WO2024259800A1 - Preparation method for titanium alloy material - Google Patents
Preparation method for titanium alloy material Download PDFInfo
- Publication number
- WO2024259800A1 WO2024259800A1 PCT/CN2023/113534 CN2023113534W WO2024259800A1 WO 2024259800 A1 WO2024259800 A1 WO 2024259800A1 CN 2023113534 W CN2023113534 W CN 2023113534W WO 2024259800 A1 WO2024259800 A1 WO 2024259800A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- titanium alloy
- powder
- feed
- blank
- sintering
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Abstract
Description
本发明涉及粉末注射成形领域,特别涉及一种钛合金材料制备方法。The invention relates to the field of powder injection molding, and in particular to a method for preparing a titanium alloy material.
钛合金因具有比强度高、耐腐蚀、耐高温、耐低温、无磁、可焊、生物相容性好等优异的综合性能,在航空航天、核工业、兵器、海洋、石油、化工、医疗、日常生活等众多领域都有着重要的用途,为越来越多的人所接受。但由于钛合金材料制备工艺复杂、流程长等原因使其成本高,限制了钛合金在的应用。降低成本已成为目前钛合金发展必须要解决的重要问题之一。Titanium alloys have excellent comprehensive properties such as high specific strength, corrosion resistance, high temperature resistance, low temperature resistance, non-magnetic, weldable, and good biocompatibility. They are used in many fields such as aerospace, nuclear industry, weapons, ocean, petroleum, chemical industry, medical treatment, and daily life, and are accepted by more and more people. However, due to the complex preparation process and long process of titanium alloy materials, the cost is high, which limits the application of titanium alloys. Reducing costs has become one of the important issues that must be solved in the development of titanium alloys.
用于金属注射成形的钛合金粉末(1-20μm)由于得粉率低,导致粉末成本居高不下。通过对钛合金粉末应用范围的研究发现:钛合金粉末中20-50μm的粉末主要用于3D打印行业,对于50-100μm的粉末由于粉末颗粒过大,几乎无任何实用价值,价格便宜,通常会进行回收处理。Titanium alloy powder (1-20μm) used for metal injection molding has a low powder yield, resulting in high powder costs. Through research on the application range of titanium alloy powder, it is found that 20-50μm titanium alloy powder is mainly used in the 3D printing industry, while 50-100μm powder has almost no practical value due to its large particles and low price, and is usually recycled.
对于钛合金粉末的粗/细粉混合,并不是添加的粗粉越多越好。需要从混合粉末的振实密度、粉末填充效果以及烧结性能多个方面进行考虑。首先,不同比例粗/细粉混合的振实密度是不同的,而用于金属注射成形的钛合金喂料的装载量设计受粉末振实密度的影响。振实密度越高,钛合金喂料的装载量也会升高,过高的装载量会影响钛合金喂料的流动性,增加注射风险。此外,只有在特定比例的粗/细粉混合状态下,才能保证细粉充分填充在粗粉间隙中。当粗粉含量过高,可能会导致部分粗粉颗粒之间的间隙无细粉填充,进而影响钛合金的烧结致密性。最后,在考虑通过钛合金粗/细粉混合降低钛合金注射成形原材料成本的同时,还应考虑烧结性能的稳定性。若粗/细粉混合后烧结的性能太差,则失去了钛合金的使用价值。For the coarse/fine powder mixing of titanium alloy powder, the more coarse powder is added, the better. It is necessary to consider the tap density of the mixed powder, the powder filling effect and the sintering performance. First of all, the tap density of coarse/fine powder mixing in different proportions is different, and the loading design of titanium alloy feed for metal injection molding is affected by the tap density of the powder. The higher the tap density, the higher the loading amount of the titanium alloy feed. Too high a loading amount will affect the fluidity of the titanium alloy feed and increase the injection risk. In addition, only when the coarse/fine powder is mixed in a specific proportion can the fine powder be fully filled in the coarse powder gap. When the coarse powder content is too high, the gaps between some coarse powder particles may not be filled with fine powder, which will affect the sintering density of the titanium alloy. Finally, while considering reducing the raw material cost of titanium alloy injection molding by mixing coarse/fine powder of titanium alloy, the stability of sintering performance should also be considered. If the sintering performance after the coarse/fine powder is mixed is too poor, the use value of the titanium alloy is lost.
