TW201431908A - Thermoplastic polyimide - Google Patents

Thermoplastic polyimide Download PDF

Info

Publication number
TW201431908A
TW201431908A TW102146827A TW102146827A TW201431908A TW 201431908 A TW201431908 A TW 201431908A TW 102146827 A TW102146827 A TW 102146827A TW 102146827 A TW102146827 A TW 102146827A TW 201431908 A TW201431908 A TW 201431908A
Authority
TW
Taiwan
Prior art keywords
polyimine
group
thermoplastic
thermoplastic polyimine
present
Prior art date
Application number
TW102146827A
Other languages
Chinese (zh)
Inventor
Takeshi Kato
Yuji Soejima
Jiro Sugiyama
Satoko Koga
Original Assignee
Mitsubishi Chem Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsubishi Chem Corp filed Critical Mitsubishi Chem Corp
Publication of TW201431908A publication Critical patent/TW201431908A/en

Abstract

The purpose of the present invention is to provide: a thermoplastic polyimide which has excellent transparency, heat resistance, thermal stability during melting, non-volatility of solvent and the like; and a thermoplastic polyimide molded body which is obtained by melt extrusion molding the thermoplastic polyimide. The present invention relates to a thermoplastic polyimide which has an alicyclic structure, while having a blocking ratio of terminal amino groups of 95.0% or more and an imidization ratio of 95.8% or more.

Description

熱可塑性聚醯亞胺 Thermoplastic polyimine

本發明係關於一種透明性、耐熱性、熔融熱穩定性、溶劑非揮發性等優異之熱可塑性聚醯亞胺及使該熱可塑性聚醯亞胺熔融擠出成形而獲得之熱可塑性聚醯亞胺成形體。 The present invention relates to a thermoplastic polyimine which is excellent in transparency, heat resistance, heat of fusion, non-volubilization of a solvent, and a thermoplastic polyazate obtained by melt-extruding the thermoplastic polyimide. Amine shaped body.

聚醯亞胺於耐熱性或機械物性、耐化學品性、電氣特性等方面具有優異之特性,因此被廣泛用於汽車、航空宇宙產業、電氣、電子、電池等領域中。 Polyimine has excellent properties in terms of heat resistance, mechanical properties, chemical resistance, electrical properties, etc., and thus is widely used in the fields of automobiles, aerospace industries, electrics, electronics, batteries, and the like.

聚醯亞胺係通常具有耐熱性優異之特徵,另一方面不具有明確之玻璃轉移溫度之熱硬化性樹脂,於用作成形材料之情形時,必須使用燒結成形等特殊之方法。又,於利用燒結成形法獲得具有複雜之形狀之加工品時,存在需要使用數值控制(NC,Numerical control)車床等切削機械自聚醯亞胺之嵌段切出目標形狀等複雜、繁雜之加工步驟,而成為高成本之問題。進而,由於聚醯亞胺通常具有全芳香族骨架,故而成形品會著色。因此,亦存在無法用於要求透明性之用途等問題。 Polyimide is generally a thermosetting resin which does not have a characteristic of excellent heat resistance, and does not have a clear glass transition temperature. When it is used as a molding material, it is necessary to use a special method such as sintering. In addition, when a processed product having a complicated shape is obtained by a sintering method, there is a need for a complicated and complicated process such as cutting out a target shape from a block of a polyimide by using a cutting machine such as a numerical control (NC) mechanical control lathe. Steps and become a high cost issue. Further, since the polyimine usually has a wholly aromatic skeleton, the molded article is colored. Therefore, there are also problems in that it cannot be used for applications requiring transparency.

因此,為了改善成形加工性,業界正開發與通用之熱可塑性樹脂同樣可於一定溫度以上進行熔融成形之熱可塑性聚醯亞胺。例如於專利文獻1中記載有以3,3',4,4'-二苯醚四羧酸骨架作為基本骨架之熱可塑性聚醯亞胺。又,於專利文獻1中,作為聚醯亞胺之製造 方法,記載有使聚醯亞胺前驅物即聚醯胺酸樹脂溶液於溶液中進行醯亞胺化之方法。 Therefore, in order to improve the formability, the industry is developing a thermoplastic polyimine which can be melt-molded at a temperature equal to or higher than a general-purpose thermoplastic resin. For example, Patent Document 1 describes a thermoplastic polyimine having a 3,3',4,4'-diphenyl ether tetracarboxylic acid skeleton as a basic skeleton. Further, in Patent Document 1, as a production of polyimine The method described is a method in which a polyamidene precursor, that is, a polyamidomate resin solution, is imidized in a solution.

另一方面,為了改善透明性,業界正開發使用脂環式四羧酸二酐及脂肪族系二胺中之至少一者之透明聚醯亞胺。例如於專利文獻2中記載有使用3,4,3',4'-二環己基四羧酸二酐骨架之透明聚醯亞胺,又,作為其製造方法,記載有藉由聚醯胺酸溶液之利用溶液流延法之成形及加熱醯亞胺化而獲得透明聚醯亞胺成形體之方法。又,於專利文獻3中記載有使具有脂肪族四羧酸骨架之聚醯胺酸樹脂於溶液中進行醯亞胺化而獲得聚醯亞胺之方法。 On the other hand, in order to improve transparency, the industry is developing a transparent polyimine which uses at least one of an alicyclic tetracarboxylic dianhydride and an aliphatic diamine. For example, Patent Document 2 describes a transparent polyimine using a 3,4,3',4'-dicyclohexyltetracarboxylic dianhydride skeleton, and a method for producing the same, which is described by polyproline The solution is formed by a solution casting method and a method of heating the yttrium to obtain a transparent polyimine molded body. Further, Patent Document 3 describes a method of obtaining a polyimine by subjecting a polyamic acid resin having an aliphatic tetracarboxylic acid skeleton to ruthenium iodide in a solution.

[先前技術文獻] [Previous Technical Literature] [專利文獻] [Patent Literature]

專利文獻1:日本專利特開平4-331231號公報 Patent Document 1: Japanese Patent Laid-Open No. 4-331231

專利文獻2:日本專利特開平8-104750號公報 Patent Document 2: Japanese Patent Laid-Open No. Hei 8-104750

專利文獻3:日本專利特開2005-15629號公報 Patent Document 3: Japanese Patent Laid-Open Publication No. 2005-15629

專利文獻4:日本專利特開2008-297360號公報 Patent Document 4: Japanese Patent Laid-Open Publication No. 2008-297360

專利文獻1中所記載之聚醯亞胺之玻璃轉移溫度較高,並且具有結晶性,因此難以於通常之工業製程中之熔融溫度之上限而製成熔融狀態,成形方法通常限制於溶劑澆鑄法。又,由於具有大量芳香族骨架,故而所獲得之聚醯亞胺亦存在色調、透明性方面之問題。 The polyimine which is described in Patent Document 1 has a high glass transition temperature and has crystallinity, so that it is difficult to form a molten state at the upper limit of the melting temperature in a usual industrial process, and the molding method is usually limited to the solvent casting method. . Further, since a large amount of aromatic skeleton is present, the obtained polyimine has problems in color tone and transparency.

又,專利文獻2中所揭示之技術係為了獲得聚醯亞胺薄膜而藉由溶劑澆鑄法(溶液流延法)使聚醯胺酸之溶液成形之技術,但存 在只能製造薄膜狀之薄膜而其用途受到限制,由於溶劑之乾燥需要時間故而生產性變差等課題。又,由於聚醯胺酸溶液容易因空氣中之水分而發生水解,故而於保管中途分子量改變,黏度降低之方面亦存在課題。進而,根據本發明者等人之研究,亦發現聚醯亞胺之醯亞胺化率不充分,又,由於在末端殘留有一級胺基故而熔融熱穩定性不充分,又,其亦成為著色之原因之課題。 Further, the technique disclosed in Patent Document 2 is a technique for forming a solution of polylysine by a solvent casting method (solution casting method) in order to obtain a polyimide film, but In the case where only a film-like film can be produced, the use thereof is limited, and the drying of the solvent takes time, and the productivity is deteriorated. Further, since the polyaminic acid solution is easily hydrolyzed by moisture in the air, there is a problem in that the molecular weight changes during storage and the viscosity is lowered. Further, according to the study by the inventors of the present invention, it has been found that the ruthenium imidization ratio of polyimine is insufficient, and since the primary amine group remains at the terminal, the thermal stability of fusion is insufficient, and it also becomes colored. The cause of the problem.

另一方面,於專利文獻3中記載有以與溶劑混合之溶液狀態使用聚醯亞胺之溶劑澆鑄法,但其亦與專利文獻2同樣,存在只能製造薄膜狀之薄膜而用途受到限制、溶劑之乾燥需要時間、及因此成本變高等問題,進而,亦發現於聚醯亞胺之末端殘留有一級胺基而成為著色原因之問題。又,於使與溶劑混合而成之聚醯亞胺溶液熔融成形而獲得聚醯亞胺成形體之方法中,由於聚醯亞胺中含有溶劑,故而發生於熔融時可見明顯之發泡,或產生可燃性氣體等問題之可能性亦較高,於該方面亦需要改善。 On the other hand, Patent Document 3 describes a solvent casting method using polyimine in a solution state mixed with a solvent. However, similarly to Patent Document 2, it is possible to produce only a film-like film and its use is limited. The drying of the solvent requires time, and therefore the cost becomes high. Further, it has been found that the primary amine group remains at the end of the polyimine and causes a coloring problem. Further, in the method of obtaining a polyimine imide formed by melt-molding a polyimine solution obtained by mixing a solvent, since the polyimine contains a solvent, significant foaming occurs when molten, or There is also a high probability of causing problems such as flammable gases, and improvements are needed in this respect.

進而,於專利文獻4中記載有藉由控制具有脂環構造之聚醯亞胺之立體構造,而獲得對有機溶劑之溶解性優異之聚醯亞胺。然而,於專利文獻4中亦使用習知之使用溶劑澆鑄法之成形方法,而存在如上述專利文獻2及3中所列舉之課題。 Further, Patent Document 4 discloses that a polyimine having excellent solubility in an organic solvent is obtained by controlling a stereostructure of a polyfluorene having an alicyclic structure. However, in Patent Document 4, a conventional molding method using a solvent casting method is also used, and there are problems as listed in Patent Documents 2 and 3 above.

如專利文獻2~4中所記載之具有脂環構造之聚醯亞胺為熱可塑性,又,透明性或耐熱性優異,因此期待用作用於撓性裝置或有機電致發光(EL,Electro-Luminescence)等用途之聚醯亞胺薄膜,但習知,發現存在:於逐漸被用於聚醯亞胺之成形之溶劑澆鑄法等方法中生產性不充分、聚醯亞胺薄膜只能以薄膜之形式獲得而難以厚膜化、以及可能產生可燃性氣體等課題。 Polyimine having an alicyclic structure as described in Patent Documents 2 to 4 is thermoplastic, and is excellent in transparency and heat resistance. Therefore, it is expected to be used as a flexible device or organic electroluminescence (EL, Electro- Luminescence) is a polyimide film which is used for other purposes, but it has been found that it is insufficient in productivity in a solvent casting method which is gradually used for the formation of polyimine, and the polyimide film can only be a film. The form is obtained, and it is difficult to thicken the film, and a problem such as a flammable gas may be generated.

本發明者等人已知:如上所述之溶劑澆鑄法中之課題可藉由熔融擠出成形法而解決,但另一方面,如專利文獻2~4中所記載之具有脂環構造之聚醯亞胺不具有可應用熔融擠出成形法之程度之熔融熱穩定性。 The inventors of the present invention have known that the problem in the solvent casting method as described above can be solved by the melt extrusion molding method, but on the other hand, the aggregation having the alicyclic structure described in Patent Documents 2 to 4 The quinone imine does not have the thermal stability of the melt to the extent that a melt extrusion process can be applied.

本發明係鑒於上述習知技術之各種問題而成者。本發明之課題在於提供一種透明性、耐熱性、熔融熱穩定性、溶劑非揮發性等優異之熱可塑性聚醯亞胺及使該熱可塑性聚醯亞胺熔融擠出成形而成之熱可塑性聚醯亞胺成形體。 The present invention has been made in view of various problems of the above-described prior art. An object of the present invention is to provide a thermoplastic polyimine which is excellent in transparency, heat resistance, heat of fusion, solvent non-volatility, and the like, and a thermoplastic polymer which is obtained by melt-extruding the thermoplastic polyimide. Yttrium imide formed body.

