JPH02236280A - Film formation method - Google Patents

Film formation method

Info

Publication number
JPH02236280A
JPH02236280A JP1057167A JP5716789A JPH02236280A JP H02236280 A JPH02236280 A JP H02236280A JP 1057167 A JP1057167 A JP 1057167A JP 5716789 A JP5716789 A JP 5716789A JP H02236280 A JPH02236280 A JP H02236280A
Authority
JP
Japan
Prior art keywords
carbon
substrate
ratio
hydrogen
diamond
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP1057167A
Other languages
Japanese (ja)
Other versions
JP2840750B2 (en
Inventor
Shinya Sumino
真也 角野
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Semiconductor Energy Laboratory Co Ltd
Original Assignee
Semiconductor Energy Laboratory Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Semiconductor Energy Laboratory Co Ltd filed Critical Semiconductor Energy Laboratory Co Ltd
Priority to JP1057167A priority Critical patent/JP2840750B2/en
Publication of JPH02236280A publication Critical patent/JPH02236280A/en
Application granted granted Critical
Publication of JP2840750B2 publication Critical patent/JP2840750B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PURPOSE:To form a diamond-like thin film on the surface of a substrate to be treated by maintaining a reduced pressure state in a reaction chamber contg. the substrate, introducing a gaseous mixture satisfying the relation of specific ratios of C, O2 and H2 into the chamber and impressing magnetic fields and microwaves from the outside. CONSTITUTION:After the substrate 8 to be treated is fixed to a holding base 6 in the reaction chamber 1, the inside of the reaction chamber 1 is evacuated and reduced in pressure. Gaseous alcoholic hydrocarbon, such as ethanol, metha nol, propyl alcohol, etc., and gaseous H2 are introduced as gaseous raw materials from a gas introducing system 10 into the chamber. The magnetic fields and microwaves are impressed to the gaseous raw materials by an external magnetic field generator 5 and a microwave generator 4 to generate high-density plasma and to form the C generated by cracking of the hydrocarbon as the diamond-like ultra-hard thin film on the surface of the substrate 8. The ratio of H/C is adjusted to 20 to 40, 7 to 15, 3 to 12 in the case of 1/1, 2/1, 3/1 O/C of the gaseous raw material mixture in this case, by which the diamond-like thin carbon film is formed on the substrate 8.

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明はマイクロ波プラスマを用いた炭素または炭素を
主成分とする被膜(いわゆるダイヤモンド状薄膜)の作
製方法に関するものである。
DETAILED DESCRIPTION OF THE INVENTION [Field of Industrial Application] The present invention relates to a method for producing carbon or a film containing carbon as a main component (so-called diamond-like thin film) using microwave plasma.

〔従来の技術〕[Conventional technology]

ダイヤモンドは従来より耐摩耗性部材や切削部材として
優れた材料であることは知られていたが、近年ダイヤモ
ンドの持つ電気絶縁性.熱伝導性硬度等の特性を活かし
、半導体の集積化に伴う絶縁膜や表面保護膜、電子材料
として注目され初めてきた。
Diamond has long been known to be an excellent material for wear-resistant materials and cutting materials, but in recent years diamond's electrical insulating properties have been greatly improved. Utilizing its properties such as thermal conductivity and hardness, it first attracted attention as an insulating film, surface protection film, and electronic material accompanying the integration of semiconductors.

このダイヤモンドを膜として形成させる方法として従来
よりメタン、エタン等の炭化水素と水素との混合ガス、
又はそれらに不活性ガスを含むものを反応性気体として
使用し、その反応性気体を真空室槽内に導入し、マイク
ロ波プラズマと、磁界とを印加してマイクロ波プラズマ
を発生させ、前記真空槽内に設置した基体上にダイヤモ
ンド薄膜を形成させるものであった。
Conventional methods for forming diamond as a film include using a mixed gas of hydrogen and hydrocarbons such as methane and ethane.
Alternatively, those containing an inert gas are used as the reactive gas, the reactive gas is introduced into the vacuum chamber, and microwave plasma and a magnetic field are applied to generate microwave plasma, and the vacuum A diamond thin film was formed on a substrate placed in a tank.

