WO2024255585A1 - Microfiltration membrane and preparation method therefor - Google Patents
Microfiltration membrane and preparation method therefor Download PDFInfo
- Publication number
- WO2024255585A1 WO2024255585A1 PCT/CN2024/095879 CN2024095879W WO2024255585A1 WO 2024255585 A1 WO2024255585 A1 WO 2024255585A1 CN 2024095879 W CN2024095879 W CN 2024095879W WO 2024255585 A1 WO2024255585 A1 WO 2024255585A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- atmosphere
- preparation
- polymer
- solvent
- membrane
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Abstract
Description
本申请要求于2023年06月12日提交国家知识产权局、申请号为CN202310691553.5、发明名称为“一种微滤膜及其制备方法”的中国专利申请的优先权,其全部内容通过引用结合在本申请中。This application claims the priority of the Chinese patent application filed with the State Intellectual Property Office on June 12, 2023, with application number CN202310691553.5 and invention name “A microfiltration membrane and its preparation method”, all contents of which are incorporated by reference in this application.
本申请涉及高分子材料技术领域,尤其涉及一种微滤膜及其制备方法。The present application relates to the technical field of polymer materials, and in particular to a microfiltration membrane and a preparation method thereof.
膜技术是当代高效分离的新技术,与传统的蒸馏、精馏等技术相比,它具有分离效率高,能耗低,占地面积小等优点,膜分离技术的核心就是分离膜。其中,聚合物滤膜是一类以有机高分子聚合物为原材料,根据一定工艺制成的分离膜。根据高分子聚合物种类的不同,聚合物滤膜可以细分为纤维素类聚合物滤膜、聚酰胺类聚合物滤膜、砜类聚合物滤膜、聚四氟乙烯类聚合物滤膜等。此外,也可以根据膜的孔径大小可以分为微滤膜、超滤膜、纳滤膜及反渗透膜。Membrane technology is a new technology for efficient separation in contemporary times. Compared with traditional distillation and rectification technologies, it has the advantages of high separation efficiency, low energy consumption, and small footprint. The core of membrane separation technology is the separation membrane. Among them, polymer filter membrane is a type of separation membrane made of organic high molecular polymers as raw materials according to a certain process. According to the different types of high molecular polymers, polymer filter membranes can be subdivided into cellulose polymer filter membranes, polyamide polymer filter membranes, sulfone polymer filter membranes, polytetrafluoroethylene polymer filter membranes, etc. In addition, according to the pore size of the membrane, it can be divided into microfiltration membranes, ultrafiltration membranes, nanofiltration membranes and reverse osmosis membranes.
微滤膜能截留0.1~1μm之间的颗粒,允许大分子和溶解性固体(无机盐)等通过,但会截留悬浮物、细菌及大分子量胶体等物质。目前,微滤膜主要用于医药行业的过滤除菌,包括无菌液体的生产、生物制剂的分离、超纯水制备以及空气过滤、生物及微生物的检测分析等方面。微滤膜的运行压力一般为0.3~7bar。微滤膜过滤是世界上开发应用最早的膜技术,以天然或人工合成的高分子化合物作为膜材料。对微滤膜而言,其分离机理主要是筛分截留。为了开发出具有更高孔隙率与水通量的微滤膜,常见的方法有非溶剂致相分离法(NIPS)、蒸汽诱导相分离法(VIPS)以及雾化预处理诱导相分离等。Microfiltration membranes can intercept particles between 0.1 and 1 μm, allowing macromolecules and soluble solids (inorganic salts) to pass through, but will intercept suspended matter, bacteria, and high molecular weight colloids. At present, microfiltration membranes are mainly used for filtration and sterilization in the pharmaceutical industry, including the production of sterile liquids, separation of biological preparations, preparation of ultrapure water, air filtration, biological and microbial detection and analysis, etc. The operating pressure of microfiltration membranes is generally 0.3 to 7 bar. Microfiltration membrane filtration is the earliest membrane technology developed and applied in the world, using natural or synthetic polymer compounds as membrane materials. For microfiltration membranes, the separation mechanism is mainly screening and interception. In order to develop microfiltration membranes with higher porosity and water flux, common methods include non-solvent induced phase separation (NIPS), vapor induced phase separation (VIPS), and atomization pretreatment induced phase separation.