本發明係鑒於以上之各種問題而成者。本發明者等人進行了努力研究,結果達成如下結論:如專利文獻2~4中所記載之聚醯亞胺之熔融熱穩定性之課題係起因於聚醯亞胺之醯亞胺化率不充分及末端胺基殘留。推測如專利文獻1中所記載之芳香族系聚醯亞胺由於其構造為剛性,故而不易殘留醯胺酸構造,而容易地進行醯亞胺化,相對於此,專利文獻2~4由於具有脂環構造,故而其構造之自由度變高,而容易殘留醯胺酸構造。 The present invention has been made in view of the above various problems. As a result of intensive studies, the inventors of the present invention have reached the following conclusions: The problem of the thermal stability of the polyamidene described in Patent Documents 2 to 4 is due to the fact that the imidization ratio of the polyimide is not Adequate and terminal amine residues. In the case of the aromatic polyimine which is described in the patent document 1, since the structure is rigid, the methionine structure is not easily retained, and the ruthenium imidization is easily performed. In contrast, Patent Documents 2 to 4 have Since the alicyclic structure is high, the degree of freedom of its structure becomes high, and the proline structure is easily left.

如上所述,本發明者等人發現:對於具有脂環構造之聚醯亞胺,藉由提高醯亞胺化率及提高胺基之封端率,可獲得可應用於熔融擠出成形之程度之熔融熱穩定性優異之聚醯亞胺,從而完成本發明。 As described above, the present inventors have found that, for the polyimine having an alicyclic structure, by increasing the sulfhydrylation rate and increasing the blocking ratio of the amine group, it is possible to obtain a degree of application for melt extrusion molding. The present invention is completed by a polyimine which is excellent in melt heat stability.

即,本發明之要旨在於以下之[1]~[9]。 That is, the present invention is intended to be the following [1] to [9].

[1]一種熱可塑性聚醯亞胺,其具有脂環構造,末端胺基之封端率為95.0%以上,且醯亞胺化率為95.8%以上。 [1] A thermoplastic polyimine having an alicyclic structure, a terminal amino group blocking ratio of 95.0% or more, and a ruthenium iodide ratio of 95.8% or more.

[2]如[1]之熱可塑性聚醯亞胺,其中,重量平均分子量 (Mw)為10,000~500,000。 [2] The thermoplastic polyimine of [1], wherein the weight average molecular weight (Mw) is 10,000 to 500,000.

[3]如[1]或[2]之熱可塑性聚醯亞胺,其中,上述脂環構造為環己烷環構造。 [3] The thermoplastic polyimine of [1] or [2], wherein the alicyclic structure is a cyclohexane ring structure.

[4]如[1]至[3]中任一項之熱可塑性聚醯亞胺,其中,上述脂環構造為與醯亞胺環構造共有2個碳原子且鄰接之構造。 [4] The thermoplastic polyimine according to any one of [1] to [3] wherein the alicyclic structure has a structure in which two carbon atoms are shared with the quinone ring structure.

[5]如[1]至[4]中任一項之熱可塑性聚醯亞胺,其中,具有下述式(1)所表示之構造單位及下述式(2)所表示之構造單位之至少一者作為上述脂環構造。 The thermoplastic polyimine of any one of the following formula (1), and the structural unit represented by the following formula (2), and the structural unit represented by the following formula (2). At least one of them is constructed as the above alicyclic ring.

[6]如[1]至[5]中任一項之熱可塑性聚醯亞胺,其中,進而具有下述式(3)所表示之構造單位。 [6] The thermoplastic polyimine of any one of [1] to [5] which further has a structural unit represented by the following formula (3).

(上述式(3)中,R1~R8可分別相互不同地為氫原子、碳數1~4之烷基、碳數1~4之氟烷基或羥基,X為直接鍵、氧原子、 硫原子、碳數1~4之伸烷基、磺醯基、亞磺醯基、硫基、羰基、醯胺基、酯基或二級胺基,n為0~4之整數) (In the above formula (3), R 1 to R 8 may each independently be a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms or a hydroxyl group, and X is a direct bond or an oxygen atom. , sulfur atom, alkyl 1 to 4 alkyl, sulfonyl, sulfinyl, thio, carbonyl, decyl, ester or secondary amine, n is an integer from 0 to 4)

[7]如[1]至[6]中任一項之熱可塑性聚醯亞胺,其中,310℃下之複數剪切黏度(complex shear viscosity)(η*)為1×102~5×105Pa.s。 [7] The thermoplastic polyimine of any one of [1] to [6] wherein the complex shear viscosity (η*) at 310 ° C is 1 × 10 2 ~ 5 × 10 5 Pa. s.

[8]如[1]至[7]中任一項之熱可塑性聚醯亞胺,其中,於310℃下經過60分鐘左右之複數剪切黏度之變化率為300%以下。 [8] The thermoplastic polyimine according to any one of [1] to [7] wherein the rate of change of the complex shear viscosity at about 310 ° C for about 60 minutes is 300% or less.

[9]一種熱可塑性聚醯亞胺成形體,其係使[1]至[8]中任一項之熱可塑性聚醯亞胺熔融擠出成形而獲得。 [9] A thermoplastic polyimine molded article obtained by melt-extruding a thermoplastic polyimine of any one of [1] to [8].

根據本發明,提供一種透明性、耐熱性、溶劑非揮發性等優異,尤其是可進行熔融擠出成形之程度之熔融熱穩定性優異之熱可塑性聚醯亞胺。又,根據本發明,提供一種使該熱可塑性聚醯亞胺熔融擠出成形而獲得之熱可塑性聚醯亞胺成形體。 According to the present invention, there is provided a thermoplastic polyimine which is excellent in transparency, heat resistance, solvent nonvolatile property, and the like, and is particularly excellent in melt heat stability to the extent of melt extrusion molding. Moreover, according to the present invention, there is provided a thermoplastic polyimine molded article obtained by melt-extruding the thermoplastic polyimide.

[熱可塑性聚醯亞胺] [thermoplastic polyimine]

本發明之熱可塑性聚醯亞胺係具有脂環構造,末端胺基之封端率為95.0%以上,且醯亞胺化率為95.8%以上者。 The thermoplastic polyimine of the present invention has an alicyclic structure, and the terminal amino group has a terminal blocking ratio of 95.0% or more and a ruthenium iodide ratio of 95.8% or more.

本發明之熱可塑性聚醯亞胺與如上述專利文獻2~4中所記載之習知之具有脂環構造之聚醯亞胺相比,實現熔融熱穩定性顯著優異之效果。根據本發明者等人之詳細之研究,可知於專利文獻2 ~4中未充分地進行醯亞胺化,而殘留醯胺酸,又,末端胺基之封端率並不充分。認為對於此種熱可塑性聚醯亞胺,於加熱至300℃以上時於聚醯亞胺分子中之醯胺酸與末端胺基之間引起反應及於聚醯亞胺之分子間之醯胺酸彼此引起反應等會影響熔融熱穩定性。 The thermoplastic polyimine of the present invention has an effect of remarkably excellent fusion heat stability as compared with the conventional polycyclic imine having an alicyclic structure as described in the above Patent Documents 2 to 4. According to the detailed study by the inventors and the like, it is known in Patent Document 2 The ruthenium imidization was not sufficiently carried out in ~4, and the proline acid remained, and the terminal amine group was not sufficiently blocked. It is considered that for such a thermoplastic polyimine, a reaction between a proline and a terminal amine group in a polyimine molecule when heated to 300 ° C or higher and a proline in the molecule of a polyimine The reaction or the like caused by each other affects the thermal stability of the fusion.

[化學構造] [Chemical Construction]

本發明之熱可塑性聚醯亞胺具有脂環構造。該脂環構造並無特別限制,通常為碳數5~12之脂環構造,較佳為碳數6~10之脂環構造,尤佳為環己烷環構造。本發明之熱可塑性聚醯亞胺藉由具有脂環構造,而成為具有熱可塑性,又,透明性優異之聚醯亞胺。再者,本發明中之「脂環構造」係以亦包含在環構造中具有雜原子者之含義使用,但較佳者為於環構造中不具有雜原子之脂環構造。 The thermoplastic polyimine of the present invention has an alicyclic structure. The alicyclic structure is not particularly limited, and is usually an alicyclic structure having a carbon number of 5 to 12, preferably an alicyclic structure having a carbon number of 6 to 10, and particularly preferably a cyclohexane ring structure. The thermoplastic polyimine of the present invention has an alicyclic structure and is a polyimide having excellent thermoplasticity and excellent transparency. Further, the "alicyclic structure" in the present invention is used in the sense of including a hetero atom in the ring structure, but is preferably an alicyclic structure having no hetero atom in the ring structure.

本發明之熱可塑性聚醯亞胺通常可如下所述以羧酸二酐(以下稱為「酸二酐」)二胺化合物作為原料而獲得。本發明之熱可塑性聚醯亞胺中之脂環構造可為源自酸二酐者,亦可為源自二胺化合物者,但較佳為源自酸二酐之脂環構造。 The thermoplastic polyimine of the present invention can be usually obtained by using a carboxylic acid dianhydride (hereinafter referred to as "acid dianhydride") diamine compound as a raw material as follows. The alicyclic structure of the thermoplastic polyimine of the present invention may be derived from an acid dianhydride or may be derived from a diamine compound, but is preferably an alicyclic structure derived from an acid dianhydride.

本發明之熱可塑性聚醯亞胺之脂環構造較佳為與醯亞胺環構造共有2個碳原子且鄰接者。若脂環構造為與醯亞胺環構造共有2個碳原子且鄰接之構造,則容易兼具基於脂環構造之透明性與源自醯亞胺環構造之耐熱性、化學穩定性,因此較佳。作為脂環構造為與醯亞胺環構造共有2個碳原子且鄰接之構造之較佳者,例如可列舉該脂環構造為環己烷環構造者(下述式(4)所表示之構造)。 The alicyclic structure of the thermoplastic polyimine of the present invention preferably has two carbon atoms in common with the quinone ring structure. When the alicyclic structure has a structure in which two carbon atoms are adjacent to the quinone ring structure, it is easy to have both transparency based on the alicyclic structure and heat resistance and chemical stability derived from the quinone ring structure. good. The alicyclic structure is preferably a structure in which the alicyclic structure has two carbon atoms and is adjacent to each other, and the alicyclic structure is a cyclohexane ring structure (the structure represented by the following formula (4)) ).

[化3] [Chemical 3]

進而,較佳為具有下述式(1)所表示之構造單位及下述式(2)所表示之構造單位之至少一者作為本發明之熱可塑性聚醯亞胺中之脂環構造。若具有式(1)所表示之構造單位及式(2)所表示之構造單位之至少一者,則成為透明性、韌性尤其優異者,因此較佳。式(1)所表示之構造單位通常可由下述式(5)所表示之酸二酐導入,又,式(2)所表示之構造單位通常可由下述式(6)所表示之酸二酐導入。 Furthermore, at least one of the structural unit represented by the following formula (1) and the structural unit represented by the following formula (2) is preferably used as the alicyclic structure of the thermoplastic polyimine of the present invention. When at least one of the structural unit represented by the formula (1) and the structural unit represented by the formula (2) is used, transparency and toughness are particularly excellent, which is preferable. The structural unit represented by the formula (1) is usually introduced by an acid dianhydride represented by the following formula (5), and the structural unit represented by the formula (2) is usually an acid dianhydride represented by the following formula (6). Import.

本發明之熱可塑性聚醯亞胺藉由末端胺基之封端率為95.0%以上,且醯亞胺化率為95.8%以上,可獲得可進行熔融擠出成形之程度之優異熔融熱穩定性。 The thermoplastic polyimine of the present invention has an end grouping ratio of 95.0% or more and a sulfhydrylation ratio of 95.8% or more, and excellent melt heat stability to the extent that melt extrusion molding can be obtained. .

本發明之熱可塑性聚醯亞胺就成為使熔融熱穩定性更加良好者之觀點而言,末端胺基之封端率較佳為96.0%以上,更佳為97.0%以上,進而較佳為98.0%以上。熱可塑性聚醯亞胺之末端胺基之封端率之上限並無限制,通常為100%。 In view of the fact that the thermoplastic polyimine of the present invention has a better melt heat stability, the terminal amine group has a blocking ratio of preferably 96.0% or more, more preferably 97.0% or more, and still more preferably 98.0. %the above. The upper limit of the capping rate of the terminal amine group of the thermoplastic polyimine is not limited and is usually 100%.

如下所述,末端胺基之封端率可藉由作為原料之酸二酐與二胺化合物之使用比率、末端封端反應步驟中之末端封端劑之使用量及其種類、化學醯亞胺化反應步驟中之觸媒、脫水劑之種類及該等之使用量等而控制。又,末端胺基之封端率可藉由1H-NMR測定而求出。將其具體例示於實施例。再者,於本發明中,所謂「末端胺基之封端」,係以不僅包含將鍵結於末端之一級胺基之氫原子藉由末端封端劑取代,亦包含化學醯亞胺化反應步驟中之末端胺基與脫水縮合劑之反應等預計外之末端封端的含義使用。 As described below, the terminal amine group can be used in the ratio of the use ratio of the acid dianhydride to the diamine compound as a raw material, the amount of the terminal blocking agent in the terminal end-capping reaction step, and the kind thereof, and the chemical quinone imine. The catalyst, the type of the dehydrating agent, the amount of use, and the like in the reaction step are controlled. Further, the terminal blocking ratio of the terminal amine group can be determined by 1 H-NMR measurement. This is specifically exemplified in the examples. Further, in the present invention, the term "end grouping of a terminal amine group" includes a chemical hydrazine imidization reaction including not only a hydrogen atom bonded to a terminal amine group at the terminal end but also a terminal blocking agent. In the step, the reaction between the terminal amine group and the dehydrating condensing agent is expected to be used for the end termination.