发明内容Summary of the invention
本发明的目的是一种钛合金材料制备方法,其通过对50-100μm的钛合金粗粉与 1-20μm的钛合金细粉进行不同比例的混合,使用部分钛合金粗粉替代钛合金细粉以降低钛合金细粉的使用量,进而降低用于金属注射成形钛合金粉末的成本。The object of the present invention is a method for preparing a titanium alloy material, which comprises: Titanium alloy fine powders of 1-20 μm are mixed in different proportions, and part of the titanium alloy coarse powder is used to replace the titanium alloy fine powder to reduce the use of the titanium alloy fine powder, thereby reducing the cost of the titanium alloy powder used for metal injection molding.
实现本发明目的的技术方案是:本发明包括以下步骤:The technical solution to achieve the purpose of the present invention is: the present invention comprises the following steps:
S1、准备钛合金细粉和钛合金粗粉,其中钛合金细粉的粒径范围为1~20μm,钛合金粗粉的粒径范围为50~100μm;将钛合金细粉和钛合金粗粉混合形成钛合金混合粉末;所述钛合金混合粉末中钛合金粗粉的占比为50%-80%;S1. Prepare titanium alloy fine powder and titanium alloy coarse powder, wherein the particle size of the titanium alloy fine powder is in the range of 1 to 20 μm, and the particle size of the titanium alloy coarse powder is in the range of 50 to 100 μm; mix the titanium alloy fine powder and the titanium alloy coarse powder to form a titanium alloy mixed powder; the titanium alloy coarse powder accounts for 50% to 80% of the titanium alloy mixed powder;
S2、将钛合金混合粉末与粘结剂混炼制备形成喂料;S2, mixing the titanium alloy mixed powder and the binder to form a feed material;
S3、将喂料置于注射成型机内,经模具注射成形为注射坯;S3, placing the feed material in an injection molding machine, and forming the feed material into an injection blank through a mold;
S4、对注射坯进行脱脂获得脱脂坯;S4, degreasing the injection blank to obtain a degreased blank;
S5、对脱脂坯进行高真空烧结,获得烧结坯。S5. Perform high vacuum sintering on the degreased blank to obtain a sintered blank.
进一步,上述钛合金细粉中D50:10~13μm;所述钛合金粗粉中D50:70~80μm。Furthermore, the D50 of the titanium alloy fine powder is 10 to 13 μm; and the D50 of the titanium alloy coarse powder is 70 to 80 μm.
进一步,上述喂料中钛合金混合粉末与粘结剂的比例为0.8≤V1/V2≤1.9,其中V1为钛合金混合粉末的体积,V2为粘结剂的体积。Furthermore, the ratio of the titanium alloy mixed powder to the binder in the above feed is 0.8≤V1/V2≤1.9, wherein V1 is the volume of the titanium alloy mixed powder, and V2 is the volume of the binder.
粉末理论装载量=振实密度(ρr)/理论密度(ρ),正常喂料制备过程中,粉末装载量可以低于理论装载量,但是不能高于理论装载量(高于理论装载量会导致粘结剂不能充分包覆所有粉末,导致喂料不均匀影响喂料流动性)。我们通过对钛合金混合粉末不同装载量的验证得到的结论是:合金粉末与高分子粘结剂的比例在0.8-1.9范围内时,喂料的流动性是最佳的。Theoretical powder loading = tap density (ρr) / theoretical density (ρ). In the normal feeding preparation process, the powder loading can be lower than the theoretical loading, but cannot be higher than the theoretical loading (higher than the theoretical loading will cause the binder to not fully cover all the powder, resulting in uneven feeding and affecting feeding fluidity). Through the verification of different loading amounts of titanium alloy mixed powder, we concluded that the feeding fluidity is optimal when the ratio of alloy powder to polymer binder is in the range of 0.8-1.9.