传统的蒸汽诱导相分离如专利CN1170620C可以明显提高膜的孔隙率,增大膜的水通量,但是一般都需要在高温蒸汽(大于100℃)放置较长时间 (大于30分钟)。采用雾化预处理和非溶剂致相分离相结合的方法如CN112973451B和CN114797484B在一定程度上可以解决传统蒸汽诱导相分离时高温且处理时间较长的问题,但是预雾化过程会产生明显的液珠,在长时间批量成膜过程中液珠下落会污染膜表面。同时,这两种方法都是蒸汽或者液珠从铸膜液表面向底层扩散,会导致表面和底层孔径形貌差别较大,且底层孔径可控性差。Traditional steam-induced phase separation, such as patent CN1170620C, can significantly increase the porosity of the membrane and increase the water flux of the membrane, but generally requires a long time in high-temperature steam (greater than 100°C). (More than 30 minutes). The method of combining atomization pretreatment and non-solvent induced phase separation, such as CN112973451B and CN114797484B, can solve the problem of high temperature and long processing time in traditional steam-induced phase separation to a certain extent. However, the pre-atomization process will produce obvious liquid droplets, and the falling liquid droplets will contaminate the membrane surface during the long-term batch film formation process. At the same time, both methods involve the diffusion of steam or liquid droplets from the surface of the casting liquid to the bottom layer, which will lead to a large difference in the pore size morphology between the surface and the bottom layer, and the controllability of the bottom layer pore size is poor.
因此,亟需研发一种具有高孔隙率,且上下表面孔径均可控的微滤膜。Therefore, there is an urgent need to develop a microfiltration membrane with high porosity and controllable pore sizes on the upper and lower surfaces.
发明内容Summary of the invention
有鉴于此,本申请要解决的技术问题在于提供一种微滤膜及其制备方法。所述微滤膜具有高孔隙率,且上下表面孔径均可控的优点。In view of this, the technical problem to be solved by the present application is to provide a microfiltration membrane and a preparation method thereof. The microfiltration membrane has the advantages of high porosity and controllable pore sizes on the upper and lower surfaces.
为达到以上目的,本申请采用的技术方案如下:In order to achieve the above objectives, the technical solutions adopted in this application are as follows:
本申请提供了一种微滤膜的制备方法,包括以下步骤:The present application provides a method for preparing a microfiltration membrane, comprising the following steps:
在封闭空间内,支撑层将空间分为上部空间和下部空间,通过上部空间的第一气氛和下部空间的第二气氛对所述支撑层的上下表面同时诱导成型,得到预成膜,然后进行相分离成型,制备得到微滤膜;所述第一气氛和第二气氛不同;所述支撑层为涂覆铸膜液的多孔结构支撑层。In a closed space, a support layer divides the space into an upper space and a lower space, and the upper and lower surfaces of the support layer are simultaneously induced to form by a first atmosphere in the upper space and a second atmosphere in the lower space to obtain a pre-film, which is then phase-separated and formed to prepare a microfiltration membrane; the first atmosphere and the second atmosphere are different; the support layer is a porous structure support layer coated with a casting liquid.
优选的,所述支撑层放置在橡胶圈上,橡胶圈为镂空状。Preferably, the support layer is placed on a rubber ring, and the rubber ring is hollow.
镂空状橡胶圈有利于上下空间内气氛对涂覆铸膜液的多孔结构支撑层上下表面同时诱导成型。The hollow rubber ring is conducive to the atmosphere in the upper and lower spaces to induce the molding of the upper and lower surfaces of the porous structure support layer coated with the casting liquid at the same time.
