JPH03224249A - Manufacture of junction wafer - Google Patents

Manufacture of junction wafer

Info

Publication number
JPH03224249A
JPH03224249A JP1786290A JP1786290A JPH03224249A JP H03224249 A JPH03224249 A JP H03224249A JP 1786290 A JP1786290 A JP 1786290A JP 1786290 A JP1786290 A JP 1786290A JP H03224249 A JPH03224249 A JP H03224249A
Authority
JP
Japan
Prior art keywords
wafer
thickness
polishing
film thickness
film
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP1786290A
Other languages
Japanese (ja)
Other versions
JP2838273B2 (en
Inventor
Tatsuo Ito
伊藤 辰夫
Yasuaki Nakazato
中里 泰章
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shin-Etsu Handotai Co Ltd
Nagano Electronics Industrial Co Ltd
Original Assignee
Shin-Etsu Handotai Co Ltd
Nagano Electronics Industrial Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shin-Etsu Handotai Co Ltd, Nagano Electronics Industrial Co Ltd filed Critical Shin-Etsu Handotai Co Ltd
Priority to JP1786290A priority Critical patent/JP2838273B2/en
Publication of JPH03224249A publication Critical patent/JPH03224249A/en
Application granted granted Critical
Publication of JP2838273B2 publication Critical patent/JP2838273B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PURPOSE:To increase production efficiency, restrain the generation of surface abnormality of a wafer, and improve quality, by measuring the thickness of an upper layer wafer in a non-contact manner by using visible light, while the wafer is dipped in water as it is during the polishing process of a junction wafer. CONSTITUTION:Silicon wafers 1 and 2 turning to an element forming surface and base material are prepared, and an SiO2 thin film 3 is formed on one surface of the wafer 1. The wafers 1, 2 are so stacked that the film 3 turns to an intermediate layer, and subjected to heat-bonding; then the wafer 1 is pre- polished until a specified thickness t1 is obtained; said wafer is further polished in thickness down to t2 by secondary polishing, and a thinned junction wafer 4 is obtained. The wafer 4 is stuck on a circular disk type glass by using wax, and is dipped in pure water of a film thickness measuring equipment, together with the glass; by automatically adjusting the focal point of a lens, the film thickness t2 is measured in a noncontact manner with high precision. Hence it can be prevented that the wafer surface is partially dried and surface abnormality is generated.

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は、2枚の半導体ウェーハを接合一体化して成る
接合ウェーハの製造方法に関する。
DETAILED DESCRIPTION OF THE INVENTION (Field of Industrial Application) The present invention relates to a method for manufacturing a bonded wafer, which is formed by bonding two semiconductor wafers together.

(従来の技術) 半導体装置の製造に当っては、単結晶の半導体ウェーハ
上に気相成長法て特定の導電型を有する半導体層を形成
し、この半導体層に機能素子を形成する技術か広く利用
されている。
(Prior art) In the manufacture of semiconductor devices, a technology is widely used in which a semiconductor layer having a specific conductivity type is formed on a single-crystal semiconductor wafer using a vapor phase growth method, and functional elements are formed in this semiconductor layer. It's being used.

ところか、上記技術においては、気相成長に長時間を要
するとともに、素子設計の自由度に制約を受けるため、
近年SOI (Si On In5ulation)ウ
ェーハの如き接合ウェーハか製造されるようになった。
However, in the above technology, vapor phase growth takes a long time and there are restrictions on the degree of freedom in device design.
In recent years, bonded wafers such as SOI (Si On Injection) wafers have been manufactured.

この接合ウェーハは42枚の半導体ウェーハの少なくと
も一方を酸化処理してそのウェーハの少なくとも一方の
表面に酸化膜を形成し、これら2枚の半導体ウェーハを
前記酸化膜が中間層になるようにして重ね合わせた後、
所定温度に加熱して両者を接着し、その上層のウェーハ
(以下、ボンドウェーハと称す)を研磨加工してこれを
薄膜化することによって得られる。
This bonded wafer is produced by oxidizing at least one of 42 semiconductor wafers to form an oxide film on at least one surface of the wafer, and stacking these two semiconductor wafers with the oxide film forming an intermediate layer. After matching,
It is obtained by heating the two to a predetermined temperature to bond them together, and polishing the upper layer wafer (hereinafter referred to as a bond wafer) to make it a thin film.

