JPH0222982B2 - - Google Patents
Info
- Publication number
- JPH0222982B2 JPH0222982B2 JP59006934A JP693484A JPH0222982B2 JP H0222982 B2 JPH0222982 B2 JP H0222982B2 JP 59006934 A JP59006934 A JP 59006934A JP 693484 A JP693484 A JP 693484A JP H0222982 B2 JPH0222982 B2 JP H0222982B2
- Authority
- JP
- Japan
- Prior art keywords
- battery
- layer
- ionomer resin
- sealing body
- metal plate
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired
Description
【発明の詳細な説明】
本発明は扁平型非水電解液電池の封口体に関す
るものである。
るものである。
近年エレクトロニクスの発達に伴ない、電卓、
時計など種々の機器が小型化、薄型化されるよう
になつてきて、それらの作動電池としての電池も
ますます小型化薄型化が要求されるようになつて
きた。
時計など種々の機器が小型化、薄型化されるよう
になつてきて、それらの作動電池としての電池も
ますます小型化薄型化が要求されるようになつて
きた。
しかしながら従来から考えられている扁平型非
水電解液電池は、負極金属板周縁に折り返し部を
設け、絶縁パツキングを介してクリンプ封口する
複雑な封口構造を有しており、電池の厚さは最低
でも1.2mm程度であり、1.0mm以下の超薄型のもの
は得られていなかつた。
水電解液電池は、負極金属板周縁に折り返し部を
設け、絶縁パツキングを介してクリンプ封口する
複雑な封口構造を有しており、電池の厚さは最低
でも1.2mm程度であり、1.0mm以下の超薄型のもの
は得られていなかつた。
そこで電池を薄型化するため、特開昭55−
133771号のように正極負極の金属板の間に発電要
素を介在させて対向させ、その周縁部を接着性の
封口体で接着し密封する構造の扁平型電池が考え
られた。こ場合、金属板は電池の外部端子、内部
集電体を兼ねている。接着性の封口体としては、
金属板に強力な接着性を有するアイオノマー樹脂
を用いることが提案されている。アイオノマー樹
脂の構造式は次のようなものである。すなわち、
エチレン・アクリル酸共重合体をアルカリ金属、
アルカリ土類金属などのイオン架橋したイオン性
共重合体である。
133771号のように正極負極の金属板の間に発電要
素を介在させて対向させ、その周縁部を接着性の
封口体で接着し密封する構造の扁平型電池が考え
られた。こ場合、金属板は電池の外部端子、内部
集電体を兼ねている。接着性の封口体としては、
金属板に強力な接着性を有するアイオノマー樹脂
を用いることが提案されている。アイオノマー樹
脂の構造式は次のようなものである。すなわち、
エチレン・アクリル酸共重合体をアルカリ金属、
アルカリ土類金属などのイオン架橋したイオン性
共重合体である。
アイオノマー樹脂を接着性封口体として用いた
扁平型非水電解液電池の場合、正極負極両金属板
の金属イオンとアイオノマー樹脂とが架橋結合
し、金属板と強力な接着性を有するため、長期貯
蔵中に内部の電解液の外部への挽散が少なく密閉
性が優れており、長期貯蔵の信頼性を有する電池
が期待される。
扁平型非水電解液電池の場合、正極負極両金属板
の金属イオンとアイオノマー樹脂とが架橋結合
し、金属板と強力な接着性を有するため、長期貯
蔵中に内部の電解液の外部への挽散が少なく密閉
性が優れており、長期貯蔵の信頼性を有する電池
が期待される。
しかしながら、アイオノマー樹脂は金属イオン
を含むため、電気絶縁性は良好でなく、アイオノ
マー樹脂を通して正極金属板と負極金属板との間
に微少電流が流れ、自己放電のため長期貯蔵の信
頼性が損なわれていた。
を含むため、電気絶縁性は良好でなく、アイオノ
マー樹脂を通して正極金属板と負極金属板との間
に微少電流が流れ、自己放電のため長期貯蔵の信
頼性が損なわれていた。
本発明の目的は、封口体の材質と構造を検討す
ることによつて、電池の長期貯蔵の信頼性を向上
させるものである。
ることによつて、電池の長期貯蔵の信頼性を向上
させるものである。
本発明は、正極負極の両金属板の間に発電要素
を介在させて対向させ、その周縁部を接着性の封
口体で密閉する扁平型非水電解液電池において、
封口体の電気絶縁性の優れたポリエチレンまたは
エチレン共重合体樹脂の層の両側に、熱接着性の
アイオノマー樹脂の層を接着した三層構造にする
とともに、アイオノマー樹脂の層を正極負極両金
属板各々に接着することによつて、長期貯蔵の信
頼性優れた扁平型非水電解液電池を提供するもの
である。第2図に本発明電池における封口部分の
拡大図を示す。封口体1はポリエチレンまたはエ
チレン共重合体の樹脂の層2の両側に、アイオノ
マー樹脂の層3を配した三層構造を有している。
アイオノマー樹脂の層3は、イオン導電性を有し
ているが、ポリエチレンの樹脂の層2は導電性を
有しない電気絶縁体なので、正極金属板4と負極