上述制备方法通过控制上下两部分空间内气氛的组成和温度,进而控制膜上下表面的成孔孔径。The preparation method controls the composition and temperature of the atmosphere in the upper and lower spaces, thereby controlling the pore sizes of the upper and lower surfaces of the membrane.
优选的,所述第一气氛和第二气氛独立地选自空气、水蒸汽、乙醇蒸汽、乙二醇蒸汽、极性非质子溶剂的蒸汽、盐溶液蒸汽、酸溶液蒸汽和碱溶液蒸汽中的一种或多种;更优选的,所述气氛选自空气、水蒸汽、乙醇蒸汽中的一种或多种。Preferably, the first atmosphere and the second atmosphere are independently selected from one or more of air, water vapor, ethanol vapor, ethylene glycol vapor, vapor of a polar aprotic solvent, salt solution vapor, acid solution vapor and alkaline solution vapor; more preferably, the atmosphere is selected from one or more of air, water vapor and ethanol vapor.
优选的,所述上部空间和下部空间的温度独立地为5℃~125℃;更优选为30℃~125℃。Preferably, the temperature of the upper space and the lower space is independently 5°C to 125°C; more preferably 30°C to 125°C.
在本申请的一些具体实施例中,所述气氛第一气氛和第二气氛独立地优选采用70%湿度的60℃空气、30%湿度的30℃空气、125℃水蒸气、质量比为 1:1的水和乙醇的60℃混合气体中的一种或多种。In some specific embodiments of the present application, the first atmosphere and the second atmosphere are independently preferably 60°C air with 70% humidity, 30°C air with 30% humidity, 125°C water vapor, and a mass ratio of One or more of a 60°C mixture of 1:1 water and ethanol.
优选的,所述预成膜成型时间为10~600s;更优选为50~300s;进一步优选为100~200s。在本申请的一些具体实施例中,所述微滤膜的预成膜成型时间为120s或180s。Preferably, the pre-film forming time is 10 to 600 seconds, more preferably 50 to 300 seconds, and further preferably 100 to 200 seconds. In some specific embodiments of the present application, the pre-film forming time of the microfiltration membrane is 120 seconds or 180 seconds.
优选的,所述铸膜液为含有聚合物的溶液;Preferably, the casting solution is a solution containing a polymer;
优选的,所述聚合物选自聚砜、聚醚砜、聚偏二氟乙烯、醋酸纤维素、聚氧化乙烯、聚丙烯腈、聚酰胺和聚酰亚胺中的一种或多种;更优选为聚醚砜或聚偏二氟乙烯。Preferably, the polymer is selected from one or more of polysulfone, polyethersulfone, polyvinylidene fluoride, cellulose acetate, polyethylene oxide, polyacrylonitrile, polyamide and polyimide; more preferably, polyethersulfone or polyvinylidene fluoride.
优选的,所述含有聚合物的溶液中还含有制孔添加剂和聚合物的溶剂;Preferably, the solution containing the polymer also contains a pore-forming additive and a solvent for the polymer;
所述聚合物的溶剂为聚合物的良溶剂和/或聚合物的不良溶剂;The solvent of the polymer is a good solvent of the polymer and/or a poor solvent of the polymer;
所述制孔添加剂选自聚乙烯吡咯烷酮、聚乙二醇、氯化锌和氯化锂中的一种或多种。The pore-forming additive is selected from one or more of polyvinyl pyrrolidone, polyethylene glycol, zinc chloride and lithium chloride.
优选的,所述聚合物的良溶剂选自N,N-二甲基甲酰胺、N,N-二甲基乙酰胺、丙酮、N-甲基-2-吡咯烷酮、二甲基亚砜、四甲基亚砜、四氢呋喃、二氧六环、乙腈、氯仿和四甲基亚砜中的一种或多种;更优选为N,N-二甲基乙酰胺或N-甲基-2-吡咯烷酮。Preferably, the good solvent for the polymer is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide, acetone, N-methyl-2-pyrrolidone, dimethyl sulfoxide, tetramethyl sulfoxide, tetrahydrofuran, dioxane, acetonitrile, chloroform and tetramethyl sulfoxide; more preferably N,N-dimethylacetamide or N-methyl-2-pyrrolidone.