ところで、前記研磨加工は、ボンドウェーハを所定の研
磨代(例えば、3#Lm)を残して所定の厚さ(例えば
、6gm)になるまて研磨するプレ研磨(1次研磨)と
、プレ研磨されたボンドウェーハを最終の厚さ(例えば
、3gm)まて研磨する2次研磨と2次研磨されたボン
ドウェーハを鏡面研磨する仕上げ研磨とから成るか、2
次研磨か施されたボンドウェーハの厚さ(例えば、3p
m)はダイヤルゲージによって空気中で測定されていた
。
By the way, the polishing process includes pre-polishing (primary polishing) in which the bond wafer is polished to a predetermined thickness (for example, 6 gm) while leaving a predetermined polishing allowance (for example, 3#Lm), and pre-polishing. The process consists of secondary polishing to polish the bond wafer to a final thickness (for example, 3 gm) and final polishing to mirror polish the secondary polished bond wafer.
The thickness of the bond wafer after subsequent polishing (e.g. 3p
m) was measured in air with a dial gauge.

(発明か解決しようとする課題) しかしながら、ボンドウェーハの厚さ(例えば、3gm
)に対してダイヤルゲージの測定精度は±0.5μmと
悪く、仕上げ研磨か終了したボンドウェーハの厚さを最
終工程の膜厚検査で測定すると、その値か許容値を逸脱
している場合があり、斯かる場合には、製品を2次研磨
工程に差し戻してこの製品に対して2次研磨以降の工程
を繰り返さねばならず、このために生産効率か低下する
という問題を生ずる。尚、膜厚検査ては、可視光を用い
た非接触式の膜厚測定器によってボンドウェーハの厚さ
か±0.01 a mの精度て測定される。
(Problem to be solved by the invention) However, the thickness of the bond wafer (for example, 3gm
), the measurement accuracy of the dial gauge is poor at ±0.5μm, and when the thickness of a bond wafer that has been finished polished is measured during the film thickness inspection in the final process, the value may deviate from the allowable value. In such a case, the product must be returned to the secondary polishing step and the steps after the secondary polishing must be repeated on this product, resulting in a problem of reduced production efficiency. In the film thickness inspection, the thickness of the bond wafer is measured with an accuracy of ±0.01 am using a non-contact film thickness measuring device using visible light.

又、2次研磨後のボンドウェーハの厚さか前述のように
空気中て測定される場合には、ボンドウェーハの空気と
の接触時間にもよるか、測定後に該ボンドウェーハの研
磨面に高さか50〜100人、直径か50〜200 p
、mの略円形の台地状突起か多数形成され、この突起は
ボンドウェーハを仕上げ研磨(通常、1μm以下の研磨
量)しても消滅しないという問題かあった。勿論、斯か
る面異常は仕上げ研磨か終了した後、研磨物を空気中に
放置したときにも起こる。
In addition, when the thickness of the bond wafer after secondary polishing is measured in air as described above, it may depend on the contact time of the bond wafer with the air, or there may be a height difference on the polished surface of the bond wafer after the measurement. 50-100 people, diameter 50-200p
, m are formed, and there is a problem in that these protrusions do not disappear even when the bond wafer is finished polished (usually by a polishing amount of 1 μm or less). Of course, such surface abnormalities also occur when the polished object is left in the air after finishing polishing.

