resin composition having a predetermined functional group, followed by a predetermined curing treatment to harden the resin composition. In this case, the wood generally also exhibits improved decay resistance and insect resistance.
(発明が解決しようとする問題点)
しかしながら、前記したような処理の場合、用いた薬剤
との関係で次のような問題・が生ずる。(Problems the invention aims to solve) However, in the case of the above-mentioned treatment, the following problems arise in relation to the chemicals used.
すなわち、一般に、上記した効能を有する薬剤は金属に
対して活性であるため、改質後の木材を合釘等の金属止
め具を用いて建築物を組立てた場合、合釘等が薬剤によ
って腐食されるという問題である。また、用いる薬剤は
一般に環境衛生面に関しても充分な注意を払うことが必
要である。In other words, since the chemicals with the above-mentioned effects are generally active against metals, if a building is constructed using metal fasteners such as nails after the wood has been modified, the nails and fasteners will corrode due to the chemicals. Furthermore, the chemicals used generally require sufficient attention to environmental hygiene.
本発明は、無害であり、金属止め具等を腐食せしめるこ
とがなく、防腐性、防虫性はいうに及ばず難燃性を高め
、また寸法安定性も向上せしめるに有効であり、しかも
それらの効果の持続性にも優れた新規な木質材料の改質
剤を提供することに目的を有する。The present invention aims to provide a novel wood material modifier that is harmless, does not corrode metal fasteners, and is effective in enhancing flame retardancy, dimensional stability, and providing excellent durability of these effects, in addition to providing anti-corrosion and insect-repellent properties.
(問題点を解決するための手段)
本発明の改質剤は1分子中にエポキシ基、ビニル基を官
能基として少なくとも1個有するブロム化有機化合物又
は/及びブロム化フェノール誘導体−ホルムアルデヒド
樹脂若しくはその初期縮合物を必須成分とする。(Means for solving the problems) The modifier of the present invention comprises a brominated organic compound and/or a brominated phenol derivative-formaldehyde resin or its initial condensate, which has at least one epoxy group or vinyl group as a functional group in one molecule.
まず、本発明における木質材料としては、粉砕若しくは
化学処理されていない有形の木材それ自体又は合板のよ
うな複合材を好適な材料として使用することができる。First, as the wood material in this invention, tangible wood itself that has not been crushed or chemically treated, or composite materials such as plywood, can be used as suitable materials.
又、パーティクルボード、ファイバーボード等を使用す
ることもできる。Additionally, particleboard, fiberboard, etc., can also be used.
本発明の改質剤は後述するブロム化有機化合物又は/及
びブロム化フェノール誘導体−ホルムアルデヒド樹脂若
しくはその初期縮合物を必須成分とする。The modifier of the present invention comprises, as described later, a brominated organic compound and/or a brominated phenol derivative-formaldehyde resin or its initial condensate as essential components.
ブロム化有機化合物は、その分子中にエポキシ基又はビ
ニル基を官能基として少なくとも1個有しているもので
あれば、環式、鎖式、脂環式のいずれであってもよい、
かかるエポキシ基又はビニル基としては、木質材料中に
おいて、重合若しくは硬化反応を生起せしめる効果的な
官能性を淘することが必要であり、かかる重合若しくは
硬化反応により改質剤の溶出、浸出、揮発等の防止が可
能となり、もって防腐性、防虫性、難燃性等の効果およ
び、それ等効果の持続性、TI境衛生の保持等の本発明
の目的を効果的に達成することが可能となる。また、分
子中のブロムの数は格別限定されるものではないが、そ
の含有率が多くなると得られる改質剤の難燃性付与効果
は向上する。Brominated organic compounds may be cyclic, linear, or alicyclic, as long as they have at least one epoxy group or vinyl group as a functional group in their molecule.
