Summary of the invention
Aiming at the problems existing in the prior art, the present invention provides a kind of side that ceramics are made using three-dimensional printing technology
Method, specifically includes previously prepared ethyl orthosilicate, the powder body material with predetermined ingredient, and by water, cosolvent and soda acid tune
The complex function reagent that section agent is mixed in a certain ratio;
In the method, threedimensional model to be printed is generated by host computer first, and will be after threedimensional model slice
It forms the corresponding plan view of multilayer and is sent in the next three-dimensional printer and printed;
Further include following steps:
Step S1 uses the ethyl orthosilicate, the powder body material and the complex function reagent in forming surface
It is mixed to form the corresponding printable layer of one layer of plan view;
Step S2 heats the printable layer using the heating device of the three-dimensional printer, complete one layer at
Type;
Step S3, repeating said steps S1-S2, until all plan views print and finish and form ceramic forerunner
Afterwards, step S4 is turned to;
Step S4 is handled the ceramic member presoma to obtain ceramic member, with backed off after random.
Preferably, the powder body material, the ethyl orthosilicate and the complex function reagent are prepared respectively, so that described
The mass ratio of ethyl orthosilicate and the powder body material is 2%-15%, and the quality of water is described in the complex function reagent
2-5 times of the quality of ethyl orthosilicate.
Preferably, the powder body material includes one of china clay, kaolin, clay, bentonite and feldspar powder powder
Or the mixing of several powder;
The particle size range of the powder is 100-8000 mesh.
Preferably, in the step S2, the heating device be infrared heating device perhaps microwave heating equipment or
Ultrasonically promoted reaction device.
Preferably, when being mixed to form the complex function reagent, the certain proportion are as follows: the content of water is not less than 50%,
The content of cosolvent is not less than 10%.
Preferably, in the complex function reagent being mixed to form:
The cosolvent includes ethyl alcohol and/or methanol and/or isopropanol and/or n-butanol and/or dioxane,
And/or formamide and/or acetone and/or tetrahydrofuran;
The acid-base modifier includes hydrochloric acid and/or hydrofluoric acid and/or sulfuric acid and/or nitric acid and/or ammonium hydroxide, and/
Or organic amino.
Preferably, the ethyl orthosilicate and the powder body material are mixed to form the first premix powders in advance;
The step S1 is specifically included:
First premix powders are laid in the forming surface by step S11a;
Step S12a is sprayed described multiple using the array piezo jets of the three-dimensional printer in the forming surface
Functional reagent is closed, to form the printable layer.
Preferably, the powder body material and the complex function reagent are mixed to form the second premix powders in advance;
The step S1 is specifically included:
Second premix powders are laid in the forming surface by step S11b;
Step S12b, using the array piezo jets of the three-dimensional printer, sprayed in the forming surface it is described just
Silester, to form the printable layer.
Preferably, the step S1 is specifically included:
The powder body material is laid in the forming surface by step S11c;
Step S12c sprays institute using the first array piezo jets on the three-dimensional printer in the forming surface
Ethyl orthosilicate is stated, while spraying institute in the forming surface using the second array formula piezo jets on the three-dimensional printer
Complex function reagent is stated, to form the printable layer.
Preferably, the ceramic member is formed after being handled by the way of sintering the ceramic forerunner, it is specific to wrap
It includes:
The ceramic forerunner is placed in ethyl orthosilicate and impregnates by step A1;
Step A2, then the ceramic forerunner is placed in the complex function reagent and is impregnated;
Step A3 is sintered again after the ceramic forerunner is taken out drying, forms the ceramic member.
Preferably, the ceramic member is formed after being handled by the way of non-sintered the ceramic forerunner, specifically
Include:
The ceramic forerunner is placed in ethyl orthosilicate and impregnates by step B1;
Step B2, then the ceramic forerunner is placed in the complex function reagent and is impregnated;
The ceramic forerunner is taken out drying by step B3;
Repeating said steps B1-B3, until liquid forms the ceramic member after can not penetrating into the ceramic forerunner.
The beneficial effects of the present invention are:
1) raw material less expensive using price, reduces 3 D-printing ceramic member cost;
2) the ceramic member defect made by is few and consistency is high;
3) stamp with the size of ceramic member is unrestricted, and printing effect is high, effective improving production efficiency;
4) molding adhesive in printing shaping process be inorganic matter silica, be ceramics itself active principle it
One, without carrying out defatting step, and without other a large amount of organic generations in sintering process, production process is more environmentally-friendly.
Specific embodiment
The present invention is described in detail with specific embodiment below in conjunction with the accompanying drawings.The present invention is not limited to the embodiment party
Formula, as long as meeting purport of the invention, other embodiments also may belong to scope of the invention.