优选的,所述聚合物的不良溶剂选自水或醇溶剂。Preferably, the poor solvent for the polymer is selected from water or alcohol solvent.
所述醇溶剂优选为小分子醇,具体包括但不限于甲醇、乙醇、苯甲醇、异丙醇中的一种或多种。The alcohol solvent is preferably a small molecule alcohol, specifically including but not limited to one or more of methanol, ethanol, benzyl alcohol, and isopropanol.
优选的,所述铸膜液的固含量为6~30wt%;更优选为10~25wt%。在本申请的一些具体实施例中,所述铸膜液的固含量为19wt%。Preferably, the solid content of the casting solution is 6 to 30 wt %, more preferably 10 to 25 wt %. In some specific embodiments of the present application, the solid content of the casting solution is 19 wt %.
优选的,所述铸膜液在多孔结构支撑层上的厚度为50~500μm;更优选为75~300μm;进一步优选为100~150μm。在本申请的一些具体实施例中,所述铸膜液在多孔支撑材料上的厚度为100μm或110μm。Preferably, the thickness of the casting liquid on the porous support layer is 50-500 μm, more preferably 75-300 μm, and further preferably 100-150 μm. In some specific embodiments of the present application, the thickness of the casting liquid on the porous support material is 100 μm or 110 μm.
本申请对上述的铸膜液的搅拌时间和温度并无特殊限定,所述搅拌时间优选为24~48h,所述搅拌温度优选为60~100℃。The present application has no particular limitation on the stirring time and temperature of the casting solution. The stirring time is preferably 24 to 48 hours, and the stirring temperature is preferably 60 to 100°C.
上述制备方法中,所述多孔结构支撑层(多孔膜)包括但不限于无纺布、有纺布和多孔陶瓷等多孔结构支撑材料。In the above preparation method, the porous structure support layer (porous membrane) includes but is not limited to porous structure support materials such as non-woven fabrics, woven fabrics and porous ceramics.
在本申请中,为了使蒸汽诱导充分进行,优选的,先用隔板将密闭空间 分为上下两部分,等上下两部分气氛稳定后,快速将隔板替换为表面涂覆铸膜液的多孔膜,使得上下两部分气氛对表面涂覆铸膜液的多孔膜同时进行蒸汽诱导成型,得到预成膜。In the present application, in order to allow the steam induction to proceed fully, preferably, the enclosed space is first separated by a partition. It is divided into two parts, the upper and lower parts. After the atmospheres in the upper and lower parts are stable, the partition is quickly replaced with a porous membrane coated with casting liquid on the surface, so that the atmospheres in the upper and lower parts simultaneously perform steam-induced molding on the porous membrane coated with casting liquid on the surface to obtain a pre-film.
上述蒸汽诱导成型前,隔板放置于镂空的橡胶圈上。Before the steam-induced molding, the partition is placed on the hollow rubber ring.
本申请中,所述相分离成型优选采用非溶剂致相分离法进行。In the present application, the phase separation molding is preferably carried out by a non-solvent induced phase separation method.
上述非溶剂致相分离法具体为将上述制备得到的预成膜在聚合物的非溶剂中浸泡一段时间进而成型制备得到微滤膜,利用预成膜中的溶剂和聚合物的非溶剂进行物理交换,使预成膜发生相分离。The non-solvent induced phase separation method is specifically to immerse the pre-film prepared above in a non-solvent of the polymer for a period of time and then shape it to prepare a microfiltration membrane, and utilize the physical exchange between the solvent in the pre-film and the non-solvent of the polymer to cause phase separation of the pre-film.