Such epoxy or vinyl groups must possess functional properties that effectively induce polymerization or curing reactions in wood materials. These polymerization or curing reactions prevent the elution, leaching, and volatilization of the modifier, thereby effectively achieving the objectives of the present invention, such as antiseptic, insecticidal, and flame-retardant effects, as well as the persistence of these effects and the maintenance of environmental hygiene. Furthermore, while the number of bromes in the molecule is not particularly limited, increasing the brome content improves the flame-retardant effect of the resulting modifier.
このようなブロム化有機化合物のうちエポキシ基を有す
るものとしては、例えば、モノブロモフェノールモノグ
リシジルエーテル、ジブロモフェノールモノグリシジル
エーテル、トリブロモフェノールモノグリシジルエーテ
ル、モノブロモクレゾールモノグリシジルエーテル、ジ
ブロモクレゾールモノグリシジルエーテル、トリブロモ
クレゾールモノグリシジルエーテル、ブロム化フェニル
フェノールモノグリシジルエーテル、ブロム化キシレノ
ールモノグリシジルエーテル、ジブロモノニルフェノー
ルモノグリシジルエーテル、ジブロモ3級ブチルフェノ
ールモノグリシジルエーテル、テトラブロモビスフェノ
ールAジグリシジルエーテル、テトラブロモビスフェノ
ールSジグリシジルエーテル、テトラブロモビスフェノ
ールFジグリシジルエーテル、ブロム化フェノールノポ
ラックエボキシ樹脂、ブロム化りレゾールノボラックエ
ポキシ樹脂、ブロム化ポリビニルフェノールエボキシ樹
脂等をあげることができる。Examples of such brominated organic compounds that have an epoxy group include monobromophenol monoglycidyl ether, dibromophenol monoglycidyl ether, tribromophenol monoglycidyl ether, monobromocresol monoglycidyl ether, dibromocresol monoglycidyl ether, tribromocresol monoglycidyl ether, brominated phenylphenol monoglycidyl ether, brominated xylenol monoglycidyl ether, dibromonolylphenol monoglycidyl ether, dibromo tertiary butylphenol monoglycidyl ether, tetrabromobisphenol A diglycidyl ether, tetrabromobisphenol S diglycidyl ether, tetrabromobisphenol F diglycidyl ether, brominated phenol novolac epoxy resin, brominated resol novolac epoxy resin, and brominated polyvinylphenol epoxy resin.
また、本発明においてビニル基とは有効なラジカル重合
反応性を有する不飽和置換基を総称する。Furthermore, in this invention, the term "vinyl group" refers collectively to unsaturated substituents that have effective radical polymerization reactivity.
かかるビニル基を有する化合物としては、例えばジブロ
モプロピルアクリレート、モノブロモフェノールアクリ
レート、ジブロモフェノールアクリレート、トリブロモ
フェノールアクリレート、ペンタブロモフェノールアク
リレート、モノブロモクレゾールアクリレート、ジブロ
モクレゾールアクリレート、テトラブロモビスフェノー
ルAジアクリレート、ジブロモプロピルメタクリレート
、モノブロモフェノールメタクリレート。Examples of compounds having such vinyl groups include dibromopropyl acrylate, monobromophenol acrylate, dibromophenol acrylate, tribromophenol acrylate, pentabromophenol acrylate, monobromocresol acrylate, dibromocresol acrylate, tetrabromobisphenol A diacrylate, dibromopropyl methacrylate, and monobromophenol methacrylate.
ジブロモフェノールメタクリレート、トリブロモフェノ
ールメタクリレート、ヘンタブロモフェノールメタクリ
レート、モノブロモクレゾールメタクリレート、ジブロ
モクレゾールメタクリレート、トリブロモクレゾールメ
タクリレート、テトラブロモビスフェノールAジメタク
リレート、ブロム化パラヒドロキシスチレン、ブロム化
スチレン、臭素化パラヒドロキシスチレンメタクリレー
ト等をあげることができる。Examples include dibromophenol methacrylate, tribromophenol methacrylate, hentabromophenol methacrylate, monobromocresol methacrylate, dibromocresol methacrylate, tribromocresol methacrylate, tetrabromobisphenol A dimethacrylate, brominated p-hydroxystyrene, brominated styrene, brominated p-hydroxystyrene methacrylate, and the like.
