RU2425183C2 - Procedures and equipment for production of mono-crystal cast silicon and items of mono-crystal cast silicon for photo cells - Google Patents

Procedures and equipment for production of mono-crystal cast silicon and items of mono-crystal cast silicon for photo cells Download PDF

Info

Publication number
RU2425183C2
RU2425183C2 RU2008134068/05A RU2008134068A RU2425183C2 RU 2425183 C2 RU2425183 C2 RU 2425183C2 RU 2008134068/05 A RU2008134068/05 A RU 2008134068/05A RU 2008134068 A RU2008134068 A RU 2008134068A RU 2425183 C2 RU2425183 C2 RU 2425183C2
Authority
RU
Russia
Prior art keywords
silicon
crucible
crystal
seed
array
Prior art date
Application number
RU2008134068/05A
Other languages
Russian (ru)
Other versions
RU2008134068A (en
Inventor
Натан Г. СТОДДАРД (US)
Натан Г. СТОДДАРД
Original Assignee
ЭйЭмДжи АЙДЕАЛКАСТ СОЛАР КОРПОРЕЙШН
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ЭйЭмДжи АЙДЕАЛКАСТ СОЛАР КОРПОРЕЙШН filed Critical ЭйЭмДжи АЙДЕАЛКАСТ СОЛАР КОРПОРЕЙШН
Publication of RU2008134068A publication Critical patent/RU2008134068A/en
Application granted granted Critical
Publication of RU2425183C2 publication Critical patent/RU2425183C2/en

Abstract

FIELD: metallurgy.
SUBSTANCE: one of versions is disclosed in procedure for production of cast silicon consisting in contacting melt silicon with at least one seeding crystal of silicon in vessel with one or several side walls heated at least to temperature of silicon melting; also, there is at least one cooled wall. Further, the procedure consists in formation of solid massif of mono-crystal silicon, not necessarily, with at least two dimensions, each at least approximately 10 cm by cooling melted silicon with control of crystallisation. Also, formation of massif includes formation of interface of solid with liquid along rib of melted silicon which at least first is parallel to at least one cooled wall. Interface is controlled during cooling so, that it is transferred in the direction where distance between melted silicon and at least one cooled wall increases. There is produced cast massif of silicon of large dimension (for example, ingots with area of cross section of at least 1 m2 and up to 4-8 m2) not containing or practically not containing radially distributed impurities and oxygen induced defects of packing.
EFFECT: more fast, efficient and less expensive procedures facilitating control of dimension, shape and orientation of grains of crystal in cast massif of crystallised silicon.
34 cl, 9 dwg, 3 ex

Description

Область техникиTechnical field

Настоящее изобретение в целом относится к области фотоэлементов и способам и аппаратуре для производства литого кремния для применения в фотоэлементах. Кроме того, изобретение относится к новым формам литого кремния, которые можно использовать в изготовляемых устройствах, таких как ячейки фотоэлементов и другие полупроводниковые устройства. Новый кремний может иметь монокристаллическую структуру, и его можно получать литьем.The present invention generally relates to the field of solar cells and methods and apparatus for the production of cast silicon for use in solar cells. In addition, the invention relates to new forms of cast silicon that can be used in manufactured devices, such as cell solar cells and other semiconductor devices. New silicon may have a single crystal structure, and it can be obtained by casting.

Предпосылки создания изобретенияBACKGROUND OF THE INVENTION

В фотоэлементах свет преобразуется в электрический ток. Одним из наиболее важных параметров фотоэлемента является эффективность превращения энергии света в электрическую энергию. Хотя фотоэлементы можно изготовить из разных полупроводников, обычно используют кремний, т.к. он легко доступен по разумной цене и обладает подходящим балансом электрических, физических и химических свойств, необходимых для применения в фотоэлементах.In photocells, light is converted into electric current. One of the most important parameters of a solar cell is the efficiency of converting light energy into electrical energy. Although solar cells can be made from different semiconductors, silicon is usually used because it is easily available at a reasonable price and has the right balance of electrical, physical and chemical properties needed for use in solar cells.

В известном способе изготовления фотоэлементов кремнийсодержащее сырье смешивают с материалом (или легирующей примесью) для индуцирования либо положительной, либо отрицательной проводимости, расплавляют и затем кристаллизуют либо путем вытягивания из зоны плавления в виде слитков монокристаллического кремния (способы Чохральского (CZ) или зонной плавки (FZ)), либо путем заливки в блоки или «кирпичи» поликристаллического кремния в зависимости от размера зерен отдельных частиц кремния. В описанной методике слитки или блоки режут на тонкие подложки или пластины известными способами резки или распиливания. Эти пластины можно затем использовать для изготовления фотоэлементов.In the known method for the manufacture of solar cells, silicon-containing raw materials are mixed with the material (or dopant) to induce either positive or negative conductivity, melted and then crystallized either by pulling single-crystal silicon ingots from the melting zone (Czochralski (CZ) or zone melting (FZ) methods )), or by pouring polycrystalline silicon into blocks or "bricks" depending on the grain size of individual silicon particles. In the described technique, ingots or blocks are cut into thin substrates or plates by known methods of cutting or sawing. These plates can then be used to make photocells.

Монокристаллический кремний для применения в производстве фотоэлементов обычно получают способами CZ или FZ в виде слитка цилиндрической формы. В способе CZ слиток медленно вытягивают из ванны с расплавленным кремнием. В способе FZ твердый материал протягивают через зону плавления, и затем он повторно затвердевает на другой стороне зоны плавления. В слитке монокристаллического кремния, полученном такими способами, радиально распределены примеси и дефекты, такие как кольцевые кислород-индуцированные дефекты упаковки (OSF) и «спиральные» дефекты междуузельных или вакантных кластеров. Даже в присутствии таких примесей и дефектов монокристаллический кремний является в целом предпочтительным источником кремния для изготовления фотоэлементов, т.к. его можно использовать для получения высокоэффективных солнечных батарей. Однако при производстве известными способами, описанными выше, монокристаллический кремний является более дорогим, чем традиционный поликристаллический кремний.Monocrystalline silicon for use in the manufacture of solar cells is usually obtained by CZ or FZ methods in the form of a cylindrical ingot. In method CZ, an ingot is slowly drawn from a bath of molten silicon. In the FZ method, solid material is pulled through the melting zone, and then it solidifies again on the other side of the melting zone. In a single-crystal silicon ingot obtained by such methods, impurities and defects, such as ring oxygen-induced stacking faults (OSF) and “spiral” defects of interstitial or vacant clusters, are radially distributed. Even in the presence of such impurities and defects, single-crystal silicon is generally the preferred source of silicon for the manufacture of solar cells, because it can be used to produce highly efficient solar cells. However, in the production by known methods described above, single-crystal silicon is more expensive than traditional polycrystalline silicon.

Традиционный поликристаллический кремний для изготовления фотоэлементов обычно получают способом литья. Способы литья для получения обычного поликристаллического кремния известны в области технологии фотоэлементов. Коротко говоря, в таких способах расплав кремния находится в тигле, например в кварцевом тигле, и его охлаждают регулируемым образом для кристаллизации. Полученный блок поликристаллического кремния обычно режут на брикеты с таким поперечным сечением, которое воспроизводит или близко к размеру пластины, которую будут использовать для изготовления фотоэлемента, и брикеты распиливают или как-то режут на такие пластины. Полученный таким образом поликристаллический кремний представляет собой агломерат кристаллических зерен, и в пластинах, полученных из него, ориентация зерен относительно друг друга совершенно беспорядочна.Conventional polycrystalline silicon for the manufacture of solar cells is usually obtained by casting. Casting methods for producing conventional polycrystalline silicon are known in the field of photocell technology. In short, in such methods, the silicon melt is in a crucible, for example in a quartz crucible, and is cooled in a controlled manner for crystallization. The obtained block of polycrystalline silicon is usually cut into briquettes with such a cross section that reproduces either close to the size of the plate that will be used to manufacture the photocell, and the briquettes are sawn or somehow cut into such plates. Polycrystalline silicon thus obtained is an agglomerate of crystalline grains, and in the wafers obtained from it, the orientation of the grains relative to each other is completely random.

Беспорядочная ориентация зерен либо в традиционном мульти- или поликристаллическом кремнии затрудняет текстурирование поверхности полученной пластины. Текстурирование используют для повышения эффективности фотоэлемента путем уменьшения отражения и увеличения поглощения энергии света поверхностью элемента. Кроме того, «уступы», которые образуются на границах зерен традиционного поликристаллического кремния, создают тенденцию к зарождению структурных дефектов в виде кластеров или рядов дислокаций. Считается, что эти дислокации и примеси, которые они стремятся к себе привлечь, вызывают быструю рекомбинацию носителей электрического заряда в работающем фотоэлементе, изготовленном из традиционного поликристаллического кремния. Это может снизить эффективность такого элемента. Фотоэлементы из такого поликристаллического кремния обычно менее эффективны по сравнению с эквивалентными фотоэлементами из монокристаллического кремния, даже принимая во внимание радиальное распределение дефектов в монокристаллическом кремнии, полученном известными способами. Однако благодаря сравнительной простоте и меньшим затратам на получение традиционного поликристаллического кремния, а также эффективной пассивации дефектов при работе фотоэлемента, поликристаллический кремний является более широко используемой формой кремния при изготовлении фотоэлементов.The random orientation of the grains in either traditional multi- or polycrystalline silicon makes texturing of the surface of the wafer difficult. Texturing is used to increase the efficiency of the photocell by reducing reflection and increasing the absorption of light energy by the surface of the element. In addition, the “ledges” that form at the grain boundaries of traditional polycrystalline silicon create a tendency to nucleation of structural defects in the form of clusters or rows of dislocations. It is believed that these dislocations and impurities that they seek to attract to themselves cause rapid recombination of electric charge carriers in a working photocell made of traditional polycrystalline silicon. This may reduce the effectiveness of such an element. Photovoltaic cells from such polycrystalline silicon are usually less efficient than equivalent solar cells from single-crystal silicon, even taking into account the radial distribution of defects in single-crystal silicon obtained by known methods. However, due to the comparative simplicity and lower cost of obtaining traditional polycrystalline silicon, as well as the effective passivation of defects during the operation of the solar cell, polycrystalline silicon is a more widely used form of silicon in the manufacture of solar cells.

Предшествующие методики литья включали использование для роста кристаллов тигля с «холодной стенкой». Термин «холодная стенка» означает, что индукционные катушки, расположенные на стенках или внутри тигля, охлаждаются водой и могут быть также щелевыми, так что обычно остаются при температуре ниже 100°С. Стенки тигля можно расположить в тесной близости между катушками и подачей сырья. Материал стенок тигля не является конкретно термически изолированным и поэтому может оставаться в термическом равновесии с охлажденными катушками. Поэтому нельзя утверждать, что нагревание кремния происходит в результате излучения от стенок тигля, т.к. индуктивное нагревание кремния в тигле означает, что кремний нагревается прямо индуцированным в нем током. Таким образом, стенки тигля остаются при температуре ниже температуры плавления кремния и могут рассматриваться как «холодные» относительно расплавленного кремния. При отверждении индуктивно нагретого расплавленного кремния эти холодные стенки тигля действуют в качестве теплоотвода. Слиток быстро охлаждается путем передачи тепла к холодным стенкам. Поэтому начальный фронт отверждения быстро становится практически искривленным, а образование центров кристаллизации по бокам слитка и рост диагонально по отношению к центру слитка делает безрезультатной любую попытку сохранить вертикальный и геометрически упорядоченный процесс кристаллизации или практически плоский фронт отверждения.Previous casting techniques included the use of a “cold wall” crucible for crystal growth. The term "cold wall" means that the induction coils located on the walls or inside the crucible are cooled by water and can also be slotted, so that they usually remain at a temperature below 100 ° C. The walls of the crucible can be located in close proximity between the coils and the feed. The material of the walls of the crucible is not specifically thermally insulated and therefore may remain in thermal equilibrium with the cooled coils. Therefore, it cannot be argued that the heating of silicon occurs as a result of radiation from the walls of the crucible, because Inductive heating of silicon in a crucible means that silicon is heated directly by the current induced in it. Thus, the crucible walls remain at a temperature below the melting temperature of silicon and can be considered as “cold” relative to molten silicon. During the curing of inductively heated molten silicon, these cold crucible walls act as a heat sink. The ingot is rapidly cooled by transferring heat to the cold walls. Therefore, the initial curing front quickly becomes practically curved, and the formation of crystallization centers on the sides of the ingot and growth diagonally with respect to the center of the ingot makes any attempt to maintain a vertical and geometrically ordered crystallization process or an almost flat curing front unsuccessful.

Ввиду сказанного выше существует необходимость в создании улучшенной формы кремния, которую можно было бы использовать для изготовления фотоэлементов. Существует также необходимость получения кремния более быстрым и менее дорогим способом, чем те, которые использовали ранее для получения монокристаллического кремния. Настоящее изобретение предлагает такой кремний и такие способы.In view of the above, there is a need to create an improved form of silicon, which could be used for the manufacture of solar cells. There is also a need to obtain silicon in a faster and less expensive way than those previously used to produce single crystal silicon. The present invention provides such silicon and such methods.

СУЩНОСТЬ ИЗОБРЕТЕНИЯSUMMARY OF THE INVENTION

Использованный здесь термин «монокристаллический кремний» относится к массиву монокристаллов кремния с одной преимущественной ориентацией кристаллов. Кроме того, традиционный поликристаллический кремний относится к кристаллическому кремнию с распределением зерен по размеру в сантиметровом диапазоне с беспорядочно ориентированными кристаллами в этом массиве кремния.The term “monocrystalline silicon” as used herein refers to an array of silicon single crystals with one preferred crystal orientation. In addition, traditional polycrystalline silicon refers to crystalline silicon with a grain size distribution in the centimeter range with randomly oriented crystals in this silicon array.

Далее, использованный здесь термин «поликристаллический кремний» относится к кристаллическому кремнию с размером зерен порядка микрона и множественной ориентацией зерен в данном массиве кремния. Например, зерна обычно имеют размеры в среднем примерно от субмикронных до субмиллиметровых (например, отдельные зерна могут быть не видны невооруженным глазом) при беспорядочной ориентации зерен в массиве.Further, the term “polycrystalline silicon” as used herein refers to crystalline silicon with a grain size of the order of a micron and multiple grain orientations in a given silicon array. For example, grains usually have an average size of about submicron to submillimeter (for example, individual grains may not be visible to the naked eye) with random orientation of the grains in the array.

Далее, использованный здесь термин «почти монокристаллический кремний» относится к массиву кристаллического кремния с одной преимущественной ориентацией кристаллов в более чем 50 об.% массива, где, например, почти монокристаллический кремний может представлять собой массив монокристаллического кремния рядом с поликристаллической областью, или он может представлять собой большой сплошной кристалл кремния, который частично или полностью содержит более мелкие кристаллы кремния других кристаллических ориентаций, причем более мелкие кристаллы составляют не более 50% общего объема. Предпочтительно, чтобы почти кристаллический кремний мог содержать более мелкие кристаллы, которые составляют не более 25% общего объема. Более предпочтительно, чтобы почти кристаллический кремний мог содержать более мелкие кристаллы, которые составляли бы не более 10% общего объема. Еще более предпочтительно, чтобы почти кристаллический кремний содержал более мелкие кристаллы, которые составляли бы не более 5% общего объема.Further, the term “almost single crystalline silicon” as used herein refers to an array of crystalline silicon with one preferred crystal orientation in more than 50 vol.% Of the array, where, for example, almost single crystal silicon can be an array of single crystal silicon near the polycrystalline region, or it can represent a large continuous silicon crystal, which partially or completely contains smaller silicon crystals of other crystalline orientations, with smaller cr comprise crystals of not more than 50% of total. Preferably, almost crystalline silicon could contain finer crystals, which make up no more than 25% of the total volume. More preferably, almost crystalline silicon could contain finer crystals, which would make up no more than 10% of the total volume. Even more preferably, the almost crystalline silicon contains finer crystals, which would comprise no more than 5% of the total volume.

Однако использованный здесь термин «геометрически упорядоченный поликристаллический кремний» (далее сокращаемый до «геометрический поликристаллический кремний») относится к кристаллическому кремнию согласно вариантам настоящего изобретения с геометрически упорядоченным распределением зерен по размерам в сантиметровом диапазоне, при котором бóльшая часть упорядоченных кристаллов находится в массиве кремния. Например, в геометрическом поликристаллическом кремнии каждое зерно обычно имеет среднюю величину поперечного сечения примерно 0.25-2500 см2 и такую высоту, как высота массива кремния, например высота может быть равна размеру массива кремния, перпендикулярному плоскости поперечного сечения, причем ориентация зерна в массиве геометрически упорядоченного поликристаллического кремния регулируется предварительно заданными ориентациями. Форма поперечного сечения зерна, которое перпендикулярно высоте или длине зерна в геометрическом поликристаллическом кремнии, обычно бывает такой же, как форма затравочного кристалла или части затравочного кристалла, на котором оно образовалось. Предпочтительно, чтобы форма поперечного сечения зерна была полигональной. Предпочтительно, чтобы углы полигональных зерен соответствовали сочленению трех разных зерен. Хотя предпочтительно, чтобы каждое зерно в массиве геометрически упорядоченного поликристаллического кремния содержало сплошной кристалл одной ориентации по зерну, одно или несколько зерен могут также содержать небольшое количество кристаллов кремния разной ориентации. Например, каждое такое зерно может частично или полностью содержать более мелкие кристаллы кремния с другими ориентациями, причем такие более мелкие кристаллы составляют не более 25% общего объема зерна, предпочтительно не более 10% общего объема зерна, предпочтительнее не более 5% общего объема зерна, еще предпочтительнее не более 1% общего объема зерна и еще предпочтительнее не более 0.1% общего объема зерна.However, the term “geometrically ordered polycrystalline silicon” (hereinafter abbreviated to “geometrical polycrystalline silicon”) as used herein refers to crystalline silicon according to embodiments of the present invention with a geometrically ordered grain size distribution in the centimeter range in which most of the ordered crystals are in a silicon array. For example, in geometric polycrystalline silicon, each grain usually has an average cross-sectional value of about 0.25-2500 cm 2 and such a height as the height of the silicon array, for example, the height can be equal to the size of the silicon array perpendicular to the plane of the cross section, and the grain orientation in the array is geometrically ordered polycrystalline silicon is regulated by predefined orientations. The cross-sectional shape of the grain, which is perpendicular to the height or length of the grain in geometric polycrystalline silicon, is usually the same as the shape of the seed crystal or part of the seed crystal on which it was formed. Preferably, the cross-sectional shape of the grain is polygonal. Preferably, the angles of the polygonal grains correspond to the articulation of three different grains. Although it is preferred that each grain in an array of geometrically ordered polycrystalline silicon contain a continuous crystal of the same grain orientation, one or more grains may also contain a small number of silicon crystals of different orientations. For example, each such grain may partially or completely contain smaller silicon crystals with different orientations, and such smaller crystals make up no more than 25% of the total grain volume, preferably not more than 10% of the total grain volume, more preferably not more than 5% of the total grain volume, even more preferably not more than 1% of the total grain volume and even more preferably not more than 0.1% of the total grain volume.

Согласно данному реализованному и подробно описанному изобретению предложен способ получения литого кремния, включающий: приведение расплавленного кремния в контакт по меньшей мере с одним затравочным кристаллом кремния в сосуде с одной или несколькими боковыми стенками, нагретыми по меньшей мере до температуры плавления кремния, и по меньшей мере с одной охлаждаемой стенкой, и формирование твердого массива монокристаллического кремния, необязательно имеющего по меньшей мере два измерения по меньшей мере по 10 см каждое, путем охлаждения расплавленного кремния при контроле кристаллизации, причем формирование включает образование границы раздела твердой фазы и жидкости на ребре расплавленного кремния, которое по меньшей мере сначала параллельно по меньшей мере одной охлаждаемой стенке, и границу раздела регулируют во время охлаждения таким образом, чтобы она перемещалась в направлении, при котором увеличивается расстояние между расплавленным кремнием и по меньшей мере одной охлаждаемой стенкой. Предполагается, что одна из стенок тигля может быть дном тигля.According to this realized and described invention, a method for producing cast silicon is provided, comprising: bringing molten silicon into contact with at least one seed silicon crystal in a vessel with one or more side walls heated at least to the melting temperature of silicon, and at least with one cooled wall, and the formation of a solid array of single-crystal silicon, optionally having at least two dimensions of at least 10 cm each, by cooling molten silicon during crystallization control, the formation including the formation of the interface between the solid phase and the liquid on the edge of the molten silicon, which is at least initially parallel to at least one cooled wall, and the interface is adjusted during cooling so that it moves in the direction at which the distance between the molten silicon and at least one cooled wall increases. It is assumed that one of the walls of the crucible may be the bottom of the crucible.

Согласно одному варианту настоящего изобретения предложен способ получения литого кремния, включающий: помещение геометрически упорядоченного множества затравочных кристаллов монокристаллического кремния по меньшей мере на одну поверхность тигля с одной или несколькими боковыми стенками, нагретыми по меньшей мере до температуры плавления кремния, и по меньшей мере одной охлаждаемой стенкой, причем геометрически упорядоченное расположение включает плотноупакованные многогранники; приведение расплавленного кремния в контакт с геометрически упорядоченным расположением затравочных кристаллов монокристаллического кремния и формирование твердого массива монокристаллического кремния, необязательно имеющего по меньшей мере два измерения по меньшей мере по 10 см каждое, путем охлаждения расплавленного кремния при контроле кристаллизации, причем формирование включает образование границы раздела твердой фазы и жидкости по ребру расплавленного кремния, параллельному по меньшей мере одной охлаждаемой стенке, и границу раздела регулируют во время охлаждения таким образом, чтобы она перемещалась в направлении, при котором увеличивается расстояние между расплавленным кремнием и по меньшей мере одной охлаждаемой стенкой.According to one embodiment of the present invention, there is provided a method for producing cast silicon, comprising: placing a geometrically ordered set of single crystals of single crystal silicon on at least one crucible surface with one or more side walls heated to at least the melting temperature of silicon and at least one cooled a wall, and a geometrically ordered arrangement includes close-packed polyhedra; bringing molten silicon into contact with a geometrically ordered arrangement of single crystal silicon seed crystals and forming a solid array of single crystal silicon, optionally having at least two dimensions of at least 10 cm each, by cooling the molten silicon while controlling crystallization, the formation comprising forming a solid interface phase and liquid along the edge of molten silicon parallel to at least one cooled wall, and faces in section is adjusted during the cooling process so that it is moved in a direction in which the distance increases between the molten silicon and at least one cooled wall.

Согласно другому варианту настоящего изобретения предложен способ получения литого кремния, включающий: размещение множества затравочных кристаллов монокристаллического кремния предварительно заданным образом по меньшей мере на двух поверхностях тигля; приведение расплавленного кремния в контакт с затравочными кристаллами монокристаллического кремния и формирование твердого массива монокристаллического кремния, необязательно имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния по меньшей мере на двух поверхностях тигля при регулировании кристаллизации, причем формирование включает регулирование границы раздела твердой фазы и жидкости по ребру расплавленного кремния во время охлаждения таким образом, чтобы она перемещалась в том направлении, в котором увеличивается расстояние между расплавленным кремнием и по меньшей мере двумя поверхностями тигля.According to another embodiment of the present invention, there is provided a method for producing cast silicon, comprising: placing a plurality of single crystal silicon seed crystals in a predetermined manner on at least two crucible surfaces; bringing molten silicon into contact with seed crystals of single crystal silicon and forming a solid array of single crystal silicon, optionally having at least two dimensions, each of at least about 10 cm, by cooling the molten silicon on at least two surfaces of the crucible while controlling crystallization, the formation includes adjusting the interface between the solid phase and the liquid along the edge of the molten silicon during cooling so that it forcibly relocated in the direction in which the distance increases between the molten silicon and at least two surfaces of the crucible.