ところで、前記突起は微分干渉顕微鏡て容易にその存在
を確認することかてきるか、面異常を生したボンドウェ
ーハの鏡面は、特に高集積度の集積回路素子形成のため
の基板表面としては不適当である。
By the way, the existence of the protrusions can be easily confirmed using a differential interference microscope, and the mirror surface of a bond wafer with surface abnormalities is not particularly suitable as a substrate surface for forming highly integrated circuit elements. Appropriate.

本発明は上記問題に鑑みてなされたもので、その目的と
する処は、研磨加工中における上層のウェーハの厚さを
高精度に測定することによって生産効率を高めることか
てきるとともに、ウェーハに面異常か発生するのを抑え
て製品の品質向上を図ることかてきる接合ウェーハの製
造方法を提供することにある。
The present invention has been made in view of the above problems, and its purpose is to increase production efficiency by measuring the thickness of the upper layer wafer during polishing with high precision, and to improve the wafer thickness. An object of the present invention is to provide a method for manufacturing bonded wafers that can suppress the occurrence of surface abnormalities and improve product quality.

(課題を解決するための手段) 上記目的を達成すべく本発明は、2枚の半導体ウェーハ
の少なくとも一方を酸化処理してそのウェーハの少なく
とも一方の表面に酸化膜を形成し、これら2枚の半導体
ウェーハを前記酸化膜か中間層になるようにして重ね合
わせた後、所定温度に加熱して両者を接着し、その上層
のウェーハを研磨加工してこれを薄膜化することによっ
て接合ウェーハを得る接合ウェーハの製造方法においで
、前記研磨加工の途中で、前記接着ウェーハを水中に浸
漬せしめた状態でその上層のウェーハの厚さを、可視光
を用いた非接触式の膜厚測定器によって測定するように
したことをその特徴とする。
(Means for Solving the Problems) In order to achieve the above object, the present invention oxidizes at least one of two semiconductor wafers to form an oxide film on the surface of at least one of the wafers. After stacking the semiconductor wafers so that the oxide film or the intermediate layer forms, the two are bonded by heating to a predetermined temperature, and the upper layer wafer is polished to make it a thin film, thereby obtaining a bonded wafer. In the method for manufacturing a bonded wafer, in the middle of the polishing process, the thickness of the wafer above the bonded wafer is immersed in water, and the thickness of the wafer is measured using a non-contact film thickness measuring device using visible light. Its characteristic is that it is made to do.

(作用) 本発明方法によれば、研磨工程(特に、2次研磨終了後
)において接合ウェーハの上層のウェーハ(ボンドウェ
ーハ)の厚さは、最終工程である膜厚検査において用い
られていると同様の膜厚測定器によって高精度に測定さ
れるため、従来のように製品を研磨工程に差し戻して該
製品に対してそれ以降の工程を繰り返す作業を省くこと
かでき、これによって生産効率か高められる。
(Function) According to the method of the present invention, the thickness of the upper layer wafer (bond wafer) of the bonded wafer in the polishing process (especially after the completion of the secondary polishing) is used in the final process, the film thickness inspection. Since the film thickness is measured with high precision using a similar film thickness measuring device, it is possible to eliminate the conventional work of returning the product to the polishing process and repeating the subsequent steps on the product, thereby increasing production efficiency. It will be done.

又、接合ウェーハは水中においてその上層のウェーハの
厚さ測定か行なわれるため、そのウェーハ表面か部分的
に乾燥することによる面異常の発生か防がれ、当該接合
ウェーハの品質か高く保たれる。
In addition, since the thickness of the wafer above the bonded wafer is measured underwater, surface abnormalities due to partial drying of the wafer surface are prevented, and the quality of the bonded wafer is maintained at a high level. .