又,本發明之熱可塑性聚醯亞胺就成為使熔融熱穩定性更加良好者之觀點而言,醯亞胺化率較佳為96.0%以上,更佳為96.5%以上,進而較佳為97.0%以上,尤佳為98.0%以上。熱可塑性聚醯亞胺之醯亞胺化率之上限並無限制,通常為100%。 Further, in view of the fact that the thermoplastic polyimine of the present invention has a better melt heat stability, the sulfiliation ratio is preferably 96.0% or more, more preferably 96.5% or more, and still more preferably 97.0. More than %, especially preferably 98.0% or more. The upper limit of the imidization ratio of the thermoplastic polyimine is not limited and is usually 100%.

於本發明中,如下所述,醯亞胺化率可藉由末端封端步驟、化學醯亞胺化反應步驟之條件等而控制。為了不經過末端封端步驟而提高醯亞胺化率,可藉由如下所述般相對多量地使用化學醯亞胺化反應步驟中所使用之脫水縮合劑,而提高醯亞胺化率。又,本發明之熱可塑性聚醯亞胺之醯亞胺化率可藉由1H-NMR測定而求出,將其具體例示於實施例。再者,於無法藉由1H-NMR測定求出醯亞胺化率之情形時,可藉由基於除氫原子以外之原子之NMR測定而求出。 In the present invention, as described below, the ruthenium iodization ratio can be controlled by the terminal end-capping step, the conditions of the chemical hydrazine imidization reaction step, and the like. In order to increase the ruthenium amide ratio without undergoing the terminal end-capping step, the ruthenium amide ratio can be increased by using a dehydration condensing agent used in the chemical hydrazylation reaction step in a relatively large amount as described below. Further, the ruthenium imidization ratio of the thermoplastic polyimine of the present invention can be determined by 1 H-NMR measurement, and specific examples thereof are shown in the examples. Further, when the ruthenium iodide ratio cannot be determined by 1 H-NMR measurement, it can be determined by NMR measurement based on an atom other than a hydrogen atom.

本發明之熱可塑性聚醯亞胺較佳為具有下述式(3)所表示之構造單位。若具有式(3)所表示之構造單位,則有耐熱性、韌性變得更加良好之傾向,因此較佳。 The thermoplastic polyimine of the present invention preferably has a structural unit represented by the following formula (3). When the structural unit represented by the formula (3) is present, heat resistance and toughness tend to be further improved, which is preferable.

[化5] [Chemical 5]

於式(3)中,R1~R8可分別相互不同地為氫原子、碳數1~4之烷基、碳數1~4之氟烷基或羥基。於該等之中,較佳為氫原子或甲基。 In the formula (3), R 1 to R 8 may each independently be a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms or a hydroxyl group. Among these, a hydrogen atom or a methyl group is preferred.

於式(3)中,X為直接鍵、氧原子、硫原子、碳數1~4之伸烷基、磺醯基、亞磺醯基、硫基、羰基、醯胺基、酯基或二級胺基。於該等之中,較佳為直接鍵、氧原子、硫原子、碳數1~4之伸烷基、磺醯基或醯胺基,尤佳為氧原子。 In the formula (3), X is a direct bond, an oxygen atom, a sulfur atom, an alkylene group having 1 to 4 carbon atoms, a sulfonyl group, a sulfinyl group, a thio group, a carbonyl group, a decylamino group, an ester group or two Amine group. Among these, a direct bond, an oxygen atom, a sulfur atom, an alkylene group having 1 to 4 carbon atoms, a sulfonyl group or a decylamino group is preferred, and an oxygen atom is particularly preferred.

於式(3)中,n為0~4之整數。n較佳為1~4之整數。 In the formula (3), n is an integer of 0 to 4. n is preferably an integer of 1 to 4.

再者,於熱可塑性聚醯亞胺1分子整體中之式(3)所表示之構造單位中,R1~R8、X、n可未必全部相同。尤其是於n為2以上之整數之情形時,X可為不同之構造。 Further, in the structural unit represented by the formula (3) in the entire molecule of the thermoplastic polyimine, R 1 to R 8 , X and n may not all be the same. In particular, when n is an integer of 2 or more, X may be a different configuration.

於式(3)所表示之構造單位之中,較佳為下述式(3-1)~式(3-6)所表示之構造單位之任一者所表示者。再者,於1分子之熱可塑性聚醯亞胺中可僅含有1種該等構造單位,亦可組合含有數種。 Among the structural units represented by the formula (3), those represented by any one of the structural units represented by the following formulas (3-1) to (3-6) are preferable. Further, in one molecule of the thermoplastic polyimine, only one type of such structural unit may be contained, or several types may be contained in combination.

[化6] [Chemical 6]

本發明之熱可塑性聚醯亞胺除了以上列舉之式(1)~(3)所表示之構造單位以外,亦可具有其他構造單位。其他構造單位可基於除下述製造方法中列舉之式(5)~(7)所表示之化合物以外之原料而導入。 The thermoplastic polyimine of the present invention may have other structural units in addition to the structural unit represented by the above formulas (1) to (3). Other structural units can be introduced based on raw materials other than the compounds represented by the formulas (5) to (7) listed in the following production methods.

[物性] [physical property]

本發明之熱可塑性聚醯亞胺之重量平均分子量(Mw)較佳為10,000以上,更佳為30,000以上,尤佳為45,000以上,另一方面,較佳為500,000以下,更佳為300,000以下,進而較佳為150,000以下,尤佳 為130,000以下。若聚醯亞胺之重量平均分子量為上述下限值以上,則於製成聚醯亞胺成形體時之韌性之觀點而言較佳,另一方面,若為上述上限值以下,則於流動性、成形性之觀點而言較佳。再者,本發明之熱可塑性聚醯亞胺之重量平均分子量可藉由凝膠滲透層析法(GPC法)而測定。關於GPC測定之更詳細之條件等記載於後揭實施例中。 The weight average molecular weight (Mw) of the thermoplastic polyimine of the present invention is preferably 10,000 or more, more preferably 30,000 or more, still more preferably 45,000 or more, and further preferably 500,000 or less, more preferably 300,000 or less. Further preferably 150,000 or less, particularly preferably It is 130,000 or less. When the weight average molecular weight of the polyimine is more than or equal to the above lower limit, it is preferable from the viewpoint of the toughness at the time of forming the polyimine molded article, and if it is at most the above upper limit, It is preferable from the viewpoint of fluidity and formability. Further, the weight average molecular weight of the thermoplastic polyimine of the present invention can be measured by gel permeation chromatography (GPC method). More detailed conditions and the like for the GPC measurement are described in the following examples.

本發明之熱可塑性聚醯亞胺於310℃下之複數剪切黏度(η*)較佳為1×102Pa.s以上,更佳為1×103Pa.s以上,且較佳為5×105Pa.s以下,更佳為1×105Pa.s以下。複數剪切黏度為上述範圍會成為適合於成形之流動性,因此較佳。複數剪切黏度可藉由分子量、分子組成等而控制,通常若分子量較大,則複數剪切黏度變大。再者,複數剪切黏度可藉由後揭實施例中記載之方法進行測定。 The complex shear viscosity (η*) of the thermoplastic polyimine of the present invention at 310 ° C is preferably 1 × 10 2 Pa. Above s, more preferably 1 × 10 3 Pa. s or more, and preferably 5 × 10 5 Pa. Below s, more preferably 1 × 10 5 Pa. s below. It is preferred that the complex shear viscosity is in the above range to be suitable for forming fluidity. The complex shear viscosity can be controlled by molecular weight, molecular composition, etc., usually, if the molecular weight is large, the complex shear viscosity becomes large. Further, the complex shear viscosity can be measured by the method described in the following examples.

進而,本發明之熱可塑性聚醯亞胺係熔融熱穩定性優異者。具體而言,本發明之熱可塑性聚醯亞胺於310℃下熔融60分鐘時、剛熔融後之初期複數剪切黏度(η*0)與經過60分鐘後之複數剪切黏度(η*60)之複數剪切黏度之變化率較佳為300%以下,更佳為200%以下,進而較佳為100%以下。複數剪切黏度之變化率係表示熔融時之流動穩定性者。因此,複數剪切黏度之變化率為上述上限值以下於熔融穩定性之觀點而言較佳,又,容易進行薄膜成形時之膜厚之控制,因此較佳。再者,複數剪切黏度之變化率之下限通常為0。複數剪切黏度之變化率有末端胺基之封端率越提高,其越變低之傾向。再者,於本發明中,複數剪切黏度之變化率可根據以下之式進行定義,藉由後揭實施例中記載之方法而測定。 Further, the thermoplastic polyimine of the present invention is excellent in fusion heat stability. Specifically, the thermoplastic shear polyimine of the present invention is melted at 310 ° C for 60 minutes, the initial complex shear viscosity (η * 0 ) immediately after melting, and the complex shear viscosity after 60 minutes (η * 60 The rate of change of the complex shear viscosity is preferably 300% or less, more preferably 200% or less, and still more preferably 100% or less. The rate of change of the complex shear viscosity indicates the flow stability at the time of melting. Therefore, the rate of change of the complex shear viscosity is preferably at least the above upper limit value from the viewpoint of melt stability, and it is preferable to control the film thickness at the time of film formation. Furthermore, the lower limit of the rate of change of the complex shear viscosity is usually zero. The rate of change of the complex shear viscosity tends to increase as the terminal blocking ratio of the terminal amine group increases. Further, in the present invention, the rate of change of the complex shear viscosity can be determined by the following formula, and can be measured by the method described in the following examples.

(複數剪切黏度之變化率)=[(η*60-η*0)/η*0]×100 (The rate of change of complex shear viscosity) = [(η * 60 - η * 0 ) / η * 0 ] × 100

本發明之熱可塑性聚醯亞胺之利用動態熱機械測定裝 置(DMS,Dynamic Mechanical Spectrometer)法所得之玻璃轉移溫度(Tg)較佳為150℃以上,更佳為200℃以上,尤佳為250℃以上。玻璃轉移溫度為上述下限值以上就耐熱性之觀點而言較佳。另一方面,關於玻璃轉移溫度之上限並無特別限制,通常為350℃以下。再者,利用DMS法所得之玻璃轉移溫度可藉由後揭實施例中記載之方法進行測定。 Dynamic thermomechanical measurement of the thermoplastic polyimine of the present invention The glass transition temperature (Tg) obtained by the DMS (Dynamic Mechanical Spectrometer) method is preferably 150 ° C or higher, more preferably 200 ° C or higher, and particularly preferably 250 ° C or higher. The glass transition temperature is preferably at least the above lower limit value from the viewpoint of heat resistance. On the other hand, the upper limit of the glass transition temperature is not particularly limited, and is usually 350 ° C or lower. Further, the glass transition temperature obtained by the DMS method can be measured by the method described in the following examples.

本發明之熱可塑性聚醯亞胺之熱膨脹率較佳為於100~200℃之範圍內為100ppm/℃以下,更佳為70ppm/℃以下。熱膨脹率為上述上限值以下於可製造尺寸精度較高之聚醯亞胺成形體之方面較佳。 The thermal expansion coefficient of the thermoplastic polyimine of the present invention is preferably 100 ppm/° C. or less, more preferably 70 ppm/° C. or less in the range of 100 to 200° C. It is preferable that the thermal expansion coefficient is not less than the above upper limit value and that the polyimine molded article having high dimensional accuracy can be produced.

[熱可塑性聚醯亞胺之製造方法] [Method for producing thermoplastic polyimine]

製造本發明之熱可塑性聚醯亞胺之方法並無限制,例如可將以下說明之特定之酸二酐與特定之二胺化合物作為原料而經過熱醯亞胺化反應步驟後,經過末端封端反應步驟及/或化學醯亞胺化步驟而獲得。再者,末端封端反應步驟與化學醯亞胺化步驟可以任意順序進行,又,亦可同時進行該等,但較佳為於經過末端封端反應步驟後,經過化學醯亞胺化反應步驟。 The method for producing the thermoplastic polyimine of the present invention is not limited, and for example, the specific acid dianhydride described below and the specific diamine compound can be used as a raw material, and after the thermal amidation reaction step, the terminal is terminated. Obtained by a reaction step and/or a chemical hydrazylation step. Furthermore, the end capping reaction step and the chemical hydrazylation step may be carried out in any order, or may be carried out simultaneously, but preferably after passing through the end-capped reaction step, passing through a chemical hydrazylation reaction step. .