〔発明が解決しようとする問題点〕[Problem that the invention seeks to solve]

しかしながら、炭化水素の分解速度が非常に遅いために
、CHやHの活性種の生成が遅く、その分解速度がダイ
ヤモンド膜形成工程の律速段階となっていた。また、炭
化水素の水素に対する容積比が小さい場合に限って膜質
の良いダイヤモンド膜が形成されるというような生産効
率という点で考えるとこの方法は非常に量産性の良くな
い方法であった。
However, since the decomposition rate of hydrocarbons is very slow, the generation of active species such as CH and H is slow, and the decomposition rate is the rate-determining step in the diamond film forming process. Furthermore, from the point of view of production efficiency, this method is extremely unsuitable for mass production, as a diamond film of good quality can be formed only when the volume ratio of hydrocarbon to hydrogen is small.

本発明人等は、上述のような分解性の良くない原料によ
る生産方法を改良し、ダイヤモンド状薄膜を高速でしか
も原料気体の混合比率の選択幅を広げることができる生
産方法を目的として検討を続けた結果、原料気体中の炭
素、酸素及び水素の間に特定の関係を満足する混合領域
においてダイヤモンド状薄膜が高速で形成でき、しかも
その領域が広範囲であるため原料気体の混合比率の選択
幅を広くとることが可能であることを見つけた。
The inventors of the present invention have improved the production method using raw materials with poor decomposability as described above, and have conducted studies with the aim of creating a production method that can produce diamond-like thin films at high speed and with a wider selection of raw material gas mixture ratios. As a result, a diamond-like thin film can be formed at high speed in a mixing region that satisfies a specific relationship between carbon, oxygen, and hydrogen in the raw material gas, and since this region is wide, there is a wide range of selection in the mixing ratio of the raw material gas. We found that it is possible to take a wide range of

〔問題点を解決するための手段〕 つまり、減圧状態に保持されたプラズマ発生室及び反応
室内に炭素と酸素との比が1対1のとき、炭素に対する
水素の比が20〜40、炭素と酸素との比が2対1のと
き、炭素に対する水素の比が7〜15、炭素と酸素との
比が3対1のとき、炭素に対する水素の比が3〜12と
なるように、炭化水素気体を含む薄膜形成気体を導入し
、該気体に対して外部より磁界及びマイクロ波を印加し
て、高密度プラズマを発生させるというものである。
[Means for solving the problem] In other words, when the ratio of carbon to oxygen is 1:1 in the plasma generation chamber and reaction chamber maintained in a reduced pressure state, the ratio of hydrogen to carbon is 20 to 40, and the ratio of hydrogen to carbon is 20 to 40. When the ratio of hydrogen to carbon is 2 to 1, the ratio of hydrogen to carbon is 7 to 15, and when the ratio of carbon to oxygen is 3 to 1, the ratio of hydrogen to carbon is 3 to 12. A thin film-forming gas containing gas is introduced, and a magnetic field and microwaves are applied to the gas from the outside to generate high-density plasma.

この原料気体中の炭素,酸素及び水素との間の混合比の
関係を示したものが第1図である。図中、15で示す領
域は炭素または炭素を主成分とする被膜を高速で形成さ
せることが可能な領域を示す。
FIG. 1 shows the relationship of the mixing ratio between carbon, oxygen, and hydrogen in this raw material gas. In the figure, a region indicated by 15 indicates a region where carbon or a film containing carbon as a main component can be formed at high speed.

この関係を満たすように原料気体の流量等を調整するこ
とによって反応室内に原料気体を導入し、マイクロ波と
磁界とを印加することで反応室内に高密度プラズマを発
生させることにより炭素または炭素を主成分とする被膜
を高速で作製することができるのである。
The raw material gas is introduced into the reaction chamber by adjusting the flow rate of the raw material gas so as to satisfy this relationship, and carbon or carbon is generated by generating high-density plasma in the reaction chamber by applying microwaves and a magnetic field. A film containing the main component can be produced at high speed.

特にこの関係を満足させるのに適した原料気体の1つと
してアルコールを挙げることができ、このアルコールの
場合、特に分解が高速で行なわれるため、ダイヤモンド
膜の形成を容易に行なわせることが可能である。
Alcohol can be cited as one of the raw material gases particularly suitable for satisfying this relationship, and in the case of this alcohol, decomposition occurs particularly rapidly, making it possible to easily form a diamond film. be.

本発明における炭素または炭素を主成分とする被膜とは
、ダイヤモンド類似の硬さを有するアモルファス(非品
質)または5〜200人の大きさの微結晶性を有する構
造のビッカース硬度2000kg/ll1が以上、熱伝
導度2. 5W/cmdeg以上のものをいう。
In the present invention, carbon or a coating mainly composed of carbon is an amorphous (non-quality) having a hardness similar to that of diamond, or a microcrystalline structure with a Vickers hardness of 2000 kg/ll1 or more in the size of 5 to 200 people. , thermal conductivity 2. 5W/cmdeg or more.