ところで、前記面異常は、既述のように表面に多数の微
少突起か形成されることによって起こるか、これの発生
理由は、研磨面か研磨中に発生した摩擦熱によって加温
されており、且つこの研磨面には残存研磨液か接触して
いるために、不均一なエツチングか進んだためと考えら
れる。即ち、研磨面上の研磨液は研磨面に部分的に存在
する疎水性領域から弾かれるため、その弾かれた部分の
エツチングか進まず、その他の部分のエッチングか進む
ためと考えることかてきる。
By the way, the surface abnormality is caused by the formation of a large number of minute protrusions on the surface as described above, or the reason for this is that the polished surface is heated by frictional heat generated during polishing. Furthermore, it is thought that this is because residual polishing liquid was in contact with this polished surface, resulting in non-uniform etching. In other words, the polishing liquid on the polishing surface is repelled from the hydrophobic regions that partially exist on the polishing surface, so it can be thought that the etching of the repelled portions does not proceed and the etching of other portions proceeds. .

(実施例) 以下に本発明の一実施例を添付図面に基づいて説明する
。
(Example) An example of the present invention will be described below based on the accompanying drawings.

第1図(a)〜(e)は本発明に係る接合ウェーハの製
造方法をその工程順示す説明図、第2図は同フローチャ
ートである。
FIGS. 1(a) to 1(e) are explanatory diagrams showing the process order of a method for manufacturing a bonded wafer according to the present invention, and FIG. 2 is a flowchart of the same.

第1図及び第2図に基づいて本発明に係る接合ウェーハ
の製造方法を概説するに、第1図(a)に示すように素
子形成面となるべき単結晶のシリコンウェーハ(以下、
ボンドウェーハと称す)lとベース材となるべき同しく
単結晶のシリコンウェーハ(以下、ベースウェーハと称
す)2とを用意しく第2図のステップl)、一方のボン
ドウェーハlを酸化処理してその一方の表面にSiO□
の薄い酸化膜3を形成する(第2図のステップ2)。
To outline the method for manufacturing a bonded wafer according to the present invention based on FIGS. 1 and 2, as shown in FIG. 1(a), a single crystal silicon wafer (hereinafter referred to as
Prepare a single-crystal silicon wafer (hereinafter referred to as a base wafer) 2, which is to be a base material (referred to as a bond wafer), and perform oxidation treatment on one of the bond wafers (l) in Fig. 2. SiO□ on one surface
A thin oxide film 3 is formed (step 2 in FIG. 2).

次に、第1図(b)に示すように、上記2枚のウェーハ
1,2を前記酸化膜3か中間層になるようにして重ね合
わせ、これらウェーハ1,2を所定温度に加熱して両者
を接着する(第2図のステップ3)。その後、第1図(
c)に示すようにプレ研磨(1次研磨)によってボンド
ウェーハ1を所定の研磨式(3μm)を残して所定の厚
さt +(= 64 m )になるまで研磨する(第2
図のステップ4)。尚、第1図(c)の斜線部分はプレ
研磨によって切除される部分を示す。
Next, as shown in FIG. 1(b), the two wafers 1 and 2 are stacked so that the oxide film 3 forms an intermediate layer, and the wafers 1 and 2 are heated to a predetermined temperature. Glue both together (step 3 in Figure 2). After that, see Figure 1 (
As shown in c), the bond wafer 1 is polished by pre-polishing (first polishing) until it reaches a predetermined thickness t + (= 64 m), leaving a predetermined polishing formula (3 μm) (second polishing).
Step 4 in the diagram). Note that the shaded portion in FIG. 1(c) indicates the portion to be removed by pre-polishing.

ところで、実際には、上記プレ研磨前に、接着されたウ
ェーハ1,2の表面を平面研削した後、その表面にマス
キンクテープを貼着し、これらウェーハ1.2をエツチ
ング液中に浸漬してその周辺をエツチングするか、ここ
てはその詳細な説明は省略する。
By the way, in reality, before the above-mentioned pre-polishing, the surfaces of the bonded wafers 1 and 2 were surface ground, masking tape was attached to the surfaces, and these wafers 1 and 2 were immersed in an etching solution. The detailed explanation will be omitted here.

而しで、前述のようにプレ研磨された厚さt。Therefore, the pre-polished thickness t as described above.