Согласно еще одному варианту настоящего изобретения предлагается способ получения литого кремния, включающий: приведение источника кремния в контакт по меньшей мере с одним затравочным кристаллом монокристаллического кремния по меньшей мере на одной поверхности; нагревание источника кремния и по меньшей мере одного затравочного кристалла монокристаллического кремния до температуры плавления кремния; регулировку нагревания таким образом, чтобы по меньшей мере один затравочный кристалл монокристаллического кремния не расплавился полностью, причем регулировка включает поддержание ΔТ на уровне примерно 0.1°С/мин или менее при измерении на внешней поверхности тигля после достижения температуры плавления кремния во всем тигле, и формирование твердого массива монокристаллического кремния путем охлаждения кремния, как только частично расплавится по меньшей мере один затравочный кристалл монокристаллического кремния.According to another embodiment of the present invention, there is provided a method for producing cast silicon, comprising: contacting a silicon source with at least one seed crystal of single crystal silicon on at least one surface; heating the source of silicon and at least one seed crystal of single crystal silicon to a melting point of silicon; adjusting the heating so that at least one seed crystal of monocrystalline silicon does not completely melt, the adjustment includes maintaining ΔT at a level of about 0.1 ° C / min or less when measured on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible, and forming solid array of single-crystal silicon by cooling silicon, as soon as at least one seed crystal of single-crystal silicon is partially melted.

Согласно еще одному варианту настоящего изобретения предлагается способ получения литого кремния, включающий: размещение геометрически упорядоченного множества затравочных кристаллов монокристаллического кремния по меньшей мере на одной поверхности в тигле, причем геометрически упорядоченное расположение включает плотноупакованные многогранники; приведение источника кремния в контакт с множеством затравочных кристаллов монокристаллического кремния по меньшей мере на одной поверхности; нагревание источника кремния и множества затравочных кристаллов монокристаллического кремния до температуры плавления кремния; регулировку нагревания таким образом, чтобы множество затравочных кристаллов не расплавилось полностью, путем поддержания ΔТ на уровне примерно 0.1°С/мин или менее при измерении на внешней поверхности тигля после достижения температуры плавления кремния во всем тигле, и, как только по меньшей мере один затравочный кристалл монокристаллического кремния частично расплавится, формирование твердого массива монокристаллического кремния путем охлаждения кремния.According to yet another embodiment of the present invention, there is provided a method for producing cast silicon, comprising: placing a geometrically ordered plurality of seed crystals of single crystal silicon on at least one surface in a crucible, the geometrically ordered arrangement comprising close-packed polyhedra; bringing the source of silicon into contact with a plurality of seed crystals of single crystal silicon on at least one surface; heating the source of silicon and many seed crystals of single crystal silicon to a melting point of silicon; adjusting the heating so that the plurality of seed crystals does not completely melt by maintaining ΔT at about 0.1 ° C / min or less when measured on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible, and as soon as at least one seed single-crystal silicon crystal is partially melted, the formation of a solid array of single-crystal silicon by cooling silicon.

Согласно следующему варианту настоящего изобретения предлагается также способ получения литого кремния, включающий: размещение множества затравочных кристаллов монокристаллического кремния предварительно заданным образом по меньшей мере на двух поверхностях тигля; приведение расплавленного кремния в контакт с множеством затравочных кристаллов монокристаллического кремния по меньшей мере на двух поверхностях; нагревание источника кремния и множества затравочных кристаллов монокристаллического кремния до температуры плавления кремния; регулировку нагревания таким образом, чтобы множество затравочных кристаллов не расплавилось полностью путем поддержания ΔТ на уровне примерно 0.1°С/мин или менее при измерении на внешней поверхности тигля после достижения температуры плавления кремния во всем тигле, и формирование твердого массива монокристаллического кремния путем охлаждения кремния, как только частично расплавится по меньшей мере один затравочный кристалл монокристаллического кремния.According to a further embodiment of the present invention, there is also provided a method for producing cast silicon, comprising: placing a plurality of single crystal silicon seed crystals in a predetermined manner on at least two crucible surfaces; bringing molten silicon into contact with a plurality of single crystal silicon seed crystals on at least two surfaces; heating the source of silicon and many seed crystals of single crystal silicon to a melting point of silicon; adjusting the heating so that the plurality of seed crystals does not completely melt by maintaining ΔT at about 0.1 ° C / min or less when measured on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible, and forming a solid array of single-crystal silicon by cooling silicon, as soon as at least one seed crystal of single-crystal silicon is partially melted.

Согласно еще одному варианту настоящего изобретения предлагается способ получения литого кремния, включающий: приведение расплавленного кремния в контакт по меньшей мере с одним затравочным кристаллом кремния в сосуде с одной или несколькими боковыми стенками, нагретыми по меньшей мере до температуры плавления кремния, причем по меньшей мере один затравочный кристалл кремния расположен так, что он покрывает всю или практически всю поверхность сосуда, и формирование твердого массива монокристаллического кремния, необязательно имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния при регулировании кристаллизации.According to another embodiment of the present invention, there is provided a method for producing cast silicon, comprising: bringing molten silicon into contact with at least one seed silicon crystal in a vessel with one or more side walls heated at least to the silicon melting temperature, at least one the silicon seed crystal is positioned so that it covers all or almost the entire surface of the vessel, and the formation of a solid array of single-crystal silicon, optionally having at least two measurements, each of at least about 10 cm each, by cooling molten silicon while controlling crystallization.

Согласно варианту настоящего изобретения предлагается массив сплошного монокристаллического кремния, не содержащий или практически не содержащий радиально распределенных примесей и дефектов и имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение величиной по меньшей мере примерно 20 см.According to an embodiment of the present invention, there is provided an array of solid monocrystalline silicon, free of or substantially free of radially distributed impurities and defects, and having at least two dimensions, each of at least about 25 cm, and a third measurement of at least about 20 cm.

Согласно еще одному варианту настоящего изобретения предлагается массив сплошного монокристаллического кремния с концентрацией углерода примерно от 2×1016 атомов/см3 до примерно 5×1017 атомов/см3, концентрацией кислорода, не превышающей 5×1017 атомов/см3, концентрацией азота по меньшей мере 1×1015 атомов/см3 и имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см.According to another embodiment of the present invention, there is provided an array of solid single-crystal silicon with a carbon concentration of from about 2 × 10 16 atoms / cm 3 to about 5 × 10 17 atoms / cm 3 , an oxygen concentration not exceeding 5 × 10 17 atoms / cm 3 , concentration nitrogen of at least 1 × 10 15 atoms / cm 3 and having at least two dimensions, each of at least about 25 cm, and a third dimension of at least about 20 cm

Согласно еще одному варианту настоящего изобретения предлагается массив сплошного литого монокристаллического кремния по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 35 см.According to yet another embodiment of the present invention, there is provided an array of solid cast single crystal silicon with at least two dimensions, each of at least about 35 cm.

Согласно другому варианту настоящего изобретения предлагается солнечная батарея, включающая: пластину из массива сплошного монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных примесей и дефектов, причем массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см; р-n переход в пластине; необязательно противоотражательное покрытие на поверхности пластины; необязательно по меньшей мере один слой, выбранный из тыльной области, и пассивирующий слой; и электропроводящие контакты на пластине.According to another embodiment of the present invention, there is provided a solar battery comprising: a wafer made of a solid single-crystal silicon array containing no or practically no radially distributed impurities and defects, the array having at least two dimensions, each of at least about 25 cm, and a third measuring at least about 20 cm; pn junction in the plate; optional anti-reflection coating on the surface of the plate; optionally at least one layer selected from the back region and a passivation layer; and conductive contacts on the plate.

Согласно другому варианту настоящего изобретения предлагается солнечная батарея, содержащая: пластину из массива сплошного литого монокристаллического кремния, причем массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 35 см; р-n переход в пластине; необязательно противоотражательное покрытие на поверхности пластины; необязательно по меньшей мере один слой, выбранный из тыльной области, и пассивирующий слой; и электропроводящие контакты на пластине.According to another embodiment of the present invention, there is provided a solar cell comprising: a solid cast single crystal silicon array plate, the array having at least two dimensions, at least about 35 cm each; pn junction in the plate; optional anti-reflection coating on the surface of the plate; optionally at least one layer selected from the back region and a passivation layer; and conductive contacts on the plate.

Согласно другому варианту настоящего изобретения предлагается также солнечная батарея, содержащая: пластину из сплошного литого монокристаллического кремния, изготовленную из массива сплошного литого монокристаллического кремния, причем пластина имеет по меньшей мере одно измерение примерно 50 мм, а массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см; р-n переход в пластине; необязательно противоотражательное покрытие на поверхности пластины; необязательно по меньшей мере один слой, выбранный из тыльной области, и пассивирующий слой; и электропроводящие контакты на пластине.According to another embodiment of the present invention, there is also provided a solar battery comprising: a solid cast single crystal silicon wafer made of a solid cast single crystal silicon array, the wafer having at least one dimension of about 50 mm, and the array has at least two dimensions, each at least about 25 cm, and a third measurement of at least about 20 cm; pn junction in the plate; optional anti-reflection coating on the surface of the plate; optionally at least one layer selected from the back region and a passivation layer; and conductive contacts on the plate.

Согласно другому варианту настоящего изобретения предлагается пластина, содержащая: кремний из массива сплошного литого монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных примесей и дефектов, причем массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см.According to another embodiment of the present invention, there is provided a wafer comprising: silicon from a solid cast monocrystalline silicon array containing no or practically no radially distributed impurities and defects, the array having at least two dimensions, each of at least about 25 cm, and a third measurement of at least about 20 cm.

Согласно другому варианту настоящего изобретения предлагается пластина, содержащая: кремний из массива сплошного литого монокристаллического кремния, причем пластина имеет по меньшей мере одно измерение по меньшей мере примерно 50 мм и массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см.According to another embodiment of the present invention, there is provided a wafer comprising: silicon from a solid cast single crystal silicon array, the wafer having at least one dimension of at least about 50 mm and the array has at least two dimensions, each of at least about 25 cm, and a third dimension of at least about 20 cm.

Согласно другому варианту настоящего изобретения предлагается способ получения литого кремния, включающий: приведение расплавленного кремния в контакт по меньшей мере с одним затравочным кристаллом кремния в сосуде с одной или несколькими боковыми стенками, нагретыми по меньшей мере до температуры плавления кремния, и по меньшей мере одной охлаждаемой стенкой и формирование твердого массива почти кристаллического кремния, необязательно имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния при контроле кристаллизации, причем формирование включает образование границы раздела твердой фазы и жидкости по ребру расплавленного кремния, которая по меньшей мере сначала параллельна по меньшей мере одной охлаждаемой стенке, причем граница раздела регулируется во время охлаждения таким образом, чтобы она перемещалась в направлении, при котором увеличивается расстояние между расплавленным кремнием и по меньшей мере одной охлаждаемой стенкой.According to another embodiment of the present invention, there is provided a method for producing cast silicon, comprising: bringing molten silicon into contact with at least one seed silicon crystal in a vessel with one or more side walls heated to at least the melting temperature of silicon, and at least one cooled wall and the formation of a solid array of almost crystalline silicon, optionally having at least two dimensions, each of at least about 10 cm, by cooling p molten silicon in a crystallization control, the formation comprising forming an interface between a solid phase and a liquid along an edge of molten silicon, which is at least parallel to at least one wall being cooled, and the interface being adjusted during cooling so that it moves in the direction at which the distance between the molten silicon and at least one cooled wall increases.

Согласно другому варианту настоящего изобретения предлагается способ получения литого кремния, включающий: приведение расплавленного кремния в контакт по меньшей мере с одним затравочным кристаллом в сосуде с одной или несколькими боковыми стенками, нагретыми по меньшей мере до температуры плавления кремния, причем по меньшей мере один затравочный кристалл кремния расположен так, что покрывает всю или практически всю поверхность сосуда, и формирование твердого массива почти монокристаллического кремния, необязательно имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния при регулировке кристаллизации.According to another embodiment of the present invention, there is provided a method for producing cast silicon, comprising: bringing molten silicon into contact with at least one seed crystal in a vessel with one or more side walls heated to at least the melting temperature of silicon, and at least one seed crystal silicon is located so that covers the entire or almost the entire surface of the vessel, and the formation of a solid array of almost single-crystal silicon, optionally having at least two measurements, each of at least about 10 cm, by cooling molten silicon while adjusting crystallization.

Согласно другому варианту настоящего изобретения предлагается массив почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных примесей и дефектов и имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см.According to another embodiment of the present invention, there is provided an array of almost monocrystalline silicon, containing no or practically no radially distributed impurities and defects, and having at least two dimensions, each of at least about 25 cm, and a third measurement of at least about 20 cm.

Согласно другому варианту настоящего изобретения предлагается массив почти монокристаллического кремния с концентрацией углерода примерно от 2×1016 атомов/см3 до примерно 5×1017 атомов/см3, концентрацией кислорода, не превышающей 5×1017 атомов/см3, концентрацией азота по меньшей мере 1×1015 атомов/см3, имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см.According to another embodiment of the present invention, there is provided an array of almost monocrystalline silicon with a carbon concentration of from about 2 × 10 16 atoms / cm 3 to about 5 × 10 17 atoms / cm 3 , an oxygen concentration not exceeding 5 × 10 17 atoms / cm 3 , and a nitrogen concentration at least 1 × 10 15 atoms / cm 3 having at least two dimensions, each of at least about 25 cm, and a third measurement of at least about 20 cm

Согласно другому варианту настоящего изобретения предлагается также массив литого почти монокристаллического кремния по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 35 см.According to another embodiment of the present invention, there is also provided an array of cast almost single crystal silicon with at least two dimensions, each of at least about 35 cm.

Согласно другому варианту настоящего изобретения предлагается также солнечная батарея, включающая: пластину из массива почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных примесей и дефектов, причем массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см; р-n переход в пластине; необязательно противоотражательное покрытие на поверхности пластины; необязательно по меньшей мере один слой, выбранный из тыльной области, и пассивирующий слой; и электропроводящие контакты на пластине.According to another embodiment of the present invention, there is also provided a solar battery, comprising: a plate of an array of almost single-crystal silicon containing no or practically no radially distributed impurities and defects, the array having at least two dimensions, each of at least about 25 cm, and a third measurement of at least about 20 cm; pn junction in the plate; optional anti-reflection coating on the surface of the plate; optionally at least one layer selected from the back region and a passivation layer; and conductive contacts on the plate.

Согласно другому варианту настоящего изобретения предлагается также солнечная батарея, включающая: пластину из массива литого почти монокристаллического кремния, причем массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 35 см; р-n переход в пластине; необязательно противоотражательное покрытие на поверхности пластины; необязательно по меньшей мере один слой, выбранный из тыльной области, и пассивирующий слой; и электропроводящие контакты на пластине.According to another embodiment of the present invention, there is also provided a solar battery comprising: a wafer made of an array of cast almost monocrystalline silicon, the array having at least two dimensions, each of at least about 35 cm; pn junction in the plate; optional anti-reflection coating on the surface of the plate; optionally at least one layer selected from the back region and a passivation layer; and conductive contacts on the plate.

Согласно другому варианту настоящего изобретения предлагается пластина, содержащая: кремний, состоящий из массива почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных примесей и дефектов, причем массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см.According to another embodiment of the present invention, there is provided a wafer comprising: silicon, consisting of an array of almost monocrystalline silicon, containing no or practically no radially distributed impurities and defects, the array having at least two dimensions, each of at least about 25 cm, and a third measurement of at least about 20 cm.

Согласно другому варианту настоящего изобретения также предлагается пластина, содержащая: кремний, состоящий из массива литого почти монокристаллического кремния, причем пластина имеет по меньшей мере одно измерение по меньшей мере примерно 50 мм и массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см.According to another embodiment of the present invention, there is also provided a wafer comprising: silicon, consisting of an array of cast almost monocrystalline silicon, the wafer having at least one dimension of at least about 50 mm and the array has at least two dimensions, each of at least about 25 cm, and a third dimension of at least about 20 cm.

Согласно еще одному варианту настоящего изобретения предлагается также солнечная батарея, включающая: пластину, вырезанную из массива сплошного монокристаллического кремния, практически не содержащего радиально распределенных дефектов, причем массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см; р-n переход в пластине; необязательно противоотражательное покрытие на поверхности пластины; необязательно по меньшей мере один слой, выбранный из тыльной области, и пассивирующий слой; и электропроводящие контакты на пластине.According to another embodiment of the present invention, there is also provided a solar battery, comprising: a plate cut from a solid monocrystalline silicon array substantially free of radially distributed defects, the array having at least two dimensions, each of at least about 25 cm, and a third dimension at least about 20 cm; pn junction in the plate; optional anti-reflection coating on the surface of the plate; optionally at least one layer selected from the back region and a passivation layer; and conductive contacts on the plate.

Согласно еще одному варианту настоящего изобретения предлагается также солнечная батарея, включающая: пластину, вырезанную из массива сплошного литого монокристаллического кремния, практически не содержащего радиально распределенных дефектов, причем массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 35 см; р-n переход в пластине; необязательно противоотражательное покрытие на поверхности пластины; необязательный тыльный слой; один или несколько необязательных пассивирующих слоев и множество электропроводящих контактов по меньшей мере на одной поверхности пластины.According to another embodiment of the present invention, there is also provided a solar battery comprising: a plate cut from a solid cast single crystal silicon array substantially free of radially distributed defects, the array having at least two dimensions, each of at least about 35 cm; pn junction in the plate; optional anti-reflection coating on the surface of the plate; optional back layer; one or more optional passivating layers and a plurality of electrically conductive contacts on at least one surface of the plate.

Согласно еще одному варианту настоящего изобретения предлагается также солнечная батарея, включающая: пластину из сплошного монокристаллического кремния, вырезанную из массива сплошного монокристаллического кремния и практически не содержащую радиально распределенных дефектов, причем пластина имеет по меньшей мере одно измерение по меньшей мере примерно 40 мм и массив имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см; р-n переход в пластине; необязательно противоотражательное покрытие на поверхности пластины; необязательный тыльный слой, один или несколько необязательных пассивирующих слоев и множество электропроводящих контактов по меньшей мере на одной поверхности пластины.According to another embodiment of the present invention, there is also provided a solar battery comprising: a solid single crystal silicon wafer cut from a solid single crystal silicon wafer and substantially free of radially distributed defects, the wafer having at least one dimension of at least about 40 mm and the array has at least two measurements, each of at least about 25 cm, and a third measurement of at least about 20 cm; pn junction in the plate; optional anti-reflection coating on the surface of the plate; an optional back layer, one or more optional passivating layers and a plurality of electrically conductive contacts on at least one surface of the plate.

Согласно еще одному варианту настоящего изобретения почти монокристаллический кремний, полученный согласно изобретению, может содержать до 5 об.% более мелких кристаллов кремния с другими ориентациями кристаллов. Согласно другому варианту настоящего изобретения предпочтительно, чтобы почти монокристаллический кремний, полученный согласно изобретению, содержал до 1 об.% более мелких кристаллов кремния с другими ориентациями кристаллов. Еще более предпочтительно согласно другому варианту настоящего изобретения, чтобы почти монокристаллический кремний, полученный согласно изобретению, содержал до 0.1 об.% более мелких кристаллов кремния с другими ориентациями кристаллов.According to yet another embodiment of the present invention, the nearly monocrystalline silicon obtained according to the invention may contain up to 5 vol.% Smaller silicon crystals with different crystal orientations. According to another embodiment of the present invention, it is preferable that the almost monocrystalline silicon obtained according to the invention contains up to 1 vol.% Smaller silicon crystals with different crystal orientations. Even more preferably, according to another embodiment of the present invention, the nearly monocrystalline silicon obtained according to the invention contains up to 0.1 vol.% Smaller silicon crystals with different crystal orientations.

Дополнительные особенности и преимущества изобретения можно будет найти в последующем описании, и они будут очевидны из описания или будут проверены на практике вариантов изобретения. Особенности и другие преимущества изобретения можно будет осмыслить и осуществить в структурах полупроводниковых устройств, способах и производственной аппаратуре, которые особенно акцентировались в приведенном описании и формуле, а также приложенных чертежах.Additional features and advantages of the invention will be found in the following description, and they will be apparent from the description or will be tested in practice variants of the invention. Features and other advantages of the invention can be comprehended and implemented in the structures of semiconductor devices, methods and industrial equipment, which are especially emphasized in the above description and formula, as well as the attached drawings.

Следует понимать, что как приведенное выше общее описание, так и последующее подробное описание служат примерами для разъяснения заявленного изобретения. Это изобретение также включает кремний, полученный способами, описанными и заявленными здесь, а также пластину и солнечные батареи, изготовленные из такого кремния.It should be understood that both the foregoing general description and the following detailed description are examples to clarify the claimed invention. This invention also includes silicon obtained by the methods described and claimed herein, as well as wafers and solar cells made from such silicon.

КРАТКОЕ ОПИСАНИЕ ЧЕРТЕЖЕЙBRIEF DESCRIPTION OF THE DRAWINGS

В сопровождающих чертежах, которые вставлены как часть данного описания, проиллюстрированы варианты изобретения, и вместе с описанием они служат для разъяснения особенностей, преимуществ и принципов изобретения. На чертежах:The accompanying drawings, which are inserted as part of this specification, illustrate embodiments of the invention and, together with the description, serve to explain the features, advantages, and principles of the invention. In the drawings:

на фиг.1 приведен пример расположения затравок кремния на дне тигля согласно варианту настоящего изобретения;figure 1 shows an example of the location of the seeds of silicon at the bottom of the crucible according to a variant of the present invention;

на фиг.2 проиллюстрирован другой пример расположения затравок кремния на дне и боковых поверхностях тигля согласно варианту настоящего изобретения;figure 2 illustrates another example of the location of the silicon seeds on the bottom and side surfaces of the crucible according to a variant of the present invention;

на фиг.3А-С показан пример расположения в тигле для отливки геометрически упорядоченного поликристаллического кремния согласно варианту настоящего изобретения;on figa-C shows an example of the location in the crucible for casting geometrically ordered polycrystalline silicon according to a variant of the present invention;

на фиг.4 приведен другой пример расположения в тигле для отливки геометрически упорядоченного поликристаллического кремния согласно варианту настоящего изобретения;figure 4 shows another example of the location in the crucible for casting geometrically ordered polycrystalline silicon according to a variant of the present invention;

на фиг.5 проведен пример плотноупакованного ряда гексагональных кристаллов согласно варианту настоящего изобретения;figure 5 shows an example of a close-packed row of hexagonal crystals according to a variant of the present invention;

на фиг.6 приведен пример расположения ряда многогранников с ромбоидальными или треугольными пустотами согласно варианту настоящего изобретения;figure 6 shows an example of the location of a number of polyhedra with rhomboid or triangular voids according to a variant of the present invention;

на фиг.7 показан пример способа по варианту настоящего изобретения, и7 shows an example of a method according to a variant of the present invention, and

на фиг.8A-G и 9 приведены примеры способов литья монокристаллического или геометрически упорядоченного поликристаллического кремния согласно вариантам настоящего изобретения.8A-G and 9 show examples of methods for casting single-crystal or geometrically ordered polycrystalline silicon according to embodiments of the present invention.

ОПИСАНИЕ ВАРИАНТОВ DESCRIPTION OF OPTIONS

Теперь подробно рассмотрим варианты настоящего изобретения, примеры которых проиллюстрированы сопровождающими чертежами. По возможности на всех чертежах будут использованы одни и те же или близкие номера ссылок, относящиеся к одним и тем же или похожим частям.Now we consider in detail variants of the present invention, examples of which are illustrated in the accompanying drawings. If possible, the same or similar reference numbers relating to the same or similar parts will be used throughout the drawings.

