JPH02145252A - Polishing method for spinning face of mouth piece for spinning of doughnut type - Google Patents
Polishing method for spinning face of mouth piece for spinning of doughnut typeInfo
- Publication number
- JPH02145252A JPH02145252A JP29743188A JP29743188A JPH02145252A JP H02145252 A JPH02145252 A JP H02145252A JP 29743188 A JP29743188 A JP 29743188A JP 29743188 A JP29743188 A JP 29743188A JP H02145252 A JPH02145252 A JP H02145252A
- Authority
- JP
- Japan
- Prior art keywords
- spinning
- polishing
- donut
- shaped
- roll
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.
Description
【発明の詳細な説明】
(産業上の利用分野)
本発明は、レーヨン、アクリル等を湿式或いは乾式紡糸
するドーナツ型紡糸用口金の紡糸面研摩方法に関する。DETAILED DESCRIPTION OF THE INVENTION (Field of Industrial Application) The present invention relates to a method of polishing the spinning surface of a donut-shaped spinning nozzle for wet or dry spinning of rayon, acrylic, etc.
(従来の技術)
第2図に示す如く断面カップ形状のドーナツ型紡糸用口
金1の紡糸面2を什摩するには、円板型のサンドベーパ
3を回転治具4に取りつけて回転させている。(Prior Art) As shown in FIG. 2, in order to polish the spinning surface 2 of the doughnut-shaped spinning nozzle 1 having a cup-shaped cross section, a disk-shaped sand vapor 3 is attached to a rotating jig 4 and rotated. .
(発明が解決しようとする課題)
ところで、上記の研摩方法では、ドーナツ型紡糸用口金
1の紡糸面2が幅方向(ドーナツの半径方向)で円弧状
となっている為、研摩中にサンドベーパ3の位置とドー
ナツ型紡糸用口金1の位置を移動しなければならず、作
業性が悪い。また荒研磨、中研摩、仕上げ研摩を行う為
、その都度所要のサンドベーパ3を回転治具4に取付け
なければならず、サンドベーパ3の交換頻度が多くて研
摩能率が悪い。さらにサンドベーパ3の目詰まりにより
紡糸面2に傷が付いたり、焼き付きにより変色したりす
るものである。その上研摩作業は熟練を要する為、未熟
な者では研摩不足、研摩オーバー等が生じ、品質を一定
にすることが難しかった。特に紡糸孔のストレート長さ
が不揃いとなって、使用時紡糸むらが生じ、断糸、デニ
ールむら等が発生することがあった。(Problem to be Solved by the Invention) By the way, in the above polishing method, since the spinning surface 2 of the donut-shaped spinning nozzle 1 has an arc shape in the width direction (the radial direction of the donut), the sand vapor 3 , and the position of the donut-shaped spinning nozzle 1 must be moved, resulting in poor workability. Furthermore, in order to perform rough polishing, medium polishing, and final polishing, the required sand vapor 3 must be attached to the rotating jig 4 each time, and the sand vapor 3 must be replaced frequently, resulting in poor polishing efficiency. Furthermore, the spinning surface 2 may be scratched due to clogging of the sand vapor 3 or discolored due to burning. Furthermore, since polishing work requires skill, inexperienced workers may end up polishing insufficiently or overpolishing, making it difficult to maintain consistent quality. In particular, the straight lengths of the spinning holes may become uneven, resulting in uneven spinning during use, resulting in yarn breakage, uneven denier, etc.
そこで本発明は、作業性、研摩能率が良く、紡糸面に傷
が付いたり、焼き付いたりすることが無く、熟練を要さ
ずに研摩作業ができて品質を一定にできるドーナツ型紡
糸用口金の紡糸面研摩方法を提供しようとするものであ
る。Therefore, the present invention has developed a donut-shaped spinning nozzle that has good workability and polishing efficiency, does not scratch or burn the spinning surface, can perform polishing operations without requiring any skill, and can maintain constant quality. It is an object of the present invention to provide a method for polishing a spinning surface.