のボンドウェーハlは、第1図(d)に示すように2次
研磨によって厚さt2 (=3gm、)まで研磨されて
薄膜化され(第2図のステップ5)、これによりて第1
図(e)に示すような接合ウェーハ4が得られる。尚、
第1図(d)の斜線部分は2次研磨によって切除される
部分を示す。
As shown in FIG. 1(d), the bond wafer l is polished and thinned to a thickness t2 (=3 gm) by secondary polishing (step 5 in FIG. 2), and as a result, the first
A bonded wafer 4 as shown in Figure (e) is obtained. still,
The shaded area in FIG. 1(d) indicates the area to be removed by secondary polishing.

上記2次研磨か終了した後、接合ウェーハ4は第3図及
び第4図に示す膜厚測定装置10によって水中に浸漬さ
れた状態でそのボンドウェーハlの厚さt2 (=3g
m)か測定される(第2図のステップ6)。
After the above-mentioned secondary polishing is completed, the bonded wafer 4 is immersed in water by the film thickness measuring device 10 shown in FIGS. 3 and 4, and the thickness t2 (=3 g
m) is measured (step 6 in Figure 2).

ここで、上記膜厚測定器WIOの概略構成を第3図及び
第4図に基づいて説明する。尚、第3図は膜厚測定装置
10の正面図、14図は同平面図である。
Here, the schematic structure of the film thickness measuring device WIO will be explained based on FIGS. 3 and 4. 3 is a front view of the film thickness measuring device 10, and FIG. 14 is a plan view thereof.

図においては、11は枠構造を成す基台であり、該基台
11上には可視光を用いた非接触式の膜厚測定器(商品
名工ナノスペック/AFT (ナノメトリクス社製))
12かX軸ステージ13及びY軸ステージ14に沿って
移動自在に設置されている。尚、膜厚側定器12は±0
.01μmの測定精度を有し、これはモータM1.M2
によって駆動されるボールネジ機構によって前記X軸ス
テージ13及びY軸ステージ14に沿って移動せしめら
れる。
In the figure, 11 is a base having a frame structure, and on the base 11 is a non-contact film thickness measuring device using visible light (trade name: Meiko Nanospec/AFT (manufactured by Nanometrics)).
12 is installed movably along an X-axis stage 13 and a Y-axis stage 14. In addition, the film thickness side regulator 12 is ±0.
.. It has a measurement accuracy of 0.01 μm, which is the same as that of motor M1. M2
It is moved along the X-axis stage 13 and the Y-axis stage 14 by a ball screw mechanism driven by.

又、前記基台11上の膜厚測定器12の手前側(第4図
の下側)には矩形の水槽15か設置されており、該水槽
15内には四方に延びるウェーハセット用のベース16
・・・か収容されており、同水槽15の底部には注水口
17と排水口18か設けられている。尚、水槽15内に
は注水口17から供給された純水か収容されている。
Further, a rectangular water tank 15 is installed in front of the film thickness measuring device 12 on the base 11 (lower side in FIG. 4), and a base for a wafer set extending in all directions is installed in the water tank 15. 16
. Note that pure water supplied from the water inlet 17 is stored in the water tank 15 .

更に、基台11の水槽15の側方には、膜厚測定器12
の作動を制御し、且つ測定データを処理するためのパー
ソナルコンピュータ19か設置されており、該パーソナ
ルコンピュータ19上には測定データ等を表示すべきC
R7表示装置20か設けられている。そして又、基台1
1上の膜厚測定器12の側方には、膜厚測定器12のレ
ンズの焦点を自動調整するためのオートフォーカスコン
トローラ21か設置されている。尚4膜厚測定器12の
レンズ部分は防水処理されており、この部分への水の浸
入が防がれる。
Further, on the side of the water tank 15 of the base 11, a film thickness measuring device 12 is installed.
A personal computer 19 is installed for controlling the operation of the computer and processing the measurement data, and a computer 19 for displaying the measurement data, etc. is installed on the personal computer 19.
An R7 display device 20 is also provided. And again, base 1
An autofocus controller 21 for automatically adjusting the focus of the lens of the film thickness measurement device 12 is installed on the side of the film thickness measurement device 12 on the top of the film thickness measurement device 1 . The lens portion of the four film thickness measuring devices 12 is waterproofed to prevent water from entering this portion.