В вариантах, соответствующих данному изобретению, кристаллизацию расплавленного кремния проводят способами литья с использованием одного или нескольких затравочных кристаллов. Показано, что такие способы литья позволяют регулировать размер, форму и ориентацию зерен кристаллов в литом массиве кристаллизующегося кремния. Использованный термин «литой» означает, что кремний получают путем охлаждения расплавленного кремния в форме или сосуде с расплавленным кремнием. Поскольку жидкость, такая как расплавленный кремний, будет принимать форму сосуда, в котором она находится, предполагается, что расплавленный кремний можно также охлаждать при ограничении объема расплавленного кремния любыми способами, а не только формой или сосудом. Например, кремний можно получать путем отверждения в тигле, где отверждение инициируют по меньшей мере на одной стенке тигля, а не путем введения в расплав постороннего предмета. Тигель может иметь любую подходящую форму, такую как чашка, цилиндр или коробка. Таким образом, способ кристаллизации расплавленного кремния согласно настоящему изобретению не регулируется путем «вытягивания» бульки или ленты. Далее, в соответствии с вариантом настоящего изобретения форма, сосуд или тигель содержат по меньшей мере одну поверхность «горячей стенки» в контакте с расплавленным кремнием. Использованный термин «горячая стенка» относится к поверхности, которая имеет ту же или более высокую температуру, что и температура расплавленного кремния, с которым она контактирует. Предпочтительно, чтобы горячая стенка оставалась неподвижной в ходе обработки кремния.In embodiments of the invention, crystallization of molten silicon is carried out by casting methods using one or more seed crystals. It is shown that such casting methods make it possible to control the size, shape, and orientation of crystal grains in a cast mass of crystallizing silicon. The term "cast" as used means that silicon is obtained by cooling molten silicon in a mold or vessel with molten silicon. Since a liquid, such as molten silicon, will take the form of the vessel in which it is located, it is assumed that molten silicon can also be cooled by limiting the volume of molten silicon by any means, and not just a shape or vessel. For example, silicon can be obtained by curing in a crucible, where curing is initiated on at least one wall of the crucible, and not by introducing a foreign object into the melt. The crucible may have any suitable shape, such as a cup, cylinder or box. Thus, the crystallization method of molten silicon according to the present invention is not controlled by “pulling” the bead or tape. Further, in accordance with an embodiment of the present invention, the mold, vessel or crucible comprises at least one “hot wall” surface in contact with molten silicon. The term "hot wall" as used refers to a surface that has the same or higher temperature as the temperature of the molten silicon with which it is in contact. Preferably, the hot wall remains stationary during the processing of silicon.

В соответствии с вариантами данного изобретения кристаллизованный кремний может быть либо сплошным монокристаллическим, почти монокристаллическим или сплошным геометрически упорядоченным поликристаллическим с регулируемой ориентацией зерен. Использованный термин «сплошной монокристаллический кремний» относится к монокристаллам кремния, когда массив кремния является массивом однородного монокристаллического кремния, а не более мелкими кусочками кремния, соединенными вместе с образованием более крупного куска кремния. Кроме того, использованный здесь термин «сплошной геометрический поликристаллический кремний» относится к геометрически упорядоченному поликристаллическому кремнию, в котором массив кремния представляет собой один однородный массив геометрически упорядоченного поликристаллического кремния, а не более мелкие кусочки кремния, соединенные вместе с образованием более крупного куска кремния.In accordance with embodiments of the invention, crystallized silicon can be either solid single crystal, nearly single crystal, or solid geometrically ordered polycrystalline with controlled grain orientation. The term “continuous single crystal silicon” as used refers to single crystals of silicon when the silicon array is an array of homogeneous single crystal silicon, and not smaller pieces of silicon connected together to form a larger piece of silicon. In addition, the term “continuous geometric polycrystalline silicon” as used herein refers to geometrically ordered polycrystalline silicon, in which the silicon array is one homogeneous array of geometrically ordered polycrystalline silicon, rather than smaller pieces of silicon joined together to form a larger piece of silicon.

В соответствии с вариантами настоящего изобретения кристаллизацию можно проводить путем помещения нужной комбинации «затравок» кристаллического кремния, например, на дно сосуда, такого как кварцевый тигель, который может вместить расплавленный кремний. Использованный термин «затравка» относится к кусочку кремния предпочтительной геометрической формы и нужной кристаллической структуры, в котором по меньшей мере одно поперечное сечение предпочтительно имеет геометрически правильную, предпочтительно многогранную, форму и предпочтительно имеет сторону, которая соответствует поверхности сосуда, в который его можно поместить. Такая затравка может быть либо куском монокристаллического кремния, либо геометрически упорядоченным поликристаллическим кремнием, например листом или горизонтальным срезом или полученным как-то иначе куском слитка монокристаллического кремния. В соответствии с настоящим изобретением затравка может иметь верхнюю поверхность, параллельную нижней поверхности, хотя это и не обязательно. Например, затравка может быть куском кремния размером примерно 2-3000 мм. Например, затравка может иметь размер 10-300 мм. Кусок кремния может иметь толщину примерно 1-1000 мм, предпочтительно примерно 5-50 мм. Подходящий размер и форма затравки могут быть выбраны в целях удобства и расположения. Расположение, которое будет более подробно описано ниже, включает размещение затравочных кристаллов кремния в предварительно заданной геометрической ориентации или способе по отношению, например, ко дну или к поверхности одной или нескольких боковых сторон и дна тигля. Предпочтительно, чтобы затравка или затравки покрывали всю поверхность тигля, рядом с которой они размещены, с тем чтобы при перемещении фронта отверждения в результате роста затравочного кристалла в сторону от затравок полный размер поперечного сечения тигля оставался в виде кристалла соответствующей геометрии.According to embodiments of the present invention, crystallization can be carried out by placing the desired combination of “seeds” of crystalline silicon, for example, on the bottom of a vessel, such as a quartz crucible, which can accommodate molten silicon. The term “seed” as used refers to a piece of silicon of a preferred geometric shape and desired crystal structure, in which at least one cross section preferably has a geometrically regular, preferably multifaceted, shape and preferably has a side that corresponds to the surface of the vessel into which it can be placed. Such a seed can be either a piece of monocrystalline silicon, or a geometrically ordered polycrystalline silicon, for example, a sheet or a horizontal slice, or otherwise obtained a piece of a single crystal silicon ingot. In accordance with the present invention, the seed may have an upper surface parallel to the lower surface, although this is not necessary. For example, the seed may be a piece of silicon about 2-3,000 mm in size. For example, the seed may have a size of 10-300 mm. A piece of silicon may have a thickness of about 1-1000 mm, preferably about 5-50 mm. The appropriate size and shape of the seed can be selected for convenience and location. The arrangement, which will be described in more detail below, includes the placement of silicon seed crystals in a predetermined geometric orientation or method with respect to, for example, the bottom or surface of one or more sides and bottom of the crucible. It is preferable that the seed or seeds cover the entire surface of the crucible next to which they are placed, so that when the curing front moves as a result of the growth of the seed crystal away from the seeds, the full cross-sectional size of the crucible remains in the form of a crystal of appropriate geometry.

Затем расплавленному кремнию дают остывать и кристаллизоваться в присутствии затравок, предпочтительно таким образом, чтобы при охлаждении расплавленного кремния кристаллизация расплавленного кремния начиналась на уровне или ниже первоначальной вершины твердых затравок и протекала в сторону, предпочтительно вверх от затравок. Сначала граница раздела твердой фазы и жидкости на ребре расплавленного кремния будет соответствовать охлаждаемой поверхности сосуда, например поверхности тигля, в который его заливают. Согласно вариантам данного изобретения границу раздела жидкости и твердой фазы между расплавленным кремнием и закристаллизованным кремнием можно поддерживать практически плоской в течение части стадии, например на начальной части, в стадии отверждения или в течение всего процесса литья. В варианте изобретения границу раздела твердой фазы и жидкости на каждом ребре расплавленного кремния регулируют в ходе охлаждения так, чтобы она перемещалась в направлении, при котором увеличивается расстояние между расплавленным кремнием и охлаждаемой поверхностью тигля, хотя предпочтительно поддерживать границу раздела твердой фазы и жидкости практически плоской.The molten silicon is then allowed to cool and crystallize in the presence of seeds, preferably so that upon cooling of the molten silicon, crystallization of the molten silicon begins at or below the initial peak of the solid seeds and flows to the side, preferably upward from the seeds. First, the interface between the solid phase and the liquid on the edge of the molten silicon will correspond to the cooled surface of the vessel, for example, the surface of the crucible into which it is poured. According to embodiments of the invention, the interface between the liquid and solid phase between the molten silicon and crystallized silicon can be kept substantially flat during part of the stage, for example, at the initial part, in the curing stage or during the entire casting process. In an embodiment of the invention, the interface between the solid phase and the liquid on each edge of the molten silicon is controlled during cooling so that it moves in a direction in which the distance between the molten silicon and the cooled surface of the crucible increases, although it is preferable to keep the interface between the solid phase and the liquid practically flat.

Поэтому в соответствии с настоящим изобретением фронт отверждения может быть параллельным охлаждаемой поверхности сосуда. Например, в тигле с плоским дном фронт отверждения может оставаться практически плоским, а граница раздела твердой фазы и жидкости будет иметь регулируемый профиль. Границу раздела твердой фазы и жидкости можно регулировать таким образом, чтобы радиус ее кривизны уменьшался по мере удаления от края к центру. Альтернативно, границу раздела твердой фазы и жидкости можно регулировать, поддерживая средний радиус кривизны, равный по меньшей мере половине ширины сосуда. Кроме того, твердая фаза может иметь слегка выпуклую границу раздела с радиусом кривизны по меньшей мере примерно в четыре раза больше ширины сосуда. Например, граница раздела твердой фазы и жидкости может иметь радиус кривизны в целом более 2 м в тигле с поверхностью 0.7 м2, он может быть более чем вдвое больше горизонтального размера тигля и предпочтительно примерно в 8-16 раз больше горизонтального размера тигля.Therefore, in accordance with the present invention, the curing front may be parallel to the cooled surface of the vessel. For example, in a crucible with a flat bottom, the curing front can remain almost flat, and the interface between the solid phase and the liquid will have an adjustable profile. The interface between the solid phase and the liquid can be adjusted so that its radius of curvature decreases with distance from the edge to the center. Alternatively, the interface between the solid phase and the liquid can be adjusted to maintain an average radius of curvature equal to at least half the width of the vessel. In addition, the solid phase may have a slightly convex interface with a radius of curvature of at least about four times the width of the vessel. For example, the interface between a solid phase and a liquid can have a radius of curvature of more than 2 m in total in a crucible with a surface of 0.7 m 2 , it can be more than twice the horizontal size of the crucible and preferably about 8-16 times the horizontal size of the crucible.

Согласно вариантам настоящего изобретения можно получить твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, предпочтительно имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 20 см, например сторону по меньшей мере примерно 20 см, и третье измерение по меньшей мере примерно 10 см. Предпочтительно получить твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 30 см, например сторону по меньшей мере примерно 30 см, и третье измерение по меньшей мере примерно 10 см. Более предпочтительно, чтобы полученный твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, имел по меньшей мере два измерения, каждое по меньшей мере примерно по 35 см, например сторону по меньшей мере примерно 35 см, и третье измерение по меньшей мере примерно 10 см. Еще более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, который имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 40 см, например сторону по меньшей мере примерно 40 см, и третье измерение по меньшей мере примерно 20 см. Еще более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, который имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 50 см, например сторону по меньшей мере примерно 50 см, и третье измерение по меньшей мере примерно 20 см. Еще более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, который имеет по меньшей мере два измерения, каждое по меньшей мере примерно по 60 см, например сторону по меньшей мере примерно 60 см, и третье измерение по меньшей мере примерно 20 см. Еще более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, который имеет по меньшей мере два измерения, каждое по меньшей мере примерно 70 см, например сторону по меньшей мере примерно 70 см, и третье измерение по меньшей мере примерно 20 см. Согласно вариантам настоящего изобретения можно получить массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных дефектов и/или примесей, предпочтительно имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 20 см, и третье измерение по меньшей мере примерно 10 см. Предпочтительно получить массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных дефектов и/или примесей, предпочтительно имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 30 см, и третье измерение по меньшей мере примерно 10 см. Более предпочтительно получить массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных дефектов и/или примесей, имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 35 см, и третье измерение по меньшей мере примерно 10 см. Еще более предпочтительно получить массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных дефектов и/или примесей, имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 40 см, и третье измерение по меньшей мере примерно 20 см. Еще более предпочтительно получить массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных дефектов и/или примесей, имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 50 см, и третье измерение по меньшей мере примерно 20 см. Еще более предпочтительно получить массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных дефектов и/или примесей, имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 60 см, и третье измерение по меньшей мере примерно 20 см. Еще более предпочтительно получить массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных дефектов и/или примесей, имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 70 см, и третье измерение по меньшей мере примерно 20 см.According to embodiments of the present invention, it is possible to obtain a solid array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, preferably having at least two dimensions, each of at least about 20 cm, for example a side of at least about 20 cm, and a third measurement of at least about 10 cm. It is preferable to obtain a solid array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, having at least two dimensions, each e at least about 30 cm, for example a side of at least about 30 cm, and a third measurement of at least about 10 cm. More preferably, the resulting solid array of single-crystal silicon or almost single-crystal silicon, preferably cast, has at least two measurements, each of at least about 35 cm, for example a side of at least about 35 cm, and a third measurement of at least about 10 cm. It is even more preferable to obtain a solid array of monocrystalline silicon or mail and monocrystalline silicon, preferably cast, which has at least two dimensions, each of at least about 40 cm, for example a side of at least about 40 cm, and a third measurement of at least about 20 cm. It is even more preferable to obtain a solid array of single crystal silicon or almost single crystal silicon, preferably cast, which has at least two dimensions, each of at least about 50 cm, for example a side of at least about 50 cm, and a third measurement of at least at least about 20 cm. It is even more preferable to obtain a solid array of single crystal silicon or almost single crystal silicon, preferably cast, which has at least two dimensions, each of at least about 60 cm, for example, a side of at least about 60 cm, and a third a measurement of at least about 20 cm. It is even more preferable to obtain a solid array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, which has at least two dimensions, each at least about 70 cm, for example a side of at least about 70 cm, and a third measurement of at least about 20 cm. According to embodiments of the present invention, it is possible to obtain an array of solid single crystal silicon or almost single crystal silicon, with little or no radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 20 cm, and a third measurement of at least about 10 cm. Preferably, массив an array of solid single-crystal silicon or almost single-crystal silicon, which does not contain or practically does not contain radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 30 cm, and the third measurement of at least about 10 cm It is more preferable to obtain an array of solid monocrystalline silicon or almost monocrystalline silicon that does not contain or practically does not contain radially distributed defects and / or of meshes having at least two measurements, each of at least about 35 cm, and a third measurement of at least about 10 cm. It is even more preferable to obtain an array of solid single-crystal silicon or almost single-crystal silicon, with little or no radially distributed defects and / or impurities having at least two dimensions, each of at least about 40 cm, and a third measurement of at least about 20 cm. It is even more preferable to obtain an array of solid mono crystalline silicon or almost monocrystalline silicon, free of or substantially free of radially distributed defects and / or impurities, having at least two dimensions, each of at least about 50 cm, and a third measurement of at least about 20 cm. Even more preferably to obtain an array of solid single-crystal silicon or almost single-crystal silicon, which does not contain or practically does not contain radially distributed defects and / or impurities, having at least two and measurements, each of at least about 60 cm, and a third measurement of at least about 20 cm. It is even more preferable to obtain an array of solid single-crystal silicon or almost single-crystal silicon, which does not contain or practically does not contain radially distributed defects and / or impurities having at least two measurements, each of at least about 70 cm, and a third measurement of at least about 20 cm.

Верхний предел горизонтального размера слитка кремния, полученного согласно вариантам настоящего изобретения, определяется только технологией литья и изготовления тигля, а не самим предлагаемым способом. Согласно данному изобретению можно получить слитки с площадью поперечного сечения по меньшей мере 1 м2 и до 4-8 м2. Аналогично верхний предел высоты слитка может быть связан с более длительными циклами, а не с фундаментальными особенностями способа литья. Возможна высота слитка до примерно 50-80 см. Таким образом, в соответствии с данным изобретением массив сплошного монокристаллического кремния или почти монокристаллического кремния можно с успехом вырастить до размера с поперечным сечением примерно 66 см × 66 см при объеме прямоугольного твердого куска сплошного монокристаллического кремния по меньшей мере 33750 см3. Кроме того, согласно настоящему изобретению предпочтительно получать твердый массив литого сплошного монокристаллического кремния или почти монокристаллического кремния по меньшей мере с двумя измерениями, каждое из которых соответствует внутренним размерам сосуда для литья, и третьим измерением, равным высоте слитка. Например, если литой массив монокристаллического кремния имеет форму куба или прямоугольника, приведенные измерения относятся к длине, ширине и высоте таких массивов.The upper limit of the horizontal size of the silicon ingot obtained according to the variants of the present invention is determined only by the technology of casting and manufacturing the crucible, and not by the proposed method. According to this invention, it is possible to obtain ingots with a cross-sectional area of at least 1 m 2 and up to 4-8 m 2 . Similarly, the upper limit of the height of the ingot may be associated with longer cycles, and not with the fundamental features of the casting method. The ingot height is possible up to about 50-80 cm. Thus, in accordance with this invention, an array of solid single-crystal silicon or almost single-crystal silicon can be successfully grown to a size with a cross section of about 66 cm × 66 cm with a volume of a rectangular solid piece of continuous single-crystal silicon over at least 33,750 cm 3 . In addition, according to the present invention, it is preferable to obtain a solid array of cast solid monocrystalline silicon or almost monocrystalline silicon with at least two dimensions, each of which corresponds to the internal dimensions of the casting vessel, and a third dimension equal to the height of the ingot. For example, if a cast array of single-crystal silicon has the shape of a cube or a rectangle, the measurements given relate to the length, width, and height of such arrays.

Аналогично можно получить твердый массив литого геометрически упорядоченного поликристаллического кремния, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 10 см, и третье измерение по меньшей мере примерно 5 см. Предпочтительно получить твердый массив литого геометрически упорядоченного поликристаллического кремния, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 20 см, и третье измерение по меньшей мере примерно 5 см. Более предпочтительно получить твердый массив литого геометрически упорядоченного поликристаллического кремния, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 30 см, и третье измерение по меньшей мере примерно 5 см. Еще более предпочтительно получить твердый массив литого геометрически упорядоченного поликристаллического кремния, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 35 см, и третье измерение по меньшей мере примерно 5 см. Еще более предпочтительно получить твердый массив литого геометрически упорядоченного поликристаллического кремния, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 40 см, и третье измерение по меньшей мере примерно 5 см. Еще более предпочтительно получить твердый массив литого геометрически упорядоченного поликристаллического кремния, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 50 см, и третье измерение по меньшей мере примерно 5 см. Еще более предпочтительно получить твердый массив литого геометрически упорядоченного поликристаллического кремния, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 60 см, и третье измерение по меньшей мере примерно 5 см. Еще более предпочтительно получить твердый массив литого геометрически упорядоченного поликристаллического кремния, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 70 см, и третье измерение по меньшей мере примерно 5 см. Таким образом, в соответствии с данным изобретением массив сплошного геометрически упорядоченного поликристаллического кремния можно с успехом вырастить до размера с поперечным сечением примерно 66 см × 66 см при объеме прямоугольного твердого куска сплошного геометрически упорядоченного поликристаллического кремния по меньшей мере 33750 см3. Кроме того, согласно настоящему изобретению предпочтительно получить твердый массив литого геометрически упорядоченного поликристаллического кремния по меньшей мере с двумя измерениями, каждое из которых соответствует внутренним размерам сосуда для литья. Например, если литой массив геометрически упорядоченного поликристаллического кремния имеет форму куба или прямоугольника, приведенные измерения относятся к длине, ширине и высоте таких массивов.Similarly, it is possible to obtain a solid array of cast geometrically ordered polycrystalline silicon, preferably having at least two dimensions, each of at least about 10 cm, and a third dimension of at least about 5 cm. It is preferable to obtain a solid array of cast geometrically ordered polycrystalline silicon, preferably having at least two measurements, each of at least about 20 cm, and a third measurement of at least about 5 cm. It is more preferable to obtain a solid an array of cast geometrically ordered polycrystalline silicon, preferably having at least two dimensions, each of at least about 30 cm, and a third dimension of at least about 5 cm. It is even more preferable to obtain a solid array of cast geometrically ordered polycrystalline silicon, preferably having at least two measurements, each of at least about 35 cm, and a third measurement of at least about 5 cm. It is even more preferable to obtain a solid cast mass geometrically ordered polycrystalline silicon, preferably having at least two dimensions, each of at least about 40 cm, and a third dimension of at least about 5 cm. It is even more preferable to obtain a solid array of cast geometrically ordered polycrystalline silicon, preferably having at least two measurements, each of at least about 50 cm, and a third measurement of at least about 5 cm. It is even more preferable to obtain a solid array of geometrically molded cast polycrystalline silicon, preferably having at least two dimensions, each of at least 60 cm, and a third dimension of at least 5 cm. It is even more preferable to obtain a solid array of cast geometrically ordered polycrystalline silicon, preferably having at least two dimensions each of at least about 70 cm, and a third measurement of at least about 5 cm. Thus, in accordance with this invention, an array of solid geometrically ordered ennogo polycrystalline silicon can be successfully grow to a size of a cross section of about 66 cm × 66 cm for a volume of a rectangular solid continuous piece of geometrically ordered polycrystalline silicon at least 33750 cm 3. In addition, according to the present invention, it is preferable to obtain a solid array of cast geometrically ordered polycrystalline silicon with at least two dimensions, each of which corresponds to the internal dimensions of the casting vessel. For example, if a cast array of geometrically ordered polycrystalline silicon has the shape of a cube or rectangle, the measurements given relate to the length, width and height of such arrays.

Путем проведения кристаллизации расплавленного кремния по способам данного изобретения можно получить литой кремний с определенными, а не беспорядочными границами зерен и определенными размерами зерен. Кроме того, путем выстраивания затравок таким образом, что все они ориентированы одинаково относительно друг друга, например так, чтобы направление оси (100) было перпендикулярно дну тигля, а направление (110) было параллельно одной из сторон тигля с прямоугольным или квадратным поперечным сечением, можно получить большие массивы литого кремния, который представляет собой полностью или почти полностью монокристаллический кремний, в котором направление оси такое же, как у затравок. Аналогично другие направления осей могут быть перпендикулярными дну тигля. Кроме того, в соответствии с вариантом изобретения затравки можно разместить таким образом, чтобы любое общее направление осей было перпендикулярно дну тигля.By crystallizing molten silicon according to the methods of the present invention, cast silicon can be produced with defined, rather than random, grain boundaries and defined grain sizes. In addition, by arranging the seeds in such a way that they are all oriented the same relative to each other, for example, so that the direction of the axis (100) is perpendicular to the bottom of the crucible, and the direction (110) is parallel to one of the sides of the crucible with a rectangular or square cross section, You can get large arrays of cast silicon, which is a fully or almost completely single-crystal silicon, in which the direction of the axis is the same as that of the seeds. Similarly, other directions of the axes may be perpendicular to the bottom of the crucible. Furthermore, according to an embodiment of the invention, the seeds can be arranged so that any general axis direction is perpendicular to the bottom of the crucible.

В случае когда монокристаллический кремний получают традиционным способом вытягивания цилиндрической отливки из резервуара с расплавленным кремнием, например способами CZ или FZ, полученный монокристаллический кремний содержит радиально распределенные примеси и дефекты, такие как спиральные (образованные из собственных дефектов, таких как вакансии и междоузельные атомы) и OSF кольцевые дефекты. Спиральные дефекты представляют собой междоузельные атомы кремния или вакансии либо в изолированной, либо в кластерной форме. Такие спиральные дефекты можно определить методами рентгеновской топографии как «спирали» в кремнии. Их также можно определить после избирательного кислотного травления кремния для визуализации дефектов.In the case where monocrystalline silicon is obtained by the traditional method of drawing a cylindrical casting from a reservoir with molten silicon, for example, by CZ or FZ methods, the obtained monocrystalline silicon contains radially distributed impurities and defects, such as helical ones (formed from intrinsic defects such as vacancies and interstitial atoms) and OSF ring defects. Spiral defects are interstitial silicon atoms or vacancies in either isolated or cluster form. Such spiral defects can be determined by X-ray topography as “spirals” in silicon. They can also be determined after selective acid etching of silicon to visualize defects.