(課題を解決するための手段)
上記課題を解決するための本発明のドーナツ型紡糸用口
金の紡糸面研摩方法は、ドーナツ型紡糸用口金を回転さ
せてその紡糸面に、ロール式の研摩シートを連続的に繰
り出して硬質ゴム製のバックアップロールにて押圧する
と共にバックアップロールを両側方に揺動させて、前記
紡糸面をロール式の研摩シートにて研摩することを特徴
とするものである。(Means for Solving the Problems) A method for polishing the spinning surface of a donut-shaped spinning nozzle according to the present invention for solving the above-mentioned problems includes rotating a donut-shaped spinning nozzle and applying a roll-type polishing sheet to the spinning surface of the donut-shaped spinning nozzle. The method is characterized in that the spinning surface is polished with a roll-type polishing sheet by continuously feeding out the spinning material and pressing it with a hard rubber backup roll, and swinging the backup roll in both directions.
(作用)
上述の如く本発明のドーナツ型紡糸用口金の紡糸面研摩
方法は、ロール式の研摩シートを連続的に繰り出して紡
糸面を研摩するのであるから、作業性が良く、また従来
のようにサンドペーパを交換する必要が無いので、研摩
能率が良く、しかも紡糸面は常に新しい砥粒で研摩され
ることとなって、安定した研摩が行われる。また硬質ゴ
ムのバックアップロールにてロール式研摩シートを抑圧
保持するので、紡糸面の幅方向の曲率へのなじみが良く
、緩衝作用もすることとなる。さらにバックアップロー
ルを両側方に揺動させてロール式の研摩シートにて紡糸
面を研摩するので、紡糸面はクロスハツチ状の方向性の
無い均一な面となるので、研摩むらが無くなり、傷の発
生も無い。(Function) As described above, the method of polishing the spinning surface of the donut-shaped spinning nozzle of the present invention has good workability because the spinning surface is polished by continuously feeding out a roll-type polishing sheet, and it does not require the conventional method. Since there is no need to replace the sandpaper every now and then, the polishing efficiency is high, and the spinning surface is always polished with new abrasive grains, resulting in stable polishing. In addition, since the rolled abrasive sheet is held down by a hard rubber backup roll, it conforms well to the curvature of the spinning surface in the width direction, and also has a buffering effect. Furthermore, since the backup roll is swung to both sides and the spinning surface is polished with a roll-type polishing sheet, the spinning surface becomes a crosshatch-like uniform surface with no directionality, eliminating uneven polishing and causing scratches. There is no.
(実施例)
本発明のドーナツ型紡糸用口金の紡糸面研摩方法の一実
施例を説明する。第1図に示す如く外径240mm、内
径169mmのドーナツ型で、断面ハツト形状の深さ1
0mm、肉厚1.01111111フランジ幅12mm
のステンレス鋼より成る紡糸用口金1を1100rpで
回転させてその紡糸面2に、幅60mm、厚さ1.25
mmのポリエストテープ上にAl1203の砥粒(9μ
m〜100μm)を塗布固定したロール式の研摩シート
3′を連続的に繰り出して、硬質ゴム(ゴム硬度40)
製の直径60mm、幅60mmのバックアップロール5
にて押圧すると共にこのバックアップロール5を両側方
に1分間に100回の割合で3 mmづつ補動させて、
前記紡糸面2を研摩シート3′にて研摩した。(Example) An example of the method for polishing the spinning surface of the donut-shaped spinning nozzle of the present invention will be described. As shown in Figure 1, it is donut-shaped with an outer diameter of 240 mm and an inner diameter of 169 mm, with a hat-shaped cross section and a depth of 1.
0mm, wall thickness 1.01111111 flange width 12mm
A spinning nozzle 1 made of stainless steel is rotated at 1100 rp, and a spinneret with a width of 60 mm and a thickness of 1.25 mm is placed on the spinning surface 2.