进一步,喂料中钛合金混合粉末体积占比为58%~66%,其余为高分子粘结剂;所述高分子粘结剂的组分按照质量百分比包括60%~70%的聚甲醛,12%~15%的聚乙烯,15%~20%的聚丙烯以及3%~5%的硬脂酸;所述喂料的装载量范围是53%-73%。Furthermore, the volume proportion of the titanium alloy mixed powder in the feed is 58% to 66%, and the rest is a polymer binder; the components of the polymer binder include 60% to 70% of polyoxymethylene, 12% to 15% of polyethylene, 15% to 20% of polypropylene and 3% to 5% of stearic acid in terms of mass percentage; the loading range of the feed is 53%-73%.
作为最优设计,上述喂料中钛合金混合粉末与粘结剂的比例为1:1;所述喂料的装载量范围为58%~66%。As the optimal design, the ratio of the titanium alloy mixed powder to the binder in the above feed is 1:1; and the loading range of the feed is 58% to 66%.
通过最佳装载量计算可得不同比例粗细粉混合的装载量范围是53%-73%,粗细粉1:1混合的振实密度最高,烧结致密化的效果理论上是最好的。但是1:1混合的理论装载量是73%,过高的装载量会影响喂料的流动性,为保证喂料的流动性,将1:1混合喂料的装载量定为58%~66%。粉末装载量可以低于理论装载量,但是不能高于理论装载量(高于理论装载量会导致粘结剂不能充分包覆所有粉末,导致喂料不均匀影响喂料流 动性)。Through the calculation of the optimal loading amount, it can be obtained that the loading amount range of different proportions of coarse and fine powders is 53%-73%. The tap density of the 1:1 mixture of coarse and fine powders is the highest, and the sintering densification effect is theoretically the best. However, the theoretical loading amount of the 1:1 mixture is 73%. Too high a loading amount will affect the fluidity of the feed. To ensure the fluidity of the feed, the loading amount of the 1:1 mixed feed is set at 58%-66%. The powder loading amount can be lower than the theoretical loading amount, but not higher than the theoretical loading amount (higher than the theoretical loading amount will cause the binder to not fully cover all the powders, resulting in uneven feeding and affecting the feeding flow. activity).
进一步,上述步骤S3中注射成形的技术参数为:模具温度为80~120℃,喂料加热温度为160~220℃,注射压力为80~120MPa;保压时间1~2.5s。Furthermore, the technical parameters of the injection molding in the above step S3 are: mold temperature of 80-120° C., feed heating temperature of 160-220° C., injection pressure of 80-120 MPa; and holding time of 1-2.5 s.
由于钛合金混合粉末的装载量较高,注射压力需偏低(高的注射压力会导致部分细粉流动到注射坯表面,起不到填充粗粉颗粒间隙的效果),一定的保压时间是为了保证注射坯注射饱满,无缺陷。Due to the high loading amount of titanium alloy mixed powder, the injection pressure needs to be low (high injection pressure will cause some fine powder to flow to the surface of the injection blank, which will not fill the gaps between the coarse powder particles). A certain holding time is to ensure that the injection blank is full and defect-free.
进一步,上述步骤S4中脱脂的技术参数为:采用草酸介质进行催化脱脂,脱脂时间为脱脂时间t≥(60+60*h)min,h为注射坯的最大厚度,单位为mm。Furthermore, the technical parameters of degreasing in the above step S4 are: catalytic degreasing is performed using oxalic acid as a medium, and the degreasing time is degreasing time t≥(60+60*h)min, where h is the maximum thickness of the injection blank, in mm.
进一步,上述步骤S5中烧结的术参数为:采用金属腔体烧结炉进行高真空烧结,炉膛内的压力≤1.0×10-3Pa,烧结温度T满足0.65TL≤T≤0.85TL。Furthermore, the technical parameters of sintering in the above step S5 are: high vacuum sintering is performed in a metal cavity sintering furnace, the pressure in the furnace is ≤1.0×10-3Pa, and the sintering temperature T satisfies 0.65TL≤T≤0.85TL.