所述聚合物的非溶剂包括但不限于水、乙醇、乙二醇、氢氧化钠水溶液等单一组份的溶剂,或者水与极性非质子溶剂的混合溶液,或者水与其它溶剂的混合溶液。The non-solvent for the polymer includes, but is not limited to, single-component solvents such as water, ethanol, ethylene glycol, sodium hydroxide aqueous solution, or a mixed solution of water and a polar aprotic solvent, or a mixed solution of water and other solvents.
预成膜进行相分离时,温度优选为10~80℃,时间优选1~60min,更优选3~10min;When the pre-film is formed for phase separation, the temperature is preferably 10 to 80°C, the time is preferably 1 to 60 minutes, more preferably 3 to 10 minutes;
本申请将铸膜液通过刮膜或流延技术涂布在多孔结构支撑层基底上,并在多孔结构支撑层的上下两侧通过控制气氛组成和温度进行蒸汽诱导相分离完成预成膜的制备,然后将预成膜浸入非溶剂浴中进一步完成相分离,从而得到具有高孔隙率,且上下表面孔径均可控的微滤膜。In the present application, the casting liquid is coated on a porous structure support layer substrate by scraping or casting technology, and steam-induced phase separation is performed on the upper and lower sides of the porous structure support layer by controlling the atmosphere composition and temperature to complete the preparation of the pre-film, and then the pre-film is immersed in a non-solvent bath to further complete the phase separation, thereby obtaining a microfiltration membrane with high porosity and controllable pore sizes on the upper and lower surfaces.
本申请所述的微滤膜的制备方法,具体包括以下步骤:The method for preparing the microfiltration membrane described in the present application specifically comprises the following steps:
1)封闭空间内,将隔板放置在镂空的橡胶圈上将空间分为上部空间和下部空间,并在上下两部分空间内通入气氛,同时分别控制上下两部分空间的温度;1) In a closed space, a partition is placed on a hollow rubber ring to divide the space into an upper space and a lower space, and the atmosphere is introduced into the upper and lower spaces, and the temperatures of the upper and lower spaces are controlled separately;
2)取出隔板,将涂有铸膜液的多孔结构支撑层放置于垫圈上,通过上下两部分空间内气氛同时诱导成型制备预成膜;2) taking out the separator, placing the porous structure support layer coated with the casting liquid on the gasket, and preparing the pre-film by simultaneously inducing molding through the atmosphere in the upper and lower spaces;
3)将预成膜进行相分离成型,制备得到微滤膜。3) The preformed membrane is subjected to phase separation and molding to prepare a microfiltration membrane.
上述制备方法中,完成步骤3)的相分离成型后,将完全成型的多孔膜用去离子水浸泡一定时间去除残余溶剂,并干燥,制备得到本申请所述的微滤膜。In the above preparation method, after the phase separation and forming in step 3) is completed, the fully formed porous membrane is soaked in deionized water for a certain period of time to remove the residual solvent, and then dried to prepare the microfiltration membrane described in the present application.
所述去离子水浸泡的时间优选为24~48h,浸泡温度优选为30~80℃。The deionized water soaking time is preferably 24 to 48 hours, and the soaking temperature is preferably 30 to 80°C.
本申请对上述干燥的方法并无特殊限定,可以为普通加热烘干、真空干 燥等本领域技术人员熟知的方法。在本申请中优选采用加热烘干的方法,所述加热烘干的温度优选为60~120℃,所述加热烘干的时间优选为24~48h。The present application does not specifically limit the drying method, which can be conventional heating drying, vacuum drying, In the present application, the heating and drying method is preferably adopted, the temperature of the heating and drying is preferably 60 to 120° C., and the time of the heating and drying is preferably 24 to 48 hours.
本申请还提供了一种微滤膜,由上述的制备方法制备得到。The present application also provides a microfiltration membrane, which is prepared by the above-mentioned preparation method.
优选的,所述微滤膜内部呈海绵孔结构。Preferably, the interior of the microfiltration membrane presents a sponge pore structure.
本申请采用蒸汽诱导的方式对涂覆铸液膜的多孔结构支撑层上下表面同时诱导成型,极大地缩短了预成膜时间。The present application adopts a steam-induced method to simultaneously induce molding of the upper and lower surfaces of the porous structure support layer coated with the casting liquid film, which greatly shortens the pre-film forming time.