更に、エポキシ基、ビニル基のいずれをも有する化合物
としては、例えば、モノブロモフェノールエポキシアク
リレート、ジブロ千フェノールエポキシアクリレート、
トリブロモフェノールエポキシアクリレート、ジブロモ
クレゾールエポキシアクリレート、テトラブロモビスフ
ェノールAエポキシアクリレート、モノブロモフェノー
ルエポキシメタクリレート、ジブロモフェノールエポキ
シメタクリレート、ジブロモクレゾールエポキシアクリ
レート、テトラブロモビスフェノールAジェポキシメタ
クリレート、ブロム化パラグリシジルエーテルスチレン
、ブロム化スチレンのエチレンオキサイド又はプロピレ
ンオキサイド等の付加物等をあげることができる。Furthermore, examples of compounds having both epoxy groups and vinyl groups include monobromophenol epoxy acrylate, dibromophenol epoxy acrylate,
Examples include tribromophenol epoxy acrylate, dibromocresol epoxy acrylate, tetrabromobisphenol A epoxy acrylate, monobromophenol epoxy methacrylate, dibromophenol epoxy methacrylate, dibromocresol epoxy acrylate, tetrabromobisphenol A dipoxymethacrylate, brominated paraglycidyl ether styrene, and adducts of brominated styrene such as ethylene oxide or propylene oxide.
本発明におけるブロム化フェノール誘導体−ホルムアル
デヒド樹脂若しくはその初期縮合物は、フロム化フェノ
ール誘導体をホルムアルデヒドを介して付加縮合して成
る樹脂若しくはその初期縮合物である。The brominated phenol derivative-formaldehyde resin or its initial condensate in the present invention is a resin or its initial condensate obtained by addition condensation of a brominated phenol derivative via formaldehyde.
この場合のブロム化フェノール誘導体は、フェノール又
はその誘導体の水酸基以外の水素の少なくとも1個をブ
ロム置換したものである。In this case, a brominated phenol derivative is one in which at least one hydrogen atom other than the hydroxyl group of phenol or its derivative is substituted with bromide.
具体的には、例えば、モノブロモフェノール。Specifically, for example, monobromophenol.
ジブロモフェノール、モノブロモクレゾール、ジブロモ
クレゾール、モノブロモレゾルシノール。Dibromophenol, monobromocresol, dibromocresol, monobromolesorcinol.
ジブロモレゾルシノール等の単独、若しくは2種以上の
混合物のホルムアルデヒド縮合物であって、それらのレ
ゾール型又はノボラック型樹脂若しくはその縮合物をあ
げることができる。Examples include formaldehyde condensates of dibromolesorcinol alone or in mixtures of two or more such substances, and resol-type or novolac-type resins or condensates thereof.