由于粗粉的烧结动能相对于细粉较高,形成烧结颈并进行致密化烧结需要更多的烧结能量。因此,粗细粉混合的烧结温度T更接近于0.85TL。Since the sintering kinetic energy of coarse powder is higher than that of fine powder, more sintering energy is required to form a sintering neck and perform densification sintering. Therefore, the sintering temperature T of the coarse and fine powder mixture is closer to 0.85TL.
在粗粉价格成本低,杂质元素含量低的基础上添加一定量的细粉,在混合过程中,细粉能够有效填充在粗粉颗粒之间,增加了粗粉的振实密度,避免了粗粉烧结致密性差,力学性能差的短板。此外,通过粗细粉比例的调整可对喂料的装载量进行微调,可以实现在不影响对烧结件力学性能的基础上对烧结件尺寸的精密微调(通过调整钛合金粗粉和钛合金细粉的比例来进行进行装载量微调,从而影响烧结件的尺寸收缩)。但是,由于粗粉的烧结致密化温度高于细粉,因此粗/细粉混合的烧结温度要以粗粉烧结的致密化温度为主,这样才能保证烧结过程中粗粉颗粒之间能够形成完整的烧结颈。A certain amount of fine powder is added on the basis of the low price and low impurity element content of coarse powder. During the mixing process, the fine powder can be effectively filled between the coarse powder particles, increasing the tap density of the coarse powder and avoiding the shortcomings of poor sintering density and poor mechanical properties of the coarse powder. In addition, the feed loading amount can be fine-tuned by adjusting the ratio of coarse and fine powders, and the precise fine-tuning of the size of the sintered part can be achieved without affecting the mechanical properties of the sintered part (the loading amount is fine-tuned by adjusting the ratio of titanium alloy coarse powder and titanium alloy fine powder, thereby affecting the size shrinkage of the sintered part). However, since the sintering densification temperature of the coarse powder is higher than that of the fine powder, the sintering temperature of the coarse/fine powder mixture should be based on the densification temperature of the coarse powder sintering, so as to ensure that a complete sintering neck can be formed between the coarse powder particles during the sintering process.
钛合金由于其活性大,易与空气中的C,O发生反应生成碳化物和氧化物,严重影响钛合金的烧结性能。因此,钛合金烧结需采用高真空烧结环境进行烧结(原理:铁基合金、不锈钢、钴合金、镍基合金、铜合金等合金材料的活泼性比氢气和C要弱,如果采用氢气/C/高真空环境烧结,合金中的氧含量将会迅速被置换出来,从而在烧结过程中迅速致密化,达不到通过高氧含量实现高孔隙率的目的,钛合金因为活泼性极高,必须采用高真空环境烧结(还原性比氢气和C气氛强),从能达到部分氧化钛被还原,实现粉末颗粒之间形成烧结颈。)Due to its high activity, titanium alloys are prone to react with C and O in the air to form carbides and oxides, which seriously affect the sintering performance of titanium alloys. Therefore, titanium alloy sintering needs to be carried out in a high vacuum sintering environment (principle: the activity of iron-based alloys, stainless steel, cobalt alloys, nickel-based alloys, copper alloys and other alloy materials is weaker than hydrogen and C. If sintering is carried out in a hydrogen/C/high vacuum environment, the oxygen content in the alloy will be quickly replaced, resulting in rapid densification during the sintering process, and the purpose of achieving high porosity through high oxygen content cannot be achieved. Titanium alloys are extremely active and must be sintered in a high vacuum environment (stronger in reducing properties than hydrogen and C atmospheres) to achieve partial reduction of titanium oxide and form sintering necks between powder particles.)
本发明具有积极的效果:(1)本发明通过对50-100μm的钛合金粗粉与1-20μm的钛合金细粉进行不同比例的混合,使用部分钛合金粗粉替代钛合金细粉以降低钛合金细 粉的使用量,进而降低用于金属注射成形钛合金粉末的成本。The present invention has positive effects: (1) The present invention reduces the titanium alloy fine powder by mixing 50-100 μm titanium alloy coarse powder and 1-20 μm titanium alloy fine powder in different proportions, and using part of the titanium alloy coarse powder to replace the titanium alloy fine powder. The amount of powder used can be reduced, thereby reducing the cost of titanium alloy powder used for metal injection molding.