[原料] [raw material]

本發明之熱可塑性聚醯亞胺通常可使用酸二酐與二胺化合物作為原料而獲得。本發明之熱可塑性聚醯亞胺之原料係使用在酸二酐與二胺化合物之至少一者中具有脂環構造之化合物,就原料準備、生產性等觀點而言,較佳為使用具有脂環構造之酸二酐。 The thermoplastic polyimine of the present invention can be usually obtained by using an acid dianhydride and a diamine compound as a raw material. The raw material of the thermoplastic polyimine of the present invention is a compound having an alicyclic structure in at least one of an acid dianhydride and a diamine compound, and it is preferred to use a fat in terms of raw material preparation, productivity, and the like. The acid dianhydride of the ring structure.

較佳為使用下述式(5)所表示之酸二酐(以下有時稱為 「H-BPDA」)及下述式(6)所表示之酸二酐(以下有時稱為「H-PMDA」)中之至少一者作為本發明之熱可塑性聚醯亞胺之原料。再者,H-BPDA為公知之化合物,例如可藉由日本專利特開2011-45877號公報中記載之方法等而獲得。又,H-PMDA亦為公知之化合物,例如可藉由日本專利特開2009-191253號公報中記載之方法等而獲得。 It is preferred to use an acid dianhydride represented by the following formula (5) (hereinafter sometimes referred to as "H-BPDA") and at least one of acid dianhydride (hereinafter sometimes referred to as "H-PMDA") represented by the following formula (6) are used as a raw material of the thermoplastic polyimine of the present invention. Further, H-BPDA is a known compound, and can be obtained, for example, by the method described in JP-A-2011-45877. Further, H-PMDA is also a known compound, and can be obtained, for example, by the method described in JP-A-2009-191253.

又,較佳為使用下述式(7)所表示之二胺化合物作為本發明之熱可塑性聚醯亞胺之原料。 Further, it is preferred to use a diamine compound represented by the following formula (7) as a raw material of the thermoplastic polyimine of the present invention.

於上述式(7)中,R1'~R8'與上述式(3)中之R1~R8同樣地定義,X'與X同樣地定義。又,n'與n同樣地定義。 In the above formula (7), R 1 ' to R 8 ' are defined similarly to R 1 to R 8 in the above formula (3), and X' is defined similarly to X. Further, n' is defined in the same manner as n.

作為上述式(7)所表示之二胺化合物,例如可列舉4,4'-二胺基二苯醚(以下有時稱為ODA)、2,2'-二甲基-4,4'-二胺基聯苯、1,4-雙(4-胺基苯氧基)苯、2,2-雙(4-(4-胺基苯氧基)苯基)丙烷、2,2-雙(4-(4- 胺基苯氧基)苯基)六氟丙烷、2,2-雙[4-(4-胺基苯氧基)苯基]丙烷、4,4'-雙(4-胺基苯氧基)聯苯、2,2'-雙(三氟甲基)-4,4'-二胺基聯苯、4,4'-二胺基苯甲醯苯胺、4-胺基苯基-4-胺基苯甲酸酯、雙(4-胺基苯基)對苯二甲酸酯、雙(4-(4-胺基苯氧基)苯基)碸、雙(4-胺基-3-羧基苯基)甲烷等。於該等之中,較佳為4,4'-二胺基二苯醚、2,2'-二甲基-4,4'-二胺基聯苯、2,2'-雙(三氟甲基)-4,4'-二胺基聯苯等。該等酸二酐可僅使用1種,亦可組合使用數種。 Examples of the diamine compound represented by the above formula (7) include 4,4'-diaminodiphenyl ether (hereinafter sometimes referred to as ODA) and 2,2'-dimethyl-4,4'-. Diaminobiphenyl, 1,4-bis(4-aminophenoxy)benzene, 2,2-bis(4-(4-aminophenoxy)phenyl)propane, 2,2-dual ( 4-(4- Aminophenoxy)phenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, 4,4'-bis(4-aminophenoxy) Biphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 4,4'-diaminobenzamide, 4-aminophenyl-4-amine Benzoate, bis(4-aminophenyl)terephthalate, bis(4-(4-aminophenoxy)phenyl)anthracene, bis(4-amino-3-carboxyl) Phenyl) methane, etc. Among these, 4,4'-diaminodiphenyl ether, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoro) are preferred. Methyl)-4,4'-diaminobiphenyl or the like. These acid dianhydrides may be used alone or in combination of several kinds.

本發明之熱可塑性聚醯亞胺亦可併用除H-BPDA及H-PMDA以外之酸二酐作為原料。作為除H-BPDA及H-PMDA以外之酸二酐,例如可列舉伸乙基四羧酸二酐、丁烷四羧酸二酐、環戊烷四羧酸二酐、1,2,3,4-環己烷四羧酸二酐、均苯四甲酸二酐、1,1-雙(2,3-二羧基苯基)乙烷二酐、雙(2,3-二羧基苯基)甲烷二酐、雙(3,4-二羧基苯基)甲烷二酐、3,3',4,4'-聯苯四羧酸二酐、2,2-雙(3,4-二羧基苯基)丙烷二酐、2,2-雙(3,4-二羧基苯基)丙烷二酐、2,2-雙(3,4-二羧基苯基)-1,1,1,3,3,3-六氟丙烷二酐、2,2-雙(2,3-二羧基苯基)-1,1,1,3,3,3-六氟丙烷二酐、雙(3,4-二羧基苯基)碸二酐、雙(3,4-二羧基苯基)醚二酐、雙(2,3-二羧基苯基)醚二酐、3,3',4,4'-二苯甲酮四羧酸二酐、2,2',3,3'-二苯甲酮四羧酸二酐、4,4-(對伸苯基二氧基)雙鄰苯二甲酸二酐、4,4-(間伸苯基二氧基)雙鄰苯二甲酸二酐、1,2,5,6-萘二羧酸二酐、1,4,5,8-萘二羧酸二酐、2,3,6,7-萘二羧酸二酐、1,2,3,4-苯四羧酸二酐、2,2',6,6'-聯苯四羧酸二酐、3,4,9,10-苝四羧酸二酐、2,3,6,7-蒽四羧酸二酐、及1,2,7,8-菲四羧酸二酐等,該等可僅使用1種,亦可組合使用數種。又,於使用除H-BPDA及H-PMDA以外之酸二酐之情形時,以相對於用作原料之全部酸二酐通常為20mol%以下、較佳為10mol%以下、更佳為5 mol%以下使用。 The thermoplastic polyimine of the present invention may be used in combination with an acid dianhydride other than H-BPDA and H-PMDA. Examples of the acid dianhydride other than H-BPDA and H-PMDA include ethyl tetracarboxylic dianhydride, butane tetracarboxylic dianhydride, cyclopentane tetracarboxylic dianhydride, and 1,2,3. 4-cyclohexanetetracarboxylic dianhydride, pyromellitic dianhydride, 1,1-bis(2,3-dicarboxyphenyl)ethane dianhydride, bis(2,3-dicarboxyphenyl)methane Dihydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, 2,2-bis(3,4-dicarboxyphenyl) Propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3, 3-hexafluoropropane dianhydride, 2,2-bis(2,3-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, bis(3,4-dicarboxyl) Phenyl) phthalic anhydride, bis(3,4-dicarboxyphenyl)ether dianhydride, bis(2,3-dicarboxyphenyl)ether dianhydride, 3,3',4,4'-diphenyl Ketotetracarboxylic dianhydride, 2,2',3,3'-benzophenonetetracarboxylic dianhydride, 4,4-(p-phenylenedioxy)diphthalic dianhydride, 4, 4-(meta-phenylenedioxy)diphthalic dianhydride, 1,2,5,6-naphthalenedicarboxylic dianhydride, 1,4,5,8-naphthalenedicarboxylic dianhydride, 2 , 3,6,7-naphthalenedicarboxylic dianhydride, 1,2,3,4-benzenetetracarboxylic dianhydride, 2,2',6,6'-biphenyltetracarboxylic acid Anhydride, 3,4,9,10-decanetetracarboxylic dianhydride, 2,3,6,7-nonanetetracarboxylic dianhydride, and 1,2,7,8-phenanthrenetetracarboxylic dianhydride, etc. Only one type may be used, and several types may be used in combination. In the case of using an acid dianhydride other than H-BPDA and H-PMDA, it is usually 20 mol% or less, preferably 10 mol% or less, more preferably 5 or less, based on the total acid dianhydride used as a raw material. Use below mol%.

本發明之熱可塑性聚醯亞胺亦可併用除上述式(7)所表示之二胺化合物以外之二胺化合物作為原料。作為除上述式(7)所表示之二胺化合物以外之二胺化合物,例如可列舉1,2-苯二胺、1,3-苯二胺、3,4'-二胺基二苯醚、1,3'-雙(4-胺基苯氧基)苯、1,3-雙(3-胺基苯氧基)苯、4,4'-雙(3-胺基苯氧基)二苯甲酮、4,4'-雙(3-胺基苯氧基)聯苯、1,3-雙[4-(3-胺基苯氧基)苯甲醯基]苯、雙(4-(3-胺基苯氧基)苯基)碸、1,3-雙(4-胺基苯氧基)新戊烷、雙(4-胺基-3-羧基苯基)甲烷、1,4-二胺基環己烷、4,4'-亞甲基雙(環己基胺)、4,4'-亞甲基雙(2-甲基環己基胺)、2-(4-胺基苯基)-5-胺基-1H-苯并咪唑、2-(4-胺基苯基)-5-1H-苯并唑、2,2-雙(3-胺基-4-羥基苯基)丙烷、2,2-雙(3-胺基-4-羥基苯基)六氟丙烷、雙(3-胺基-4-羥基苯基)碸等,該等可僅使用1種,亦可組合使用數種。又,於使用除上述式(7)所表示之二胺化合物以外之二胺化合物之情形時,以相對於用作原料之全部二胺化合物通常為20mol%以下、較佳為10mol%以下、更佳為5mol%以下使用。 The thermoplastic polyimine of the present invention may be used in combination with a diamine compound other than the diamine compound represented by the above formula (7). Examples of the diamine compound other than the diamine compound represented by the above formula (7) include 1,2-phenylenediamine, 1,3-phenylenediamine, and 3,4'-diaminodiphenyl ether. 1,3'-bis(4-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)benzene, 4,4'-bis(3-aminophenoxy)diphenyl Methyl ketone, 4,4'-bis(3-aminophenoxy)biphenyl, 1,3-bis[4-(3-aminophenoxy)benzylidene]benzene, bis(4-( 3-aminophenoxy)phenyl)indole, 1,3-bis(4-aminophenoxy) neopentane, bis(4-amino-3-carboxyphenyl)methane, 1,4- Diaminocyclohexane, 4,4'-methylenebis(cyclohexylamine), 4,4'-methylenebis(2-methylcyclohexylamine), 2-(4-aminophenyl) -5-Amino-1H-benzimidazole, 2-(4-aminophenyl)-5-1H-benzo Azole, 2,2-bis(3-amino-4-hydroxyphenyl)propane, 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, bis(3-amino-4) -Hydroxyphenyl)anthracene or the like, these may be used alone or in combination of several kinds. In the case of using a diamine compound other than the diamine compound represented by the above formula (7), it is usually 20 mol% or less, preferably 10 mol% or less, based on the total amount of the diamine compound used as a raw material. It is preferably used at 5 mol% or less.

對於本發明之熱可塑性聚醯亞胺,用作原料之酸二酐與二胺化合物之使用比率係相對於酸二酐1mol使用二胺化合物較佳為通常0.8mol以上,又,更佳為多於1.0mol。另一方面,較佳為使用1.2mol以下,更佳為使用1.1mol以下。若將用作原料之酸二酐與二胺化合物之使用比率設為上述範圍,則容易獲得分子量較大之聚醯亞胺,可獲得聚醯亞胺之韌性,因此較佳。尤其是藉由相對於酸二酐使用多於1.0mol之二胺化合物,而控制為使末端胺基多於酸酐末端,提高藉由將其進行末端封端而最終獲得之聚醯亞胺之末端胺基的封端率,因此較佳。其原因在於:於酸二酐多於二胺化合物之情形時,容 易獲得末端為酸酐之聚醯亞胺,於將酸酐末端進行封端時,必須使用具有胺基之封端劑。 With respect to the thermoplastic polyimine of the present invention, the use ratio of the acid dianhydride and the diamine compound used as a raw material is preferably 0.8 mol or more, more preferably more, based on 1 mol of the acid dianhydride. At 1.0 mol. On the other hand, it is preferably used in an amount of 1.2 mol or less, more preferably 1.1 mol or less. When the ratio of use of the acid dianhydride and the diamine compound used as a raw material is in the above range, it is easy to obtain a polyimine having a large molecular weight, and the toughness of the polyimine is obtained, which is preferable. In particular, by using more than 1.0 mol of the diamine compound relative to the acid dianhydride, it is controlled such that the terminal amine group is more than the anhydride end, and the end of the polyimine finally obtained by end-capping it is increased. The capping ratio of the amine group is therefore preferred. The reason is that when the acid dianhydride is more than the diamine compound, the capacity is A polyimine having an acid anhydride at the end is easily obtained, and when the acid anhydride terminal is blocked, a terminal blocking agent having an amine group must be used.