本発明の改質剤は、上記したブロム化有機化合物、ブロ
ム化フェノール誘導体−ホルムアルデヒド樹脂若しくは
その初期縮合物のそれぞれ1種をそのままで、又は両者
を混合し、必要に応じて硬化剤とともに溶媒に溶解せし
めて調製することができる。用いる溶媒としては、例え
ば、灯油;メタノール、エタノールのようなアルコール
;アセトン、MEKのようなケトン;トルエン、キシレ
ン、ベンゼンのような芳香族系のものをあげることがで
きる。溶媒の使用量は、得られた改質剤を例えば木質材
料に注入・含浸せしめるに好適な粘度となり、しかも含
浸せしめられた上記薬効成分が適正な効果を発揮するに
必要な量となるように適宜法められる。具体的には、改
質後の木質材料中におけるブロム量が1重量%以上、好
ましくは3重量%以上となるように、上記成分と溶媒と
を混合すればよい。The modifier of the present invention can be prepared by dissolving one of the above-mentioned brominated organic compounds, brominated phenol derivative-formaldehyde resin, or their initial condensate, either as is or as a mixture of both, in a solvent together with a curing agent as needed. Examples of solvents that can be used include kerosene; alcohols such as methanol and ethanol; ketones such as acetone and MEK; and aromatic solvents such as toluene, xylene, and benzene. The amount of solvent used is appropriately determined so that the resulting modifier has a viscosity suitable for injection and impregnation into, for example, wood material, and is sufficient for the impregnated active ingredient to exert its proper effect. Specifically, the above-mentioned ingredients and the solvent should be mixed so that the amount of brome in the modified wood material is 1% by weight or more, preferably 3% by weight or more.
本発明の改質剤を用いた木質材料の改質処理は次のよう
にして行なわれる。すなわち、上記した改質剤の溶液を
まず木質材料に注入・含浸する。注入・含浸法としては
常圧注入法、減圧注入法、加圧注入性等公知の方法を使
用することができ、これら各方法を適宜に組合わせた方
法を適用することができる。かくして、木質材料内に改
質剤を注入中含浸処理した後に、適宜な方法により重合
、あるいは硬化処理をすればよい。The wood material modification treatment using the modifier of the present invention is carried out as follows. That is, the above-mentioned modifier solution is first injected and impregnated into the wood material. Known methods such as atmospheric pressure injection, reduced pressure injection, and pressurized injection can be used as the injection and impregnation method, and methods that combine these methods as appropriate can be applied. Thus, after the wood material has been treated with injection and impregnation of the modifier, polymerization or hardening treatment can be carried out by an appropriate method.
(発明の実施例) 実施例1〜6.比較例1,2 米松、ブナの各木材からそれぞれ防腐試験。(Examples of the Invention) Examples 1-6. Comparative Examples 1 and 2 Preservative tests were conducted on Douglas fir and beech wood, respectively.
防蟻試験を行うために木口面2cmX2cm、軸方向1
cm、又難燃試験、全針腐食試験を行うために木目方向
30cmX横20cmX厚さ5mmとなるように木材ブ
ロックを切り出した。これらブロックにアセトン抽出処
理を施したのち乾燥し、更に熱水抽出処理を施し、絶乾
燥してそれぞれの重rを測定した。To conduct the termite resistance test, measure 2cm x 2cm on the end grain and 1cm in the axial direction.
To conduct flame retardancy tests and total needle corrosion tests, wood blocks were cut to measure 30 cm in the grain direction, 20 cm in width, and 5 mm in thickness. These blocks were subjected to acetone extraction treatment, dried, then subjected to hot water extraction treatment, and then air-dried, after which their respective weights were measured.
つぎに、以下の4種類の改質剤を調製した。Next, the following four types of modifiers were prepared.
すなわち、ジブロモフェノールモノグリシジルエーテル
98重量部とトリエチルアミン2重量部とから成る溶液
(実施例1〜3)、フェノールモノグリシジルエーテル
98重量部とトリエチルアミン2重量部とから成る溶液
(比較例1)、テトラブロモビスフェノールAジグリシ
ジルエーテル98重量部とトリエチルアミン2重量部と
トルエン100重量部とから成る溶液(実施例4〜6)
、ビスフェノールAジグリシジルエーテル98重量部と
トリエチルアミン2重量部とトルエン100重量部とか
ら成る溶液(比較例2)である。Specifically, a solution consisting of 98 parts by weight of dibromophenol monoglycidyl ether and 2 parts by weight of triethylamine (Examples 1-3), a solution consisting of 98 parts by weight of phenol monoglycidyl ether and 2 parts by weight of triethylamine (Comparative Example 1), and a solution consisting of 98 parts by weight of tetrabromobisphenol A diglycidyl ether, 2 parts by weight of triethylamine and 100 parts by weight of toluene (Examples 4-6).