(2)本发明通过钛合金粗粉和钛合金细粉的混合比例设计,使得钛合金细粉能够完全填充在钛合金粗粉的间隙处,解决了钛合金粗粉烧结不致密的难点。(2) The present invention designs the mixing ratio of titanium alloy coarse powder and titanium alloy fine powder so that the titanium alloy fine powder can be completely filled in the gaps of the titanium alloy coarse powder, thereby solving the problem of the coarse sintering of the titanium alloy coarse powder being not dense.
(3)本发明中钛合金粗粉的氧含量低于钛合金细粉的氧含量,因此钛合金混合粉末能够有效降低产品氧含量,从而有利于烧结致密化。(3) The oxygen content of the titanium alloy coarse powder in the present invention is lower than that of the titanium alloy fine powder. Therefore, the titanium alloy mixed powder can effectively reduce the oxygen content of the product, which is beneficial to sintering densification.
为了使本发明的内容更容易被清楚地理解,下面根据具体实施例并结合附图,对本发明作进一步详细的说明,其中In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments and in conjunction with the accompanying drawings, wherein
图1为本发明实施例1中烧结坯的金相显微组织;FIG1 is a metallographic microstructure of a sintered blank in Example 1 of the present invention;
图2为本发明实施例2中烧结坯的金相显微组织;FIG2 is a metallographic microstructure of a sintered blank in Example 2 of the present invention;
图3为本发明对比实施例中烧结坯的金相显微组织。FIG. 3 is a metallographic microstructure of a sintered blank in a comparative example of the present invention.
(实施例1)(Example 1)
本发明包括以下步骤:The present invention comprises the following steps:
S1、准备钛合金细粉和钛合金粗粉,其中钛合金细粉的粒径范围为1~20μm(D50:10~13μm),钛合金粗粉的粒径范围为50~100μm(D50:70~80μm);将钛合金细粉和钛合金粗粉混合形成钛合金混合粉末;所述钛合金混合粉末中钛合金粗粉和钛合金细粉的比例为1:1;S1. Prepare titanium alloy fine powder and titanium alloy coarse powder, wherein the particle size range of the titanium alloy fine powder is 1-20 μm (D50: 10-13 μm), and the particle size range of the titanium alloy coarse powder is 50-100 μm (D50: 70-80 μm); mix the titanium alloy fine powder and the titanium alloy coarse powder to form a titanium alloy mixed powder; the ratio of the titanium alloy coarse powder to the titanium alloy fine powder in the titanium alloy mixed powder is 1:1;
S2、将钛合金混合粉末与粘结剂混炼制备形成喂料;其中钛合金混合粉末与粘结剂的比例为1.6;说述喂料中钛合金混合粉末体积占比为66%,其余为高分子粘结剂;所述高分子粘结剂的组分按照质量百分比包括60%~70%的聚甲醛,12%~15%的聚乙烯,15%~20%的聚丙烯以及3%~5%的硬脂酸;S2. Mixing titanium alloy mixed powder and binder to form feed; wherein the ratio of titanium alloy mixed powder to binder is 1.6; the volume proportion of titanium alloy mixed powder in the feed is 66%, and the rest is polymer binder; the components of the polymer binder include 60% to 70% of polyoxymethylene, 12% to 15% of polyethylene, 15% to 20% of polypropylene and 3% to 5% of stearic acid according to mass percentage;
S3、将喂料置于注射成型机内,经模具注射成形为注射坯;注射参数为:模具温度为80~120℃,喂料加热温度为160~220℃,注射压力为80~120MPa;保压时间1~2.5s;S3, placing the feed material in an injection molding machine, and injecting it into an injection blank through a mold; the injection parameters are: mold temperature of 80-120°C, feed material heating temperature of 160-220°C, injection pressure of 80-120MPa; holding time of 1-2.5s;