[熱醯亞胺化反應步驟] [Thermal imidization reaction step]

於本發明中,所謂「熱醯亞胺化反應步驟」,意指藉由視需要將溶劑及觸媒與上述原料混合並加熱而進行醯亞胺化反應(縮合及脫水環化反應)之步驟。 In the present invention, the "hot hydrazine imidization reaction step" means a step of performing a ruthenium amide reaction (condensation and dehydration cyclization reaction) by mixing and heating a solvent and a catalyst with the above-mentioned raw materials as necessary. .

作為熱醯亞胺化反應中所使用之溶劑,可列舉N,N-二甲基甲醯胺、N,N-二甲基乙醯胺及N-甲基-2-吡咯啶酮、二甲基亞碸等。於該等之中,較佳為N,N-二甲基乙醯胺、N-甲基-2-吡咯啶酮等。該等溶劑可僅使用1種,亦可組合使用2種以上。再者,較佳為使此處所使用之溶劑直接殘留而進行末端封端反應或化學醯亞胺化反應。 Examples of the solvent used in the hydrazine imidization reaction include N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, and dimethyl. Kea and others. Among these, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and the like are preferred. These solvents may be used alone or in combination of two or more. Further, it is preferred to carry out the terminal blocking reaction or the chemical oxime imidization reaction by directly leaving the solvent used herein.

作為熱醯亞胺化反應中所使用之觸媒,可列舉三甲胺、三乙胺、三丙胺、三丁胺、三乙醇胺、吡啶、N,N-二甲基乙醇胺、N,N-二乙基乙醇胺、三伸乙基二胺、N-甲基吡咯啶、N-乙基吡咯啶、N-甲基哌啶、N-乙基哌啶、咪唑、喹啉、異喹啉等。該等觸媒可僅使用1種,亦可組合使用2種以上。 Examples of the catalyst used in the thermal imidization reaction include trimethylamine, triethylamine, tripropylamine, tributylamine, triethanolamine, pyridine, N,N-dimethylethanolamine, and N,N-diethyl. Ethylethanolamine, tri-ethylenediamine, N-methylpyrrolidine, N-ethylpyrrolidine, N-methylpiperidine, N-ethylpiperidine, imidazole, quinoline, isoquinoline and the like. These catalysts may be used alone or in combination of two or more.

熱醯亞胺化反應中之反應溫度較佳為120~200℃,更佳為130~190℃。又,熱醯亞胺化反應可於常壓(0.1MPa)下、減壓下及加壓下之任一者進行,但通常係於常壓下進行。又,熱醯亞胺化反應之反應時間通常為2小時,較佳為4小時~20小時。 The reaction temperature in the thermal imidization reaction is preferably from 120 to 200 ° C, more preferably from 130 to 190 ° C. Further, the thermal hydrazine imidization reaction can be carried out under normal pressure (0.1 MPa), under reduced pressure, and under pressure, but it is usually carried out under normal pressure. Further, the reaction time of the thermal imidization reaction is usually 2 hours, preferably 4 hours to 20 hours.

又,熱醯亞胺化反應較佳為於惰性氣體環境下進行,例如較佳為於氮氣環境下進行。進而,為了使熱醯亞胺化反應充分地進行,較佳為去除因醯亞胺化反應而產生之水,若於溶劑中添加甲苯或 二甲苯等共沸脫水劑,則可提高水之去除效率。 Further, the heat imidization reaction is preferably carried out under an inert gas atmosphere, for example, preferably under a nitrogen atmosphere. Further, in order to sufficiently carry out the thermal hydrazine imidization reaction, it is preferred to remove water generated by the hydrazine imidization reaction, and if toluene is added to the solvent or An azeotropic dehydrating agent such as xylene can improve water removal efficiency.

[末端封端反應步驟] [End capping reaction step]

於本發明中,所謂「末端封端反應步驟」,意指藉由末端封端劑將聚醯亞胺之末端胺基進行封端之步驟。 In the present invention, the "end capping reaction step" means a step of blocking the terminal amine group of the polyimine by a terminal blocking agent.

作為末端封端反應步驟中所使用之末端封端劑,只要為與胺基反應而形成穩定之構造者,則無特別限制,例如可列舉鄰苯二甲酸酐、琥珀酸酐、1,2-環己烷二羧酸酐、4-甲基環己烷-1,2-二接酸酐、(2-甲基-2-丙烯基)琥珀酸酐等酸酐;苯甲醯氯等有機醯氯等。以上列舉之末端封端劑可僅使用1種,亦可組合使用數種。再者,於將本發明之熱可塑性聚醯亞胺之末端酸酐基進行封端之情形時,亦可使用3-胺基苯基乙炔、苯胺、環己胺等胺化合物作為末端封端劑。但是,末端酸酐基之封端不符合本發明中之末端胺基之封端。 The terminal blocking agent used in the terminal end-capping reaction step is not particularly limited as long as it forms a stable structure by reacting with an amine group, and examples thereof include phthalic anhydride, succinic anhydride, and 1,2-ring. An acid anhydride such as hexane dicarboxylic anhydride, 4-methylcyclohexane-1,2-dihydroanhydride or (2-methyl-2-propenyl) succinic anhydride; or organic ruthenium chloride such as benzamidine chloride. The above-mentioned terminal blocking agents may be used alone or in combination of several kinds. Further, when the terminal acid anhydride group of the thermoplastic polyimine of the present invention is blocked, an amine compound such as 3-aminophenylacetylene, aniline or cyclohexylamine may be used as the terminal blocking agent. However, the termination of the terminal anhydride group does not conform to the termination of the terminal amine group in the present invention.

關於末端封端劑之使用量,相對於用作原料之二胺化合物之mol數與酸二酐之mol數之差(未反應之一級胺基量),較佳為1~10倍之當量數,更佳為2~8倍之當量數。若末端封端劑之使用量為上述下限值以上,則提高末端胺基之封端率,因此較佳,另一方面,若為上述上限值以下,則未反應之末端封端劑之精製處理變少,因此較佳。再者,於不進行下述化學醯亞胺化反應步驟之情形時,增加末端封端劑之使用量可提高末端胺基之封端率,因此較佳。 Regarding the amount of the terminal blocking agent used, the difference between the number of moles of the diamine compound used as the raw material and the number of moles of the acid dianhydride (the amount of the unreacted primary amine group) is preferably from 1 to 10 times the equivalent amount. More preferably, it is 2 to 8 times the equivalent number. When the amount of the terminal blocking agent used is at least the above lower limit value, the terminal blocking ratio of the terminal amine group is increased, which is preferable. On the other hand, if it is at most the above upper limit value, the unreacted terminal blocking agent is used. Since the refining treatment is small, it is preferable. Further, in the case where the chemical imidization reaction step described below is not carried out, it is preferred to increase the amount of the terminal blocking agent to increase the terminal blocking ratio of the terminal amine group.

末端封端反應較佳為於溶劑中進行。作為末端封端反應中所使用之溶劑,可列舉N,N-二甲基甲醯胺、N,N-二甲基乙醯胺及N-甲基-2-吡咯啶酮、二甲基亞碸等。於該等之中,較佳為N,N-二甲基乙醯胺、N-甲基-2-吡咯啶酮等。該等溶劑可僅使用1種,亦可組合使用 2種以上。 The end capping reaction is preferably carried out in a solvent. Examples of the solvent used in the terminal end-capping reaction include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and dimethylene. Hey. Among these, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and the like are preferred. These solvents may be used alone or in combination. 2 or more types.

末端封端反應步驟中之反應溫度通常為80~200℃,較佳為120~200℃。又,熱醯亞胺化反應可於常壓(0.1MPa)下、減壓下及加壓下之任一者進行,但通常係於常壓下進行。又,末端封端反應之反應時間通常為1小時以上,較佳為2小時~10小時。 The reaction temperature in the terminal end-capping reaction step is usually from 80 to 200 ° C, preferably from 120 to 200 ° C. Further, the thermal hydrazine imidization reaction can be carried out under normal pressure (0.1 MPa), under reduced pressure, and under pressure, but it is usually carried out under normal pressure. Further, the reaction time of the terminal end-capping reaction is usually 1 hour or longer, preferably 2 hours to 10 hours.

[化學醯亞胺化反應步驟] [Chemical hydrazine imidation reaction step]

於本發明中,所謂「化學醯亞胺化反應步驟」,通常意指將聚醯亞胺與有機胺化合物及脫水縮合劑於溶劑中混合而進行醯亞胺化反應之步驟。 In the present invention, the "chemical hydrazine imidation reaction step" generally means a step of mixing a polyimine with an organic amine compound and a dehydrating condensing agent in a solvent to carry out a hydrazine imidization reaction.

作為化學醯亞胺化反應步驟中所使用之有機胺化合物,可列舉三甲胺、三乙胺、三丙胺、三丁胺等三級烷基胺類;三乙醇胺、N,N-二甲基乙醇胺、N,N-二乙基乙醇胺等烷醇胺類;三伸乙基二胺等伸烷基二胺類;吡啶等吡啶類;N-甲基吡咯啶、N-乙基吡咯啶等吡咯啶類;N-甲基哌啶、N-乙基哌啶等哌啶類;咪唑等咪唑類;喹啉、異喹啉等喹啉類等。該等觸媒可僅使用1種,亦可組合使用2種以上。有機胺化合物之使用量相對於聚醯亞胺樹脂之固形份,較佳為0.1重量%以上且未滿15重量%,更佳為0.5重量%以上且未滿5重量%。 Examples of the organic amine compound used in the chemical hydrazine imidization reaction step include tertiary alkylamines such as trimethylamine, triethylamine, tripropylamine and tributylamine; triethanolamine and N,N-dimethylethanolamine. , alkanolamines such as N,N-diethylethanolamine; alkyldiamines such as tri-ethylidene diamine; pyridines such as pyridine; pyrrolidines such as N-methylpyrrolidine and N-ethylpyrrolidine Classes; piperidines such as N-methylpiperidine and N-ethylpiperidine; imidazoles such as imidazole; quinolines such as quinoline and isoquinoline. These catalysts may be used alone or in combination of two or more. The amount of the organic amine compound to be used is preferably 0.1% by weight or more and less than 15% by weight, more preferably 0.5% by weight or more and less than 5% by weight based on the solid content of the polyimide resin.

作為化學醯亞胺化反應步驟中所使用之脫水縮合劑,可列舉乙酸酐、三氟乙酸酐、氯乙酸酐等酸酐;N,N-二環己基碳二醯亞胺、N,N-二苯基碳二醯亞胺等N,N-二取代碳二醯亞胺等。該等脫水劑可僅使用1種,亦可組合使用2種以上。脫水劑之使用量相對於聚醯亞胺樹脂固形份,較佳為0.1重量%以上,更佳為0.5重量%以上,尤 其是為了不經過末端封端步驟而獲得本發明之熱可塑性聚醯亞胺,較佳為使用大量脫水縮合劑,具體而言,較佳為使用15重量%以上。另一方面,脫水縮合劑之使用量之上限較佳為30重量%以下,更佳為25重量%以下。 Examples of the dehydrating condensing agent used in the chemical hydrazine imidization reaction step include acid anhydrides such as acetic anhydride, trifluoroacetic anhydride, and chloroacetic anhydride; N,N-dicyclohexylcarbodiimide, N,N-di N,N-disubstituted carbodiimide or the like such as phenylcarbodiimide. These dehydrating agents may be used alone or in combination of two or more. The amount of the dehydrating agent used is preferably 0.1% by weight or more, more preferably 0.5% by weight or more, based on the solid content of the polyimide component. This is to obtain the thermoplastic polyimine of the present invention without undergoing the terminal blocking step, and it is preferred to use a large amount of the dehydrating condensing agent. Specifically, it is preferably 15% by weight or more. On the other hand, the upper limit of the amount of use of the dehydrating condensing agent is preferably 30% by weight or less, more preferably 25% by weight or less.

作為化學醯亞胺化反應步驟中所使用之溶劑,可列舉N,N-二甲基甲醯胺、N,N-二甲基乙醯胺、N-甲基-2-吡咯啶酮、二甲基亞碸等。於該等之中,較佳為N,N-二甲基乙醯胺、N-甲基-2-吡咯啶酮等。該等溶劑可僅使用1種,亦可組合使用2種以上。 Examples of the solvent used in the chemical hydrazine imidization reaction step include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, and Methyl hydrazine and the like. Among these, N,N-dimethylacetamide, N-methyl-2-pyrrolidone and the like are preferred. These solvents may be used alone or in combination of two or more.