与现有技术相比,本申请提供的微滤膜利用多孔结构支撑层可以透过气氛的特点,通过上部空间的第一气氛和下部空间的第二气氛对涂覆铸液膜的多孔结构支撑层上下表面同时进行蒸汽诱导成型,极大地缩短了预成膜时间。同时,通过调节多孔结构支撑层上部空间的第一气氛和下部空间第二气氛的组成和温度,实现了对预成膜上下表面孔径的同步控制,使得所述微滤膜具有高孔隙率且上下表面孔径均可控的优点。Compared with the prior art, the microfiltration membrane provided by the present application utilizes the characteristic that the porous structure support layer can pass through the atmosphere, and simultaneously performs steam induction molding on the upper and lower surfaces of the porous structure support layer coated with the casting liquid membrane through the first atmosphere in the upper space and the second atmosphere in the lower space, which greatly shortens the pre-filming time. At the same time, by adjusting the composition and temperature of the first atmosphere in the upper space of the porous structure support layer and the second atmosphere in the lower space, the pore size of the upper and lower surfaces of the pre-filming is synchronously controlled, so that the microfiltration membrane has the advantages of high porosity and controllable pore size on the upper and lower surfaces.
图1为微滤膜的制备工艺示意图;FIG1 is a schematic diagram of the preparation process of a microfiltration membrane;
图2为实施例1中微滤膜的截面,其中,a为纵截面,b为上表面,c为下表面;FIG2 is a cross section of the microfiltration membrane in Example 1, wherein a is a longitudinal cross section, b is an upper surface, and c is a lower surface;
图3为实施例2中微滤膜的截面,其中,d为纵截面,e为上表面,f为下表面。Figure 3 is a cross section of the microfiltration membrane in Example 2, wherein d is a longitudinal section, e is an upper surface, and f is a lower surface.
为了进一步说明本申请,下面结合实施例对本申请提供的微滤膜及其制备方法进行详细描述。In order to further illustrate the present application, the microfiltration membrane and the preparation method thereof provided by the present application are described in detail below in conjunction with embodiments.
实施例1Example 1
第一步:将隔板放置在镂空的橡胶圈上,将空间隔开为上部空间和下部空间,将湿度70%的60℃空气注入上部空间作为气氛A,将湿度30%的30℃空气注入下部空间作为气氛B,待上部空间和下部空间的气氛组成与温度稳定;Step 1: Place the partition on the hollow rubber ring to separate the space into the upper space and the lower space, inject 60°C air with 70% humidity into the upper space as atmosphere A, and inject 30°C air with 30% humidity into the lower space as atmosphere B, and wait until the atmosphere composition and temperature of the upper space and the lower space are stable;
第二步:将12g聚醚砜、4g聚乙烯吡咯烷酮溶解在84g的N,N-二甲基 乙酰胺中,60℃搅拌24h得到均匀铸膜液;Step 2: Dissolve 12g polyethersulfone and 4g polyvinylpyrrolidone in 84g N,N-dimethyl In acetamide, stir at 60°C for 24h to obtain a uniform casting solution;
第三步:将得到的铸膜液通过刮膜技术涂布在多孔陶瓷上,控制涂布厚度为100μm;Step 3: coating the obtained casting solution on the porous ceramic by scraping film technology, and controlling the coating thickness to be 100 μm;
第四步:快速取出隔板,然后将涂有铸膜液的多孔陶瓷放在气氛A和B之间,铸膜液上层受上部空间气氛A影响,底层受下部空间气氛B影响同时进行蒸汽诱导相分离,控制时间为2min得到预成膜;Step 4: quickly take out the partition, and then place the porous ceramic coated with the casting liquid between atmospheres A and B. The upper layer of the casting liquid is affected by the upper space atmosphere A, and the bottom layer is affected by the lower space atmosphere B. At the same time, steam-induced phase separation is carried out, and the control time is 2 minutes to obtain a pre-film.