Согласно традиционным способам CZ или FZ распределение атомов кислорода в кремнии и дефектов, обусловленных этими атомами кислорода, является радиальным. Это означает, что они имеют тенденцию образовывать кольца, спирали или наплывы, симметричные относительно центральной оси. Дефекты в виде колец OSF являются конкретными примерами, в которых нанометровые атомы кислорода вызывают дефекты упаковки в цилиндрической полосе в слитке монокристаллического кремния, полученного вытягиванием, или отливке кремния, что приводит к образованию полос круговых дефектов на пластинах, сделанных из такого кремния. Такие полосы можно наблюдать на кремнии после избирательного кислотного травления.According to traditional CZ or FZ methods, the distribution of oxygen atoms in silicon and the defects caused by these oxygen atoms is radial. This means that they tend to form rings, spirals or bursts that are symmetrical about the central axis. OSF ring defects are specific examples in which nanometer oxygen atoms cause stacking faults in a cylindrical strip in a single-crystal silicon ingot obtained by drawing or casting silicon, which leads to the formation of circular defect bands on wafers made of such silicon. Such bands can be observed on silicon after selective acid etching.

Как спиральные дефекты, так и кольцевые дефекты OSF наблюдаются в отливках монокристаллического кремния при вытягивании цилиндрической бульки из резервуара расплавленного кремния, например, традиционными способами CZ или FZ благодаря вращательной симметрии способа вытягивания, аксиальным термическим градиентам и вращению, присущему этому способу. Напротив, кремний можно получить способом литья согласно вариантам изобретения, при котором не образуются такие спиральные дефекты и кольцевые дефекты OSF. Это обусловлено тем, что инкорпорирование дефектов во время литья может быть реально беспорядочным на растущей поверхности раздела, на которую не влияет вращение, в массиве кремния, не обладающем цилиндрической симметрией, и в рамках способа, при котором во время отверждения и охлаждения изотермы являются практически плоскими по слитку.Both spiral defects and OSF ring defects are observed in single-crystal silicon castings when a cylindrical bobble is drawn from a molten silicon reservoir, for example, by traditional CZ or FZ methods due to rotational symmetry of the drawing method, axial thermal gradients and rotation inherent in this method. On the contrary, silicon can be obtained by a casting method according to embodiments of the invention in which such helical defects and OSF ring defects are not formed. This is due to the fact that the incorporation of defects during casting can be really random on a growing interface that is not affected by rotation in a silicon array that does not have cylindrical symmetry, and within the framework of the method in which isotherms are almost flat during curing and cooling by ingot.

Что касается концентраций примесей легких элементов в кремнии, выращенном разными способами, характеристическими считаются следующие концентрации, приведенные в Таблице 1.With regard to the concentrations of impurities of light elements in silicon grown in different ways, the following concentrations are listed as characteristic, given in Table 1.

Таблица 1Table 1   Концентрация (атомов/см3)Concentration (atoms / cm 3 )   КислородOxygen УглеродCarbon АзотNitrogen Зонная плавкаZone melting <1×1016 <1 × 10 16 <1×1016 <1 × 10 16 <1×1014 <1 × 10 14 Метод ЧохральскогоCzochralski method 2×1017 - ×1018 2 × 10 17 - × 10 18 <1×1016 <1 × 10 16 <5×1014 <5 × 10 14 ЛитьеCasting 2-3×1017 2-3 × 10 17 2×1016-5×1017 2 × 10 16 -5 × 10 17 >1×1015 > 1 × 10 15

Часть слитков CZ можно получить с концентрацией кислорода всего 5×1017 атомов/см3, но не меньше. Концентрацию углерода и азота в слитках FZ и CZ можно увеличить путем интенсивного легирования, но легирование не превышало предела растворимости в твердой фазе, возможного в таких методиках (как это происходит с литым материалом), и легированные слитки не получали размером более 20 см в диаметре. Напротив, литые слитки обычно пересыщены углеродом и азотом из-за антиадгезионных покрытий и конструкции горячей зоны в печи. В результате благодаря жидкофазной инициации и роста кристаллов везде образуются осажденные нитриды и карбиды. Кроме того, согласно вариантам данного изобретения были изготовлены литые слитки монокристаллов с указанными выше концентрациями примесей и размерами до 50×50×20 см3 и 60×60×5 см3. Эти размеры являются только примерами и не служат верхними пределами для способов литья в данном изобретении.Some CZ ingots can be obtained with an oxygen concentration of only 5 × 10 17 atoms / cm 3 , but not less. The concentration of carbon and nitrogen in the FZ and CZ ingots can be increased by intensive alloying, but the alloying did not exceed the solubility limit in the solid phase, which is possible in such methods (as happens with cast material), and alloyed ingots did not get larger than 20 cm in diameter. In contrast, cast ingots are usually supersaturated with carbon and nitrogen due to release coatings and the design of the hot zone in the furnace. As a result, due to liquid-phase initiation and crystal growth, precipitated nitrides and carbides are everywhere formed. In addition, according to the variants of the present invention, cast single crystal ingots with the above impurity concentrations and sizes up to 50 × 50 × 20 cm 3 and 60 × 60 × 5 cm 3 were made . These sizes are only examples and do not serve as upper limits for the casting methods in this invention.

Например, относительно концентраций примесей в слитке кремния согласно настоящему изобретению предпочтительно, чтобы концентрация растворенного углерода составляла примерно 1-5×1017 атомов/см3 (а именно, от примерно 1×1017 атомов/см3 до примерно 5×1017 атомов/см3), концентрация растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрация растворенного азота примерно 1-5×1015 атомов/см3. Согласно вариантам настоящего изобретения предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, который имел бы по меньшей мере два измерения, каждое по меньшей мере примерно по 20 см, например сторону примерно 20 см, и третье измерение по меньшей мере примерно 10 cм, с концентрацией растворенного углерода примерно 1-5×1017 атомов/см3, концентрацией растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрацией растворенного азота примерно 1-5×1015 атомов/см3.For example, with respect to the concentration of impurities in the silicon ingot according to the present invention, it is preferable that the concentration of dissolved carbon is about 1-5 × 10 17 atoms / cm 3 (namely, from about 1 × 10 17 atoms / cm 3 to about 5 × 10 17 atoms / cm 3 ), the concentration of dissolved oxygen is about 2-3 × 10 17 atoms / cm 3 and the concentration of dissolved nitrogen is about 1-5 × 10 15 atoms / cm 3 . According to variants of the present invention, it is preferable to obtain a solid array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, which would have at least two dimensions, each of at least about 20 cm, for example, the side of about 20 cm, and the third dimension of at least about 10 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1-5 × 10 15 atoms / cm 3 .

Предпочтительно получать массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 30 см, например со стороной по меньшей мере примерно 30 см, и третьим измерением по меньшей мере примерно 10 см, при концентрации растворенного углерода примерно 1-5×1017 атомов/см3, концентрации растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрации растворенного азота примерно 1-5×1015 атомов/см3. Более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, по меньшей мере с двумя измерениями, каждое по меньшей мере примерно 35 см, например со стороной по меньшей мере примерно 35 см, и третьим измерением по меньшей мере примерно 10 см, при концентрации растворенного углерода примерно 1-5×1017 атомов/см3, концентрации растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрации растворенного азота примерно 1-5×1015 атомов/см3. Еще более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 40 см, например со стороной по меньшей мере примерно 40 см, и третьим измерением по меньшей мере примерно 20 см, при концентрации растворенного углерода примерно 1-5×1017 атомов/см3, концентрации растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрации растворенного азота примерно 1-5×1015 атомов/см3. Еще более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 50 см, например со стороной по меньшей мере примерно 50 см, и третьим измерением по меньшей мере примерно 20 см, при концентрации растворенного углерода примерно 1-5×1017 атомов/см3, концентрации растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрации растворенного азота примерно 1-5×1015 атомов/см3. Еще более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 60 см, например со стороной по меньшей мере примерно 60 см, и третьим измерением по меньшей мере примерно 20 см, при концентрации растворенного углерода примерно 1-5×1017 атомов/см3, концентрации растворенного кислорода примерно 2-3×1017атомов/см3 и концентрации растворенного азота примерно 1-5×1015 атомов/см3. Еще более предпочтительно получать твердый массив монокристаллического кремния или почти монокристаллического кремния, предпочтительно литого, по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 70 см, например со стороной по меньшей мере примерно 70 см, и третьим измерением по меньшей мере примерно 20 см, при концентрации растворенного углерода примерно 1-5×1017 атомов/см3, концентрации растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрации растворенного азота примерно 1-5×1015 атомов/см3.It is preferable to obtain an array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, with at least two dimensions, each of at least about 30 cm, for example with a side of at least about 30 cm, and a third measurement of at least about 10 cm, with the concentration of dissolved carbon is about 1-5 × 10 17 atoms / cm 3 the concentration of dissolved oxygen is about 2-3 × 10 17 atoms / cm 3 and the concentration of dissolved nitrogen is about 1-5 × 10 15 atoms / cm 3 . It is more preferable to obtain a solid array of single crystal silicon or almost single crystal silicon, preferably cast, with at least two dimensions, each of at least about 35 cm, for example with a side of at least about 35 cm, and a third measurement of at least about 10 cm, when the concentration of dissolved carbon is about 1-5 × 10 17 atoms / cm 3 , the concentration of dissolved oxygen is about 2-3 × 10 17 atoms / cm 3 and the concentration of dissolved nitrogen is about 1-5 × 10 15 atoms / cm 3 . It is even more preferable to obtain a solid array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, with at least two dimensions, each of at least about 40 cm, for example with a side of at least about 40 cm, and a third dimension of at least about 20 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1-5 × 10 15 atoms / cm 3 . It is even more preferable to obtain a solid array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, with at least two dimensions, each of at least about 50 cm, for example with a side of at least about 50 cm, and a third dimension of at least about 20 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1-5 × 10 15 atoms / cm 3 . It is even more preferable to obtain a solid array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, with at least two dimensions, each of at least about 60 cm, for example with a side of at least about 60 cm, and a third dimension of at least about 20 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1-5 × 10 15 atoms / cm 3 . It is even more preferable to obtain a solid array of monocrystalline silicon or almost monocrystalline silicon, preferably cast, with at least two dimensions, each of at least about 70 cm, for example with a side of at least about 70 cm, and a third measurement of at least about 20 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1-5 × 10 15 atoms / cm 3 .

Согласно вариантам настоящего изобретения можно получить массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащий или практически не содержащий радиально распределенных дефектов и/или примесей, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 20 см, и третье измерение по меньшей мере примерно 10 см, с концентрацией растворенного углерода примерно 1-5×1017 атомов/см3, концентрацией растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрацией растворенного азота примерно 1-5×1015 атомов/см3. Предпочтительно получать массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащий или практически не содержащий радиально распределенных дефектов и/или примесей, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 30 см, и третье измерение по меньшей мере примерно 10 см, с концентрацией растворенного углерода примерно 1-5×1017 атомов/см3, концентрацией растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрацией растворенного азота примерно 1-5×1015 атомов/см3. Более предпочтительно получать массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащий или практически не содержащий радиально распределенных дефектов и/или примесей, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 35 см, и третье измерение по меньшей мере примерно 10 см, с концентрацией растворенного углерода примерно 1-5×1017 атомов/см3, концентрацией растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрацией растворенного азота примерно 1-5×1015 атомов/см3. Еще более предпочтительно получать массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащий или практически не содержащий радиально распределенных дефектов и/или примесей, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 40 см, и третье измерение по меньшей мере примерно 20 см, с концентрацией растворенного углерода примерно 1-5×1017 атомов/см3, концентрацией растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрацией растворенного азота примерно 1-5×1015 атомов/см3. Еще более предпочтительно получать массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащий или практически не содержащий радиально распределенных дефектов и/или примесей, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 50 см, и третье измерение по меньшей мере примерно 20 см, с концентрацией растворенного углерода примерно 1-5×1017 атомов/см3, концентрацией растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрацией растворенного азота примерно 1-5×1015 атомов/см3. Еще более предпочтительно получать массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащий или практически не содержащий радиально распределенных дефектов и/или примесей, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 60 см, и третье измерение по меньшей мере примерно 20 см, с концентрацией растворенного углерода примерно 1-5×1017 атомов/см3, концентрацией растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрацией растворенного азота примерно 1-5×1015 атомов/см3. Еще более предпочтительно получать массив сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащий или практически не содержащий радиально распределенных дефектов и/или примесей, предпочтительно имеющий по меньшей мере два измерения, каждое по меньшей мере примерно по 70 см, и третье измерение по меньшей мере примерно 20 см, с концентрацией растворенного углерода примерно 1-5×1017 атомов/см3, концентрацией растворенного кислорода примерно 2-3×1017 атомов/см3 и концентрацией растворенного азота примерно 1-5×1015 атомов/см3.According to the variants of the present invention, it is possible to obtain an array of solid single-crystal silicon or almost single-crystal silicon, containing no or practically no radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 20 cm, and the third measurement at least about 10 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a solution concentration Nitrogen content of approximately 1-5 × 10 15 atoms / cm 3 . It is preferable to obtain an array of solid monocrystalline silicon or almost monocrystalline silicon, containing no or practically no radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 30 cm, and the third dimension of at least about 10 cm, with a concentration of dissolved carbon of about 1-5 × 10 17 atoms / cm 3 , a concentration of dissolved oxygen of about 2-3 × 10 17 atoms / cm 3 and a concentration of dissolved nitrogen of about 1-5 × 10 15 atom o / cm 3 . It is more preferable to obtain an array of solid monocrystalline silicon or almost monocrystalline silicon, containing no or practically no radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 35 cm, and the third measurement of at least about 10 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1-5 × 10 15 atoms / cm 3 . It is even more preferable to obtain an array of solid monocrystalline silicon or almost monocrystalline silicon, which does not contain or practically does not contain radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 40 cm, and the third measurement of at least about 20 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1 -5 × 10 15 atoms / cm 3 . It is even more preferable to obtain an array of solid monocrystalline silicon or almost monocrystalline silicon, containing no or practically no radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 50 cm, and a third measurement of at least about 20 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1 -5 × 10 15 atoms / cm 3 . It is even more preferable to obtain an array of solid monocrystalline silicon or almost monocrystalline silicon, which does not contain or practically does not contain radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 60 cm, and the third measurement of at least about 20 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1 -5 × 10 15 atoms / cm 3 . It is even more preferable to obtain an array of solid monocrystalline silicon or almost monocrystalline silicon, free or practically free of radially distributed defects and / or impurities, preferably having at least two dimensions, each of at least about 70 cm, and a third measurement of at least about 20 cm, with a dissolved carbon concentration of about 1-5 × 10 17 atoms / cm 3 , a dissolved oxygen concentration of about 2-3 × 10 17 atoms / cm 3 and a dissolved nitrogen concentration of about 1 -5 × 10 15 atoms / cm 3 .

Верхний предел горизонтального размера слитка кремния, полученного согласно вариантам данного изобретения, определяется только технологией литья и изготовления тигля, а не самим предлагаемым способом. Согласно настоящему изобретению предпочтительно получать твердый массив литого сплошного монокристаллического кремния или почти монокристаллического кремния, содержащего указанные выше концентрации примесей, который может иметь по меньшей мере два измерения, каждое из которых соответствует внутренним размерам сосуда для литья, и третье измерение, равное высоте слитка. Например, если литой массив монокристаллического кремния имеет форму куба или прямоугольника, приведенные измерения относятся к длине, ширине и высоте таких массивов.The upper limit of the horizontal size of the silicon ingot obtained according to the variants of the present invention is determined only by the technology of casting and manufacturing the crucible, and not by the proposed method. According to the present invention, it is preferable to obtain a solid array of cast solid monocrystalline silicon or almost monocrystalline silicon containing the above impurity concentrations, which may have at least two dimensions, each of which corresponds to the internal dimensions of the casting vessel, and a third dimension equal to the height of the ingot. For example, if a cast array of single-crystal silicon has the form of a cube or a rectangle, the measurements given relate to the length, width, and height of such arrays.

Затравки, используемые в способах литья согласно вариантам изобретения, могут быть любой нужной формы и размера, в том числе кусками подходящей геометрической формы монокристаллического кремния, почти монокристаллического кремния или геометрически упорядоченного поликристаллического кремния, такими как куски кремния квадратной, прямоугольной, гексагональной, ромбоидальной или шестиугольной формы. Они могут иметь форму, удобную для укладки, с тем чтобы их можно было разместить или «уложить» ребро-к-ребру нужным образом по дну тигля. Также в соответствии с вариантами изобретения затравки можно помещать на одну или несколько, в том числе на все стороны тигля. Такие затравки можно получить, например, путем разрезания источника кристаллического кремния, такого как слиток монокристаллического кремния, на куски нужной формы. Такие затравки можно получить путем отрезания их от образца либо сплошного монокристаллического, почти кристаллического или сплошного геометрически упорядоченного поликристаллического кремния, полученного по способу вариантов данного изобретения, так что затравки для использования в последующих процессах литья можно изготовить начальным способом литья. Таким образом, например, лист либо сплошного монокристаллического, либо почти монокристаллического кремния, вырезанный или полученный иначе из слитка сплошного монокристаллического или почти монокристаллического кремния, может служить матрицей для последующего литья монокристаллического или почти монокристаллического кремния. Такой затравочный кристалл может быть такого размера и формы или почти такого размера и формы, как сторона, например дно, тигля или другого сосуда, в который помещают затравку. В целях монокристаллического литья предпочтительно иметь по возможности несколько затравок, чтобы во избежание внедрения дефектов покрыть дно тигля. Таким образом, затравка или затравки могут быть такого размера и формы или почти такого размера и формы, как одна или несколько сторон, таких как дно тигля или другого сосуда, в который помещают затравку или затравки для осуществления способа литья согласно данному изобретению.The seeds used in the casting methods according to embodiments of the invention can be of any desired shape and size, including pieces of a suitable geometric shape of single crystal silicon, almost single crystal silicon or geometrically ordered polycrystalline silicon, such as pieces of silicon square, rectangular, hexagonal, rhomboidal or hexagonal forms. They can have a shape convenient for stacking so that they can be placed or “laid” rib-to-rib in the desired way along the bottom of the crucible. Also, in accordance with embodiments of the invention, the seeds can be placed on one or more, including on all sides of the crucible. Such seeds can be obtained, for example, by cutting a source of crystalline silicon, such as a single crystal silicon ingot, into pieces of the desired shape. Such seeds can be obtained by cutting them from a sample or a solid single crystal, almost crystalline or continuous geometrically ordered polycrystalline silicon obtained by the method of the variants of the present invention, so that seeds for use in subsequent casting processes can be made by the initial casting method. Thus, for example, a sheet of either solid single-crystal or almost single-crystal silicon, cut or otherwise obtained from an ingot of solid single-crystal or almost single-crystal silicon, can serve as a matrix for subsequent casting of single-crystal or almost single-crystal silicon. Such a seed crystal may be of such size and shape, or of almost such size and shape as the side, for example, the bottom, crucible or other vessel into which the seed is placed. For single-crystal casting, it is preferable to have as few seeds as possible in order to avoid the introduction of defects to cover the bottom of the crucible. Thus, the seed or seeds can be of such a size and shape, or of nearly the same size and shape as one or more sides, such as the bottom of a crucible or other vessel, in which the seed or seeds are placed to carry out the casting method according to this invention.

Далее будут описаны способы и аппаратура для получения кремния согласно некоторым вариантам данного изобретения. Однако следует понимать, что это не единственные способы получения кремния согласно принципам изобретения.Next will be described methods and apparatus for producing silicon according to some variants of the present invention. However, it should be understood that these are not the only methods for producing silicon according to the principles of the invention.

На ФИГ.1 затравки 100 помещают на дно тигля, имеющего дно и боковые стенки 110, например кварцевого тигля, таким образом, чтобы они тесно примыкали друг к другу, будучи ориентированы одинаково, с образованием большого листа 120 с непрерывной ориентацией. Альтернативно, они плотно примыкают без предварительно заданной ориентации с образованием специфических границ зерен, чтобы конечный кремний содержал зерна выбранного размера. Т.е. при литье геометрически упорядоченного поликристаллического кремния размер поперечного сечения и предпочтительно форма поперечного сечения полученного закристаллизованного поликристаллического кремния будут такими же или приблизительно такими же, как у затравочных кристаллов, и высота зерна будет равна размеру кремния, перпендикулярному поперечному сечению. Если в качестве кристалла или кристаллов затравки при литье геометрически упорядоченного поликристаллического кремния используют затравочный кристалл геометрически упорядоченного поликристаллического кремния, например лист геометрически упорядоченного поликристаллического кремния, вырезанный или иначе полученный из слитка геометрически упорядоченного поликристаллического кремния, размер поперечного сечения зерна и предпочтительно форма поперечного сечения зерен полученного геометрически упорядоченного поликристаллического кремния будут приблизительно такими же, как у зерен затравочного кристалла или кристаллов геометрически упорядоченного поликристаллического кремния. Таким образом, лист геометрически упорядоченного поликристаллического кремния, вырезанный или иначе полученный из слитка геометрически упорядоченного поликристаллического кремния, может быть «затравочным кристаллом геометрически упорядоченного поликристаллического кремния» (также называемый «затравочным кристаллом геометрически упорядоченного поликристаллического кремния») и может функционировать в качестве матрицы для последующего литья геометрически упорядоченного поликристаллического кремния. Такой затравочный кристалл может иметь такой размер и форму или практически такой же размер и форму, как и сторона, например дно, тигля или другого сосуда, в который помещена затравка. При использовании такого затравочного кристалла в способе данного изобретения полученный геометрически упорядоченный поликристаллический кремний будет предпочтительно состоять из кристаллических зерен, которые имеют такие же или практически такие же размеры и форму поперечного сечения, как у зерен затравки.In FIG. 1, the seeds 100 are placed on the bottom of a crucible having a bottom and side walls 110, for example a quartz crucible, so that they closely adjoin each other, being oriented identically, to form a large sheet 120 with a continuous orientation. Alternatively, they are closely adjacent without a predetermined orientation with the formation of specific grain boundaries so that the final silicon contains grains of a selected size. Those. when casting geometrically ordered polycrystalline silicon, the cross-sectional size and preferably the cross-sectional shape of the obtained crystallized polycrystalline silicon will be the same or approximately the same as the seed crystals, and the grain height will be equal to the size of silicon perpendicular to the cross-section. If a seed crystal of a geometrically ordered polycrystalline silicon, for example a sheet of geometrically ordered polycrystalline silicon, cut or otherwise obtained from an ingot of geometrically ordered polycrystalline silicon, grain cross-sectional size, and preferably grain cross section shape geometrically ordered polycrystalline about silicon will be approximately the same as the grains of the seed crystal or crystals of geometrically ordered polycrystalline silicon. Thus, a sheet of geometrically ordered polycrystalline silicon, cut out or otherwise obtained from an ingot of geometrically ordered polycrystalline silicon, can be a “seed crystal of geometrically ordered polycrystalline silicon” (also called a “seed crystal of geometrically ordered polycrystalline silicon”) and can function as a matrix for subsequent casting geometrically ordered polycrystalline silicon. Such a seed crystal may have such a size and shape, or substantially the same size and shape as the side, for example, the bottom, crucible or other vessel in which the seed is placed. When using such a seed crystal in the method of the present invention, the obtained geometrically ordered polycrystalline silicon will preferably consist of crystalline grains that have the same or substantially the same size and cross-sectional shape as the seed grains.