化學醯亞胺化反應步驟之反應溫度通常為40~200℃,較佳為50~160℃。又,化學醯亞胺化反應可於常壓(0.1MPa)下、減壓下及加壓下之任一者進行,但通常係於常壓下進行。又,化學醯亞胺化反應之反應時間通常為30分鐘以上,較佳為1小時~6小時。 The reaction temperature of the chemical hydrazine imidization reaction step is usually 40 to 200 ° C, preferably 50 to 160 ° C. Further, the chemical hydrazine imidization reaction can be carried out under normal pressure (0.1 MPa), under reduced pressure, and under pressure, but it is usually carried out under normal pressure. Further, the reaction time of the chemical hydrazine imidization reaction is usually 30 minutes or longer, preferably 1 hour to 6 hours.

再者,所獲得之聚醯亞胺較佳為藉由再沈澱、洗淨、過濾等而精製。藉由該精製,可去除殘留於系統中之原料或觸媒。 Further, the obtained polyimine is preferably purified by reprecipitation, washing, filtration, or the like. By this refining, the raw materials or catalyst remaining in the system can be removed.

[添加劑之調配] [Additive Addition]

於本發明之熱可塑性聚醯亞胺中,可於不損害本發明之效果之範圍內調配各種添加劑。作為添加劑,例如可列舉抗氧化劑、紫外線吸收劑、光穩定劑、抗靜電劑等。 In the thermoplastic polyimine of the present invention, various additives can be formulated within a range not impairing the effects of the present invention. Examples of the additive include an antioxidant, an ultraviolet absorber, a light stabilizer, an antistatic agent, and the like.

於以上列舉之添加劑之中,較佳為使用抗氧化劑。作為抗氧化劑,例如可列舉酚系抗氧化劑、硫系抗氧化劑、磷系抗氧化劑等。該等抗氧化劑可僅使用1種,亦可組合使用2種以上。 Among the above-exemplified additives, it is preferred to use an antioxidant. Examples of the antioxidant include a phenol-based antioxidant, a sulfur-based antioxidant, and a phosphorus-based antioxidant. These antioxidants may be used alone or in combination of two or more.

[聚醯亞胺成形體] [Polyimide molded body]

藉由使本發明之熱可塑性聚醯亞胺成形,可獲得聚醯亞胺成形體。 By molding the thermoplastic polyimine of the present invention, a polyimine molded article can be obtained.

[成形方法] [Forming method]

於本發明中,熱可塑性聚醯亞胺成形體之成形方法並無特別限制。成形方法可配合各種用途採用,例如可列舉擠出成形法、射出成形法、中空成形法、壓縮成型法等。進而,利用該等方法形成而獲得之熱可塑性聚醯亞胺形成體可藉由積層成形法、輥加工法、延伸加工法、衝壓加工法、熱壓法等加工方法進行加工。於該等之中,如上所述,本發明之熱可塑性聚醯亞胺之熔融熱穩定性顯著優異,因此可進行利用熔融擠出成形之成形,又,熔融擠出成形於製造時間、步驟數等觀點而言可有效率地製造,因此較佳。 In the present invention, the method of forming the thermoplastic polyimide body is not particularly limited. The molding method can be used in various applications, and examples thereof include an extrusion molding method, an injection molding method, a hollow molding method, and a compression molding method. Further, the thermoplastic polyimine formed body formed by these methods can be processed by a processing method such as a laminate molding method, a roll processing method, an extension processing method, a press working method, or a hot pressing method. Among these, as described above, the thermoplastic polyimine of the present invention has remarkably excellent melt heat stability, so that it can be formed by melt extrusion molding, and melt extrusion molding can be carried out in the production time and the number of steps. It is preferable to manufacture it efficiently, and it is preferable.

關於熱可塑性聚醯亞胺成形體之成形條件並無特別限制。於進行擠出成形之情形時,亦可使用單軸擠出機或雙軸擠出機中之任一擠出機。擠出機之缸體之溫度通常為280℃~380℃,自模具擠出之聚醯亞胺係利用冷卻輥進行冷卻。冷卻輥之溫度通常為0℃~60℃。 The molding conditions of the thermoplastic polyimine molded body are not particularly limited. In the case of extrusion molding, either one of a single screw extruder or a twin screw extruder may be used. The temperature of the cylinder of the extruder is usually 280 ° C to 380 ° C, and the polyimide extruded from the die is cooled by a cooling roll. The temperature of the chill roll is usually from 0 ° C to 60 ° C.

[物性] [physical property]

本發明之熱可塑性聚醯亞胺成形體係透明性優異者。熱可塑性聚醯亞胺成形體之透明性係藉由基於JIS K7105(1981年)之全光線透過率進行評價,較佳為70%以上,更佳為75%以上,進而較佳為80%以上,尤佳為85%以上。此時之熱可塑性聚醯亞胺薄膜之厚度並無特別限制,通常為0.01~10mm,較佳為0.02~5mm,尤佳為0.03~1mm。 The thermoplastic polyimine molding system of the present invention is excellent in transparency. The transparency of the thermoplastic polyimide polyimide is evaluated by the total light transmittance based on JIS K7105 (1981), preferably 70% or more, more preferably 75% or more, still more preferably 80% or more. , especially good for more than 85%. The thickness of the thermoplastic polyimide film at this time is not particularly limited and is usually 0.01 to 10 mm, preferably 0.02 to 5 mm, and particularly preferably 0.03 to 1 mm.

[用途] [use]

由本發明之熱可塑性聚醯亞胺所獲得之熱可塑性聚醯亞胺成形體係透明性、耐熱性、耐溶劑性、成形性、溶劑非揮發性等優異者。因此,不僅可應用於聚醯亞胺成形體之代表性之用途即薄膜用途,亦可應用於廣泛之用途。例如可用於撓性太陽能電池用構件、顯示器用構件、IC包裝用托盤、IC製造步驟用托盤、IC插座、晶圓載體、連接器、插座、硬碟載體、液晶顯示器載體、晶體振盪器製造用托盤、影印機用分離爪、影印機用隔熱軸承、影印機用齒輪、推力墊圈、傳輸環、活塞環、油封環、軸承護圈、齒輪泵、輸送鏈、拉伸機用滑套、耐熱絕緣帶、耐熱黏著帶、高密度磁記錄基底、電容器或軟性印刷基板用之薄膜等。又,例如亦可用於利用玻璃纖維或碳纖維等進行補強之構造構件、小型線圈之線軸或終端絕緣用管之成形品之製造。又,可用於絕緣間隔件、磁頭間隔件或變壓器之間隔件等積層材料之製造。又,可用於電線/電纜絕緣被覆材料、低溫儲存罐、宇宙隔熱材料或積體電路等之搪瓷塗層材料之製造。進而,亦可用於具有耐熱性之紗、織物或不織布等之製造。 The thermoplastic polyimine molding system obtained from the thermoplastic polyimine of the present invention is excellent in transparency, heat resistance, solvent resistance, moldability, solvent non-volatility and the like. Therefore, it can be applied not only to a representative use of a polyimide bismuth molded article, that is, to a film, but also to a wide range of applications. For example, it can be used for flexible solar cell members, display members, IC packaging trays, IC manufacturing step trays, IC sockets, wafer carriers, connectors, sockets, hard disk carriers, liquid crystal display carriers, and crystal oscillators. Separating claws for trays and photocopiers, heat-insulating bearings for photocopiers, gears for photocopiers, thrust washers, transmission rings, piston rings, oil seal rings, bearing retainers, gear pumps, conveyor chains, sliding sleeves for stretching machines, heat-resistant Insulating tape, heat-resistant adhesive tape, high-density magnetic recording substrate, capacitor or film for flexible printed circuit board, etc. Further, for example, it can be used for the production of a molded article which is reinforced by a glass fiber, a carbon fiber or the like, a bobbin of a small coil, or a tube for terminal insulation. Moreover, it can be used for the manufacture of a laminated material such as an insulating spacer, a magnetic head spacer or a spacer of a transformer. Moreover, it can be used for the manufacture of enamel coating materials such as wire/cable insulation coating materials, low temperature storage tanks, cosmic heat insulating materials or integrated circuits. Further, it can also be used for the production of heat-resistant yarns, woven fabrics, nonwoven fabrics, and the like.

[實施例] [Examples]

以下,藉由實施例更具體地說明本發明,但本發明只要不超出其要旨,則不限定於以下之例。再者,以下之實施例中之各種製造條件或評價結果之值係具有作為本發明之實施態樣中之上限或下限之較佳值之含義者,較佳之範圍可為以上述上限或下限之值與後揭實施例之值或實施例彼此之值的組合所規定之範圍。 Hereinafter, the present invention will be specifically described by way of examples, but the present invention is not limited to the following examples as long as the gist of the invention is not exceeded. In addition, the values of various manufacturing conditions or evaluation results in the following examples have the meanings of the preferred values of the upper or lower limit in the embodiment of the present invention, and the preferred range may be the above upper or lower limit. The values are within the ranges specified by the combination of the values of the examples or the values of the embodiments.

[聚醯亞胺之評價方法] [Evaluation method of polyimine]

以下之實施例中所製造之聚醯亞胺之構造、物性等之評價方法如下所述。 The evaluation methods of the structure, physical properties and the like of the polyimine produced in the following examples are as follows.

[末端胺基之封端率] [End-capped amine group capping rate]

末端胺基之封端率係進行1H-NMR測定,以下述方式求出。 The blocking ratio of the terminal amine group was measured by 1 H-NMR and determined in the following manner.

相對於聚醯亞胺中之由ODA構成單位所得之末端胺基將鄰位峰(6.75ppm)之積分值設為S1,將胺基末端被封端而移位之峰(7.61ppm)之積分值設為S2。根據以下之式,由該等值求出末端胺基之封端率。 The terminal amino group obtained from the ODA constituent unit in the polyimine has an integral value of the ortho peak (6.75 ppm) as S 1 and a peak at which the amine terminal is blocked and displaced (7.61 ppm). The integral value is set to S 2 . The blocking ratio of the terminal amine group was determined from the equivalent value according to the following formula.

(末端胺基之封端率)=100×[S2/(S1+S2)] (end capping rate of terminal amine group) = 100 × [S 2 / (S 1 + S 2 )]

(1H-NMR測定條件) ( 1 H-NMR measurement conditions)

溶劑:DMF-d7(N,N-二甲基甲醯胺-d7) Solvent: DMF-d7 (N,N-dimethylformamide-d7)

頻率:400MHz Frequency: 400MHz

標準物質:DMF-d7 2.74ppm Reference material: DMF-d7 2.74ppm

累積次數:256次 Cumulative number: 256 times

弛豫時間(relaxation time):1秒 Relaxation time: 1 second

[醯亞胺化率] [醯imination rate]

醯亞胺化率係根據末端胺基之封端率之測定中獲得之NMR圖表,以下述方式由醯胺酸殘留率而求出。 The ruthenium iodide ratio was determined from the methionine residual ratio in the following manner based on the NMR chart obtained by measuring the terminal group ratio of the terminal amine group.

觀測聚醯亞胺中之H-BPDA構成單位中之5個質子為1.0~2.0ppm。 It was observed that 5 protons of the H-BPDA constituent units in the polyimine were 1.0 to 2.0 ppm.

將該峰群之積分值之合計設為S3。將由殘留於聚醯亞胺中之醯胺酸構造之醯胺氫產生之峰(9.3~10.3ppm)之積分值設為S4。根據以下之式,由該等值求出醯亞胺化率。 The total of the integrated values of the peak group is set to S 3 . The integral value of the peak (9.3 to 10.3 ppm) generated by the hydrogenation of the indoleamine structure of the proline acid remaining in the polyimine was set to S 4 . The ruthenium imidization ratio was determined from the above values according to the following formula.

(醯亞胺化率)=100×[1-(5S4/S3)] (醯imination rate)=100×[1-(5S 4 /S 3 )]

[重量平均分子量(Mw)] [Weight average molecular weight (Mw)]

本發明之聚醯亞胺之聚苯乙烯換算之重量平均分子量係藉由凝膠滲透層析法(GPC),利用下述方法求出。首先,於下述條件下測定標準聚苯乙烯之GPC,並製作檢量線。繼而藉由相同之條件測定試樣(聚醯亞胺)之GPC,而求出聚苯乙烯換算之平均分子量。 The polystyrene-equivalent weight average molecular weight of the polyimine of the present invention is determined by gel permeation chromatography (GPC) by the following method. First, GPC of standard polystyrene was measured under the following conditions, and a calibration curve was prepared. Then, the GPC of the sample (polyimine) was measured under the same conditions to obtain an average molecular weight in terms of polystyrene.