The solution (Comparative Example 2) consists of 98 parts by weight of bisphenol A diglycidyl ether, 2 parts by weight of triethylamine, and 100 parts by weight of toluene.
上記の各木材ブロック100重量部に対する各改質剤の
使用量は、実施例の場合、5重量部。In the example, the amount of each modifier used per 100 parts by weight of each wood block was 5 parts by weight.
10重量部、20重量部の3水準二また比較例の場合は
20重量部とし〈実施例4〜6.比較例2の場合はトル
エン以外の成分の量)を各種の木材ブロックと改質剤の
組につき、オートクレーブ処理を行った。即ち木材ブロ
ックと改質剤をオートクレーブに収容し、減圧下にて4
0℃で10分間1次いで6気圧の加圧下にて40℃で1
0分間、続いて減圧下にて40℃で1時間、最後に6気
圧の加圧下にて150℃で2時間処理した。Three levels were used: 10 parts by weight, 20 parts by weight, and in the case of comparative examples, 20 parts by weight (Examples 4-6. In the case of Comparative Example 2, the amount of components other than toluene). These were autoclaved for various combinations of wood blocks and modifiers. That is, the wood blocks and modifiers were placed in an autoclave and autoclaved under reduced pressure for 4
1 minute at 0°C, then 1 minute at 40°C under a pressure of 6 atmospheres.
The sample was treated for 0 minutes, then under reduced pressure at 40°C for 1 hour, and finally under pressure at 6 atmospheres at 150°C for 2 hours.
オートクレーブ処理後、処理ブロックを取り出し風乾し
たのちそれぞれの重量を測定した。After autoclaving, the processed blocks were removed, air-dried, and then their weights were measured.
各処理ブロックにつき下記仕様で防腐効力試験、防蟻試
験、難燃性試験、合釘腐食試験を行なった0以上の結果
を第1表に示した。Table 1 shows the results of the following tests conducted on each treatment block: anti-corrosion efficacy test, termite resistance test, flame retardancy test, and nail corrosion test, with results of 0 or higher.
防腐効力試験二日木木材保存協会規格 (JWPA)第1号(1979) の方法に準拠し、菌としてはオ オウズラタケを使用し、無処理 の木材ブロックサンプルの重量 減との比較により、防腐効力値 を算出した。The wood preservative efficacy test was conducted in accordance with the Japan Wood Preservation Association Standard (JWPA) No. 1 (1979). The fungus used was *Ophiopogon pulcherrimus*, and the wood preservative efficacy value was calculated by comparing it with the weight reduction of an untreated wood block sample.
防蟻試験:上記JWPA第11号(1)(1981)に
準拠して行い、
21日後の重量減少率により評
価を行った。Termite control test: Conducted in accordance with JWPA No. 11 (1) (1981) above, and evaluated by the weight loss rate after 21 days.
難燃性試験:JIS A 1322(建築用薄物材
料の難燃性試験方法)に
準拠し、材料の木目方向を縦方
向において試験を行い、/<−
ナーによる加熱時間は3分と
し、試験後の炭化長、残炎、残
じんを測定した。Flame retardancy test: In accordance with JIS A 1322 (Test method for flame retardancy of thin building materials), the test was conducted with the wood grain direction in the longitudinal direction, the heating time with a heater was 3 minutes, and the carbonization length, afterflame, and dust after the test were measured.
なお、試験時に3分以内に燃 焼がすすみ試験装置内で試験の 継続が不可能になったものに ついては、試験後の測定項目 に(−)を記入しである。Furthermore, for samples that burned within 3 minutes during the test, making it impossible to continue the test within the test apparatus, a (-) should be entered in the measurement item after the test.