以下に実施例とともに本発明を詳細に説明する.〔実施
例1〕 第2図に本発明にて用いた磁場印加可能なマイクロ波プ
ラズマCVD装置を示す。
The present invention will be explained in detail below along with examples. [Example 1] FIG. 2 shows a microwave plasma CVD apparatus capable of applying a magnetic field used in the present invention.

同図において、この装置は減圧状態に保持可能な反応室
(1)と磁場を発生する外部磁場発生器(5)とマイク
ロ波発振器(4),排気系(9),予備室(2),ガス
導入系0■,基板位置移動機構OI),より構成されて
いる。
In the figure, this device includes a reaction chamber (1) that can be maintained in a reduced pressure state, an external magnetic field generator (5) that generates a magnetic field, a microwave oscillator (4), an exhaust system (9), a preliminary chamber (2), It consists of a gas introduction system (0) and a substrate position movement mechanism (OI).

まず、薄膜形成用基板(8)を基板保持台(6)に基板
押さえ(7)で固定する。つぎに、水素ガスをIOOS
CC阿同時に炭化水素気体としてエタノール( C z
 H sOH)ガスをガス系00)を通して反応室(1
)に導入し外部よりマイクロ波5 kW,磁界2.2K
ガウスを印加し高密度なプラズマを発生させる。エタノ
ールの他にその他のアルコール類、例えばメタノール(
CH30H).プロビルアルコール( C 3H ? 
O H )が代表的なものである。この時反応室内(1
)の圧力は10Paに保持されている。この圧力は10
0Pa〜10−”Paの間で変えることは可能である。
First, the thin film forming substrate (8) is fixed to the substrate holding table (6) with the substrate presser (7). Next, add hydrogen gas to IOOS
At the same time, ethanol (C z
H sOH) gas is passed through the gas system 00) into the reaction chamber (1
) and externally introduced microwaves of 5 kW and magnetic field of 2.2 K.
A Gaussian voltage is applied to generate high-density plasma. In addition to ethanol, other alcohols such as methanol (
CH30H). Proyl alcohol (C3H?
O H ) is a typical example. At this time, the reaction chamber (1
) is maintained at 10 Pa. This pressure is 10
It is possible to vary between 0 Pa and 10-''Pa.

この時発散磁界により、高エネルギーに加熱された炭素
原子が基板表面上に生成され基板上に、この炭素原子が
堆積し、ビッカース硬度が4000kg/n+m”を有
する炭素または炭素を主成分とする被膜が形成された。
At this time, due to the divergent magnetic field, carbon atoms heated to high energy are generated on the substrate surface, and these carbon atoms are deposited on the substrate to form a carbon or carbon-based coating having a Vickers hardness of 4000 kg/n+m. was formed.

本実施例におけるダイヤモンド状薄膜の成長速度は90
0人/winであり従来の成長速度の倍以上の速度とな
った。
The growth rate of the diamond-like thin film in this example was 90
0 people/win, which is more than double the previous growth rate.

本実施例の場合、マイクロ波導入口02)と基板との間
隔は150 〜250mmであり、その時直径100m
m範囲で±10%以内の膜圧分布を有するダイヤモンド
状薄膜が得られた。
In the case of this example, the distance between the microwave inlet 02) and the substrate is 150 to 250 mm, and the diameter is 100 m.
A diamond-like thin film having a film pressure distribution within ±10% in the m range was obtained.

また、同条件下で磁場を印加しなければブラズマは発生
しなくなった。
Furthermore, under the same conditions, plasma was no longer generated unless a magnetic field was applied.

さらに、プラズマ加熱により基板を400゜Cまで上昇
させた場合、ダイヤモンド状薄膜が形成された。
Furthermore, when the temperature of the substrate was raised to 400° C. by plasma heating, a diamond-like thin film was formed.

本実施例にて形成された薄膜のラマン分先による測定の
結果は1331cm− ’にかなり強いピークが認めら
れた。
As a result of Raman spectroscopy measurements of the thin film formed in this example, a fairly strong peak was observed at 1331 cm-'.