(GPC測定條件) (GPC measurement conditions)

管柱:昭和電工公司製造之Shodex AD-80M/S 3根 Pipe column: Shodex AD-80M/S 3 manufactured by Showa Denko

前置管柱:昭和電工公司製造之Shodex KF-G 1根 Front column: Shodex KF-G 1 manufactured by Showa Denko

溶劑:N,N-二甲基甲醯胺(含有50mmol/L之LiBr) Solvent: N,N-dimethylformamide (containing 50 mmol/L of LiBr)

流速:1.0mL/min Flow rate: 1.0mL/min

溫度:管柱35℃ Temperature: column 35 ° C

試樣濃度:0.5重量% Sample concentration: 0.5% by weight

檢測器:UV檢測器 Detector: UV detector

校準試樣:單分散標準聚苯乙烯 Calibration sample: monodisperse standard polystyrene

[複數剪切黏度(η*)、複數剪切黏度之變化率] [complex shear viscosity (η*), rate of change of complex shear viscosity]

使用旋轉型流變儀(TA Instruments公司製造,ARES-100),於下述測定條件下測定頻率1Hz時之初期複數剪切黏度(η*0)及60分鐘後之複數剪切黏度(η*60)。 The initial complex shear viscosity (η* 0 ) at a frequency of 1 Hz and the complex shear viscosity after 60 minutes (η*) were measured using a rotary rheometer (manufactured by TA Instruments, ARES-100) under the following measurement conditions. 60 ).

(旋轉型流變儀測定條件) (rotation type rheometer measurement conditions)

旋轉型流變儀(ARES)之時間分散測定之治具係使用直徑25mm之水平板。 A time-dispersion measuring tool for a rotary rheometer (ARES) uses a horizontal plate having a diameter of 25 mm.

測定溫度:310℃ Measurement temperature: 310 ° C

角頻率:1rad/s Angular frequency: 1rad/s

應變:1% Strain: 1%

預熱時間:5分鐘 Warm-up time: 5 minutes

測定時間:0~60分鐘 Measurement time: 0~60 minutes

[3,3',4,4'-聯環己基四羧酸二酐(H-BPDA)之合成] Synthesis of [3,3',4,4'-bicyclohexyltetracarboxylic dianhydride (H-BPDA)] <合成例1> <Synthesis Example 1>

將3,3',4,4'-聯苯四羧酸二酐(三菱化學股份有限公司製造)150重量份溶解於使氫氧化鈉83.3重量份溶解於水593重量份而成之溶液中,而製作3,3',4,4'-聯苯四羧酸四鈉鹽之水溶液,並對該鹽使用釕/碳觸媒,於10MPaG(相對於大氣之相對壓力)、120℃下使芳香環氫化。其次,滴加49%硫酸水溶液429重量份,並將所析出之固體過濾,藉此獲得3,3',4,4'-聯環己基四羧酸(H-BTC)。 150 parts by weight of 3,3',4,4'-biphenyltetracarboxylic dianhydride (manufactured by Mitsubishi Chemical Corporation) was dissolved in a solution obtained by dissolving 83.3 parts by weight of sodium hydroxide in 593 parts by weight of water. An aqueous solution of 3,3',4,4'-biphenyltetracarboxylic acid tetrasodium salt is prepared, and the salt is scented at 10 MPaG (relative pressure relative to the atmosphere) at 120 ° C using a ruthenium/carbon catalyst. Ring hydrogenation. Next, 429 parts by weight of a 49% aqueous sulfuric acid solution was added dropwise, and the precipitated solid was filtered, whereby 3,3',4,4'-bicyclohexyltetracarboxylic acid (H-BTC) was obtained.

將所獲得之H-BTC 33.7重量份及乙酸酐90重量份於氮氣下添加至反應器中。一面攪拌該混合物一面升溫,並於迴流溫度(130℃~140℃)下反應3小時。於反應後,將反應溶液冷卻至10℃,並將固體過濾,藉此獲得白色之結晶。將所獲得之結晶利用甲苯洗淨,並利用減壓乾燥機進行乾燥,藉此獲得3,3',4,4'-聯環己基四羧酸二酐(H-BPDA)。 33.7 parts by weight of the obtained H-BTC and 90 parts by weight of acetic anhydride were added to the reactor under nitrogen. The mixture was heated while stirring, and reacted at a reflux temperature (130 ° C to 140 ° C) for 3 hours. After the reaction, the reaction solution was cooled to 10 ° C, and the solid was filtered, whereby white crystals were obtained. The obtained crystals were washed with toluene and dried by a vacuum dryer to obtain 3,3',4,4'-bicyclohexyltetracarboxylic dianhydride (H-BPDA).

[聚醯亞胺之製造] [Manufacture of polyimine] <實施例1-1> <Example 1-1>

於設置有乾燥氮氣導入管、冷卻器、冷凝器、攪拌機之反應器中, 添加合成例1中獲得之H-BPDA 60.0重量份、4,4-二胺基二苯醚(ODA)40.0重量份、N,N-二甲基乙醯胺200重量份及甲苯95重量份。其次,將反應器內設為氮氣環境,並將內溫加熱至145℃而進行熱醯亞胺化反應。將伴隨醯亞胺化產生之水與甲苯一同共沸去除。繼續加熱12小時、迴流、攪拌,可不再認為有水之產生。 In a reactor provided with a dry nitrogen introduction pipe, a cooler, a condenser, and a mixer, 60.0 parts by weight of H-BPDA obtained in Synthesis Example 1, 40.0 parts by weight of 4,4-diaminodiphenyl ether (ODA), 200 parts by weight of N,N-dimethylacetamide, and 95 parts by weight of toluene were added. Next, the inside of the reactor was set to a nitrogen atmosphere, and the internal temperature was heated to 145 ° C to carry out a thermal hydrazine imidization reaction. The water produced by the imidization of hydrazine is azeotropically removed together with toluene. Heating is continued for 12 hours, refluxed, and stirred, and no water is considered to be produced.

繼而,添加鄰苯二甲酸酐2.2重量份,並於145℃下攪拌3小時,而進行末端封端反應。於攪拌3小時後,一面於減壓下去除甲苯一面加熱1小時。將內溫冷卻至60℃後,添加三乙胺1.0重量份、乙酸酐2.0重量份,並於60℃下攪拌3小時進行化學醯亞胺化反應,而獲得聚醯亞胺溶液。將所獲得之聚醯亞胺溶液滴加至甲醇中,將所析出之聚醯亞胺過濾回收,於減壓下以80℃乾燥3小時後,於減壓下以150℃乾燥3小時,而獲得聚醯亞胺之固體。將所獲得之聚醯亞胺之物性示於表1。 Then, 2.2 parts by weight of phthalic anhydride was added, and the mixture was stirred at 145 ° C for 3 hours to carry out a terminal end-capping reaction. After stirring for 3 hours, the toluene was removed under reduced pressure while heating for 1 hour. After cooling the internal temperature to 60 ° C, 1.0 part by weight of triethylamine and 2.0 parts by weight of acetic anhydride were added, and the mixture was stirred at 60 ° C for 3 hours to carry out a chemical hydrazine imidization reaction to obtain a polyimine solution. The obtained polyimine solution was added dropwise to methanol, and the precipitated polyimine was collected by filtration, dried at 80 ° C for 3 hours under reduced pressure, and then dried at 150 ° C for 3 hours under reduced pressure. A solid of polyimine is obtained. The physical properties of the obtained polyimine are shown in Table 1.

<實施例1-2> <Example 1-2>

於實施例1-1中,將原料組成變更為表1所示之組成,除此以外,以與實施例1-1同樣之方式製造,而獲得聚醯亞胺。將所獲得之聚醯亞胺之物性示於表1。 In the same manner as in Example 1-1, except that the composition of the raw material was changed to the composition shown in Table 1, except that the composition of the raw material was changed, the polyimine was obtained. The physical properties of the obtained polyimine are shown in Table 1.

<實施例1-3> <Example 1-3>

於實施例1-1中,使用吡啶代替三乙胺,並將原料組成變更為表1-1所示之組成,除此以外,以與實施例1-1同樣之方式製造,而獲得聚醯亞胺。將所獲得之聚醯亞胺之物性示於表1。 In the same manner as in Example 1-1, except that pyridine was used instead of triethylamine, and the composition of the raw material was changed to the composition shown in Table 1-1, the polyfluorene was obtained. Imine. The physical properties of the obtained polyimine are shown in Table 1.

<實施例1-4> <Example 1-4>

於設置有乾燥氮氣導入管、冷卻器、冷凝器、攪拌機之反應器中,添加合成例1中獲得之H-BPDA 59.1重量份、4,4-二胺基二苯醚(ODA)40.9重量份、N,N-二甲基乙醯胺200重量份及甲苯95重量份。其次,將反應器內設為氮氣環境,將內溫加熱至145℃,並將伴隨醯亞胺化產生之水與甲苯一同共沸去除。繼續加熱12小時、迴流、攪拌,可不再認為有水之產生。 59.1 parts by weight of H-BPDA obtained in Synthesis Example 1 and 40.9 parts by weight of 4,4-diaminodiphenyl ether (ODA) were added to a reactor equipped with a dry nitrogen gas introduction tube, a cooler, a condenser, and a stirrer. 200 parts by weight of N,N-dimethylacetamide and 95 parts by weight of toluene. Next, the inside of the reactor was set to a nitrogen atmosphere, the internal temperature was heated to 145 ° C, and the water produced by the imidization of hydrazine was azeotropically removed together with toluene. Heating is continued for 12 hours, refluxed, and stirred, and no water is considered to be produced.

繼而,添加鄰苯二甲酸酐6.0重量份,並於145℃下攪拌3小時。於攪拌3小時後,一面於減壓下去除甲苯一面加熱1小時,而獲得聚醯亞胺溶液。將所獲得之聚醯亞胺溶液滴加至甲醇中,將所析出之聚醯亞胺過濾回收,於減壓下以80℃乾燥3小時後,於減壓下以150℃乾燥3小時,而獲得聚醯亞胺之固體。將所獲得之聚醯亞胺之物性示於表1。 Then, 6.0 parts by weight of phthalic anhydride was added, and the mixture was stirred at 145 ° C for 3 hours. After stirring for 3 hours, the toluene was removed under reduced pressure while heating for 1 hour to obtain a polyimine solution. The obtained polyimine solution was added dropwise to methanol, and the precipitated polyimine was collected by filtration, dried at 80 ° C for 3 hours under reduced pressure, and then dried at 150 ° C for 3 hours under reduced pressure. A solid of polyimine is obtained. The physical properties of the obtained polyimine are shown in Table 1.

<實施例1-5~1-7> <Examples 1-5 to 1-7>

於實施例1-1中,將原料組成變更為表1所示之組成,除此以外,以與實施例1-1同樣之方式製造,而獲得聚醯亞胺。將所獲得之各個聚醯亞胺之物性示於表1。 In the same manner as in Example 1-1, except that the composition of the raw material was changed to the composition shown in Table 1, except that the composition of the raw material was changed, the polyimine was obtained. The physical properties of each of the obtained polyimines are shown in Table 1.

<實施例1-8> <Example 1-8>

於設置有乾燥氮氣導入管、冷卻器、冷凝器、攪拌機之反應器中,添加合成例1中獲得之H-BPDA 60.0重量份、4,4-二胺基二苯醚(ODA)40.0重量份、N,N-二甲基乙醯胺200重量份及甲苯95重量份。其次,將反應器內設為氮氣環境,將內溫加熱至145℃,並將伴隨醯亞 胺化產生之水與甲苯一同共沸去除。繼續加熱12小時、迴流、攪拌,可不再認為有水之產生。 60.0 parts by weight of H-BPDA obtained in Synthesis Example 1 and 40.0 parts by weight of 4,4-diaminodiphenyl ether (ODA) were added to a reactor equipped with a dry nitrogen gas introduction tube, a cooler, a condenser, and a stirrer. 200 parts by weight of N,N-dimethylacetamide and 95 parts by weight of toluene. Next, set the inside of the reactor to a nitrogen atmosphere, and heat the internal temperature to 145 ° C. The water produced by the amination is azeotropically removed together with toluene. Heating is continued for 12 hours, refluxed, and stirred, and no water is considered to be produced.

繼而,將內溫冷卻至60℃後,添加三乙胺10重量份、乙酸酐20重量份,並於60℃下攪拌3小時,而獲得聚醯亞胺溶液。將所獲得之聚醯亞胺溶液滴加至甲醇中,將所析出之聚醯亞胺過濾回收,於減壓下以80℃乾燥3小時後,於減壓下以150℃乾燥3小時,而獲得聚醯亞胺之固體。將所獲得之各個聚醯亞胺之物性示於表1。 Then, after cooling the internal temperature to 60 ° C, 10 parts by weight of triethylamine and 20 parts by weight of acetic anhydride were added, and the mixture was stirred at 60 ° C for 3 hours to obtain a polyimine solution. The obtained polyimine solution was added dropwise to methanol, and the precipitated polyimine was collected by filtration, dried at 80 ° C for 3 hours under reduced pressure, and then dried at 150 ° C for 3 hours under reduced pressure. A solid of polyimine is obtained. The physical properties of each of the obtained polyimines are shown in Table 1.

<實施例1-9> <Example 1-9>

於實施例1-4中,將原料組成變更為表1所示之組成,除此以外,以與實施例1-1同樣之方式製造,而獲得聚醯亞胺。將所獲得之聚醯亞胺之物性示於表1。 In the same manner as in Example 1-1, except that the composition of the raw material was changed to the composition shown in Table 1, except that the composition of the raw material was changed, the polyimine was obtained. The physical properties of the obtained polyimine are shown in Table 1.