Предпочтительно размещать и укладывать затравки 100 так, чтобы покрыть практически все дно тигля 110. Также предпочтительно, чтобы тигель 110 имел противоадгезионное покрытие, например, из оксида кремния, нитрида кремния или жидкого герметика, с тем чтобы облегчить удаление закристаллизованного кремния из тигля 110. Кроме того, затравки могут представлять собой лист или листы монокристаллического кремния с нужной ориентацией кристаллов толщиной примерно 3-100 мм. Хотя на ФИГ.1 показаны конкретные число и размер затравок 100, специалисту в данной области будет очевидно, что как число, так и размер затравок можно увеличить или уменьшить в зависимости от применения.It is preferable to place and stack the seeds 100 so as to cover practically the entire bottom of the crucible 110. It is also preferable that the crucible 110 has a release coating, for example of silicon oxide, silicon nitride or liquid sealant, in order to facilitate the removal of crystallized silicon from the crucible 110. In addition Moreover, the seeds can be a sheet or sheets of single crystal silicon with the desired orientation of the crystals with a thickness of about 3-100 mm Although FIG. 1 shows the specific number and size of the seeds 100, one skilled in the art will appreciate that both the number and size of the seeds can be increased or decreased depending on the application.

На ФИГ.2 показано, что затравки 100 можно также поместить на одну или несколько боковых стенок 130, 140 тигля 110. Затравки 100 можно поместить на все четыре стенки тигля 110, хотя для иллюстрации затравки 100 показаны только на стенках 130, 140. Для облегчения роста кристаллов предпочтительно, чтобы затравки 100, помещенные на любой из четырех стенок тигля 110, были столбчатыми. Предпочтительно, чтобы каждая столбчатая затравка, помещенная на любую из четырех стенок тигля 110, имела ту же ориентацию зерен, что и затравка, помещенная ниже нее на поверхности дна тигля 110. В случае роста геометрически упорядоченного поликристаллического кремния такое размещение столбчатых затравок будет облегчать рост зерен геометрически упорядоченного поликристаллического кремния на высоту тигля 110.Figure 2 shows that the seeds 100 can also be placed on one or more side walls 130, 140 of the crucible 110. The seeds 100 can be placed on all four walls of the crucible 110, although to illustrate the seeds 100 are shown only on the walls 130, 140. To facilitate crystal growth, it is preferable that the seed 100, placed on any of the four walls of the crucible 110, were columnar. Preferably, each columnar seed placed on any of the four walls of the crucible 110 has the same grain orientation as the seed placed below it on the bottom surface of the crucible 110. In the case of growth of geometrically ordered polycrystalline silicon, such placement of the columnar seeds will facilitate grain growth geometrically ordered polycrystalline silicon to a height of 110 crucible.

Кроме того, из ФИГ.2 следует, что преимуществом такого расположения затравок 110 является более быстрый и простой саморазвивающийся способ литья кремния с более высокой кристалличностью и более высокими скоростями роста. Например, кремний можно расплавить в кремниевой «чашке», состоящей из множества затравок, уложенных вместе с образованием полости, например из дна и четырех стенок, внутри тигля 110. Альтернативно расплавленный кремний можно вылить в кремниевую «чашку», состоящую из множества затравок, уложенных вместе с образованием полости, например из дна и четырех стенок, внутри тигля 110. В альтернативном примере принимающую «чашку» сначала доводят до температуры плавления кремния, но оставляют в твердом состоянии и затем выливают расплавленный кремний и дают ему прийти в термическое равновесие. Затем в любом приведенном выше примере тигель 110 охлаждают, а тепло отводят через дно и стенки тигля 110, например, с помощью твердого теплопоглотителя (не показан), который передает тепло в окружающую среду, когда тепло еще подают к открытой вершине тигля 110. Таким образом, полученный слиток кремния может быть либо монокристаллическим, либо геометрически упорядоченным поликристаллическим кремнием (в зависимости от типа использованных затравок 100 и их ориентации), и кристаллизация протекает быстрее, чем в известных способах литья поликристаллического кремния. Для повторения способа часть затравок и дно слитка закристаллизованного кремния удаляют с помощью известных методик, и их можно использовать в последующих циклах литья. Предпочтительно располагать множество затравочных кристаллов, например затравок 100, таким образом, чтобы общее направление оси затравок 100 было перпендикулярным к дну и стенке тигля 110, тогда границы зерен между дном и стенкой тигля 110 не образуются.In addition, it follows from FIG. 2 that the advantage of this arrangement of the seeds 110 is a faster and easier self-developing silicon casting process with higher crystallinity and higher growth rates. For example, silicon can be melted in a silicon “cup” consisting of a plurality of seeds placed together to form a cavity, for example of a bottom and four walls, inside the crucible 110. Alternatively, molten silicon can be poured into a silicon “cup” consisting of a plurality of seeds placed together with the formation of a cavity, for example from the bottom and four walls, inside the crucible 110. In an alternative example, the receiving “cup” is first brought to the melting temperature of silicon, but left in the solid state and then molten silicon is poured second and give it to come to thermal equilibrium. Then, in any example above, the crucible 110 is cooled, and heat is removed through the bottom and walls of the crucible 110, for example, using a solid heat sink (not shown) that transfers heat to the environment when heat is still supplied to the open top of the crucible 110. Thus , the obtained silicon ingot can be either single-crystal or geometrically ordered polycrystalline silicon (depending on the type of seeds used 100 and their orientation), and crystallization proceeds faster than in the known polycrystal casting methods -crystal silicon. To repeat the method, part of the seeds and the bottom of the crystallized silicon ingot are removed using known methods and can be used in subsequent casting cycles. It is preferable to arrange a plurality of seed crystals, for example, seeds 100, so that the general direction of the axis of the seeds 100 is perpendicular to the bottom and wall of the crucible 110, then grain boundaries between the bottom and the wall of the crucible 110 are not formed.

ФИГ.3А-С иллюстрируют пример укладки для литья геометрически упорядоченного поликристаллического кремния в тигле 110. Технологию кристаллических зерен можно осуществить тщательным приготовлением затравки, ориентацией, размещением и ростом кристалла. На ФИГ.3А и 3В, например, показаны два листа 155, 165, на которых обозначены различные направления (110). Оба листа имеют общее направление (100), перпендикулярное их поверхностям. Затем каждый лист монокристаллического кремния 155, 165 режут на много кусочков кремния, которые становятся затравками 150, 160. Поверхность может быть однородной, например (100), благодаря текстурированию или может быть выбрана любой. Форму и размер зерен можно выбрать при нарезании кусочков из листов монокристаллического кремния 155 и 165, как показано на ФИГ.3B. Углы относительной ориентации между соседними плитками кусков 150, 160 определяют тип границ зерен (например, большой угол, малый угол или двойной) в полученном литом геометрически упорядоченном поликристаллическом кремнии. На ФИГ.3А, например, показаны две ориентации осей зерен (100).FIGS. 3A-C illustrate an example of a styling for casting geometrically ordered polycrystalline silicon in a crucible 110. The technology of crystalline grains can be accomplished by thoroughly preparing the seed, orientation, placement and growth of the crystal. FIGS. 3A and 3B, for example, show two sheets 155, 165, which indicate different directions (110). Both sheets have a common direction (100) perpendicular to their surfaces. Then, each sheet of monocrystalline silicon 155, 165 is cut into many pieces of silicon, which become seeds 150, 160. The surface can be uniform, for example (100), due to texturing, or can be selected any. The shape and size of the grains can be selected when cutting pieces from sheets of monocrystalline silicon 155 and 165, as shown in FIG.3B. The relative orientation angles between adjacent tiles of pieces 150, 160 determine the type of grain boundaries (for example, a large angle, a small angle, or a double) in a cast geometrically ordered polycrystalline silicon. FIG. 3A, for example, shows two orientations of the grain axes (100).

Затравки, показанные на ФИГ.3С, состоят из уложенных кусочков монокристаллического кремния 150, 160, которые характеризуются специально выбранными соотношениями с соседними плитками. Кусочки кремния 150, 160 затем укладывают на дне тигля 110, показанного на ФИГ.3С, таким образом, что два направления (110) чередуются, как показано стрелками, изображенными на кусочках 150, 160. Важно отметить, что кусочки 150, 160 изображены в виде примерно квадратных блоков только в целях иллюстрации и по причинам, описанным ниже, могут иметь другую форму.The seeds shown in FIG. 3C consist of stacked pieces of monocrystalline silicon 150, 160, which are characterized by specially selected ratios with adjacent tiles. The pieces of silicon 150, 160 are then stacked on the bottom of the crucible 110 shown in FIG. 3C, so that the two directions (110) alternate, as shown by the arrows depicted in pieces 150, 160. It is important to note that the pieces 150, 160 are shown in in the form of approximately square blocks, for illustration purposes only and for the reasons described below, may have a different shape.

Хотя это и не показано на ФИГ.3С, затравки также могут располагаться на стенках тигля, как на ФИГ.2. Источник кремния (не показан) можно ввести в тигель 110 в виде кусков 150, 160 и затем расплавить. Альтернативно, расплавленный кремний можно вылить в тигель 110. В альтернативном примере тигель 110 сначала доводят вплотную до температуры плавления кремния и затем расплавленный кремний выливают. В соответствии с вариантами изобретения тонкий слой затравок можно расплавить до того, как начинается отверждение.Although not shown in FIG. 3C, the seeds can also be located on the walls of the crucible, as in FIG. 2. A silicon source (not shown) can be introduced into the crucible 110 in the form of pieces 150, 160 and then melted. Alternatively, molten silicon can be poured into crucible 110. In an alternative example, crucible 110 is first brought close to the melting point of silicon and then molten silicon is poured. In accordance with embodiments of the invention, a thin layer of seeds can be melted before curing begins.

Затем во всех приведенных примерах тигель 110 охлаждают, причем тепло отводят через дно тигля 110 (и стенки, только если затравки укладывают также и на стенках) с помощью, например, твердого теплоносителя, который передает тепло в окружающую среду, в то время как тепло подводят к открытому верху тигля 110. Таким образом, расплавленный кремний вводят тогда, когда затравка находится в твердом состоянии и направленное отверждение расплава вызывает указанный рост столбчатых зерен. В результате полученный слиток геометрически упорядоченного поликристаллического кремния запомнит ориентацию зерен уложенных затравок кремния 150, 160. После точного применения этой техники полученный слиток можно разрезать, например, на горизонтальный листы, которые могут служить слоями затравок для других способов литья. Лист может иметь, например, такой размер и форму или почти такой размер и форму, как у поверхности, например, дна тигля или другого сосуда, используемого для литья. Например, для литья можно использовать только один такой лист.Then, in all the examples cited, the crucible 110 is cooled, and heat is removed through the bottom of the crucible 110 (and the walls, only if the seeds are also laid on the walls) using, for example, a solid heat transfer medium that transfers heat to the environment, while heat is supplied to the open top of the crucible 110. Thus, molten silicon is introduced when the seed is in a solid state and directional solidification of the melt causes the indicated growth of columnar grains. As a result, the obtained ingot of geometrically ordered polycrystalline silicon will remember the orientation of the grains of the deposited silicon seeds 150, 160. After the exact application of this technique, the obtained ingot can be cut, for example, into horizontal sheets, which can serve as seed layers for other casting methods. The sheet may, for example, be of such a size and shape, or nearly the same size and shape as that of the surface of, for example, the bottom of a crucible or other vessel used for casting. For example, only one such sheet can be used for casting.

ФИГ.4 иллюстрирует варианты укладки, показанной на ФИГ.3С. В качестве примера ориентации зерен для литья геометрически упорядоченного поликристаллического кремния кусочки затравки 150, 160 укладывают с общим направлением оси (001), перпендикулярным дну тигля 110. На ФИГ.4 все варианты семейства направлений (110) представлены при укладке кусочков 150, 160, как показано направлениями стрелок. Хотя они не показаны на отдельной фигуре, затравки могут находиться на одной или нескольких стенках тигля 110.FIG. 4 illustrates the styling options shown in FIG. 3C. As an example of the orientation of the grains for casting geometrically ordered polycrystalline silicon, the seed pieces 150, 160 are stacked with the general axis direction (001) perpendicular to the bottom of the crucible 110. In FIG. 4, all variants of the direction family (110) are presented when stacking the pieces 150, 160, as shown by arrow directions. Although not shown in a separate figure, the seeds can be on one or more walls of the crucible 110.

Таким образом, ориентацию затравочных кристаллов в тигле, используемом для получения кремния, можно выбрать такой, чтобы в отлитом геометрически упорядоченном поликристаллическом кремнии образовались определенные границы зерен и такие границы зерен соответствовали определенным геометрическим формам. В отличие от вариантов данного изобретения известные способы литья включают литье поликристаллических зерен нерегулируемым образом путем направленного отверждения полностью расплавленной массы кремния. Полученные зерна характеризуются в основном беспорядочной ориентацией и распределением по размерам. Беспорядочная ориентация зерен затрудняет эффективное текстурирование поверхности кремния. Кроме того, было показано, что углы на границах зерен - естественных продуктах типичных методик роста - имеют тенденцию образовывать зародыши структурных дефектов, включая кластеры или линии дислокаций. Эти дислокации и примеси, которые они к себе притягивают, вызывают быструю рекомбинацию электрических носителей и снижение фотоэлектрической активности получаемого материала. Поэтому в соответствии с вариантом данного изобретения тщательное планирование и внесение затравок регулярной сети границ зерен при литье либо монокристаллического, либо геометрически упорядоченного поликристаллического кремния проводят таким образом, чтобы размер, форма и ориентация зерен были точно подобраны для достижения максимального срока жизни меньшинства носителей и геттерирования примесей при минимизации структурных дефектов.Thus, the orientation of the seed crystals in the crucible used to produce silicon can be chosen such that certain grain boundaries form in the cast geometrically ordered polycrystalline silicon and such grain boundaries correspond to certain geometric shapes. In contrast to the embodiments of the present invention, known casting methods include casting polycrystalline grains in an unregulated manner by directed curing of a completely molten mass of silicon. The resulting grains are characterized mainly by random orientation and size distribution. The random orientation of the grains makes it difficult to texturize the silicon surface efficiently. In addition, it has been shown that angles at grain boundaries — the natural products of typical growth techniques — tend to form nuclei of structural defects, including clusters or dislocation lines. These dislocations and the impurities that they attract to themselves cause a rapid recombination of electrical carriers and a decrease in the photoelectric activity of the resulting material. Therefore, in accordance with an embodiment of the invention, careful planning and seeding of a regular network of grain boundaries when casting either single-crystal or geometrically ordered polycrystalline silicon is carried out in such a way that the size, shape and orientation of the grains are precisely matched to achieve the maximum lifetime of a minority of carriers and gettering of impurities while minimizing structural defects.

Границы зерен можно выбрать в виде плоскостей с тем, чтобы минимизировать образование дислокаций при сохранении их вертикального направления во время роста. Типы границ зерен выбирают с учетом максимального геттерирования примесей и снятия напряжений. Ориентацию зерен (и особенно ориентацию поверхности) выбирают так, чтобы происходило текстурирование, улучшалась пассивация поверхности и повышалась прочность зерен. Размер зерен выбирают таким образом, чтобы оптимизировать баланс между расстояниями эффективного геттерирования и большими поверхностями поглощения. Например, литье геометрически упорядоченного поликристаллического кремния можно проводить так, чтобы геометрически упорядоченный поликристаллический кремний содержал зерна со средним минимальным размером поперечного сечения по меньшей мере примерно 0.5-10 см с общим направлением главной оси, перпендикулярным поверхности литого геометрически упорядоченного поликристаллического кремния, как показано, например, на ФИГ.3С и 4. Размер поперечного сечения среднего зерна кристалла может составлять примерно 0.5-70 см или более. Как показано выше, под размером поперечного сечения понимают наибольший размер поперечного сечения зерна, перпендикулярный высоте или длине зерна. Общим результатом является увеличение эффективности полученного фотоэлектрика.Grain boundaries can be selected in the form of planes in order to minimize the formation of dislocations while maintaining their vertical direction during growth. The types of grain boundaries are selected taking into account the maximum gettering of impurities and stress relief. The orientation of the grains (and especially the orientation of the surface) is chosen so that texturing occurs, surface passivation is improved, and grain strength is increased. The grain size is chosen so as to optimize the balance between the effective gettering distances and large absorption surfaces. For example, the casting of geometrically ordered polycrystalline silicon can be carried out so that the geometrically ordered polycrystalline silicon contains grains with an average minimum cross-sectional size of at least about 0.5-10 cm with a common direction of the main axis perpendicular to the surface of the cast geometrically ordered polycrystalline silicon, as shown, for example , FIGS and 4. The size of the cross section of the average grain of the crystal may be approximately 0.5-70 cm or more. As shown above, the cross-sectional size refers to the largest grain cross-sectional size perpendicular to the grain height or length. The overall result is an increase in the efficiency of the resulting photoelectric.

В соответствии с вариантом изобретения множество затравочных кристаллов монокристаллического кремния можно геометрически расположить по меньшей мере на одной поверхности тигля, например на поверхности дна тигля, причем геометрическое расположение включает плотноупакованные многогранники. Альтернативно, множество затравочных кристаллов монокристаллического кремния могут быть расположены так, что геометрическое расположение включит плотноупакованные многогранники или совокупность многогранников с ромбоидальными или треугольными пустотами, как показано, например, на ФИГ.5 и 6. Еще одной альтернативой при литье монокристаллического кремния или почти монокристаллического кремния в соответствии с данным изобретением является использование вместо множества монокристаллических затравочных кристаллов части или среза от слитка кремния, полученного предшествующим литьем монокристаллического кремния или почти монокристаллического кремния, в качестве одного затравочного кристалла. Такой единичный затравочный кристалл может иметь такой же размер и форму или практически такой же размер и форму, как поверхность тигля или другого сосуда, используемого для проведения литья. Более конкретно, на ФИГ.5 приведен пример плотноупакованных шестигранников 170. Напротив, ФИГ.6 иллюстрирует пример ряда многогранников с ромбоидальными или треугольными пустотами 180, 190. Оба ряда рассмотрены ниже более подробно. Любое расположение, обсужденное выше, также применимо в варианте литья либо твердого массива монокристаллического кремния, твердого массива почти кристаллического кремния, либо твердого массива геометрически упорядоченного поликристаллического кремния, где затравочные кристаллы находятся как на дне, так и на боковых стенках тигля.According to an embodiment of the invention, a plurality of single crystals of single crystal silicon can be geometrically positioned on at least one surface of the crucible, for example, on the surface of the bottom of the crucible, the geometrical arrangement including close-packed polyhedra. Alternatively, a plurality of single crystal silicon seed crystals may be arranged such that the geometrical arrangement includes densely packed polyhedra or a plurality of polyhedra with rhomboid or triangular voids, as shown, for example, in FIGS. 5 and 6. Another alternative when casting single crystal silicon or almost single crystal silicon in accordance with this invention is the use, instead of many single crystal seed crystals of a part or a cut from Litke silicon, monocrystalline silicon obtained by the previous injection, or nearly single crystalline silicon, as a seed crystal. Such a single seed crystal may have the same size and shape, or substantially the same size and shape as the surface of a crucible or other vessel used for casting. More specifically, FIG. 5 shows an example of close-packed hexahedrons 170. In contrast, FIG. 6 illustrates an example of a series of polyhedra with rhomboid or triangular voids 180, 190. Both rows are discussed in more detail below. Any arrangement discussed above is also applicable in the casting variant of either a solid array of monocrystalline silicon, a solid array of almost crystalline silicon, or a solid array of geometrically ordered polycrystalline silicon, where the seed crystals are located both on the bottom and on the side walls of the crucible.

Кристаллические зерна кремния, полученные литьем массива геометрически упорядоченного поликристаллического кремния в соответствии с вариантами изобретения, можно вырастить в виде столбиков. Кроме того, такие кристаллические зерна могут иметь поперечное сечение, которое повторяет форму кристалла, на котором оно образуется, или имеет близкую к ней форму. При получении кремния с такими специфически выбранными границами зерен предпочтительно, чтобы только три границы между зернами сходились в одном углу. Как показано на ФИГ.5, гексагональное расположение затравочных кристаллов 170 желательно для укладки затравочных кристаллов с такой ориентацией кристалла, при которой атомы в горизонтальной плоскости имеют тройную или шестикратную симметрию, например (111) для кремния. Таким образом, ФИГ.5 показывает план части набора затравочных кристаллов гексагональной формы на дне подходящего тигля, такого как на ФИГ.1 и 2. Стрелки показывают ориентацию направления (110) в кристалле кремния в этих затравках.Crystalline silicon grains obtained by casting an array of geometrically ordered polycrystalline silicon in accordance with embodiments of the invention can be grown in columns. In addition, such crystalline grains can have a cross section that repeats the shape of the crystal on which it is formed, or has a shape close to it. When producing silicon with such specifically selected grain boundaries, it is preferable that only three boundaries between the grains converge in one corner. As shown in FIG. 5, a hexagonal arrangement of seed crystals 170 is desirable for stacking seed crystals with a crystal orientation such that the atoms in the horizontal plane have triple or six-fold symmetry, for example, (111) for silicon. Thus, FIG. 5 shows a plan of a portion of a set of hexagonal seed crystals at the bottom of a suitable crucible, such as in FIGS. 1 and 2. The arrows show the orientation of the (110) direction in the silicon crystal in these seeds.

Альтернативно, для ориентации с четырехкратной симметрией можно использовать разные геометрические конфигурации затравочных кристаллов, с тем чтобы сохранить стабильные симметричные границы зерен во многих зернах, когда три границы зерен сходятся в одном углу. Например, если θ означает угол расхождения между направлением (110) и первичными сторонами шестигранника с главной осью (100) и α является углом при вершине междуузельного ромба, как показано на ФИГ.6, то все кристаллические зерна будут иметь симметричную границу зерна по отношению к направлению (110), если α=90°-θ. В этом примере все кристаллические зерна характеризуются направлением главной оси (100), перпендикулярным плоскости, на которой изображена ФИГ.6. Таким образом, ФИГ.6 представляет собой план части набора затравочных шестигранных кристаллов наряду с ромбическими затравками 180, 190 на дне соответствующего тигля, такого как на ФИГ.1 и 2. Стрелки показывают ориентацию направления (110) в кристалле кремния в затравках.Alternatively, for orientations with fourfold symmetry, different geometric configurations of seed crystals can be used in order to maintain stable symmetrical grain boundaries in many grains when the three grain boundaries converge in one corner. For example, if θ means the angle of divergence between the direction (110) and the primary sides of the hexagon with the main axis (100) and α is the angle at the apex of the interstitial rhombus, as shown in FIG. 6, then all crystalline grains will have a symmetrical grain boundary with respect to direction (110) if α = 90 ° -θ. In this example, all crystalline grains are characterized by the direction of the main axis (100) perpendicular to the plane in which FIG. 6 is depicted. Thus, FIG. 6 is a plan of a portion of a set of seed hex crystals along with rhombic seeds 180, 190 at the bottom of the corresponding crucible, such as in FIGS. 1 and 2. The arrows indicate the orientation of the direction (110) in the silicon crystal in the seeds.