而しで、前記2次研磨か終了した接合ウェーハ4は、第
4図に示すように円板状のガラス5上にワックスによっ
て貼着され、ガラス5と共に水槽l5内の純水中に浸漬
せしめられ、膜厚測定器12によってそのボンドウェー
ハlの厚さt2(=3gm)か測定される。具体的には
、ボンドウェーハlは、第5図に示すようにその中心位
置■と、該中心位置■を通る互いに直交する2本の直線
上の点であっで、該ボンドウェーハ1の周縁からlO■
謹内側内側■、■、■、■及びボンドウェーハlの半径
γの半分子 / 2の点■、■、■。
Then, the bonded wafer 4, which has undergone the secondary polishing, is adhered with wax to a disc-shaped glass 5, as shown in FIG. 4, and is immersed together with the glass 5 in pure water in a water tank 15. Then, the thickness t2 (=3 gm) of the bond wafer l is measured by the film thickness measuring device 12. Specifically, as shown in FIG. 5, the bond wafer 1 is located at its center position (■) and points on two straight lines passing through the center position (2) orthogonal to each other, and from the periphery of the bond wafer 1. lO■
Inner side ■, ■, ■, ■ and half molecule of radius γ of bond wafer l / 2 points ■, ■, ■.

■の9点においてその厚さt2か測定され、膜厚測定器
12の各測定点■〜■への移動はパーソナルコンピュー
タ19に予め入力されたプログラムに従ってなされる。
The thickness t2 is measured at nine points (1), and the film thickness measuring device 12 is moved to each measurement point (2) to (2) according to a program input into the personal computer 19 in advance.

ところで、本膜厚測定装置lOによるボンドウェーハl
の厚さt2の水中での測定の信頼性を確認するために直
径150曹■のボンドウェーハに対して水中と空気中で
厚さ測定した結果の一例を下表に示す(表中の数字の単
位は4mである)。
By the way, bond wafer l using this film thickness measuring device lO
The table below shows an example of the results of measuring the thickness of a bond wafer with a diameter of 150 mm in water and air in order to confirm the reliability of underwater measurements of the thickness t2. The unit is 4m).

尚、測定器として可視光を用いた膜厚測定器12を採用
したのは、可視光は水中での吸収か少ない理由による。
The reason why the film thickness measuring device 12 using visible light was adopted as the measuring device is because visible light is poorly absorbed in water.

上表より、水中と空気中における膜厚測定データは高い
精度(相関係数=0.998 )で一致しており、水中
での膜厚測定の高い信頼性が確認された。
From the table above, the film thickness measurement data in water and in air matched with high accuracy (correlation coefficient = 0.998), confirming the high reliability of film thickness measurement in water.

尚1本実施例にて使用された膜厚測定器(商品名:ナノ
スペック/AFT (ナノメトリクス社製))12は、
光源としてタングステンランプ。
1. The film thickness measuring device (product name: Nanospec/AFT (manufactured by Nanometrics)) 12 used in this example was as follows:
Tungsten lamp as light source.

回折格子としてホログラフィック凹格子を用いており、
その測定範囲は100人〜50pmであり、シリコン基
板上或いはガラス基板上での各種の膜厚測定か可能てあ
っで、本実施例に係るボンドウェーハlの厚さ測定につ
いては、厚さ3gmに対して少なくとも±2%の精度で
測定し得る。
A holographic concave grating is used as a diffraction grating,
The measurement range is from 100 people to 50 pm, and it is possible to measure various film thicknesses on silicon substrates or glass substrates. can be measured with an accuracy of at least ±2%.