〔実施例2〕 実施例1に示した装置により、実施例と同様の方法によ
り反応室内圧力を13Pa、水素ガスをIOOSCCM
メタノールを40SCCMの流量で流した他は実施例l
と同様に実施したところ基板表面上にビッカース硬度4
500kg/ms”を脊する炭素または炭素を主成分と
する被膜が形成された。この被膜の成長速度は850人
/winであり、この場合も従来の成長速度の倍以上の
速度となった。
[Example 2] Using the apparatus shown in Example 1, the pressure in the reaction chamber was set at 13 Pa, and the hydrogen gas was set at IOOSCCM in the same manner as in Example.
Example 1 except that methanol was flowed at a flow rate of 40 SCCM
When carried out in the same manner as above, a Vickers hardness of 4 was obtained on the substrate surface.
A film of carbon or carbon-based film having a growth rate of 500 kg/ms was formed. The growth rate of this film was 850 people/win, which was also more than double the conventional growth rate.

本実施例の場合もラマン分光による測定の結果1331
cm− ’にかなり強いピークが認められた。
In the case of this example as well, the result of measurement by Raman spectroscopy is 1331
A fairly strong peak was observed at cm-'.

〔効果〕〔effect〕

本発明は原料気体中の炭素、酸素及び水素の混合比率を
特定の関係を満足させる混合領域内に定めることにより
、高速で炭素または炭素を主成分とする被膜を形成させ
ることが可能となるばかりか、前記の混合領域が広いた
め材料の選択に幅が出て量産性に極めて優れたものであ
った。
In the present invention, by setting the mixing ratio of carbon, oxygen, and hydrogen in the raw material gas within a mixing range that satisfies a specific relationship, it becomes possible to form carbon or a film mainly composed of carbon at high speed. Moreover, since the above-mentioned mixing area is wide, there is a wide range of materials to choose from, making it extremely suitable for mass production.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は炭素,酸素及び水素の間の混合比を示した図。 第2図は本発明で用いる磁場印加可能なマイクロ波CV
D装置の概略を示す図。 反応室 予備室 整合器 マイクロ波発振器 外部磁場発生器 基板保持台 基板押さえ 基板 排気系 10・・・・ガス導入系 11・・・・基板位置移動機構
Figure 1 is a diagram showing the mixing ratio between carbon, oxygen and hydrogen. Figure 2 shows a microwave CV capable of applying a magnetic field used in the present invention.
A diagram showing an outline of the D device. Reaction chamber preliminary chamber matching device microwave oscillator external magnetic field generator substrate holding table substrate holding substrate exhaust system 10...gas introduction system 11...substrate position movement mechanism

Claims (1)

【特許請求の範囲】 1、減圧状態に保持されたプラズマ発生室及び反応室内
に、炭素と酸素との比が1対1のとき、炭素に対する水
素の比が20〜40、炭素と酸素との比が2対1のとき
、炭素に対する水素の比が7〜15、炭素と酸素との比
が3対1のとき、炭素に対する水素の比が3〜12とな
るように、炭化水素気体を含む薄膜形成気体を導入し、
該気体に対して外部より磁界及びマイクロ波を印加して
、高密度プラズマを発生させ、基板表面上に炭素または
炭素を主成分とする被膜を形成することを特徴とする被
膜形成方法。 2、特許請求の範囲第1項において炭化水素気体を含む
薄膜形成気体としてメタノールと水素あるいはエタノー
ルと水素、もしくはプロパノールと水素を用いたことを
特徴とする被膜形成方法。
[Claims] 1. When the ratio of carbon to oxygen is 1:1 in the plasma generation chamber and reaction chamber maintained in a reduced pressure state, the ratio of hydrogen to carbon is 20 to 40, and the ratio of carbon to oxygen is 1:1. Contains hydrocarbon gases such that when the ratio is 2 to 1, the ratio of hydrogen to carbon is 7 to 15, and when the ratio of carbon to oxygen is 3 to 1, the ratio of hydrogen to carbon is 3 to 12. Introducing a thin film forming gas,
A film forming method comprising applying a magnetic field and microwaves to the gas from the outside to generate high-density plasma to form carbon or a film containing carbon as a main component on the surface of a substrate. 2. A film forming method according to claim 1, characterized in that methanol and hydrogen, ethanol and hydrogen, or propanol and hydrogen are used as the thin film forming gas containing a hydrocarbon gas.
JP1057167A 1989-03-09 1989-03-09 Coating method Expired - Fee Related JP2840750B2 (en)