第五步:将预成膜浸入到40%的DMAc溶液中浸泡7min进一步进行相分离成型;Step 5: Immerse the pre-film in 40% DMAc solution for 7 minutes to further perform phase separation molding;
第六步:将完全成型的多孔膜用去30℃离子水中浸泡24h去除残余溶剂,并在80℃烘干24h得到微滤膜。Step 6: Soak the fully formed porous membrane in deionized water at 30°C for 24 hours to remove residual solvent, and dry it at 80°C for 24 hours to obtain a microfiltration membrane.
实施例2Example 2
第一步:将隔板放置在镂空的橡胶圈上,将空间隔开为上部空间和下部空间,将125℃水蒸气注入上部空间作为气氛A,将60℃水:乙醇为100g:100g的混合气体注入下部空间作为气氛B,待上部空间和下部空间的气氛组成与温度稳定;Step 1: Place the partition on the hollow rubber ring to separate the space into an upper space and a lower space, inject 125°C water vapor into the upper space as atmosphere A, and inject a mixed gas of 60°C water and ethanol (100g:100g) into the lower space as atmosphere B, and wait until the atmosphere composition and temperature of the upper space and the lower space are stable;
第二步:将10g聚偏二氟乙烯、6g聚乙烯吡咯烷酮溶解在84g的N-甲基吡咯烷酮,80℃搅拌24h得到均匀铸膜液;Step 2: Dissolve 10 g of polyvinylidene fluoride and 6 g of polyvinyl pyrrolidone in 84 g of N-methyl pyrrolidone, and stir at 80° C. for 24 h to obtain a uniform casting solution;
第三步:将得到的铸膜液通过刮膜技术涂布在无纺布上,控制涂布厚度为110μm;Step 3: coating the obtained casting solution on the non-woven fabric by scraping film technology, and controlling the coating thickness to be 110 μm;
第四步:快速取出隔板,然后将涂有铸膜液的无纺布放在气氛A和B之间,铸膜液上层受上部空间气氛A影响,底层受下部空间气氛B影响同时进行蒸汽诱导相分离,控制时间为3min得到预成膜;Step 4: quickly take out the partition, and then place the non-woven fabric coated with the casting liquid between atmospheres A and B. The upper layer of the casting liquid is affected by the upper space atmosphere A, and the bottom layer is affected by the lower space atmosphere B. At the same time, steam-induced phase separation is carried out, and the control time is 3 minutes to obtain a pre-film;
第五步:将预成膜浸入到30%的DMAc溶液中浸泡3min进一步相分离成型;Step 5: Immerse the pre-formed film in a 30% DMAc solution for 3 minutes for further phase separation and molding;
第六步:将完全成型的多孔膜用去60℃离子水中浸泡24h去除残余溶剂,并在60℃烘干36h得到微滤膜。Step 6: Soak the fully formed porous membrane in deionized water at 60°C for 24 hours to remove residual solvent, and dry it at 60°C for 36 hours to obtain a microfiltration membrane.
对上述实施例所制备的微滤膜进行下列相关测试,具体数据见表1。The following relevant tests were performed on the microfiltration membrane prepared in the above examples, and the specific data are shown in Table 1.
1)扫描电镜测试1) Scanning electron microscope test
使用日立SU3800对微滤膜上下表面的孔径进行扫描统计,得到上下表 面的平均孔径。详见图2(实施例1制备的微滤膜)、图3(实施例2制备的微滤膜)。Hitachi SU3800 was used to scan and count the pore sizes on the upper and lower surfaces of the microfiltration membrane, and the upper and lower tables were obtained. See Figure 2 (microfiltration membrane prepared in Example 1) and Figure 3 (microfiltration membrane prepared in Example 2) for details.