S4、对注射坯进行脱脂获得脱脂坯;脱脂的具体技术参数是:脱脂采用草酸介质进行催化脱脂,脱脂时间为脱脂时间t≥(60+60*h)min,h为注射坯的最大厚度,单位为mm; S4, degreasing the injection blank to obtain a degreasing blank; the specific technical parameters of the degreasing are: the degreasing is carried out by catalytic degreasing with oxalic acid medium, the degreasing time is the degreasing time t≥(60+60*h)min, h is the maximum thickness of the injection blank, the unit is mm;
S5、对脱脂坯进行高真空烧结,获得烧结坯;烧结的具体技术参数是:采用金属腔体烧结炉进行高真空烧结,炉膛内的压力≤1.0×10-3Pa,烧结温度T满足0.65TL≤T≤0.85TL。由于粗粉的烧结动能相对于细粉较高,形成烧结颈并进行致密化烧结需要更多的烧结能量。因此,粗细粉混合的烧结温度T更接近于0.85TL。S5. The degreased blank is subjected to high vacuum sintering to obtain a sintered blank. The specific technical parameters of the sintering are: high vacuum sintering is performed in a metal cavity sintering furnace, the pressure in the furnace is ≤1.0×10-3Pa, and the sintering temperature T satisfies 0.65TL≤T≤0.85TL. Since the sintering kinetic energy of the coarse powder is higher than that of the fine powder, more sintering energy is required to form a sintering neck and perform densification sintering. Therefore, the sintering temperature T of the coarse and fine powder mixture is closer to 0.85TL.
烧结件密度为4.36g/cm3,屈服强度达到了870MPa,延伸率在5%左右(ISO22068-TC4指标:屈服强度≥600MPa,延伸率≥3%,密度≥4.2g/cm3)。图1为本实施例中烧结坯的金相显微组织。The density of the sintered part is 4.36 g/cm3, the yield strength reaches 870 MPa, and the elongation is about 5% (ISO22068-TC4 index: yield strength ≥ 600 MPa, elongation ≥ 3%, density ≥ 4.2 g/cm3). FIG1 is the metallographic microstructure of the sintered blank in this embodiment.
(实施例2)(Example 2)
本发明包括以下步骤:The present invention comprises the following steps:
S1、准备钛合金细粉和钛合金粗粉,其中钛合金细粉的粒径范围为1~20μm(D50:10~13μm),钛合金粗粉的粒径范围为50~100μm(D50:70~80μm);将钛合金细粉和钛合金粗粉混合形成钛合金混合粉末;所述钛合金混合粉末中钛合金粗粉和钛合金细粉的比例为3:2;S1. Prepare titanium alloy fine powder and titanium alloy coarse powder, wherein the particle size range of the titanium alloy fine powder is 1-20 μm (D50: 10-13 μm), and the particle size range of the titanium alloy coarse powder is 50-100 μm (D50: 70-80 μm); mix the titanium alloy fine powder and the titanium alloy coarse powder to form a titanium alloy mixed powder; the ratio of the titanium alloy coarse powder to the titanium alloy fine powder in the titanium alloy mixed powder is 3:2;
S2、将钛合金混合粉末与粘结剂混炼制备形成喂料;其中钛合金混合粉末与粘结剂的比例为1.6;所述喂料中钛合金粉末体积占比为64%,其余为高分子粘结剂。所述高分子粘结剂的组分按照质量百分比包括60%~70%的聚甲醛,12%~15%的聚乙烯,15%~20%的聚丙烯以及3%~5%的硬脂酸;S2. Mix the titanium alloy mixed powder and the binder to form a feed material; wherein the ratio of the titanium alloy mixed powder to the binder is 1.6; the volume proportion of the titanium alloy powder in the feed material is 64%, and the rest is the polymer binder. The components of the polymer binder include 60% to 70% of polyoxymethylene, 12% to 15% of polyethylene, 15% to 20% of polypropylene and 3% to 5% of stearic acid in terms of mass percentage;