<實施例1-10> <Example 1-10>

於實施例1-1中,將原料組成變更為表1所示之組成,除此以外,以與實施例1-1同樣之方式製造,而獲得聚醯亞胺。將所獲得之聚醯亞胺之物性示於表1。 In the same manner as in Example 1-1, except that the composition of the raw material was changed to the composition shown in Table 1, except that the composition of the raw material was changed, the polyimine was obtained. The physical properties of the obtained polyimine are shown in Table 1.

<實施例1-11> <Example 1-11>

於實施例1-8中,將原料組成變更為表1所示之組成,除此以外,以與實施例1-1同樣之方式製造,而獲得聚醯亞胺。將所獲得之聚醯亞胺之物性示於表1。 In the same manner as in Example 1-1, except that the composition of the raw material was changed to the composition shown in Table 1, except that the composition of the raw material was changed, the polyimine was obtained. The physical properties of the obtained polyimine are shown in Table 1.

<比較例1-1~1-5> <Comparative Example 1-1~1-5>

於實施例1-1中,將原料組成變更為表2所示之組成,且不進行末端封端步驟及化學醯亞胺化步驟,除此以外,以與實施例1-1同樣之方式製造,而獲得聚醯亞胺。將所獲得之聚醯亞胺之物性示於表2。 In the same manner as in Example 1-1, except that the composition of the raw material was changed to the composition shown in Table 2, and the end blocking step and the chemical imidization step were not carried out, in the same manner as in Example 1-1. And obtain polyimine. The physical properties of the obtained polyimine are shown in Table 2.

由表1及表2可知,實施例1-1~1-11中獲得之聚醯亞胺之任一者之複數剪切黏度之變化率均為300%以下,與比較例1-1~1-5相比,係熔融熱穩定性優異,而適合於熔融擠出成形之聚醯亞胺。尤其是實施例1-1~1-8中複數剪切黏度之變化率為100%以下,係熔融熱穩定性顯著優異者。 As can be seen from Tables 1 and 2, the rate of change of the complex shear viscosity of any of the polyimine obtained in Examples 1-1 to 1-11 was 300% or less, and Comparative Example 1-1 to 1 Compared with -5, it is excellent in melt heat stability and is suitable for melt extrusion molding of polyimine. In particular, in Examples 1-1 to 1-8, the rate of change of the complex shear viscosity was 100% or less, and the melt heat stability was remarkably excellent.

[聚醯亞胺成形體之評價] [Evaluation of Polyimine Molded Articles]

以下之實施例中所製造之聚醯亞胺之構造、物性等之評價方法如下所述。 The evaluation methods of the structure, physical properties and the like of the polyimine produced in the following examples are as follows.

[耐熱性:玻璃轉移溫度(Tg)] [Heat resistance: glass transition temperature (Tg)]

使用動態熱機械測定裝置(SII Nano Technology股份有限公司製造,DMS/SS6100),於下述測定條件下測定相對於樣品之振動負重之樣品之儲存彈性模數、損失彈性模數,並根據損失正切而求出玻璃轉移溫度(Tg)。Tg越高則評價為耐熱性越優異者。 Using a dynamic thermomechanical measuring device (manufactured by SII Nano Technology Co., Ltd., DMS/SS6100), the storage elastic modulus, the loss elastic modulus of the sample with respect to the vibration load of the sample were measured under the following measurement conditions, and the tangent was calculated according to the loss. The glass transition temperature (Tg) was determined. The higher the Tg, the more excellent the heat resistance was evaluated.

(DMS測定條件) (DMS measurement conditions)

將以試片之儲存彈性模數(E')除以損失彈性模數(E")所得之損失正切(tanδ)之峰頂定義為玻璃轉移溫度。 The peak top of the loss tangent (tan δ) obtained by dividing the storage elastic modulus (E') of the test piece by the loss elastic modulus (E") is defined as the glass transition temperature.

測定溫度範圍:50℃~400℃(升溫速度:2℃/min) Measuring temperature range: 50 ° C ~ 400 ° C (temperature rising rate: 2 ° C / min)

拉伸負荷:5g Tensile load: 5g

樣品形狀:10mm×10mm Sample shape: 10mm × 10mm

樣品厚度:記載於表3中 Sample thickness: as described in Table 3

[透明性:全光線透過率] [Transparency: total light transmittance]

對於聚醯亞胺薄膜,按照JIS標準K7105(1981年)測定全光線透過率。全光線透過率越高,評價為透明性越優異者,只要全光線透過率為70%以上,則設為合格。 For the polyimide film, the total light transmittance was measured in accordance with JIS Standard K7105 (1981). The higher the total light transmittance, the more excellent the transparency was evaluated, and the total light transmittance was 70% or more.

[溶劑非揮發性:殘留溶劑量] [Solvent non-volatile: amount of residual solvent]

使用熱重示差熱同步測定裝置(SII Nano Technology股份有限公司製造之TG/DTA6200),按照下述測定條件進行測定。將聚醯亞胺片或聚醯亞胺熔融成形體20mg以升溫速度20℃/min自40℃加溫至100℃後,於100℃下靜置30分鐘。其後,以升溫速度10℃/min自100℃加溫至350℃,將自150℃至300℃之過程中之重量損失定義為殘留溶劑含量。該值越低,評價為溶劑非揮發性越優異者。 The measurement was carried out in accordance with the following measurement conditions using a thermogravimetric differential thermal synchronization measuring apparatus (TG/DTA6200 manufactured by SII Nano Technology Co., Ltd.). 20 mg of the polyimide sheet or the polyimide melt-molded body was heated from 40 ° C to 100 ° C at a temperature increase rate of 20 ° C / min, and then allowed to stand at 100 ° C for 30 minutes. Thereafter, the temperature was increased from 100 ° C to 350 ° C at a heating rate of 10 ° C / min, and the weight loss during the process from 150 ° C to 300 ° C was defined as the residual solvent content. The lower the value, the more excellent the solvent non-volatility was evaluated.

[聚醯亞胺成形體之製造] [Manufacture of polyimine molded body] <實施例2-1> <Example 2-1>

將實施例1-1中獲得之聚醯亞胺供給至單軸擠出機中,於330℃下 熔融後,擠出至設定為120℃之冷卻輥上進行冷卻固化,而獲得厚度100μm之聚醯亞胺薄膜。對所獲得之聚醯亞胺薄膜進行上述評價。將其結果示於表3。 The polyimine obtained in Example 1-1 was supplied to a single screw extruder at 330 ° C After melting, it was extruded onto a cooling roll set to 120 ° C to carry out cooling solidification to obtain a polyimine film having a thickness of 100 μm. The above evaluation was carried out on the obtained polyimide film. The results are shown in Table 3.

<實施例2-2> <Example 2-2>

將實施例1-2中獲得之聚醯亞胺供給至雙軸延伸擠出機中,將於330℃下熔融而獲得之樹脂股線水冷後,利用製粒機切割股線,而獲得聚醯亞胺顆粒。將所獲得之聚醯亞胺顆粒供給至單軸擠出機中,於330℃下熔融後,擠出至設定為120℃之冷卻輥上進行冷卻固化,而獲得厚度100μm之聚醯亞胺薄膜。對所獲得之聚醯亞胺薄膜進行上述評價。將其結果示於表3。 The polyimine obtained in Example 1-2 was supplied to a biaxial stretching extruder, and the resin strand obtained by melting at 330 ° C was water-cooled, and then the strand was cut by a granulator to obtain a polyfluorene. Imine particles. The obtained polyimine particles were supplied to a single-axis extruder, melted at 330 ° C, and then extruded onto a cooling roll set to 120 ° C to be cooled and solidified to obtain a polyimide film having a thickness of 100 μm. . The above evaluation was carried out on the obtained polyimide film. The results are shown in Table 3.

<實施例2-3> <Example 2-3>

使聚醯亞胺薄膜之厚度變為50μm,除此以外,以與實施例2-2同樣之方式實施,而獲得聚醯亞胺薄膜。又,對所獲得之聚醯亞胺薄膜進行上述評價。將其結果示於表3。 A polyimide film was obtained in the same manner as in Example 2-2 except that the thickness of the polyimide film was changed to 50 μm. Further, the obtained polyimide film was subjected to the above evaluation. The results are shown in Table 3.

由表3可知,實施例2-1~2-3中獲得之聚醯亞胺薄膜之透明性、耐熱性優異。可知尤其是加熱前後之重量損失較少,溶劑非 揮發性優異。 As is clear from Table 3, the polyimide films obtained in Examples 2-1 to 2-3 were excellent in transparency and heat resistance. It can be seen that especially the weight loss before and after heating is less, the solvent is not Excellent volatility.

參照特定實施態樣而詳細地說明了本發明,但從業者明瞭可在不脫離本發明之精神與範圍之情況下施加各種變更或修正。本申請案係基於2012年12月17日提出申請之日本專利申請案(日本專利特願2012-274901)者,其內容作為參照而併入本文中。 The present invention has been described in detail with reference to the specific embodiments thereof, but it is understood that various changes and modifications may be made without departing from the spirit and scope of the invention. The present application is based on Japanese Patent Application No. 2012-274901, filed on Dec.

Claims (9)

一種熱可塑性聚醯亞胺,其具有脂環構造,末端胺基之封端率為95.0%以上,且醯亞胺化率為95.8%以上。 A thermoplastic polyimine having an alicyclic structure, a terminal amine group having a terminal blocking ratio of 95.0% or more, and a quinone imidization ratio of 95.8% or more. 如申請專利範圍第1項之熱可塑性聚醯亞胺,其中,重量平均分子量(Mw)為10,000~500,000。 The thermoplastic polyimine of claim 1, wherein the weight average molecular weight (Mw) is from 10,000 to 500,000. 如申請專利範圍第1或2項之熱可塑性聚醯亞胺,其中,上述脂環構造為環己烷環構造。 The thermoplastic polyimine of claim 1 or 2, wherein the alicyclic structure is a cyclohexane ring structure. 如申請專利範圍第1至3項中任一項之熱可塑性聚醯亞胺,其中,上述脂環構造為與醯亞胺環構造共有2個碳原子且鄰接之構造。 The thermoplastic polyimine according to any one of claims 1 to 3, wherein the alicyclic structure has a structure in which two carbon atoms are adjacent to the quinone ring structure. 如申請專利範圍第1至4項中任一項之熱可塑性聚醯亞胺,其中,具有下述式(1)所表示之構造單位及下述式(2)所表示之構造單位之至少一者作為上述脂環構造, The thermoplastic polyimine of any one of the following formula (1), wherein at least one of the structural unit represented by the following formula (1) and the structural unit represented by the following formula (2); As the above alicyclic structure, 如申請專利範圍第1至5項中任一項之熱可塑性聚醯亞胺,其中,進而具有下述式(3)所表示之構造單位,[化2] (上述式(3)中,R1~R8可分別相互不同地為氫原子、碳數1~4之烷基、碳數1~4之氟烷基或羥基,X為直接鍵、氧原子、硫原子、碳數1~4之伸烷基、磺醯基、亞磺醯基、硫基、羰基、醯胺基、酯基或二級胺基,n為0~4之整數)。 The thermoplastic polyimine according to any one of the first to fifth aspects of the present invention, further comprising a structural unit represented by the following formula (3), [Chemical 2] (In the above formula (3), R 1 to R 8 may each independently be a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a fluoroalkyl group having 1 to 4 carbon atoms or a hydroxyl group, and X is a direct bond or an oxygen atom. A sulfur atom, an alkylene group having 1 to 4 carbon atoms, a sulfonyl group, a sulfinyl group, a thio group, a carbonyl group, a decylamino group, an ester group or a secondary amine group, and n is an integer of 0 to 4). 如申請專利範圍第1至6項中任一項之熱可塑性聚醯亞胺,其中,310℃下之複數剪切黏度(η*)為1×102~5×105Pa.s。 The thermoplastic polyimine of any one of claims 1 to 6, wherein the complex shear viscosity (η*) at 310 ° C is 1 × 10 2 ~ 5 × 10 5 Pa. s. 如申請專利範圍第1至7項中任一項之熱可塑性聚醯亞胺,其中,於310℃下經過60分鐘左右之複數剪切黏度之變化率為300%以下。 The thermoplastic polyimine of any one of claims 1 to 7, wherein the rate of change of the complex shear viscosity at about 310 ° C for about 60 minutes is 300% or less. 一種熱可塑性聚醯亞胺成形體,其係使申請專利範圍第1至8項中任一項之熱可塑性聚醯亞胺熔融擠出成形而獲得。 A thermoplastic polyimine molded article obtained by melt-extruding a thermoplastic polyimine of any one of claims 1 to 8.
TW102146827A 2012-12-17 2013-12-17 Thermoplastic polyimide TW201431908A (en)