A method of using three-dimensional printing technology make ceramics, including previously prepared ethyl orthosilicate, have make a reservation for into
The powder body material divided, and the complex function reagent that water, cosolvent and acid-base modifier are mixed in a certain ratio;
In this method, threedimensional model to be printed is generated by host computer first, and is formed after threedimensional model is sliced more
The corresponding plan view of layer and being sent in the next three-dimensional printer is printed;
As shown in Figure 1, further including following steps:
Step S1 is mixed to form one layer using ethyl orthosilicate, powder body material and complex function reagent in forming surface
The corresponding printable layer of plan view;
Step S2 heats printable layer using the heating device of three-dimensional printer, completes one layer of molding;
Step S3 repeats step S1-S2, until all plan views print after finishing and forming ceramic forerunner, turns to
Step S4;
Step S4 is handled ceramic member presoma to obtain ceramic member, with backed off after random.
Specifically, in the present embodiment, the thickness of printable layer can be configured as needed on upper computer software, thickness
Setting value can be between 0.05-1mm.
In preferred embodiment of the invention, powder body material, ethyl orthosilicate and complex function reagent are prepared respectively, so that
The mass ratio of ethyl orthosilicate and powder body material is 2%-15%, and the quality of water is ethyl orthosilicate in complex function reagent
2-5 times of quality.
Specifically, in the present embodiment, the dosage of ethyl orthosilicate is less, and the dosage of powder body material is more, and positive silicic acid second
The mass ratio of ester and powder body material includes but is not limited to 2%-15%, and wherein ethyl orthosilicate also can be used with ethyl orthosilicate
Liquid as main component replaces.
In preferred embodiment of the invention, powder body material includes china clay, kaolin, clay, bentonite and feldspar powder
One of powder or several powder mixing;And the particle size range of powder is 100-8000 mesh.
Specifically, in the present embodiment, powder body material is the mixing of one or several kinds of powder of ceramic primary raw material, this hair
It is not specifically limited in bright.
In preferred embodiment of the invention, in step S2, heating device is infrared heating device or microwave heating dress
It sets or ultrasonically promoted reaction device.
In preferred embodiment of the invention, when being mixed to form complex function reagent, certain proportion are as follows: the content of water is not small
In 50%, the content of cosolvent is not less than 10%.
In preferred embodiment of the invention, in the complex function reagent that is mixed to form:
Cosolvent includes ethyl alcohol and/or methanol and/or isopropanol and/or n-butanol and/or dioxane, and/or
Formamide and/or acetone and/or tetrahydrofuran;
Acid-base modifier includes hydrochloric acid and/or hydrofluoric acid and/or sulfuric acid and/or nitric acid and/or ammonium hydroxide, and/or is had
Machine ammonia.
Specifically, in the present embodiment, the cosolvent in complex function reagent includes but is not limited to ethyl alcohol and/or methanol,
And/or isopropanol and/or n-butanol and/or dioxane and/or formamide and/or acetone and/or tetrahydrofuran;It is multiple
The acid-base modifier closed in functional reagent includes but is not limited to hydrochloric acid and/or hydrofluoric acid and/or sulfuric acid and/or nitric acid, and/
Or ammonium hydroxide and/or organic amino.
In a preferred embodiment of the invention, ethyl orthosilicate and powder body material are mixed to form the first premix in advance
Powder;
Then in the embodiment, as shown in Fig. 2, step S1 is specifically included:
First premix powders are laid in forming surface by step S11a;
Step S12a sprays complex function reagent using the array piezo jets of three-dimensional printer in forming surface, with
Form printable layer.
Specifically, in the present embodiment, the array piezo jets of three-dimensional printer are mobile in the top of forming surface, and according to
Plan view sprays complex function reagent on the specific area, and the amount of injection of complex function reagent is controlled so that unit volume
In powder body material, the quality of water is 2-5 times of the quality of the ethyl orthosilicate in the first premix powders in complex function reagent.
In another preferred embodiment of the invention, powder body material and complex function reagent are mixed to form second in advance
Premix powders;
Then in the embodiment, as shown in figure 3, step S1 is specifically included:
Second premix powders are laid in forming surface by step S11b;
Step S12b sprays ethyl orthosilicate, in forming surface using the array piezo jets of three-dimensional printer with shape
At printable layer.
In another preferred embodiment of the invention, as shown in figure 4, step S1 is specifically included:
Step S11c, powder body material is laid in forming surface;
Step S12c sprays positive silicic acid second using the first array piezo jets on three-dimensional printer in forming surface
Ester, while complex function reagent is sprayed in forming surface using the second array formula piezo jets on three-dimensional printer, to be formed
Printable layer.
In other words, in technical solution of the present invention, as long as mixed powder material, ethyl orthosilicate in each layer of forming surface
And complex function reagent, do not limit powder body material, ethyl orthosilicate and complex function reagent addition manner and add
The sequencing added.
In the present invention, in above-mentioned steps S1, being laid with powder body material (is either the first premix powders or the second premixing flour
Material) after, the region of ethyl orthosilicate and/or complex function reagent is sprayed for the specific region in forming surface, that is, is formed
There is the region for the figure for needing to carry out 3 D-printing on face, do not need to carry out spraying in the white space in forming surface.