而しで、膜厚測定器WIOによるボンドウェーハlの厚
さt2の測定が終了すると、その厚さt2が許容値内に
あるか否かか判定され(!s2図のステップ7)、厚さ
t2か許容値から外れている場合にはその接合ウェーハ
4は2次研磨工程(第2図のステップ5)に戻され、再
び2次研磨され、前記と同様にボンドウェーハlの厚さ
t2か測定される(第2図のステップ6)、そして。
Therefore, when the measurement of the thickness t2 of the bond wafer l by the film thickness measuring device WIO is completed, it is determined whether the thickness t2 is within the allowable value (step 7 in the !s2 diagram), and the thickness If t2 is outside the allowable value, the bonded wafer 4 is returned to the secondary polishing process (step 5 in FIG. 2) and is polished again, and the thickness t2 of the bonded wafer l is measured (step 6 in Figure 2), and.

ボンドウェーハlの厚さt2が許容値内に入るまて以上
の作業(ステップ5からステップ7までの作業)か繰り
返される。
The above operations (operations from step 5 to step 7) are repeated until the thickness t2 of the bond wafer l falls within the allowable value.

一方、ボンドウェーハlの厚さt2が許容値内に入って
いる場合には、次工程の仕上げ研磨によってボンドウェ
ーハlの表面か鏡面化され(w42図のステップ8)、
その後、当該接合ウェーハ4はガラス5から剥され(第
2図のステップ9)、処理液て洗浄されてこれに付着し
たワツク不か除去される(第2図のステップlO)、そ
して最後に、接合ウェーハ4は前記膜厚測定器12と同
型式の膜厚測定器によってそのボンドウェーハlの厚さ
t2か空気中て測定される(第2図のステップ11)。
On the other hand, if the thickness t2 of the bond wafer l is within the allowable value, the surface of the bond wafer l is mirror-finished in the next step of final polishing (step 8 in Figure W42),
Thereafter, the bonded wafer 4 is peeled off from the glass 5 (step 9 in FIG. 2), cleaned with a treatment solution to remove any stuck wafers (step 1O in FIG. 2), and finally, The thickness t2 of the bonded wafer 4 is measured in air by a film thickness measuring device of the same type as the film thickness measuring device 12 (step 11 in FIG. 2).

以上説明した一連の製造工程においで、2次研磨が終了
した接合ウェーハ4のボンドウェーハ1の厚さt2は、
最終工程である膜厚検査において用いられると同型式の
可視光を用いた非接触式の膜厚測定器12によって高精
度に測定されるため、従来要していた膜厚検査か終了し
た製品を研磨工程に差し戻してそれ以降の工程を繰り返
す作業を省くことができ、これによって生産効率を高め
ることができる。
In the series of manufacturing steps explained above, the thickness t2 of the bonded wafer 1 of the bonded wafer 4 after the secondary polishing is
Since the film thickness measurement device 12 uses the same type of non-contact visible light as used in the film thickness inspection, which is the final process, to measure with high precision, the film thickness test that was previously required can be performed on finished products. It is possible to eliminate the work of returning to the polishing process and repeating the subsequent steps, thereby increasing production efficiency.

又、接合ウェーハ4は膜厚測定装置10によって水中で
そのボンドウェーハ1の厚さt2か測定されるため、そ
の表面が部分的に乾燥することによる面異常の発生か防
がれ、当該接合ウェーA4の品質が高く保たれる。
Furthermore, since the thickness t2 of the bonded wafer 1 is measured underwater by the film thickness measuring device 10, surface abnormalities due to partial drying of the surface of the bonded wafer 4 are prevented from occurring, and the thickness of the bonded wafer 1 is The quality of A4 paper is kept high.