ФИГ.7 представляет собой блок-схему примера способа получения кремния согласно данному изобретению. В соответствии с ФИГ.7 процесс 700 можно начинать с выбора затравочных кристаллов монокристаллического кремния для роста монокристаллического или геометрически упорядоченного поликристаллического кремния и размещения затравочных кристаллов монокристаллического кремния в тигле (стадия 705). Альтернативно, в качестве единственного затравочного кристалла можно использовать один срез или иным способом полученный фрагмент слитка монокристаллического или геометрически упорядоченного поликристаллического кремния. Затем в тигель можно добавить источник кремния (стадия 710). Затем тигель нагревают сверху, в то время как дно тигля охлаждают снизу (пассивно или активно; см. стадию 715). Во время плавления за стадией плавления кремния следят для того, чтобы направлять и регулировать положение границы раздела твердой фазы и жидкости (стадия 720). Стадию плавления кремния продолжают до расплавления части затравочных кристаллов монокристаллического кремния (стадия 725). Как только нужная часть затравочных кристаллов монокристаллического кремния расплавится, стадию плавления заканчивают и начинается стадия роста кристаллов (стадия 730). Рост кристаллов продолжают в тигле в одном направлении и вертикально до завершения кристаллизации кремния (стадия 735). Если затравочные кристаллы расположены для роста геометрически упорядоченного поликристаллического кремния, на стадии кристаллизации 735 образуется слиток геометрически упорядоченного поликристаллического кремния со столбчатыми зернами (стадия 740). Альтернативно, если затравочные кристаллы расположены для роста монокристаллического кремния, на стадии кристаллизации 735 образуется слиток монокристаллического кремния (стадия 745). Наконец, слиток, полученный либо на стадии 740, либо на стадии 745, удаляют для дальнейшей обработки (стадия 750).7 is a flowchart of an example of a method for producing silicon according to this invention. In accordance with FIG. 7, process 700 can be started by selecting seed crystals of single crystal silicon to grow single crystal or geometrically ordered polycrystalline silicon and placing seed crystals of single crystal silicon in a crucible (step 705). Alternatively, as a single seed crystal, a single slice or otherwise obtained fragment of a single-crystal or geometrically ordered polycrystalline silicon ingot can be used. Then, a silicon source can be added to the crucible (step 710). Then, the crucible is heated from above, while the bottom of the crucible is cooled from below (passively or actively; see step 715). During melting, the silicon melting stage is monitored in order to direct and adjust the interface of the solid phase and the liquid (step 720). The silicon melting step is continued until a part of the seed crystals of single crystal silicon is melted (step 725). Once the desired portion of the single crystal silicon seed crystals has melted, the melting step is completed and the crystal growth step begins (step 730). Crystal growth is continued in the crucible in one direction and vertically until the crystallization of silicon is complete (step 735). If the seed crystals are arranged for the growth of geometrically ordered polycrystalline silicon, an ingot of geometrically ordered polycrystalline silicon with columnar grains is formed at crystallization stage 735 (step 740). Alternatively, if the seed crystals are arranged to grow single-crystal silicon, an ingot of single-crystal silicon is formed in the crystallization step 735 (step 745). Finally, the ingot obtained in either step 740 or step 745 is removed for further processing (step 750).

Как показано на ФИГ.8А, источник кремния 200 можно внести в тигель 210, содержащий затравочные кристаллы 220, например, одним из двух способов. В первом из них тигель 210 заполняют доверху твердым источником кремния 200, как правило, в виде кусков обычного размера, и заполненный тигель 210 помещают в аппарат для литья (не показан).As shown in FIG. 8A, the silicon source 200 can be introduced into the crucible 210 containing seed crystals 220, for example, in one of two ways. In the first of these, the crucible 210 is filled to the top with a solid source of silicon 200, usually in the form of pieces of normal size, and the filled crucible 210 is placed in a casting apparatus (not shown).

Как показано на ФИГ.8В, термический профиль в тигле 210 устанавливают так, что верхнюю часть порции кремния в тигле 110 нагревают до плавления, в то время как дно активно или пассивно охлаждают для сохранения твердой фазы затравок 220 на дне тигля 210, т.е. они не всплывают при плавлении сырья 200. Твердый теплопоглотитель 230 находится в контакте с дном тигля 210 для передачи тепла к охлаждаемым водой стенкам. Например, теплопоглотитель 230 может представлять собой твердый блок графита и предпочтительно может иметь такие же измерения, как у дна тигля, или бóльшие. В соответствии с данным изобретением теплопоглотитель может иметь, например, размеры 66 см × 66 см × 20 см, когда используют тигель с поверхностью дна 66 см × 66 см. Предпочтительно боковые стенки тигля 210 совсем не охлаждать при условии, что затравки 220 находятся только на дне тигля 210. Если затравки 220 расположены на дне и стенках тигля 210, то для поддержания нужного термического профиля теплопоглотитель 230 надо помещать как на дне, так и на стенках тигля 210.As shown in FIG. 8B, the thermal profile in the crucible 210 is set so that the upper portion of the portion of silicon in the crucible 110 is heated to melting, while the bottom is actively or passively cooled to maintain the solid phase of the seeds 220 at the bottom of the crucible 210, i.e. . they do not float when the raw materials 200 are melted. The solid heat sink 230 is in contact with the bottom of the crucible 210 to transfer heat to the walls cooled by water. For example, heat sink 230 may be a solid block of graphite, and may preferably have the same dimensions as or larger at the bottom of the crucible. According to the invention, the heat sink may, for example, be 66 cm × 66 cm × 20 cm when a crucible with a bottom surface of 66 cm × 66 cm is used. Preferably, the side walls of the crucible 210 are not cooled at all, provided that the seeds 220 are only on the bottom of the crucible 210. If the seeds 220 are located on the bottom and walls of the crucible 210, then to maintain the desired thermal profile, the heat sink 230 must be placed both on the bottom and on the walls of the crucible 210.

Фазу расплава источника кремния 200 тщательно отслеживают с тем, чтобы контролировать положение границы раздела между расплавленным кремнием и затравочными кристаллами. Предпочтительно плавление 240 (показано на ФИГ.8В) продолжать до тех пор, пока весь источник кремния 200 за исключением затравок 220 полностью расплавится, после чего частично плавят затравочные кристаллы кремния 220. Например, нагревание тщательно регулируют так, чтобы затравки 220 не расплавились полностью, путем поддержания ΔТ на уровне примерно 0.1°С/мин или менее согласно измерениям на внешней поверхности тигля после достижения температуры плавления кремния по всему тиглю. Предпочтительно тщательно регулировать нагрев, поддерживая ΔТ примерно равным 0.05°С/мин или меньше согласно измерениям на внешней поверхности тигля после достижения температуры плавления кремния по всему тиглю. Например, в соответствии с изобретением ΔТ можно измерять на внешней поверхности тигля между тиглем и большим блоком графита и для измерения глубины расплава в расплав 240 вводить погружаемый стержень, чтобы рассчитать долю расплавившихся затравочных кристаллов 220.The melt phase of the silicon source 200 is carefully monitored in order to control the position of the interface between the molten silicon and the seed crystals. Preferably, melting 240 (shown in FIG. 8B) is continued until the entire silicon source 200, with the exception of the seeds 220, is completely melted, after which the silicon seed crystals 220 are partially melted. For example, the heating is carefully controlled so that the seeds 220 do not completely melt. by maintaining ΔT at about 0.1 ° C / min or less according to measurements on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible. It is preferable to carefully control the heating, keeping ΔT approximately equal to 0.05 ° C / min or less according to measurements on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible. For example, in accordance with the invention, ΔT can be measured on the outer surface of the crucible between the crucible and a large block of graphite, and to measure the depth of the melt, an immersion rod is introduced into the melt 240 to calculate the proportion of the molten seed crystals 220.

Как показано на ФИГ.8С, доля 250 иллюстрирует расплавленную часть общей толщины затравок 220, расположенных под расплавом 240. После того как доля 250 затравочных кристаллов 220 под расплавом 240 расплавится, стадию плавления быстро заканчивают и начинают стадию роста кристаллов, в которой нагревание верхней части тигля 210 уменьшают и/или усиливают охлаждение дна рядом с теплопоглотителем 230. В качестве примера этого способа блок-схема, показанная на ФИГ.8D, иллюстрирует плавление доли 250 затравок 220 как функцию времени. Как показано на ФИГ.8D, часть затравок с начальной толщиной слоя 5-6 см постепенно расплавляют до тех пор, пока не останется слоя твердых затравок толщиной менее 2 см. Например, нагрев можно тщательно регулировать таким образом, чтобы затравки 220 не расплавились полностью, путем поддержания ΔТ на уровне примерно 0.1°С/мин или меньше согласно измерению на внешней поверхности тигля (например, термопарой, вмонтированной в блок охлаждения), после достижения температуры плавления кремния по всему тиглю. Предпочтительно контролировать нагрев, поддерживая ΔТ примерно 0.05°С/мин или меньше, согласно измерениям на внешней поверхности тигля после достижения температуры плавления кремния по всему тиглю. В этот момент стадию плавления быстро завершают и начинают стадию роста кристалла, о которой свидетельствует увеличение толщины твердого материала, как показано на ординате схемы.As shown in FIG. 8C, the fraction 250 illustrates the molten portion of the total thickness of the seeds 220 located under the melt 240. After the fraction 250 of the seed crystals 220 under the melt 240 melts, the melting step is quickly completed and the crystal growth stage begins, in which the heating of the upper part crucible 210 reduces and / or enhances bottom cooling near the heat sink 230. As an example of this method, the flowchart shown in FIG. 8D illustrates the melting of a fraction of 250 seeds 220 as a function of time. As shown in FIG. 8D, part of the seeds with an initial layer thickness of 5-6 cm are gradually melted until there is a layer of solid seeds less than 2 cm thick. For example, the heating can be carefully controlled so that the seeds 220 do not completely melt. by maintaining ΔТ at a level of about 0.1 ° C / min or less as measured on the outer surface of the crucible (for example, a thermocouple mounted in the cooling unit), after reaching the melting temperature of silicon throughout the crucible. It is preferable to control the heating by maintaining ΔT of about 0.05 ° C / min or less, as measured on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible. At this point, the melting stage is quickly completed and the stage of crystal growth begins, which is indicated by an increase in the thickness of the solid material, as shown in the ordinate of the diagram.

Затем, как показано на ФИГ.8Е, затравочные кристаллы растут в одном направлении и вертикально в тигле 210, пока кристаллизация кремния не закончится. Цикл литья заканчивается, когда градиент тепла от верхушки до дна тигля 210 выравнивается. Затем весь слиток 260 медленно охлаждают до комнатной температуры. При литье геометрически упорядоченного поликристаллического кремния, как показано на ФИГ.8Е, этот одномерный рост на затравках приводит к зернам 270 в виде столбиков, имеющих в общем случае горизонтальное поперечное сечение по форме такое же, как отдельная затравка 220, на которой он образуется. Таким образом, можно заранее выбрать границы зерен литого геометрического упорядоченного поликристаллического кремния. В этом способе литья применимы любые типы затравок из указанных выше.Then, as shown in FIG. 8E, the seed crystals grow in one direction and vertically in the crucible 210 until the crystallization of silicon is complete. The casting cycle ends when the heat gradient from the top to the bottom of the crucible 210 is leveled. Then, the entire ingot 260 is slowly cooled to room temperature. When casting geometrically ordered polycrystalline silicon, as shown in FIG. 8E, this one-dimensional growth on the seeds leads to the grains 270 in the form of columns having, in the general case, the horizontal cross section in shape is the same as the separate seed 220 on which it is formed. Thus, it is possible to preselect grain boundaries of ordered geometric ordered polycrystalline silicon. In this casting method, any type of seed from the above is applicable.

Альтернативно, для изготовления отливок монокристаллического кремния затравки 220 можно расположить так, чтобы границ зерен не было вообще, что приводит к литому монокристаллическому кремнию. Как показано на ФИГ.8F, доля 250 иллюстрирует долю расплава в общей толщине затравок 220 под расплавом 240. После того как доля 250 затравочных кристаллов 220 под расплавом 240 расплавится, стадию плавления быстро заканчивают и начинают стадию роста кристаллов, в которой нагревание верхушки тигля 210 уменьшают и/или усиливают охлаждение дна рядом с теплопоглотителем 230. Затем, как показано на ФИГ.8G, рост затравочных кристаллов продолжается в одном направлении и вертикально в тигле 210, пока кристаллизация кремния не закончится. Предпочтительная практически плоская граница раздела 285 между твердой фазой и жидкостью растет вверх и в сторону от поверхности дна тигля 210. Цикл литья заканчивается после того, как завершается рост кристаллов, когда термический градиент от верхушки до дна тигля 210 выравнивается. Затем весь слиток 280 медленно охлаждают до комнатной температуры. При литье монокристаллического кремния, как показано на ФИГ.8G, этот одномерный рост на затравках приводит к сплошному твердому массиву литого монокристаллического кремния 290.Alternatively, for the manufacture of single-crystal silicon castings, seeds 220 can be positioned so that there are no grain boundaries at all, which leads to cast single-crystal silicon. As shown in FIG. 8F, the fraction 250 illustrates the fraction of the melt in the total thickness of the seeds 220 under the melt 240. After the fraction 250 of the seed crystals 220 under the melt 240 melts, the melting step is quickly completed and the crystal growth stage is started in which heating of the crucible tip 210 reduce and / or increase cooling of the bottom near the heat sink 230. Then, as shown in FIG. 8G, the growth of seed crystals continues in one direction and vertically in the crucible 210 until the crystallization of silicon is complete. The preferred substantially planar interface 285 between the solid phase and the liquid grows upward and away from the surface of the bottom of the crucible 210. The casting cycle ends after the crystal growth is completed when the thermal gradient from the top to the bottom of the crucible 210 is leveled. Then, the entire ingot 280 is slowly cooled to room temperature. When casting single-crystal silicon, as shown in FIG. 8G, this one-dimensional growth on the seeds leads to a continuous solid mass of cast single-crystal silicon 290.

В другом способе, проиллюстрированном на ФИГ.9, источник кремния 200 можно сначала расплавить в отдельном отсеке или отдельном сосуде для плавления 300. Затравки 220 можно частично расплавить сверху или не стоит их плавить до подачи расплавленного источника кремния 305 или его сливания в тигель 210 через трубу для расплава 310, после чего охлаждение и рост кристаллов проводят, как показано на ФИГ.8B-G. В другом варианте затравочные кристаллы кремния могут быть размещены на стенках тигля 210 (не показаны) и рост затравок может протекать по сторонам тигля, а также на дне тигля 210, как показано выше. Альтернативно, источник кремния 200 плавят в сосуде 300 отдельно от тигля 210 и одновременно тигель 210 нагревают до температуры плавления кремния, причем нагревание регулируют таким образом, чтобы затравочные кристаллы 220 не расплавились полностью. После частичного плавления затравок 220 расплавленное сырье 305 можно перенести из сосуда с расплавом 300 в тигель 210 и начать охлаждение и кристаллизацию. Таким образом, в соответствии с вариантом изобретения часть твердого массива закристаллизованного кремния может включать затравки 220. Альтернативно, затравочные кристаллы можно сохранять в твердом состоянии до подачи расплава. В этом случае расплавленный кремний в сосуде с расплавом 300 нагревают выше температуры плавления, и при введении перегретой жидкости в ней плавится часть затравочных кристаллов.In another method illustrated in FIG. 9, the silicon source 200 can first be melted in a separate compartment or in a separate melting vessel 300. The seeds 220 can be partially melted on top or not worth melting before the molten silicon source 305 is fed or drained into the crucible 210 through a melt pipe 310, after which cooling and crystal growth are carried out as shown in FIG. 8B-G. In another embodiment, the seed crystals of silicon can be placed on the walls of the crucible 210 (not shown) and the growth of seeds can occur on the sides of the crucible, as well as on the bottom of the crucible 210, as shown above. Alternatively, the source of silicon 200 is melted in a vessel 300 separately from the crucible 210 and at the same time, the crucible 210 is heated to the melting temperature of silicon, and the heating is controlled so that the seed crystals 220 are not completely melted. After partial melting of the seeds 220, the molten feed 305 can be transferred from the melt 300 to the crucible 210 and cooling and crystallization can begin. Thus, in accordance with an embodiment of the invention, part of the solidified crystallized silicon massif may include seed 220. Alternatively, seed crystals may be stored in a solid state until the melt is fed. In this case, molten silicon in a vessel with a melt 300 is heated above the melting temperature, and when a superheated liquid is introduced, a part of the seed crystals melts in it.

В двухстадийной установке для изготовления отливок, такой как показанная на ФИГ.9, расплавленное сырье 305 выливают из сосуда с расплавом 300 на затравочные кристаллы 220 и наблюдают их кристаллизацию во время отверждения. Альтернативно, плавку можно проводить в центральном сосуде с расплавом 300, в котором предлагается распределенное расположение тиглей для отверждения, таких как один тигель 210 или несколько аналогичных тиглей (не показаны). В соответствии с вариантами изобретения тигли для отверждения могут содержать затравочные кристаллы 220 на одной или обеих сторонах и на дне тиглей. Преимущества такого подхода включают: разделение систем плавления и отверждения для оптимизации каждой стадии литья; полунепрерывное плавление кремния, когда плавление новой порции материала можно проводить регулярно, что необходимо для поддержания подачи в тигель; удаление шлака с кремния сверху тигля (и потенциально очищение кремния на дне), в то время как в установку для отверждения подается расплав из середины расплава, что повышает чистоту исходного кремния, и возможность установления равновесия между сосудом с расплавом 300 и расплавленным сырьем 305, в результате чего он перестает быть заметным источником примесей.In a two-stage casting plant, such as that shown in FIG. 9, molten feed 305 is poured from the molten vessel 300 onto seed crystals 220 and crystallization is observed during curing. Alternatively, smelting can be carried out in a central vessel with a melt 300, in which a distributed arrangement of curing crucibles such as one crucible 210 or several similar crucibles (not shown) is proposed. In accordance with embodiments of the invention, curing crucibles may contain seed crystals 220 on one or both sides and on the bottom of the crucibles. Advantages of this approach include: separation of melting and curing systems to optimize each casting stage; semi-continuous melting of silicon, when the melting of a new portion of the material can be carried out regularly, which is necessary to maintain the flow into the crucible; removing slag from silicon on top of the crucible (and potentially purifying silicon at the bottom), while the melt from the middle of the melt is fed into the curing unit, which increases the purity of the initial silicon, and the possibility of establishing equilibrium between the vessel with the melt 300 and the molten feed 305, as a result, it ceases to be a noticeable source of impurities.

Таким образом, после того как слиток 260 или 280 был изготовлен одним из описанных выше способов, полученный слиток можно обрабатывать дальше, например отрезать дно или другую часть слитка и использовать ее в качестве затравочного монокристалла в последующих циклах литья для получения массива монокристаллического кремния, почти монокристаллического кремния или геометрически упорядоченного поликристаллического кремния в соответствии с настоящим изобретением, причем размер и форма такого затравочного монокристалла будут такими же, как у дна тигля, используемого для последующего литья, а остальной слиток можно нарезать на блоки и пластины для использования в фотоэлектрических элементах. Альтернативно, весь слиток можно разрезать, например, на горизонтальные листы для использования в качестве затравочных кристаллов в последующих опытах и во многих других установках для литья.Thus, after the ingot 260 or 280 was made by one of the methods described above, the obtained ingot can be processed further, for example, to cut the bottom or other part of the ingot and use it as a seed single crystal in subsequent casting cycles to obtain an array of single-crystal silicon, almost single-crystal silicon or geometrically ordered polycrystalline silicon in accordance with the present invention, the size and shape of such a seed single crystal being the same as the bottom of the crucible used for subsequent casting, and the rest of the ingot can be cut into blocks and plates for use in photovoltaic cells. Alternatively, the entire ingot can be cut, for example, into horizontal sheets for use as seed crystals in subsequent experiments and in many other casting plants.

Источник кремния, используемый в способах по вариантам данного изобретения, может содержать одну или несколько легирующих добавок, таких как: бор, алюминий, литий, галлий, фосфор, сурьма, мышьяк и висмут. Общее количество такой легирующей добавки может составлять примерно от 0.01 частей на миллион в атомных процентах (ppma) до примерно 2 ppma. Предпочтительно, чтобы количество такой легирующей добавки в кремнии было таким, чтобы пластина из кремния имела сопротивление примерно 0.1-50 Ом·см, предпочтительно примерно 0.5-5.0 Ом·см.The silicon source used in the methods of the embodiments of the present invention may contain one or more dopants, such as boron, aluminum, lithium, gallium, phosphorus, antimony, arsenic and bismuth. The total amount of such a dopant can be from about 0.01 ppm in atomic percent (ppma) to about 2 ppma. Preferably, the amount of such a dopant in silicon is such that the silicon wafer has a resistance of about 0.1-50 Ohm · cm, preferably about 0.5-5.0 Ohm · cm.

Таким образом, в соответствии с настоящим изобретением кремний может быть в виде массива литого сплошного монокристаллического кремния, литого почти кристаллического кремния или литого сплошного геометрически упорядоченного поликристаллического кремния, который предпочтительно не содержит или практически не содержит радиально распределенных дефектов, таких как OSF и/или спиральные дефекты, и предпочтительно, чтобы по меньшей мере два измерения массива составляли по меньшей мере примерно 10 см, предпочтительно по меньшей мере примерно 20 см, более предпочтительно по меньшей мере 30 см, еще более предпочтительно по меньшей мере 40 см, еще более предпочтительно по меньшей мере 50 см, еще более предпочтительно по меньшей мере 60 см и наиболее предпочтительно по меньшей мере примерно 70 см. Наиболее предпочтительно, чтобы третье измерение такого массива кремния составляло по меньшей мере примерно 5 см, более предпочтительно по меньшей мере примерно 15 см и наиболее предпочтительно по меньшей мере примерно 20 см. Массив кремния может иметь вид одного отдельного куска, или он может содержаться или быть окруженным, полностью или частично, другим кремнием. Массив кремния может иметь предпочтительно по меньшей мере два измерения, каждое из них такое же по величине, как внутренние размеры сосуда для литья. Как описано здесь, варианты изобретения можно использовать для получения больших массивов монокристаллического кремния, почти кристаллического кремния или геометрически упорядоченного поликристаллического кремния с помощью простого и эффективного по стоимости способа литья.Thus, in accordance with the present invention, the silicon may be in the form of an array of cast solid single crystal silicon, cast almost crystalline silicon, or cast solid geometrically ordered polycrystalline silicon, which preferably does not contain or practically does not contain radially distributed defects, such as OSF and / or spiral defects, and preferably at least two dimensions of the array are at least about 10 cm, preferably at least about 20 cm, more preferably at least 30 cm, even more preferably at least 40 cm, even more preferably at least 50 cm, even more preferably at least 60 cm and most preferably at least about 70 cm. Most preferably, so that the third dimension of such a silicon array is at least about 5 cm, more preferably at least about 15 cm, and most preferably at least about 20 cm. The silicon array may be in the form of one single piece, or it may contain stick or be surrounded, in whole or in part, by other silicon. The silicon array may preferably have at least two dimensions, each of which is the same size as the internal dimensions of the casting vessel. As described herein, embodiments of the invention can be used to produce large amounts of single-crystal silicon, near-crystalline silicon, or geometrically ordered polycrystalline silicon using a simple and cost-effective casting method.

Далее следуют примеры экспериментальных результатов в соответствии с вариантами данного изобретения. Эти примеры представлены только для иллюстрации вариантов изобретения, и никоим образом не следует считать, что они ограничивают объем изобретения.The following are examples of experimental results in accordance with variants of the present invention. These examples are presented only to illustrate embodiments of the invention, and in no way should be considered that they limit the scope of the invention.

Пример 1Example 1

Приготовление затравок: Слиток полученного от МЕМС, Inc. чистого (монокристаллического) кремния, изготовленного по методу Чохральского (CZ) и содержащего 0.3 ppma бора, разрезали по длине, используя алмазную ленточную пилу, так что получилось квадратное поперечное сечение со стороной 14 см. Полученный блок монокристаллического кремния разрезали той же пилой через поперечное сечение на листы толщиной примерно 2-3 см. Эти листы использовали как затравочные кристаллы монокристаллического кремния, или «затравки». Ориентация кристаллографической оси (100) слитка кремния при этом сохраняется. Полученные листы монокристалла кремния затем разместили на дне кварцевого тигля таким образом, чтобы направление (100) было направлено вверх, а направление (110) было параллельно одной стороне тигля. Кварцевый тигель имеет квадратное поперечное сечение со стороной 68 см, глубиной примерно 40 см и толщиной стенок примерно 1.8 см. Листы расположили на дне тигля так, чтобы их длинный размер был параллелен дну тигля и их стороны касались друг друга с образованием одного заполненного слоя таких листов на дне тигля.Seed preparation: An ingot obtained from MEMS, Inc. Pure (single-crystal) silicon manufactured by the Czochralski method (CZ) and containing 0.3 ppma boron was cut in length using a diamond band saw, so that a square cross section with a side of 14 cm was obtained. The obtained block of single-crystal silicon was cut with the same saw through a cross section on sheets with a thickness of about 2-3 cm. These sheets were used as seed crystals of single crystal silicon, or "seed". The orientation of the crystallographic axis (100) of the silicon ingot is retained. The resulting silicon single crystal sheets were then placed on the bottom of the quartz crucible so that the direction (100) was directed upward and the direction (110) was parallel to one side of the crucible. A quartz crucible has a square cross section with a side of 68 cm, a depth of about 40 cm and a wall thickness of about 1.8 cm. The sheets are placed on the bottom of the crucible so that their long size is parallel to the bottom of the crucible and their sides touch each other to form one filled layer of such sheets at the bottom of the crucible.