腐食試験:各木材ブロックに対し、亜鉛メツキの施され
た鉄釘を打ち込
み、温度30℃、相対湿度75
%の恒温恒温器中に30日間
放置した後、その腐食状態を観
察した。その腐食程度を(全
く腐食を認めない O1腐食を
僅かに認める Δ、腐食 ×)
で表わした。Corrosion Test: Zinc-plated iron nails were driven into each wood block and left in a constant temperature chamber at 30°C and 75% relative humidity for 30 days. The corrosion state was then observed. The degree of corrosion was expressed as follows: (O1: No corrosion at all, Δ: Slight corrosion, ×: Corrosion).
なお、この試験において同時 に、臭化アンモニウムを使用し た市販の難燃合板の切片を用い て同様の試験を行ったところ、 鉄釘には著しい腐食がみられ た。Furthermore, in the same test conducted simultaneously using sections of commercially available flame-retardant plywood treated with ammonium bromide, significant corrosion was observed in the iron nails.
なお、上記改質剤で処理しない場合の結果も表に示した
。The results for cases where the above-mentioned modifier was not used are also shown in the table.
実施例7〜12.比較例3.4
改質剤としては、トリブロモフェノールメタクリレート
100重量部とアセトン100重量部とから成る溶液(
実施例7〜9)、フェノールメタクリレート100重量
部とアセトン100重量部とから成る溶液(比較例3)
、モノブロモフェノールとジブロモフェノールとの混合
物のホルムアルデヒド樹脂(分子量:4500)10(
l置部をメタノール100重量部に溶解せしめて成る溶
液(li例1O−12)、フェノール−ホルムアルデヒ
ド樹脂(分子量:4000)too重量部をメタノール
100重量部に溶解せしめて成る溶液(比較例4)を用
いた。Examples 7-12. Comparative Example 3.4 As a modifier, a solution consisting of 100 parts by weight of tribromophenol methacrylate and 100 parts by weight of acetone (
Examples 7-9), a solution consisting of 100 parts by weight of phenol methacrylate and 100 parts by weight of acetone (Comparative Example 3)
, a formaldehyde resin (molecular weight: 4500) of a mixture of monobromophenol and dibromophenol 10 (
A solution was prepared by dissolving the 1 part in 100 parts by weight of methanol (Example 10-12), and a solution was prepared by dissolving too much by weight of phenol-formaldehyde resin (molecular weight: 4000) in 100 parts by weight of methanol (Comparative Example 4).
試験ブロックと、各試験ブロック100重量部に対する
各改質剤の使用量は前記実施例1〜6の場合と同様に5
重量部、10重量部、20重量部、又比較例では20重
量部(溶媒を除いた成分の量)とし実施例1〜6の場合
と同一の条件によりオートクレーブ処理を行った。The number of test blocks and the amount of each modifier used per 100 parts by weight of each test block are the same as in Examples 1 to 6 above.
Autoclave treatment was performed using parts by weight, 10 parts by weight, 20 parts by weight, and in the comparative example, 20 parts by weight (amount of component excluding solvent) under the same conditions as in Examples 1 to 6.
得られた各処理プロッタについて、実施例1〜6と同様
の方法で防腐効力試験、防蟻試験、難燃性試験、合釘腐
食試験を行ない、その結果を第2表に示した。For each of the obtained treated plotters, anti-corrosion efficacy tests, termite resistance tests, flame retardancy tests, and nail corrosion tests were performed using the same methods as in Examples 1 to 6, and the results are shown in Table 2.
実施例13.14.比較例5.6
改質剤としては、ジブロモフェノールモノグリシジルエ
ーテル48重量部、臭素化クレゾールノボランク樹脂(
分子14200:臭素含有率35%)50重量部、ジエ
チルアミン2重量部。Examples 13.14. Comparative Examples 5.6. The modifiers were 48 parts by weight of dibromophenol monoglycidyl ether and brominated cresol novolank resin (
Molecular weight 14200 (bromine content 35%) 50 parts by weight, diethylamine 2 parts by weight.