(発明の効果) 以上の説明て明らかな如く本発明によれば、2枚の半導
体ウェーハの少なくとも一方を酸化処理してそのウェー
ハの少なくとも一方の表面に酸化膜を形成し、これら2
枚の半導体ウェーハを前記酸化膜か中間層になるように
して重ね合わせた後、所定温度に加熱して両者を接着し
、その上層のウェーハを研磨加工してこれを薄膜化する
ことによって接合ウェーハを得る接合ウェーハの製造方
法においで、前記研磨加工の途中で、前記接合ウェーハ
を水中に浸漬せしめた状態でその上層のウェーハの厚さ
を、可視光を用いた非接触式の膜厚測定器によって測定
するようにしたため、研磨加工中における上層のウェー
ハの厚さを高精度に測定することによって生産効率を高
めることができるとともに、ウェーハに面異常か発生す
るのを抑えて製品の品質向上を図ることかできるという
効果か得られる。
(Effects of the Invention) As is clear from the above description, according to the present invention, at least one of two semiconductor wafers is oxidized to form an oxide film on the surface of at least one of the wafers.
After stacking two semiconductor wafers so that the oxide film or intermediate layer forms, the two are bonded by heating to a predetermined temperature, and the upper layer wafer is polished to make it a thin film, thereby creating a bonded wafer. In the method for manufacturing a bonded wafer, in the middle of the polishing process, the thickness of the upper layer of the wafer is measured with a non-contact film thickness measuring device using visible light while the bonded wafer is immersed in water. By measuring the thickness of the upper layer wafer with high precision during polishing, it is possible to increase production efficiency and improve product quality by suppressing the occurrence of surface abnormalities on the wafer. You can get the effect of being able to do something.

【図面の簡単な説明】[Brief explanation of drawings]

第1図(a)〜(e)は本発明に係る接合ウェーハの製
造方法をその工程順示す説明図、第2図は同フローチャ
ート、第3図は膜厚測定装置の正面図、第4図は同平面
図、第5図は測定点を示すウェーハの平面図である。 l・・・ボンドウェーハ(上層のウェーハ)、2・・・
ベースウェーハ、3・・・酸化膜、4・・・接合ウェー
ハ、12・・・膜厚測定器。
1(a) to 1(e) are explanatory diagrams showing the process order of the bonded wafer manufacturing method according to the present invention, FIG. 2 is the same flowchart, FIG. 3 is a front view of the film thickness measuring device, and FIG. 4 is the same plan view, and FIG. 5 is a plan view of the wafer showing measurement points. l... Bond wafer (upper layer wafer), 2...
Base wafer, 3... Oxide film, 4... Bonded wafer, 12... Film thickness measuring device.

Claims (1)

【特許請求の範囲】[Claims] 2枚の半導体ウェーハの少なくとも一方を酸化処理して
そのウェーハの少なくとも一方の表面に酸化膜を形成し
、これら2枚の半導体ウェーハを前記酸化膜が中間層に
なるようにして重ね合わせた後、所定温度に加熱して両
者を接着し、その上層のウェーハを研磨加工してこれを
薄膜化することによって接合ウェーハを得る接合ウェー
ハの製造方法において、前記研磨加工の途中で、前記接
合ウェーハを水中に浸漬せしめた状態でその上層のウェ
ーハの厚さを、可視光を用いた非接触式の膜厚測定器に
よって測定するようにしたことを特徴とする接合ウェー
ハの製造方法。
At least one of the two semiconductor wafers is oxidized to form an oxide film on the surface of at least one of the wafers, and the two semiconductor wafers are stacked so that the oxide film becomes an intermediate layer, and then In a method for manufacturing a bonded wafer, in which a bonded wafer is obtained by heating the two to a predetermined temperature and bonding the two, and polishing the upper layer wafer to reduce the thickness of the bonded wafer, the bonded wafer is soaked in water during the polishing process. 1. A method for manufacturing a bonded wafer, characterized in that the thickness of an upper layer of the wafer is measured by a non-contact film thickness measuring device using visible light while the wafer is immersed in the wafer.
JP1786290A 1990-01-30 1990-01-30 Manufacturing method of bonded wafer Expired - Fee Related JP2838273B2 (en)