2)水通量测试2) Water flux test
水通量是单位时间通过单位膜面积的水的体积或质量简称,用于评价膜分离效率的重要指标,也是用于衡量微滤膜性能的关键指标之一,水通量越大表明膜的分离效率越高,膜内部孔隙越通透,实施例1和2所制备的微滤膜水通量较高。其参考GB/T 34242-2017标准进行测试。Water flux is the volume or mass of water passing through a unit membrane area per unit time. It is an important indicator for evaluating membrane separation efficiency and one of the key indicators for measuring microfiltration membrane performance. The larger the water flux, the higher the separation efficiency of the membrane and the more transparent the pores inside the membrane. The microfiltration membranes prepared in Examples 1 and 2 have higher water flux. The test was conducted with reference to GB/T 34242-2017 standard.
3)最可几孔径3) Most probable aperture
最可几孔径是指最可能出现的孔径大小,也就是孔最多的孔径,用于评价膜分离效果的重要指标,也是用于衡量微滤膜性能的关键指标之一,最可几孔径大小决定了膜分离物质颗粒的大小,表1表明了实施例1和2所制备的微滤膜具有优异的分离性能。其参考GB/T 5249-2013标准进行测试。The most probable pore size refers to the most likely pore size, that is, the pore size with the most pores. It is an important indicator for evaluating the membrane separation effect and one of the key indicators for measuring the performance of microfiltration membranes. The most probable pore size determines the size of the particles of the membrane-separated substances. Table 1 shows that the microfiltration membranes prepared in Examples 1 and 2 have excellent separation performance. The test was carried out with reference to the GB/T 5249-2013 standard.
4)孔隙率4) Porosity
孔隙率是指多孔介质内相互连通的微小空隙的总体积与该多孔介质的外表体积的比值。一般来说,孔隙率越高,膜内部越通透,分离效率也越高。孔隙率大于80%,属于高孔隙率。其参考GB/T 33052-2016标准进行测试。Porosity refers to the ratio of the total volume of interconnected micro-voids in a porous medium to the surface volume of the porous medium. Generally speaking, the higher the porosity, the more permeable the inside of the membrane and the higher the separation efficiency. A porosity greater than 80% is considered high porosity. It is tested with reference to the GB/T 33052-2016 standard.
表1实施例的水通量、孔径以及孔隙率
Table 1 Water flux, pore size and porosity of the examples
通过表1数据,结合图2和图3可以看出,本申请通过改变上下两部分空间内气氛的组成与温度来控制预成膜上下表面的孔径,制备得到的微滤膜内部呈海绵孔结构,且拥有优异的分离性能与高孔隙率。并且,本申请所述微滤膜的制备方法可以根据需要制备不同孔径大小的、上下表面孔径可调的微滤膜,具有较强的实际应用性;另外,所述制备方法工艺简单,采用上下表面同时蒸汽诱导使得预成膜时间大大缩短,可满足不同的工业生产需要,具有广阔的市场应用前景。 From the data in Table 1, combined with Figures 2 and 3, it can be seen that the present application controls the pore size of the upper and lower surfaces of the pre-film by changing the composition and temperature of the atmosphere in the upper and lower spaces, and the prepared microfiltration membrane has a sponge pore structure inside and has excellent separation performance and high porosity. In addition, the preparation method of the microfiltration membrane described in the present application can prepare microfiltration membranes with different pore sizes and adjustable pore sizes on the upper and lower surfaces as needed, and has strong practical applicability; in addition, the preparation method is simple in process, and the use of steam induction on the upper and lower surfaces simultaneously greatly shortens the pre-filming time, which can meet different industrial production needs and has broad market application prospects.
以上实施例的说明只是用于帮助理解本申请的方法及其核心思想。应当指出,对于本技术领域的普通技术人员来说,在不脱离本申请原理的前提下,还可以对本申请进行若干改进和修饰,这些改进和修饰也落入本申请权利要求的保护范围内。 The description of the above embodiments is only used to help understand the method and core idea of the present application. It should be pointed out that, for ordinary technicians in this technical field, several improvements and modifications can be made to the present application without departing from the principles of the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.
Claims (14)