In preferred embodiment of the invention, ceramics are formed after being handled by the way of sintering ceramic forerunner
Part, as shown in figure 5, specifically including:
Ceramic forerunner is placed in ethyl orthosilicate and impregnates by step A1;
Step A2, then ceramic forerunner is placed in complex function reagent and is impregnated;
Step A3 is sintered again after ceramic forerunner is taken out drying, forms ceramic member.
In preferred embodiment of the invention, ceramics are formed after being handled by the way of non-sintered ceramic forerunner
Part, as shown in fig. 6, specifically including:
Ceramic forerunner is placed in ethyl orthosilicate and impregnates by step B1;
Step B2, then ceramic forerunner is placed in complex function reagent and is impregnated;
Ceramic forerunner is taken out drying by step B3;
Step B1-B3 is repeated, until liquid forms ceramic member after can not penetrating into ceramic forerunner.
In a preferred embodiment of the invention, the production of ceramic member is carried out according to Fig. 1 and step shown in Fig. 2:
By silicone content be 40% ethyl orthosilicate and granularity to be the china clay of 600 mesh use muller with the mass ratio of 2:100
Formula batch mixer or other equipment are sufficiently mixed, and the first premix powders are obtained;The hydrochloric acid that water, ethyl alcohol and concentration are 35% is pressed
The mass ratio of 78:21.5:0.5, which pours into container, to be thoroughly mixed, and complex function reagent is obtained.
Threedimensional model to be printed is established in host computer, and above-mentioned model is sliced by setting thickness with software,
Several corresponding plan views are generated, host computer reads above-mentioned plan view, generates the dot array data of above-mentioned plan view and be sent to
In the next three-dimensional printer.
As shown in fig. 7, cleaning work table top 4, controls transmission mechanism by control circuit and drives piston rod 2, make to lead to therewith
It crosses the powder bed 3 being threadedly coupled and moves down 0.3mm.
As shown in figure 8, control powdering roller 51 is pre- one layer of 3 upper berth of powder bed along the direction parallel with work top 4
Mixed powder 6, the premix powders 6 spread are flushed with work top 4.
As shown in Figure 9 and Figure 10, control array piezo jets 8 are moved after the dot array data of three-dimensional printer acquisition plan view
It is dynamic, and complex function reagent is sprayed in forming area 7, the amount of injection is controlled, so that by jeting area powder body material and complex function
The mass ratio of reagent is 100:6.
As shown in figure 11, the infrared heating device 9 for being located at 7 top of forming area is opened, forming area 7 is made by irradiation
Temperature rises to about 60 DEG C, prolonged exposure 3~5 seconds, accelerates the hydrolysis and polycondensation of ethyl orthosilicate, generates silicon dioxide molecules and hands over
Networking network, to realize that powder bonds, because above-mentioned powder bed 3 moves down 0.3mm, thus the resulting as 0.3mm thick layer by layer.
Above-mentioned the step of moving down powder bed 3, powdering, injection complex function reagent and heating to forming area is repeated, successively
Remaining all printable layers are printed, as shown in figure 12, bonding is successively stacked in forming area 7 and forms ceramic member presoma 10.
After standing 12 hours, ceramic forerunner 10 is taken out from powder bed, simultaneously by unglued molding powder removal
It recycles;Ceramic forerunner 10 is first placed in 2 hours of immersion in ethyl orthosilicate, then is placed in complex function reagent and impregnates
Then as shown in figure 13 2 hours are put into 12 hours of heat preservation in the constant baking oven 11 for being 60 DEG C of temperature, placing after taking-up makes
It is spontaneously dried, and is put into Muffle furnace after dry, sinters high-intensitive and high-densit ceramic member at 1300 DEG C;
In the present embodiment, by ceramic forerunner 10 after taking out in powder bed, non-sintered processing mode can also be taken:
Ceramic forerunner 10 is first soaked in ethyl orthosilicate, then is soaked in complex function reagent, is taken out and is spontaneously dried, then will be above-mentioned
It impregnates and drying process is repeated as many times, until liquid, which can not penetrate into, obtains high-intensitive and high-densit ceramic member;
In the present embodiment, power spreading device is roll type, can also according to circumstances be changed to scraper-type as shown in figure 14.
In another preferred embodiment of the invention, the production of ceramic member is carried out according to Fig. 1 and step shown in Fig. 3,
Wherein,
After powder body material and complex function reagent are first thoroughly mixed to form the second premix powders, then sprayed using array
Head injection ethyl orthosilicate;
Remaining step is identical as embodiment before, and details are not described herein.
In another preferred embodiment of the invention, the production of ceramic member is carried out according to Fig. 1 and step shown in Fig. 4,
Wherein,
Directly powder body material is laid in powder bed, is then sprayed respectively just using two groups of independent array formula piezo jets
Silester and complex function reagent;
Remaining step is identical as embodiment before, and details are not described herein.
The foregoing is merely preferred embodiments of the present invention, are not intended to limit embodiments of the present invention and protection model
It encloses, to those skilled in the art, should can appreciate that and all be equal with made by present specification and diagramatic content
It replaces and obviously changes obtained scheme, should all be included within the scope of the present invention.