WO2024133473A1 - Préparation de bois d'érable pour la production de ctmp - Google Patents

Préparation de bois d'érable pour la production de ctmp Download PDF

Info

Publication number
WO2024133473A1
WO2024133473A1 PCT/EP2023/086978 EP2023086978W WO2024133473A1 WO 2024133473 A1 WO2024133473 A1 WO 2024133473A1 EP 2023086978 W EP2023086978 W EP 2023086978W WO 2024133473 A1 WO2024133473 A1 WO 2024133473A1
Authority
WO
WIPO (PCT)
Prior art keywords
chips
impregnation
steamed
impregnated
maple wood
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/EP2023/086978
Other languages
English (en)
Inventor
Thomas Lindstedt
Thomas Granfeldt
Per Engstrand
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Billerud AB
Original Assignee
Billerud AB
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Billerud AB filed Critical Billerud AB
Publication of WO2024133473A1 publication Critical patent/WO2024133473A1/fr
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Abstract

L'invention concerne un procédé de préparation de CTMP chimiothermomécanique à partir de bois d'érable, ledit procédé comprenant les étapes consistant à : a) fournir des copeaux de bois d'érable ayant une longueur moyenne inférieure à 20 mm, par exemple inférieure à 19 mm ; b) laver les copeaux de bois d'érable avec de l'eau ; c) cuire à la vapeur les copeaux de bois d'érable lavés pendant une période d'au moins 15 minutes pour obtenir des copeaux pré-cuits à la vapeur ; d) imprégner les copeaux pré-cuits à la vapeur pour obtenir des copeaux imprégnés ; e) chauffer les copeaux imprégnés pour obtenir des copeaux pré-traités ; et f) défibrer les copeaux pré-traités.
PCT/EP2023/086978 2022-12-21 2023-12-20 Préparation de bois d'érable pour la production de ctmp Ceased WO2024133473A1 (fr)

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
SE2251535-7 2022-12-21
SE2251535 2022-12-21

Publications (1)

Publication Number Publication Date
WO2024133473A1 true WO2024133473A1 (fr) 2024-06-27

Family

ID=89509095

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/EP2023/086978 Ceased WO2024133473A1 (fr) 2022-12-21 2023-12-20 Préparation de bois d'érable pour la production de ctmp

Country Status (1)

Country Link
WO (1) WO2024133473A1 (fr)

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US4152197A (en) * 1974-09-23 1979-05-01 Mo Och Domsjo Ab Process for preparing high-yield cellulose pulps by vapor phase pulping an unpulped portion of lignocellulosic material and a partially chemically pulped portion
NO300225B1 (no) * 1991-04-17 1997-04-28 Atochem Elf Sa Fremgangsmåte for fremstilling av bleket papirmasse i höyt utbytte
CN1321571A (zh) * 2001-03-23 2001-11-14 福建腾荣达制浆有限公司 用杉木生产的木绒毛浆板及其生产方法和应用
CN112726252A (zh) * 2020-11-30 2021-04-30 山东华泰纸业股份有限公司 一种造纸厂废渣的综合利用方法

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US4152197A (en) * 1974-09-23 1979-05-01 Mo Och Domsjo Ab Process for preparing high-yield cellulose pulps by vapor phase pulping an unpulped portion of lignocellulosic material and a partially chemically pulped portion
NO300225B1 (no) * 1991-04-17 1997-04-28 Atochem Elf Sa Fremgangsmåte for fremstilling av bleket papirmasse i höyt utbytte
CN1321571A (zh) * 2001-03-23 2001-11-14 福建腾荣达制浆有限公司 用杉木生产的木绒毛浆板及其生产方法和应用
CN112726252A (zh) * 2020-11-30 2021-04-30 山东华泰纸业股份有限公司 一种造纸厂废渣的综合利用方法

Similar Documents

Publication Publication Date Title
AU705185B2 (en) A light drainability, bulky chemimechanical pulp that has a low shive content and a low fine-material content
US11352746B2 (en) Processes and systems for the pulping of lignocellulosic materials
WO2004050983A1 (fr) Procede et systeme de traitement de copeaux de bois
US4968385A (en) Method of preparing a plup using a fluidizing centrifugal pump during impregnation
WO2024133473A1 (fr) Préparation de bois d'érable pour la production de ctmp
EP0199481B1 (fr) Procédé de fabrication de pâtes cellulosiques
EP4590895B1 (fr) Imprégnation en deux étapes dans la production de ht-ctmp
CA1145107A (fr) Methode de raffinage des pates a papier
EP4590894B1 (fr) Production de ctmp à partir d'un mélange de bois dur/bois mou
EP4389963A1 (fr) Ctmp à grand volume
WO2024133425A1 (fr) Imprégnation en deux étapes dans la production de ctmp à partir de bois d'érable
WO2024133442A1 (fr) Pctm-ht d'érable
EP4590893B1 (fr) Procédé de production de ht-ctmp ayant une résistance à la traction élevée
EP4389967B1 (fr) Procédé de production de ctmp ayant une faible teneur en produits d'extraction
EP4389965A1 (fr) Procédé de production de ctmp ayant une faible teneur en produits d'extraction
WO2024136742A1 (fr) Ht-ctmp formé à partir d'un mélange bois d'érable/bois de résineux et procédé de production d'un ht-ctmp à partir d'un mélange de bois d'érable/bois de résineux
WO2000052256A1 (fr) Preconditionnement de l'alimentation pour reduction en pate chimique
WO2025259170A1 (fr) Procédé de production de pâte de cellulose à haut rendement et produits à base de pâte de cellulose à haut rendement

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 23837244

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 23837244

Country of ref document: EP

Kind code of ref document: A1