Литье: Затем тигель заполнили при комнатной температуре твердым источником кремния общей массой 265 кг. Заполненный тигель затем поместили в установку литья с in-situ плавлением/направленным отверждением, предназначенной для литья поликристаллического кремния. Плавление проводили нагреванием с помощью резистивных электронагревателей до примерно 1550°С, и нагреватели были расположены таким образом, что нагрев шел сверху и тепловой поток отводили от дна через 6 см просвет в теплоизолирующем материале. Такая конфигурация обеспечивала плавление в направлении сверху-вниз ко дну тигля. Пассивное охлаждение через дно приводило к тому, что затравочные кристаллы оставались в твердом состоянии при температуре плавления, что определяли с помощью термопары. Степень плавления определяли кварцевым стержнем, который погружали в расплав каждые десять минут. Для определения высоты оставшегося твердого материала высоту стержня сравнивали с измерением на пустом тигле в той же установке. С помощью измерений на стержне сначала сырье плавили и затем фазу расплава выдерживали до тех пор, пока высота затравочных кристаллов не достигала примерно 1.5 см. В этот момент интенсивность нагрева уменьшали до достижения температуры 1500°С, в то время как тепловой поток со дна увеличивали путем открывания просвета в теплоизоляторе до 12 см. Один-два миллиметра затравочных кристаллов плавились до начала отверждения, как показывали замеры на стержне. Затем происходил рост монокристаллической затравки до конца стадии отверждения. Стадию роста и остальную часть цикла литья проводили при нормальных параметрах до выравнивания теплового градиента в направлении сверху-вниз и затем весь слиток медленно охлаждали до комнатной температуры. Полученный продукт литья имел вид слитка размером 66 см × 66 см × 24 см, центральная часть которого в виде горизонтального поперечного сечения размером 50 см × 50 см представляла собой монокристаллический кремний сверху донизу. Монокристаллическая структура кремния была видна при визуальном обследовании поверхности слитка. Кроме того, травление кремния щелочью, способное очертить границы зерен, также подтвердило отсутствие границ зерен в полученном материале. В среднем объемное легирование составило 1.2 Ом·см, и эффективность по току фотоэлектрических элементов, изготовленных из этого кремния, была равна 16.0%.Casting: The crucible was then filled at room temperature with a solid source of silicon with a total weight of 265 kg. The filled crucible was then placed in an in situ melting / directional curing casting machine for casting polycrystalline silicon. Melting was carried out by heating using resistive electric heaters to about 1550 ° C, and the heaters were arranged so that the heating came from above and the heat flux was diverted from the bottom through a 6 cm gap in the heat-insulating material. This configuration ensured melting from top to bottom to the bottom of the crucible. Passive cooling through the bottom led to the fact that the seed crystals remained in the solid state at the melting temperature, which was determined using a thermocouple. The degree of melting was determined by a quartz rod, which was immersed in the melt every ten minutes. To determine the height of the remaining solid material, the height of the rod was compared with the measurement on an empty crucible in the same setup. Using measurements on the rod, the raw material was first melted and then the melt phase was kept until the height of the seed crystals reached about 1.5 cm. At this point, the heating intensity was reduced until a temperature of 1500 ° C was reached, while the heat flux from the bottom was increased by openings of the lumen in the heat insulator up to 12 cm. One to two millimeters of seed crystals melted before curing began, as measurements on the rod showed. Then there was a growth of single crystal seed until the end of the curing stage. The growth stage and the rest of the casting cycle were carried out at normal parameters until the thermal gradient was equalized in the top-down direction, and then the entire ingot was slowly cooled to room temperature. The obtained casting product had the form of an ingot of 66 cm × 66 cm × 24 cm in size, the central part of which in the form of a horizontal cross section of 50 cm × 50 cm in size was monocrystalline silicon from top to bottom. The single-crystal structure of silicon was visible by visual inspection of the surface of the ingot. In addition, alkali etching of silicon, capable of delineating grain boundaries, also confirmed the absence of grain boundaries in the resulting material. On average, the volume doping was 1.2 Ohm · cm, and the current efficiency of the photovoltaic cells made of this silicon was 16.0%.

В других опытах по литью, проведенных согласно этому примеру, было установлено, что полученный слиток представлял собой контактно согласованный кристалл кремния, который содержал более мелкие кристаллы кремния с другими ориентациями кристаллов, или это был массив монокристаллического кремния с соседними областями поликристаллического кремния.In other casting experiments carried out according to this example, it was found that the obtained ingot was a contact-matched silicon crystal that contained smaller silicon crystals with different crystal orientations, or it was an array of single-crystal silicon with neighboring regions of polycrystalline silicon.

Пример 2Example 2

Приготовление затравки: Затравки получали, как в примере 1, за исключением того, что затравочные кристаллы монокристаллического кремния были нарезаны так, что у половины затравочных кристаллов направление (110) составляло угол 45 градусов со стороной квадрата затравочных кристаллов, в то время как у другой половины этот угол составлял примерно 20 градусов. Квадратные кусочки уложили слоем на дно тигля в шахматном порядке, чередуя две разные ориентации затравок, т.е. с направлением (110) под углом 45 градусов и 20 градусов к ориентации сторон тигля. Относительно друг друга затравки были повернуты либо на 25 градусов, либо на 155 градусов. Однако из-за несогласования размеров затравок квадратной формы в слое затравок оставались непокрытые места. Тигель имел измерения примерно 33 см на сторонах квадрата и примерно 22 см в высоту.Preparation of the seed: The seeds were obtained as in Example 1, except that the seed crystals of single crystal silicon were cut so that for half of the seed crystals the direction (110) was 45 degrees with the square side of the seed crystals, while in the other half this angle was about 20 degrees. The square pieces were layered on the bottom of the crucible in a checkerboard pattern, alternating two different orientations of the seeds, i.e. with a direction of (110) at an angle of 45 degrees and 20 degrees to the orientation of the sides of the crucible. Relative to each other, the seeds were rotated either 25 degrees or 155 degrees. However, due to a mismatch in the size of the square-shaped seeds in the seed layer, uncovered spots remained. The crucible had dimensions of approximately 33 cm on the sides of the square and approximately 22 cm in height.

Литье: Тигель, содержащий затравочные кристаллы, и отдельный тигель, содержащий все 56 кг кусков источника кремния, были помещены в двухстадийную установку литья по способу Ubiquitous Casting Process (UCP). Тигель-приемник (с затравочными кристаллами внутри) нагрели до температуры плавления кремния, но не расплавили их полностью. Кремний в другом тигле расплавили с помощью резистивных графитовых нагревателей до температуры по меньшей мере на 50°С выше температуры плавления кремния и затем вылили в тигель-приемник. В этот момент сразу же начиналось отверждение, и тепло отводили со дна тигеля-приемника для обеспечения направленного отверждения и роста кристаллов на затравках. Стандартный цикл роста укоротили с учетом массы уже отвержденного материала на затравочных кристаллах. Таким образом, вместо времени, необходимого для отверждения всех 66 кг (10 кг затравочных кристаллов и 56 кг источника кремния) до начала охлаждения, было предоставлено время для отверждения 56 кг расплавленного кремния, чтобы избежать потерь энергии на нагрев. Продуктом этого опыта был слиток кремния с большими, обычно столбчатыми зернами, имеющими квадратное поперечное сечение с формой и размерами, которые остались близкими к размерам первоначальных затравочных кристаллов на наружной поверхности, на которых они образуются. В некоторых случаях положение боковых границ зерен смещалось по мере роста.Casting: A crucible containing seed crystals and a separate crucible containing all 56 kg of pieces of a silicon source were placed in a two-stage casting plant using the Ubiquitous Casting Process (UCP). The receiver crucible (with seed crystals inside) was heated to the melting temperature of silicon, but they were not completely melted. Silicon in another crucible was melted using resistive graphite heaters to a temperature of at least 50 ° C above the melting temperature of silicon and then poured into a receiving crucible. At this point, curing immediately began, and heat was removed from the bottom of the receiver crucible to provide directional curing and crystal growth on the seeds. The standard growth cycle was shortened taking into account the mass of already cured material on the seed crystals. Thus, instead of the time needed to cure all 66 kg (10 kg of seed crystals and 56 kg of a silicon source) before cooling began, time was given to cure 56 kg of molten silicon to avoid heating energy loss. The product of this experiment was an ingot of silicon with large, usually columnar grains having a square cross-section with a shape and size that remained close to the size of the initial seed crystals on the outer surface on which they are formed. In some cases, the position of the lateral grain boundaries shifted with growth.

Пример 3Example 3

Приготовление затравочных кристаллов: Затравки готовили из 23 кг квадратных пластинок (100), уложенных на дно тигля так, что была покрыта площадь 63 см × 63 см при толщине от 3 см в центре до 1.8 см по сторонам. Все пластинки были расположены так, что направления (110) составляли угол 45° со стенками тигля.Preparation of seed crystals: Seeds were prepared from 23 kg of square plates (100) laid on the bottom of the crucible so that an area of 63 cm × 63 cm was covered with a thickness of 3 cm in the center to 1.8 cm on the sides. All plates were arranged so that (110) directions made an angle of 45 ° with the crucible walls.

Литье: Тигель, содержащий затравочные кристаллы, заполнили дополнительным количеством источника кремния в кусках, всего 242 кг, представляющим собой смесь собственно кремния, кремния, возвращенного от предыдущих слитков, и кремния удвоенной стоимости с удельным сопротивлением p-типа более 9 Ом·см. Тигель с загруженным кремнием поместили в печь одностадийного направленного отверждения. Тигель (с затравочными кристаллами) нагрели до температуры 1550°С, в то время как дно охлаждали путем увеличения просвета в теплоизоляторе до 12 см. Во время плавления граница раздела твердой фазы и жидкости оставалась практически плоской, так что в конце плавления затравочные кристаллы не были расплавлены. За толщиной слоя кремния следили с помощью погружаемого кварцевого стержня. Когда толщина в центре составила 2.5 см, стадию плавления остановили, температуру нагревателя снизили до 1440°С и просвет в теплоизоляторе увеличили до 15 см. С того момента, как начиналось изменение фазы расплава, скорость подъема температуры поддерживали на уровне 0.1°С/мин или ниже, определяя температуру на внешней поверхности тигля после того, как температура плавления кремния устанавливалась по всему тиглю. Затем процесс отверждения довели до конца при почти постоянной мощности нагревателя, поддерживаемой до конца роста кристаллов. После окончания роста кристаллов температура слитка закристаллизованного кремния выравнивалась и затем снижалась по всему слитку до комнатной температуры. После извлечения слитка из тигля дно слитка отрезали одним большим куском для дальнейшего использования в качестве затравки в другом последующем опыте, а оставшуюся часть слитка нарезали на квадратные блоки со стороной 12.5 см для дальнейшей обработки. Способ с успехом обеспечивает рост монокристаллов практически на всем поперечном сечении слоя затравочных кристаллов вплоть до верхушки слитка. Монокристалличность была очевидна при рассмотрении среза кремния.Casting: A crucible containing seed crystals was filled with an additional amount of a silicon source in pieces, only 242 kg, which is a mixture of silicon itself, silicon returned from previous ingots, and doubled silicon with a p-type resistivity of more than 9 Ohm · cm. A silicon-loaded crucible was placed in a single-stage directional curing oven. The crucible (with seed crystals) was heated to a temperature of 1550 ° C, while the bottom was cooled by increasing the clearance in the heat insulator to 12 cm. During melting, the interface between the solid phase and the liquid remained almost flat, so that at the end of melting the seed crystals were not melted. The thickness of the silicon layer was monitored using an immersed quartz rod. When the thickness in the center was 2.5 cm, the melting stage was stopped, the temperature of the heater was reduced to 1440 ° C and the clearance in the heat insulator was increased to 15 cm. From the moment the melt phase began to change, the temperature rise rate was maintained at 0.1 ° C / min or below, determining the temperature on the outer surface of the crucible after the melting temperature of silicon was established throughout the crucible. Then, the curing process was brought to an end with an almost constant heater power, maintained until the end of crystal growth. After the end of the crystal growth, the temperature of the crystallized silicon ingot was leveled off and then decreased throughout the ingot to room temperature. After removing the ingot from the crucible, the bottom of the ingot was cut in one large piece for further use as a seed in another subsequent experiment, and the remainder of the ingot was cut into square blocks with a side of 12.5 cm for further processing. The method successfully ensures the growth of single crystals over practically the entire cross section of the seed crystal layer up to the top of the ingot. Monocrystallinity was evident when considering a silicon slice.

В других опытах по литью согласно этому примеру было найдено, что полученный литой кремний представлял собой контактно согласованный кристалл кремния, содержащий более мелкие кристаллы кремния с другими ориентациями, или массив монокристаллического кремния с соседними областями поликристаллического кремния.In other casting experiments according to this example, it was found that the obtained cast silicon was a contact matched silicon crystal containing smaller silicon crystals with different orientations, or an array of single-crystal silicon with neighboring regions of polycrystalline silicon.

Пластины, изготовленные из кремния в соответствии с этими вариантами изобретения, достаточно тонкие, и их можно использовать в фотоэлектрических элементах. Пластины могут быть n-типа или p-типа. Например, пластины могут иметь толщину 10-700 мкм. Кроме того, предпочтительно, чтобы пластины, используемые в фотоэлектрических элементах, имели диффузионную длину (Lp), которая превышает толщину пластины (t). Например, отношение Lp к t составляет по меньшей мере 0.5. Оно может быть равно, например, по меньшей мере примерно 1.1 или по меньшей мере примерно 2. Диффузионная длина является средним расстоянием, на которое неосновные носители заряда (такие, как электроны в материале p-типа) могут диффундировать до рекомбинации с большинством носителей (дырками в материале p-типа). Величина Lp относится ко времени жизни меньшинства носителей τ по соотношению Lp=(Dτ)1/2, где D является константой диффузии. Диффузионную длину можно определить многими методами, такими как измерение тока, индуцированного протонным пучком, или методом фотозарядки поверхности. См. описание определения диффузионной длины, например, в книге «Основы солнечных батарей», "Fundamentals of Solar Cells", A.Fahrenbruch and R.Bube, Academic Press, 1983, p.90-102.The wafers made of silicon in accordance with these embodiments of the invention are quite thin and can be used in photovoltaic cells. The plates may be n-type or p-type. For example, the plates may have a thickness of 10-700 microns. In addition, it is preferable that the plates used in the photovoltaic cells have a diffusion length (L p ) that is greater than the thickness of the plate (t). For example, the ratio of L p to t is at least 0.5. It can be, for example, at least about 1.1 or at least about 2. The diffusion length is the average distance over which minority carriers (such as electrons in p-type material) can diffuse before recombination with most carriers (holes) in p-type material). The value of L p refers to the lifetime of a minority of carriers τ in the relation L p = (Dτ) 1/2 , where D is the diffusion constant. The diffusion length can be determined by many methods, such as measuring the current induced by a proton beam, or by photo-charging the surface. See the description of the definition of diffusion length, for example, in the book Fundamentals of Solar Cells, A. Fahrenbruch and R. Bube, Academic Press, 1983, p.90-102.

Пластины могут иметь ширину примерно 100-600 мм. Предпочтительно, чтобы пластины имели по меньшей мере одно измерение по меньшей мере примерно 50 мм. Пластины, изготовленные из кремния согласно настоящему изобретению, и, следовательно, фотоэлектрические элементы, изготовленные по данному изобретению, могут иметь величину поверхности примерно 50-3600 см2. Предпочтительно, чтобы передняя поверхность пластины была текстурирована. Например, пластина может быть текструрирована путем химического травления, плазменного травления, а также лазерного или механического гравирования. При использовании пластины с ориентацией оси (100) пластину можно травить с образованием анизотропно текстурированной поверхности путем обработки пластины водным раствором основания, такого как гидроксид натрия, при повышенной температуре, например примерно 70-90°С, в течение примерно 10-120 мин. Водный раствор может содержать спирт, например изопропиловый спирт.The plates may have a width of about 100-600 mm. Preferably, the plates have at least one dimension of at least about 50 mm. The wafers made of silicon according to the present invention, and therefore the photovoltaic cells made according to this invention, can have a surface value of about 50-3600 cm 2 . Preferably, the front surface of the plate is textured. For example, a wafer may be textured by chemical etching, plasma etching, and laser or mechanical engraving. When using a plate with a (100) axis orientation, the plate can be etched to form an anisotropically textured surface by treating the plate with an aqueous solution of a base, such as sodium hydroxide, at an elevated temperature, for example about 70-90 ° C, for about 10-120 minutes. The aqueous solution may contain alcohol, for example isopropyl alcohol.

Таким образом, солнечные батареи можно изготовить, используя пластины, полученные из слитков кремния согласно вариантам данного изобретения путем нарезания твердого массива литого кремния с образованием по меньшей мере одной пластины; необязательно очистки поверхности пластины; необязательно проведения стадии текстурирования поверхности; формирования p-n перехода, например, путем легирования поверхности; необязательно нанесения противоотражательного покрытия на поверхность; необязательно образования по меньшей мере одного слоя, выбранного из тыльной области, и пассивирующего слоя, например, с помощью стадии спекания с алюминием и формирования электропроводящих контактов на пластине. Пассивирующий слой представляет собой слой, который является границей раздела с чистой поверхностью пластины, который фиксирует свободные связи атомов на поверхности. Примеры пассивирующих слоев на кремнии включают нитрид кремния, диоксид кремния и аморфный кремний. Этот слой обычно тоньше одного микрона и является либо прозрачным для света, либо действует как противоотражательный слой.Thus, solar cells can be manufactured using wafers made from silicon ingots according to embodiments of the present invention by cutting a solid cast silicon array to form at least one wafer; optionally cleaning the surface of the plate; optionally conducting a surface texture step; forming a pn junction, for example, by doping a surface; optionally applying an antireflection coating to the surface; optionally forming at least one layer selected from the back region and a passivating layer, for example, using the stage of sintering with aluminum and the formation of electrically conductive contacts on the plate. A passivating layer is a layer that is an interface with a clean plate surface that captures the free bonds of atoms on the surface. Examples of passivating layers on silicon include silicon nitride, silicon dioxide, and amorphous silicon. This layer is usually thinner than one micron and is either transparent to light or acts as an antireflection layer.

В типичном и общем способе изготовления фотоэлектрического элемента с использованием, например, кремниевой пластины p-типа пластина контактирует одной стороной с подходящей n-легирующей добавкой с образованием слоя эмиттера и p-n перехода спереди или на светоприемной стороне пластины. Обычно слой n-типа или слой эмиттера образуется при нанесении сначала n-легирующей добавки на переднюю поверхность пластины p-типа по методике, обычно используемой в данной области, такой как химическое или физическое нанесение, и после такого нанесения n-легирующую добавку, например фосфор, перемещают на переднюю поверхность кремниевой пластины для дальнейшей диффузии n-легирующей добавки вглубь поверхности пластины. Эту стадию «перемещения» обычно осуществляют путем воздействия на пластину высоких температур. Таким образом, р-n переход происходит в граничной области между слоем n-типа и субстратом p-типа кремниевой пластиной. Поверхность пластины перед введением фосфора или другой легирующей добавки с образованием слоя эмиттера можно текстурировать. Для дальнейшего повышения поглощения света необязательное противоотражательное покрытие, например, из нитрида кремния, обычно можно нанести на переднюю поверхность пластины, что приводит иногда к одновременной пассивации поверхности или объема.In a typical and general method for manufacturing a photovoltaic cell using, for example, a p-type silicon wafer, the wafer contacts one side with a suitable n-dopant to form an emitter layer and a pn junction in front or on the light receiving side of the wafer. Typically, an n-type layer or an emitter layer is formed by first applying an n-dopant to the front surface of a p-type plate according to a technique commonly used in the art, such as chemical or physical deposition, and after such an application an n-dopant, for example phosphorus , move to the front surface of the silicon wafer for further diffusion of the n-dopant into the surface of the wafer. This "moving" stage is usually carried out by exposing the plate to high temperatures. Thus, the pn junction occurs in the boundary region between the n-type layer and the p-type substrate with a silicon wafer. The surface of the plate before the introduction of phosphorus or other dopants to form an emitter layer can be textured. To further increase light absorption, an optional antireflection coating, such as silicon nitride, can usually be applied to the front surface of the wafer, which sometimes leads to simultaneous passivation of the surface or volume.

Для использования электрического потенциала, возникающего при взаимодействии p-n перехода со световой энергией, в фотоэлектрическом элементе обычно создают проводящий передний электрический контакт на передней стороне пластины и проводящий обратный электрический контакт на задней стороне пластины, хотя оба контакта могут быть позади пластины. Такие контакты обычно изготавливают из одного или нескольких металлов с высокой электропроводностью, и поэтому они обычно являются непрозрачными.To exploit the electrical potential arising from the interaction of the pn junction with light energy, a conductive front electrical contact on the front side of the wafer and a conductive electrical reverse contact on the back side of the wafer are usually created in the photovoltaic cell, although both contacts can be behind the wafer. Such contacts are usually made of one or more metals with high electrical conductivity, and therefore they are usually opaque.

Таким образом, солнечные батареи в соответствии с вариантами, описанными выше, могут содержать пластину, изготовленную из массива сплошного монокристаллического кремния или почти монокристаллического кремния, не содержащего или практически не содержащего радиально распределенных дефектов, причем массив может быть таким, как описано выше, и, например, иметь по меньшей мере два измерения, каждое по меньшей мере примерно по 25 см, и третье измерение по меньшей мере примерно 20 см; p-n переход в пластине; необязательное противоотражательное покрытие на поверхности пластины; предпочтительно иметь по меньшей мере один слой, выбранный из тыльной области, и пассивирующий слой; и электропроводящие контакты на пластине, причем массив может не содержать или практически не содержать спиральных дефектов и не содержать или практически не содержать OSF-дефектов.Thus, solar cells in accordance with the options described above may contain a plate made of an array of solid monocrystalline silicon or almost monocrystalline silicon that does not contain or practically does not contain radially distributed defects, and the array may be as described above, and, for example, have at least two dimensions, each of at least about 25 cm, and a third measurement of at least about 20 cm; pn junction in the plate; optional anti-reflection coating on the surface of the plate; it is preferable to have at least one layer selected from the back region and a passivation layer; and electrically conductive contacts on the plate, and the array may or may not contain spiral defects and not contain or practically no OSF defects.

Кроме того, солнечные батареи в соответствии с вариантами, описанными выше, могут содержать пластину, полученную из массива сплошного геометрически упорядоченного поликристаллического кремния, причем массив имеет предварительно определенное расположение ориентации зерен, предпочтительно такое, при котором направление главной оси перпендикулярно поверхности массива, а массив предпочтительно также имеет по меньшей мере два измерения, каждое предпочтительно по меньшей мере примерно по 10 см; p-n переход в пластине; необязательное противоотражательное покрытие на поверхности пластины, предпочтительно содержащее по меньшей мере один слой, выбранный из тыльной области, и пассивирующий слой, и электропроводящие контакты на пластине, причем геометрически упорядоченный поликристаллический кремний включает зерна кремния со средним размером поперечного сечения зерен кристаллов примерно 0.5-30 см, а массив может не содержать или практически не содержать спиральных дефектов и не содержать или практически не содержать OSF-дефектов.In addition, solar cells in accordance with the options described above may contain a plate obtained from an array of solid geometrically ordered polycrystalline silicon, the array having a predetermined grain orientation, preferably such that the direction of the main axis is perpendicular to the surface of the array, and the array is preferably also has at least two dimensions, each preferably at least about 10 cm; pn junction in the plate; an optional antireflection coating on the wafer surface, preferably containing at least one layer selected from the back region, and a passivating layer, and electrically conductive contacts on the wafer, the geometrically ordered polycrystalline silicon comprising silicon grains with an average crystal grain cross section of about 0.5-30 cm , and the array may or may not contain spiral defects and may or may not contain OSF defects.