金属板5との間で全く電流を通さない。従つて、
第2図に示した封口体1を有する本発明の扁平型
非水電解液電池は、優れた長期貯蔵の信頼性を有
する。
を介在させて対向させ、その周縁部を接着性の封
口体で密閉する扁平型非水電解液電池において、
封口体の電気絶縁性の優れたポリエチレンまたは
エチレン共重合体樹脂の層の両側に、熱接着性の
アイオノマー樹脂の層を接着した三層構造にする
とともに、アイオノマー樹脂の層を正極負極両金
属板各々に接着することによつて、長期貯蔵の信
頼性優れた扁平型非水電解液電池を提供するもの
である。第2図に本発明電池における封口部分の
拡大図を示す。封口体1はポリエチレンまたはエ
チレン共重合体の樹脂の層2の両側に、アイオノ
マー樹脂の層3を配した三層構造を有している。
アイオノマー樹脂の層3は、イオン導電性を有し
ているが、ポリエチレンの樹脂の層2は導電性を
有しない電気絶縁体なので、正極金属板4と負極
金属板5との間で全く電流を通さない。従つて、
第2図に示した封口体1を有する本発明の扁平型
非水電解液電池は、優れた長期貯蔵の信頼性を有
する。
以下実施例によつてさらに詳細に説明する。リ
チウム・二酸化マンガン扁平型非水電解液電池に
ついて、実施例の電池構造を第1図に示す。
チウム・二酸化マンガン扁平型非水電解液電池に
ついて、実施例の電池構造を第1図に示す。
幅20mm、長さ70mmのステンレス鋼製の正極金属
板4上に二酸化マンガン正極合剤6、非水電解液
を含んだセレータ7、リチウム負極8、正極金属
板4との同形状のステンレス鋼製の負極棄金属板
5を配し、アイオノマー樹脂の層3−ポリエチレ
ンの樹脂の層2−アイオノマー樹脂の層3の三層
構造を有する封口体1を用いて、アイオノマー樹
脂の層3を正極負極両金属板4,5に各々熱接着
して封口することによつて、電池厚さ0.7mmの超
薄型密閉型の本発明の扁平型非水電解液電池Aを
組み立てた。
板4上に二酸化マンガン正極合剤6、非水電解液
を含んだセレータ7、リチウム負極8、正極金属
板4との同形状のステンレス鋼製の負極棄金属板
5を配し、アイオノマー樹脂の層3−ポリエチレ
ンの樹脂の層2−アイオノマー樹脂の層3の三層
構造を有する封口体1を用いて、アイオノマー樹
脂の層3を正極負極両金属板4,5に各々熱接着
して封口することによつて、電池厚さ0.7mmの超
薄型密閉型の本発明の扁平型非水電解液電池Aを
組み立てた。
比較例として、三層構造の封口体の代りにアイ
オノマー樹脂単独の封口体を用いて同型の従来電
池Bを組み立てた。第3図にA,Bの電池を長期
間放置した場合の放電曲線を示した。放電条件
は、20℃、2MΩの定抵抗放電である。図より明
らかなように、本発明電池Aは比較例電池Bに比
較して、持続時間が長く長期信頼性が優れてい
る。これは、比較例電池は封口体であるアイオノ
マー樹脂を通して正極負極金属板間に微少流が流
れ、いわゆる自己放電するために持続時間が短く
なつたものと考えられる。一方本発明電池では、
電気絶縁性のポリエチレン樹脂の層を間に配した
三層構造の封口体を用いるため、このような自己
放電がほとんど無く、長期の持続時間が得られた
ものである。なおポリエチレの樹脂の層の代りに
電気絶縁性のエチレン共重合体の樹脂の層を用い
た場合も同様な効果が得られた。
オノマー樹脂単独の封口体を用いて同型の従来電
池Bを組み立てた。第3図にA,Bの電池を長期
間放置した場合の放電曲線を示した。放電条件
は、20℃、2MΩの定抵抗放電である。図より明
らかなように、本発明電池Aは比較例電池Bに比
較して、持続時間が長く長期信頼性が優れてい
る。これは、比較例電池は封口体であるアイオノ
マー樹脂を通して正極負極金属板間に微少流が流
れ、いわゆる自己放電するために持続時間が短く
なつたものと考えられる。一方本発明電池では、
電気絶縁性のポリエチレン樹脂の層を間に配した
三層構造の封口体を用いるため、このような自己
放電がほとんど無く、長期の持続時間が得られた
ものである。なおポリエチレの樹脂の層の代りに
電気絶縁性のエチレン共重合体の樹脂の層を用い
た場合も同様な効果が得られた。
以上詳述したように、本発明は長期貯蔵の信頼
性の優れた超薄型の扁平型非水電解液を提供する
ことができる。
性の優れた超薄型の扁平型非水電解液を提供する
ことができる。
第1図は本発明実施例の扁平型非水電解液電池
の断面図、第2図は本発明電池の封口部の拡大断
面図、第3図は本発明電池Aと従来電池Bとの放
電曲線比較図である。 1……封口体、2……ポリエチレン樹脂の層、
3……アイオノマー樹脂の層、4……正極金属
板、5……負極金属板。
の断面図、第2図は本発明電池の封口部の拡大断
面図、第3図は本発明電池Aと従来電池Bとの放
電曲線比較図である。 1……封口体、2……ポリエチレン樹脂の層、
3……アイオノマー樹脂の層、4……正極金属
板、5……負極金属板。
Claims (1)
- 1 正極、負極両金属板の間に発電要素を介在さ
せて対向させ、該金属板の周縁部を接着性の封口
体で密閉する構造の扁平型非水電解液電池におい
て、該封口体がポリエチレンまたはエチレン共重
合体樹脂の層の両側に、アイオノマー樹脂の層を
配した三層構造であり、かつ該アイオノマー樹脂
の層が上記正極負極両金属板に接着していること
を特徴とする扁平型非水電解液電池。