S3、将喂料置于注射成型机内,经模具注射成形为注射坯;注射参数为:模具温度为80~120℃,喂料加热温度为160~220℃,注射压力为80~120MPa;保压时间1~2.5s;S3, placing the feed material in an injection molding machine, and injecting it into an injection blank through a mold; the injection parameters are: mold temperature of 80-120°C, feed material heating temperature of 160-220°C, injection pressure of 80-120MPa; holding time of 1-2.5s;
S4、对注射坯进行脱脂获得脱脂坯;脱脂的具体技术参数是:脱脂采用草酸介质进行催化脱脂,脱脂时间为脱脂时间t≥(60+60*h)min,h为注射坯的最大厚度,单位为mm;S4, degreasing the injection blank to obtain a degreasing blank; the specific technical parameters of the degreasing are: the degreasing is carried out by catalytic degreasing with oxalic acid medium, the degreasing time is the degreasing time t≥(60+60*h)min, h is the maximum thickness of the injection blank, the unit is mm;
S5、对脱脂坯进行高真空烧结,获得烧结坯;烧结的具体技术参数是:采用金属腔体烧结炉进行高真空烧结,炉膛内的压力≤1.0×10-3Pa,烧结温度T满足0.65TL≤T≤0.85TL。由于粗粉的烧结动能相对于细粉较高,形成烧结颈并进行致密化烧结需要更多的烧结能量。因此,粗细粉混合的烧结温度T更接近于0.85TL;S5. Perform high vacuum sintering on the degreased blank to obtain a sintered blank. The specific technical parameters of sintering are: high vacuum sintering in a metal cavity sintering furnace, the pressure in the furnace is ≤1.0×10-3Pa, and the sintering temperature T satisfies 0.65TL≤T≤0.85TL. Since the sintering kinetic energy of coarse powder is higher than that of fine powder, more sintering energy is required to form a sintering neck and perform densification sintering. Therefore, the sintering temperature T of the mixture of coarse and fine powders is closer to 0.85TL.
烧结件密度为4.35g/cm3,屈服强度达到了875MPa,延伸率在5%左右(ISO22068-TC4指标:屈服强度≥600MPa,延伸率≥3%,密度≥4.2g/cm3)。图2为本实施 例中烧结坯的金相显微组织。The density of the sintered part is 4.35g/cm3, the yield strength reaches 875MPa, and the elongation is about 5% (ISO22068-TC4 index: yield strength ≥600MPa, elongation ≥3%, density ≥4.2g/cm3). Metallographic microstructure of the sintered blank in the example.
(对比实施例)(Comparative Example)
本发明包括以下步骤:The present invention comprises the following steps:
S1、准备钛合金细粉和钛合金粗粉,其中钛合金细粉的粒径范围为1~20μm(D50:10~13μm),钛合金粗粉的粒径范围为50~100μm(D50:70~80μm);将钛合金细粉和钛合金粗粉混合形成钛合金混合粉末;所述钛合金混合粉末中钛合金粗粉和钛合金细粉的比例为4:1;S1. Prepare titanium alloy fine powder and titanium alloy coarse powder, wherein the particle size range of the titanium alloy fine powder is 1 to 20 μm (D50: 10 to 13 μm), and the particle size range of the titanium alloy coarse powder is 50 to 100 μm (D50: 70 to 80 μm); mix the titanium alloy fine powder and the titanium alloy coarse powder to form a titanium alloy mixed powder; the ratio of the titanium alloy coarse powder to the titanium alloy fine powder in the titanium alloy mixed powder is 4:1;
S2、将钛合金混合粉末与粘结剂混炼制备形成喂料;其中钛合金混合粉末与粘结剂的比例为1.3;上述喂料中钛合金粉末体积占比为58%,其余为高分子粘结剂。所述高分子粘结剂的组分按照质量百分比包括60%~70%的聚甲醛,12%~15%的聚乙烯,15%~20%的聚丙烯以及3%~5%的硬脂酸;S2. Mix the titanium alloy mixed powder and the binder to prepare a feed material; wherein the ratio of the titanium alloy mixed powder to the binder is 1.3; the volume proportion of the titanium alloy powder in the above feed material is 58%, and the rest is a polymer binder. The components of the polymer binder include 60% to 70% of polyoxymethylene, 12% to 15% of polyethylene, 15% to 20% of polypropylene and 3% to 5% of stearic acid in terms of mass percentage;