Специалистам в данной области будет очевидно, что в раскрытые структуры и способы можно внести различные модификации и вариации, не отклоняясь от объема или духа изобретения. Например, раскрытые способы получения монокристаллического кремния применимы также для получения почти монокристаллического кремния или их комбинаций. Кроме того, хотя здесь был описан способ литья кремния, можно отливать и другие полупроводниковые материалы, и неметаллические кристаллические материалы, не отклоняясь от объема и духа изобретения. Например, изобретатель имел в виду литье других материалов в соответствии с вариантами изобретения, таких как арсенид галлия, кремний-германий, оксид алюминия, нитрид галлия, оксид цинка, арсенид галлия-индия, антимонид индия, германий, оксиды иттрия-бария, оксиды лантанидов, оксид магния и другие полупроводники, оксиды и интерметаллиды с жидкой фазой. Другие варианты изобретения будут очевидны специалистам в данной области из рассмотрения описания и практики раскрытого здесь изобретения. Полагаем, что описания и примеры являются только примерами, а объем и сущность изобретения показаны в его формуле.It will be apparent to those skilled in the art that various modifications and variations can be made to the disclosed structures and methods without departing from the scope or spirit of the invention. For example, the disclosed methods for producing monocrystalline silicon are also applicable for the production of almost monocrystalline silicon or combinations thereof. In addition, although a silicon casting method has been described herein, other semiconductor materials and non-metallic crystalline materials can be cast without deviating from the scope and spirit of the invention. For example, the inventor meant casting other materials in accordance with embodiments of the invention, such as gallium arsenide, silicon germanium, aluminum oxide, gallium nitride, zinc oxide, gallium indium arsenide, indium antimonide, germanium, yttrium barium oxides, lanthanide oxides , magnesium oxide and other semiconductors, oxides and intermetallic compounds with a liquid phase. Other embodiments of the invention will be apparent to those skilled in the art from consideration of the description and practice of the invention disclosed herein. We believe that the descriptions and examples are only examples, and the scope and essence of the invention are shown in its formula.

Claims (34)

1. Способ получения литого кремния, включающий:
приведение расплавленного кремния в контакт по меньшей мере с одним затравочным кристаллом кремния в сосуде, имеющем одну или несколько боковых стенок, нагретых по меньшей мере до температуры плавления кремния, и по меньшей мере одну охлаждаемую стенку; и
образование твердого массива монокристаллического кремния необязательно по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния при регулировании кристаллизации, причем образование массива включает формирование границы раздела твердого тела с жидкостью по ребру расплавленного кремния, которая по меньшей мере сначала параллельна по меньшей мере одной охлаждаемой стенке, и граница раздела регулируется во время охлаждения таким образом, что она перемещается в направлении, при котором увеличивается расстояние между расплавленным кремнием и по меньшей мере одной охлаждаемой стенкой.
1. The method of producing cast silicon, including:
bringing molten silicon into contact with at least one seed silicon crystal in a vessel having one or more side walls heated at least to the melting temperature of silicon and at least one cooled wall; and
the formation of a solid array of single-crystal silicon, optionally with at least two measurements, each of at least about 10 cm, by cooling the molten silicon while controlling crystallization, the formation of the array including the formation of a solid-liquid interface at the edge of the molten silicon, which is at least first parallel to at least one cooled wall, and the interface is adjusted during cooling so that it moves in the direction n and wherein the increasing the distance between the molten silicon and at least one cooled wall.
2. Способ по п.1, в котором по меньшей мере один затравочный кристалл кремния помещают на дно тигля, и в котором при охлаждении граница раздела твердой фазы и жидкости перемещается в направлении от дна тигля при сохранении ребра, параллельного по меньшей мере одной охлаждаемой стенке.2. The method according to claim 1, in which at least one seed crystal of silicon is placed on the bottom of the crucible, and in which, when cooled, the interface between the solid phase and the liquid moves in the direction from the bottom of the crucible while maintaining the rib parallel to at least one cooled wall . 3. Способ по п.2, включающий такое расположение по меньшей мере одного затравочного кристалла, что основная ось кристалла направлена перпендикулярно дну тигля.3. The method according to claim 2, including the location of at least one seed crystal such that the main axis of the crystal is directed perpendicular to the bottom of the crucible. 4. Способ по п.2, в котором расплавленный кремний размещают таким образом, что источник кремния плавят в контейнере для плавления, отдельном от тигля, затем нагревают тигель и кремний до температуры плавления кремния, регулируют нагревание таким образом, чтобы по меньшей мере один затравочный кристалл в тигле не расплавился полностью, и переносят расплавленный кремний из контейнера для плавления в тигель.4. The method according to claim 2, in which the molten silicon is placed so that the silicon source is melted in a melting container separate from the crucible, then the crucible and silicon are heated to the melting temperature of silicon, the heating is controlled so that at least one seed the crystal in the crucible has not completely melted, and molten silicon is transferred from the melting container to the crucible. 5. Способ по п.2, включающий формирование части массива с внесением в него по меньшей мере одного затравочного кристалла.5. The method according to claim 2, including the formation of part of the array with the introduction of at least one seed crystal. 6. Способ получения литого кремния, включающий:
геометрически упорядоченное расположение множества затравочных кристаллов кремния, включая монокристаллический кремний, по меньшей мере на одной поверхности тигля с одной или несколькими боковыми стенками, нагретого по меньшей мере до температуры плавления кремния, и по меньшей мере с одной охлаждаемой стенкой, причем геометрически упорядоченное расположение включает плотно упакованные многогранники;
приведение расплавленного кремния в контакт с геометрически упорядоченным расположением затравочных кристаллов кремния; и
формирование твердого массива, содержащего монокристаллический кремний, необязательно по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния под контролем кристаллизации, причем это формирование включает формирование границы раздела твердая фаза - жидкость по ребру расплавленного кремния, которое параллельно по меньшей мере одной охлаждаемой стенке, причем границу раздела регулируют во время охлаждения так, чтобы она перемещалась в направлении, при котором увеличивается расстояние между расплавленным кремнием и по меньшей мере одной охлаждаемой стенкой.
6. A method of producing cast silicon, including:
a geometrically ordered arrangement of a plurality of silicon seed crystals, including monocrystalline silicon, on at least one crucible surface with one or more side walls, heated to at least the silicon melting temperature, and at least one cooled wall, the geometrically ordered arrangement comprising packaged polyhedra;
bringing molten silicon into contact with a geometrically ordered arrangement of silicon seed crystals; and
the formation of a solid array containing monocrystalline silicon, optionally with at least two measurements, each of at least about 10 cm, by cooling molten silicon under crystallization control, and this formation includes the formation of a solid phase - liquid interface along the edge of molten silicon, which parallel to at least one wall being cooled, the interface being adjusted during cooling so that it moves in the direction in which it increases The distance between the molten silicon and at least one cooled wall.
7. Способ получения литого кремния, включающий:
расположение заданным образом множества затравочных кристаллов кремния, содержащих монокристаллический кремний, по меньшей мере на двух поверхностях тигля;
приведение расплавленного кремния в контакт с затравочными кристаллами монокристаллического кремния; и
формирование твердого массива, содержащего монокристаллический кремний, необязательно по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния по меньшей мере по двум поверхностям тигля под контролем кристаллизации, причем это формирование включает регулирование границы раздела твердая фаза - жидкость по ребру расплавленного кремния во время охлаждения так, чтобы она перемещалась в направлении, при котором увеличивается расстояние между расплавленным кремнием и по меньшей мере двумя поверхностями тигля.
7. A method of producing cast silicon, including:
positioning in a predetermined manner a plurality of seed crystals of silicon containing monocrystalline silicon on at least two surfaces of the crucible;
bringing molten silicon into contact with seed crystals of single crystal silicon; and
the formation of a solid array containing monocrystalline silicon, optionally with at least two measurements, each of at least about 10 cm, by cooling molten silicon along at least two surfaces of the crucible under crystallization control, and this formation involves adjusting the solid phase interface - liquid along the edge of molten silicon during cooling so that it moves in a direction in which the distance between the molten silicon and at least Leray two surfaces of the crucible.
8. Способ получения литого кремния, включающий:
приведение кремниевого сырья в контакт по меньшей мере с одним затравочным кристаллом кремния, содержащим монокристаллический кремний, по меньшей мере на одной поверхности;
нагревание источника кремния и по меньшей мере одного затравочного кристалла кремния до температуры плавления кремния;
регулирование нагревания таким образом, чтобы по меньшей мере один затравочный кристалл кремния не расплавился полностью, путем поддержания ΔT на уровне примерно 0,1°С/мин или менее, измеренного на внешней поверхности тигля после достижения температуры плавления кремния по всему тиглю; и как только по меньшей мере один затравочный кристалл кремния частично расплавится,
формирование твердого массива, содержащего монокристаллический кремний, путем охлаждения кремния.
8. A method of producing cast silicon, including:
bringing the silicon raw material into contact with at least one seed crystal of silicon containing monocrystalline silicon on at least one surface;
heating the source of silicon and at least one seed crystal of silicon to a melting point of silicon;
adjusting the heating so that at least one seed silicon crystal does not completely melt by maintaining ΔT of about 0.1 ° C / min or less, measured on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible; and as soon as at least one seed crystal of silicon is partially melted,
the formation of a solid array containing monocrystalline silicon by cooling silicon.
9. Способ по п.7 или 8, который включает размещение по меньшей мере одного затравочного кристалла кремния на дне тигля.9. The method according to claim 7 or 8, which includes placing at least one seed crystal of silicon at the bottom of the crucible. 10. Способ по п.7 или 8, включающий дополнительно формирование части массива, содержащего по меньшей мере один затравочный кристалл.10. The method according to claim 7 or 8, further comprising forming a part of the array containing at least one seed crystal. 11. Способ получения литого кремния, включающий:
геометрически упорядоченное расположение множества затравочных кристаллов кремния, содержащих монокристаллический кремний, по меньшей мере на одной поверхности тигля, причем геометрически упорядоченное расположение включает плотно упакованные многогранники;
приведение расплавленного кремния в контакт со множеством затравочных кристаллов кремния по меньшей мере на одной поверхности;
нагревание источника кремния и множества затравочных кристаллов кремния до температуры плавления кремния;
регулирование нагрева таким образом, чтобы множество затравочных кристаллов кремния не расплавилось полностью, путем поддержания ΔT на уровне примерно 0,1°С/мин или менее, измеренного на внешней поверхности тигля после достижения температуры плавления кремния по всему тиглю; и как только по меньшей мере один затравочный кристалл кремния частично расплавится,
формирование твердого массива, содержащего монокристаллический кремний, путем охлаждения кремния.
11. A method of producing cast silicon, including:
a geometrically ordered arrangement of a plurality of silicon seed crystals containing monocrystalline silicon on at least one surface of the crucible, the geometrically ordered arrangement comprising densely packed polyhedra;
bringing molten silicon into contact with a plurality of silicon seed crystals on at least one surface;
heating the source of silicon and many seed crystals of silicon to the melting temperature of silicon;
adjusting the heating so that the plurality of seed crystals of silicon does not melt completely by maintaining ΔT at about 0.1 ° C / min or less, measured on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible; and as soon as at least one seed crystal of silicon is partially melted,
the formation of a solid array containing monocrystalline silicon by cooling silicon.
12. Способ получения литого кремния, включающий:
расположение множества затравочных кристаллов кремния, содержащих монокристаллический кремний, по меньшей мере на двух поверхностях тигля;
приведение расплавленного кремния в контакт со множеством затравочных кристаллов кремния по меньшей мере на двух поверхностях;
нагревание источника кремния и множества затравочных кристаллов кремния до температуры плавления кремния;
регулирование нагревания таким образом, чтобы множество затравочных кристаллов кремния не расплавились полностью, путем поддержания ΔТ на уровне примерно 0,1°С/мин или менее, измеренного на внешней поверхности тигля после достижения температуры плавления кремния по всему тиглю; и как только по меньшей мере один затравочный кристалл монокристаллического кремния частично расплавится,
формирование твердого массива, содержащего монокристаллический кремний, путем охлаждения кремния.
12. A method of producing cast silicon, including:
the location of many seed crystals of silicon containing monocrystalline silicon, at least two surfaces of the crucible;
bringing molten silicon into contact with a plurality of silicon seed crystals on at least two surfaces;
heating the source of silicon and many seed crystals of silicon to the melting temperature of silicon;
adjusting the heating so that the plurality of seed crystals of silicon does not completely melt by maintaining ΔT of about 0.1 ° C / min or less, measured on the outer surface of the crucible after reaching the melting temperature of silicon throughout the crucible; and as soon as at least one seed crystal of single-crystal silicon is partially melted,
the formation of a solid array containing monocrystalline silicon by cooling silicon.
13. Способ получения литого кремния, включающий: приведение расплавленного кремния в контакт по меньшей мере с одним затравочным кристаллом кремния в сосуде с одной или несколькими боковыми стенками, нагретым по меньшей мере до температуры плавления кремния, причем по меньшей мере один затравочный кристалл кремния расположен так, чтобы покрыть всю или практически всю поверхность сосуда; и
формирование твердого массива, содержащего монокристаллический кремний, необязательно по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния при регулируемой кристаллизации.
13. A method of producing cast silicon, comprising: bringing molten silicon into contact with at least one seed crystal of silicon in a vessel with one or more side walls heated at least to the melting temperature of silicon, and at least one seed crystal of silicon is located so to cover the entire or almost the entire surface of the vessel; and
the formation of a solid array containing monocrystalline silicon, optionally with at least two measurements, each of at least about 10 cm, by cooling molten silicon with controlled crystallization.
14. Способ по пп.1, 6-8, 11 и 12 или 13, в котором охлаждение включает использование теплопоглотителя для переноса тепла к охлаждаемым водой стенкам.14. The method according to claims 1, 6-8, 11 and 12 or 13, in which cooling includes the use of a heat sink to transfer heat to the walls cooled by water. 15. Способ по пп.1, 6-8, 11 и 12 или 13, включающий также формирование массива, не содержащего спиральных дефектов и практически не содержащего кислород-индуцированных дефектов упаковки.15. The method according to claims 1, 6-8, 11 and 12 or 13, which also includes the formation of an array that does not contain spiral defects and practically does not contain oxygen-induced packaging defects. 16. Способ по пп.1, 6-8, 11 и 12 или 13, включающий также изготовление пластины по меньшей мере с одним измерением, равным по меньшей мере примерно 50 мм.16. The method according to claims 1, 6-8, 11 and 12 or 13, which also includes the manufacture of a plate with at least one dimension equal to at least about 50 mm 17. Способ по п.16, включающий также изготовление пластины, не содержащей спиральных дефектов и практически не содержащей кислород-индуцированных дефектов упаковки.17. The method according to clause 16, which also includes the manufacture of a plate that does not contain spiral defects and practically does not contain oxygen-induced packaging defects. 18. Способ по пп.6-8, 11 или 12, включающий также формирование части массива с включением множества затравочных кристаллов.18. The method according to PP.6-8, 11 or 12, also including the formation of part of the array with the inclusion of many seed crystals. 19. Способ по любому из пп.6 и 7, 11 и 12, в котором размещение расплавленного кремния включает плавление источника кремния в контейнере для плавления, отдельном от тигля, нагревание тигля и кремния до температуры плавления кремния, регулирование нагревания таким образом, чтобы множество затравочных кристаллов в тигле не расплавились полностью, и перенос расплавленного кремния из контейнера для плавления в тигель.19. The method according to any one of claims 6 and 7, 11 and 12, in which the placement of molten silicon includes melting the silicon source in a melting container separate from the crucible, heating the crucible and silicon to the melting temperature of silicon, adjusting the heating so that the seed crystals in the crucible were not completely melted, and the transfer of molten silicon from the container for melting into the crucible. 20. Способ по любому из пп.1, 8 и 13, в котором размещение расплавленного кремния включает плавление источника кремния в контейнере для плавления, отдельном от тигля, нагревание тигля и кремния до температуры плавления кремния, регулирование нагревания таким образом, чтобы по меньшей мере один затравочный кристалл в тигле не расплавился полностью, и перенос расплавленного кремния из контейнера для плавления в тигель.20. The method according to any one of claims 1, 8 and 13, in which the placement of molten silicon includes melting the silicon source in a melting container separate from the crucible, heating the crucible and silicon to the melting temperature of silicon, adjusting the heating so that at least one seed crystal in the crucible did not melt completely, and the transfer of molten silicon from the container for melting into the crucible. 21. Способ по любому из пп.6 или 11, включающий также размещение множества затравочных кристаллов таким образом, чтобы общая главная ось затравочных кристаллов была перпендикулярна дну тигля.21. The method according to any one of claims 6 or 11, further comprising placing a plurality of seed crystals such that the common major axis of the seed crystals is perpendicular to the bottom of the crucible. 22. Способ по любому из пп.1, 6-8, 11 и 12 или 13, включающий также формирование другого твердого массива кремния с использованием затравочного кристалла, вырезанного из массива кремния, предварительно полученного литьем по указанному способу.22. The method according to any one of claims 1, 6-8, 11 and 12 or 13, which also includes the formation of another solid silicon array using a seed crystal cut from a silicon array previously obtained by casting according to the specified method. 23. Способ по любому из пп.6 или 7, в котором размещение расплавленного кремния включает также нагревание тигля и кремния до температуры плавления кремния и регулирование нагревания путем поддержания ΔТ на уровне примерно 0,1°С/мин или менее, измеренного на внешней поверхности тигля после достижения температуры плавления кремния по всему тиглю.23. The method according to any one of claims 6 or 7, in which the placement of molten silicon also includes heating the crucible and silicon to the melting temperature of silicon and regulating the heating by maintaining ΔT at about 0.1 ° C / min or less, measured on the outer surface crucible after reaching the melting point of silicon throughout the crucible. 24. Способ по любому из пп.1 или 13, в котором размещение расплавленного кремния включает также нагревание тигля и кремния до температуры плавления кремния и регулирование нагревания путем поддержания ΔT на уровне примерно 0,1°С/мин или менее, измеренного на внешней поверхности тигля после достижения температуры плавления кремния по всему тиглю.24. The method according to any one of claims 1 or 13, in which the placement of molten silicon also includes heating the crucible and silicon to the melting temperature of silicon and controlling the heating by maintaining ΔT at about 0.1 ° C / min or less, measured on the outer surface crucible after reaching the melting point of silicon throughout the crucible. 25. Способ по любому из пп.7 или 8, включающий также размещение множества затравочных кристаллов таким образом, что общая главная ось затравочных кристаллов перпендикулярна одной из по меньшей мере двух поверхностей тигля, с тем чтобы между по меньшей мере двумя поверхностями тигля не образовывались границы зерен.25. The method according to any one of claims 7 or 8, further comprising arranging a plurality of seed crystals such that the common major axis of the seed crystals is perpendicular to one of the at least two crucible surfaces so that no boundaries are formed between at least two crucible surfaces grains. 26. Способ по любому из пп.7 или 8, включающий также размещение множества затравочных кристаллов таким образом, чтобы максимум шесть ребер затравочных кристаллов сходились в любом углу предварительно определенной схемы.26. The method according to any one of claims 7 or 8, further comprising arranging a plurality of seed crystals so that a maximum of six edges of the seed crystals converge in any corner of a predetermined pattern. 27. Способ по любому из пп.7, 8, 12 или 13, включающий также расположение предварительно заданной схемы в гексагональной и октагональной ориентации вдоль по меньшей мере одной поверхности тигля.27. The method according to any one of claims 7, 8, 12, or 13, further comprising arranging a predetermined pattern in a hexagonal and octagonal orientation along at least one surface of the crucible. 28. Способ по любому из пп.7, 8, 12 или 13, в котором по меньшей мере две поверхности тигля перпендикулярны друг другу.28. The method according to any one of claims 7, 8, 12 or 13, in which at least two surfaces of the crucible are perpendicular to each other. 29. Способ по любому из пп.1, 6-8, 11 и 12 или 13, включающий также наблюдение за плавлением с помощью погружаемого стержня.29. The method according to any one of claims 1, 6-8, 11 and 12 or 13, which also includes monitoring the melting using an immersed rod. 30. Способ по любому из пп.1, 6-8, 11 и 12 или 13, в котором формируют твердый массив монокристаллического или почти монокристаллического кремния.30. The method according to any one of claims 1, 6-8, 11 and 12 or 13, in which a solid array of single-crystal or almost single-crystal silicon is formed. 31. Способ по п.1, который включает размещение по меньшей мере одного затравочного кристалла кремния таким образом, чтобы покрыть всю или практически всю поверхность сосуда.31. The method according to claim 1, which includes placing at least one seed crystal of silicon in such a way as to cover the entire or almost the entire surface of the vessel. 32. Способ получения литого кремния, включающий:
приведение расплавленного кремния в контакт по меньшей мере с одним затравочным кристаллом кремния в сосуде, имеющем одну или несколько боковых стенок, нагретых по меньшей мере до температуры плавления кремния, и по меньшей мере одну охлаждаемую стенку; и
образование твердого массива почти монокристаллического кремния необязательно по меньшей мере с двумя измерениями, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния при регулировании кристаллизации, причем это образование включает формирование границы раздела твердое тело-жидкость по ребру расплавленного кремния, которая по меньшей мере сначала параллельна по меньшей мере одной охлаждаемой стенке, причем граница раздела регулируется во время охлаждения таким образом, что она перемещается в направлении, при котором увеличивается расстояние между расплавленным кремнием и по меньшей мере одной охлаждаемой стенкой.
32. A method for producing cast silicon, including:
bringing molten silicon into contact with at least one seed silicon crystal in a vessel having one or more side walls heated at least to the melting temperature of silicon and at least one cooled wall; and
the formation of a solid array of almost monocrystalline silicon, optionally with at least two measurements, each of at least about 10 cm, by cooling the molten silicon while controlling crystallization, this formation including the formation of a solid-liquid interface along the edge of the molten silicon, which is at least at least parallel to at least one wall being cooled, the interface being adjusted during cooling so that it moves in the direction In which the distance increases between the molten silicon and at least one cooled wall.
33. Способ получения литого кремния, включающий:
приведение расплавленного кремния в контакт по меньшей мере с одним затравочным кристаллом кремния в сосуде, имеющем одну или несколько боковых стенок, нагретых по меньшей мере до температуры плавления кремния, причем по меньшей мере один затравочный кристалл кремния располагают так, чтобы он покрывал всю или практически всю поверхность сосуда;
образование твердого массива почти монокристаллического кремния, необязательно имеющего по меньшей мере два измерения, каждое по меньшей мере примерно по 10 см, путем охлаждения расплавленного кремния под контролем кристаллизации.
33. A method for producing cast silicon, including:
bringing molten silicon into contact with at least one seed crystal of silicon in a vessel having one or more side walls heated at least to the melting temperature of silicon, and at least one seed crystal of silicon is arranged so that it covers all or almost all vessel surface;
the formation of a solid array of almost monocrystalline silicon, optionally having at least two dimensions, each of at least about 10 cm, by cooling molten silicon under crystallization control.
34. Кремний, полученный способом по любому из пп.1, 6-8, 11-13, 32 или 33. 34. Silicon obtained by the method according to any one of claims 1, 6-8, 11-13, 32 or 33.
RU2008134068/05A 2006-01-20 2007-01-18 Procedures and equipment for production of mono-crystal cast silicon and items of mono-crystal cast silicon for photo cells RU2425183C2 (en)