アセトン100重量部とからなる溶液(実施例13)、
ジブロモフェノールメタクリレート50rfXrJt部
、臭素化クレゾールノボラック樹脂(分子量4200
:臭素含有率35%)50重量部。A solution consisting of 100 parts by weight of acetone (Example 13),
Dibromophenol methacrylate 50 rfXrJt parts, brominated cresol novolac resin (molecular weight 4200)
:bromine content 35%) 50 parts by weight.
アセトン100重量部とからなる溶液(実施例14)、
フェノールモノグリシジルエーテル48重量部、クレゾ
ールノポラ7り樹脂(分子量4000)50重量部、ジ
エチルアミン2重量部とからなる溶液(比較例5)、フ
ェノールメタクリレート50重量部、クレゾールノボラ
ック樹脂(分子量4000)50重量部、アセトン10
0TI¥贋部とからなる溶液(比較例6)を用いた。A solution consisting of 100 parts by weight of acetone (Example 14),
A solution consisting of 48 parts by weight of phenol monoglycidyl ether, 50 parts by weight of cresol novolac resin (molecular weight 4000), and 2 parts by weight of diethylamine (Comparative Example 5), 50 parts by weight of phenol methacrylate, 50 parts by weight of cresol novolac resin (molecular weight 4000), and 10 parts by weight of acetone.
A solution consisting of 0TI\fake part (Comparative Example 6) was used.
試験ブロックと、各試験ブロック100重量部に対する
各改質剤の使用量はいずれの試験の場合も20重量部(
溶媒を除いた成分の量)とし、実施例1〜6の場合と同
一の条件によりオートクレーブ処理を行った。The amount of each modifier used per 100 parts by weight of each test block is 20 parts by weight in all tests.
The amount of the component excluding the solvent was used, and autoclaving was performed under the same conditions as in Examples 1 to 6.
得られた各処理ブロックについて、実施例1〜6と同様
の方法で、防腐効力試験、防蟻試験、難燃性試験(ただ
し、比較例5.6は行なわず)。Each of the obtained treated blocks was subjected to anti-corrosion efficacy tests, termite resistance tests, and flame retardancy tests in the same manner as in Examples 1 to 6 (however, Comparative Examples 5 and 6 were not subjected to these tests).
全針腐食試験を行ない、その結果を第3表に示した。A total needle corrosion test was conducted, and the results are shown in Table 3.
(発明の効果)
以上の説明で明らかなように、本発明の改質剤は、木質
材料への防腐性、防虫性付与効果を有するのみならず難
燃性付与効果も有している。また、毒性はなく全針等を
腐食させることもない。(Effects of the Invention) As is clear from the above description, the modifier of the present invention not only has the effect of imparting preservative and insecticidal properties to wood materials, but also has the effect of imparting flame retardancy. Furthermore, it is non-toxic and does not corrode needles, etc.
更には、注入・含浸された改質剤が硬化して安定化する
ため上記の効果の持続性にも優れ、又改質後の木質材料
の寸法安定性も良好になる。Furthermore, because the injected and impregnated modifier hardens and stabilizes, the above effects are highly durable, and the dimensional stability of the modified wood material is also good.
したがって、建築用、建設用、各種内装用、家具調度用
に用いる木材の改質剤としてその工業的価値は大である
。Therefore, it has great industrial value as a wood modifier used for building, construction, various interior finishes, and furniture.
Claims (1)
も1個有するブロム化有機化合物又は/及びブロム化フ
ェノール誘導体−ホルムアルデヒド樹脂若しくはその初
期縮合物を必須成分とする木質材料の改質剤。A wood material modifier comprising a brominated organic compound having at least one epoxy group or vinyl group as a functional group in its molecule, and/or a brominated phenol derivative-formaldehyde resin or its initial condensate as essential components.