S3、将喂料置于注射成型机内,经模具注射成形为注射坯;注射参数为:模具温度为80~120℃,喂料加热温度为160~220℃,注射压力为80~120MPa;保压时间1~2.5s;S3, placing the feed material in an injection molding machine, and injecting it into an injection blank through a mold; the injection parameters are: mold temperature of 80-120°C, feed material heating temperature of 160-220°C, injection pressure of 80-120MPa; holding time of 1-2.5s;
S4、对注射坯进行脱脂获得脱脂坯;脱脂的具体技术参数是:脱脂采用草酸介质进行催化脱脂,脱脂时间为脱脂时间t≥(60+60*h)min,h为注射坯的最大厚度,单位为mm;S4, degreasing the injection blank to obtain a degreasing blank; the specific technical parameters of the degreasing are: the degreasing is carried out by catalytic degreasing with oxalic acid medium, the degreasing time is the degreasing time t≥(60+60*h)min, h is the maximum thickness of the injection blank, the unit is mm;
S5、对脱脂坯进行高真空烧结,获得烧结坯。烧结的具体技术参数是:采用金属腔体烧结炉进行高真空烧结,炉膛内的压力≤1.0×10-3Pa,烧结温度T满足0.65TL≤T≤0.85TL。由于粗粉的烧结动能相对于细粉较高,形成烧结颈并进行致密化烧结需要更多的烧结能量。因此,粗细粉混合的烧结温度T更接近于0.85TL。S5. Perform high vacuum sintering on the degreased blank to obtain a sintered blank. The specific technical parameters of sintering are: high vacuum sintering in a metal cavity sintering furnace, the pressure in the furnace is ≤1.0×10-3Pa, and the sintering temperature T satisfies 0.65TL≤T≤0.85TL. Since the sintering kinetic energy of coarse powder is higher than that of fine powder, more sintering energy is required to form a sintering neck and perform densification sintering. Therefore, the sintering temperature T of the mixture of coarse and fine powders is closer to 0.85TL.
烧结件密度为4.18g/cm3,屈服强度达到了490MPa,延伸率在2%左右(ISO22068-TC4指标:屈服强度≥600MPa,延伸率≥3%,密度≥4.2g/cm3)。图3为本实施例中烧结坯的金相显微组织。The density of the sintered part is 4.18 g/cm3, the yield strength reaches 490 MPa, and the elongation is about 2% (ISO22068-TC4 index: yield strength ≥ 600 MPa, elongation ≥ 3%, density ≥ 4.2 g/cm3). FIG3 is the metallographic microstructure of the sintered blank in this embodiment.
由实施例1、实施例2和对比实施例可以看出,钛合金混合粉末中钛合金粗粉和钛合金细粉的比例对于烧结件的密度、屈服强度以及延伸率都有很大的影响。并不是钛合金细粉比例越高,产品性能越强。范围是在本发明所给出的范围内进行合理化混合才能获得性能优异的钛合金材料。同时从图1至图3的金相显微组织也能够看到整体区别。 It can be seen from Example 1, Example 2 and the comparative example that the ratio of titanium alloy coarse powder and titanium alloy fine powder in the titanium alloy mixed powder has a great influence on the density, yield strength and elongation of the sintered part. It is not the case that the higher the ratio of titanium alloy fine powder, the stronger the product performance. The range is that a titanium alloy material with excellent performance can be obtained by rationally mixing within the range given by the present invention. At the same time, the overall difference can also be seen from the metallographic microstructures of Figures 1 to 3.
以上所述的具体实施例,对本发明的目的、技术方案和有益效果进行了进一步详细说明,所应理解的是,以上所述仅为本发明的具体实施例而已,并不用于限制本发明,凡在本发明的精神和原则之内,所做的任何修改、等同替换、改进等,均应包含在本发明的保护范围之内。 The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims (8)