Al1203 abrasive grains (9μ
A roll-type abrasive sheet 3' coated with hard rubber (rubber hardness 40) is continuously rolled out.
Backup roll 5 with a diameter of 60 mm and a width of 60 mm
At the same time, the backup roll 5 is assisted by 3 mm on both sides at a rate of 100 times per minute.
The spinning surface 2 was polished with a polishing sheet 3'.
こうして研摩したドーナツ型紡糸用口金の紡糸面を検査
した処、該紡糸面はクロスハツチ状の方向性の無い均一
な面となっていて、研摩むらが無く、研摩シートの目詰
りによる傷の発生も無かった。そしてこのドーナツ型紡
糸用口金を使用した処、紡糸孔のストレート長さが一定
している為、紡糸むらが生ぜず、断糸、デニールむら等
が生じることが無かった。When the spinning surface of the donut-shaped spinning nozzle polished in this way was inspected, the spinning surface was a crosshatch-like uniform surface with no directionality, and there was no unevenness in polishing, and there was no occurrence of scratches due to clogging of the polishing sheet. There wasn't. When this doughnut-shaped spinning nozzle was used, since the straight length of the spinning hole was constant, uneven spinning did not occur, and yarn breakage, uneven denier, etc. did not occur.
(発明の効果)
以上の説明で判るように本発明のドーナツ型紡糸用口金
の紡糸面研摩方法は、作業性が良く、また従来のように
サンドベーパを交換する必要が無いので、研摩能率が良
く、しかも紡糸面は常に新しい砥粒で研摩されることと
なって安定した研摩が行われる。またその紡糸面はクロ
スハツチ状の方向性の無い均一な面となって、研摩むら
が無く、傷の発生も無くて、紡糸孔のストレート長さが
一定している。従って、使用時紡糸むらが生ぜず、断糸
、デニールむら等の生じることの無いドーナツ型紡糸用
口金が得られる。(Effects of the Invention) As can be seen from the above explanation, the method of polishing the spinning surface of the donut-shaped spinning nozzle of the present invention has good workability, and there is no need to replace the sand vapor as in the conventional method, so the polishing efficiency is high. Moreover, the spinning surface is constantly polished with new abrasive grains, resulting in stable polishing. Further, the spinning surface is a crosshatch-like uniform surface with no directionality, and there is no uneven polishing, no scratches, and the straight length of the spinning hole is constant. Therefore, it is possible to obtain a donut-shaped spinning nozzle that does not cause uneven spinning during use, and is free from yarn breakage, uneven denier, and the like.
第1図は本発明のドーナツ型紡糸用口金の紡糸面研摩方
法の実施例を示す斜視図、第2図は従来のドーナツ型紡
糸用口金の紡糸面研摩方法を示す斜視図である。
出願人 田中貴金属工業株式会社FIG. 1 is a perspective view showing an embodiment of the method for polishing the spinning surface of a donut-shaped spinning nozzle according to the present invention, and FIG. 2 is a perspective view showing a conventional method for polishing the spinning surface of a donut-shaped spinning nozzle. Applicant Tanaka Kikinzoku Kogyo Co., Ltd.
Claims (1)
ロール式の研摩シートを連続的に繰り出して硬質ゴム製
のバックアップロールにて押圧すると共にバックアップ
ロールを両側方に揺動させて、前記紡糸面をロール式の
研摩シートにて研摩することを特徴とするドーナツ型紡
糸用口金の紡糸面研摩方法。1. Rotate the donut-shaped spinning nozzle and apply it to the spinning surface.
The spinning surface is polished with the roll-type abrasive sheet by continuously feeding out a roll-type abrasive sheet and pressing it with a hard rubber backup roll and swinging the backup roll in both directions. A method for polishing the spinning surface of a donut-shaped spinning nozzle.