JPH04200882A - 電子ビーム溶接法 - Google Patents

電子ビーム溶接法

Info

Publication number
JPH04200882A
JPH04200882A JP32897590A JP32897590A JPH04200882A JP H04200882 A JPH04200882 A JP H04200882A JP 32897590 A JP32897590 A JP 32897590A JP 32897590 A JP32897590 A JP 32897590A JP H04200882 A JPH04200882 A JP H04200882A
Authority
JP
Japan
Prior art keywords
electron beam
penetration
electron
base metal
welding
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP32897590A
Other languages
English (en)
Inventor
Sadao Shibakita
柴北 貞雄
Kazuyuki Ishimaru
石丸 一行
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hitachi Ltd
Original Assignee
Hitachi Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hitachi Ltd filed Critical Hitachi Ltd
Priority to JP32897590A priority Critical patent/JPH04200882A/ja
Publication of JPH04200882A publication Critical patent/JPH04200882A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 [産業上の利用分野1 本発明は電子ビームン岩接における溶け込みン某さの自
動制御法に関するものである。
[従来の技術1 従来の方法6:J−1あらがしめ試料にて溶け込み深さ
を確認L−Cその時の適正条件−Cもって実機を施I−
シていた。なお、この種の技術として関連するものには
、例えば、文献 産業出版、現代溶接技術大系「溶接法
の基礎」第(33亘へ第65亘記載のものがある。
「発明が解決しようとする課題1 手記従来技術は、破細lL物の板厚や開先精度のバラツ
ギで試料と溶け込み深さが異なったり、溶接執のび; 
4に’4ゝで同し開先内でも浩1)〉開始部と終了部ど
ではその)hけ込み深さが違ってくる。又、電子銃陰極
部の消耗でビーム焦点距離が経時変化し、同様Gごイー
の溶け込み深さが違ってくる。つまり、同一条件で施工
しても、その時、その部位で溶け込み深さが異なってく
るもので、−4の点についての対策がなされていなかっ
た。
本発明の[]的は、溜は込み深さを自動的に制御Jろ′
1[了ビーム溶接法を提供することにある。
[課題を解決するだめの手段1 手記目的を達成するためG乙FI材をV[通、つまり透
過する電工の量や一すイクルを検出し、これを基じ、溶
け込み深さの諸元である加速電圧やヒーノ\電?A1、
ビーム焦点位置を;演算 制御して、常に一定の謂は込
み深さとなるようにしたものである。
[作   用] 透過電子の量やサイクルを検出するために、母材や電子
ビーム溶接機から絶縁されている状態の導電体でその透
過電子を受け、アース線へ流ず。
その途中に電流計を設け、電流として測定をする。
母材を貫通する透過電子の量やサイクルは、溶け込み深
さに比例して増加する。この関係を利用して、溶接条件
を制御して溶け込み深さをコン1−ロールすることがで
きる。
〔実 施 例] 以下、本発明の一実施例を第1図により説明する。図に
おいて、電子銃1から発射された電子ビーム(入射電子
)2は母材3へ衝突し、そのエネルギーでもって溶融部
4を形成して溶接する。溶融部の板厚方向の長さ、つま
り溶け込み深さが増ずと母材固体部の厚さが薄くなり、
電子の透過率が増ずにの透過電子5を導電体7で受ける
。この導電体7は、セラミックスなどの非導電体6でも
って、母材3や電子ビーム溶接機などと絶縁された状態
に保持される。導電体7からアース線8でもってアース
する。この中間に電流計9を設け、透過電子の流れを電
流として測定する。この電子ビーム溶接における溶け込
み深さと透過電子(電流)との関係の一例を第2図に示
す。第2図において、横軸に母材3厚み(1)から溶融
部4厚み(d)を差し引いた状態の寸法、縦軸にその状
態におりる電流計9での検出電流(Iし)を示す電子ビ
ーム溶接時の入射電子(例えば60KVx100mA)
の透過電流の特性図である。つまり、このデータを随時
、マイクロコンピュータ−0で演算−解析して、溶接込
み深さに影響する加速電圧、ビーム電流、ビーム焦点位
置の諸条件を選定し直し、溶け込み深さが常に一定にな
るように指令信号を電子ビーム溶接機へ流し、その溶け
込み深さを制御する。
本実施例によれば、溶融部の板厚方向の長さ・つまり溶
け込み深さを上手にコントロールできるので、溶け込み
不足による開先未溶着部の発生、溶け過ぎによる溶融金
属の流出つまり溶け落ち等を防止できる。
[発明の効果] 本発明によれば、常に溶け込み深さを一定にコントロー
ルできるので、安定した溶接品質を得ることができる。
【図面の簡単な説明】
第1図は本発明の一実施例の電子ビーム溶接法の系統図
、第2図は第1図における電子ビーム(h接時の溶け込
み深さと透過電流との特性図である。 1−−−−−一電子銃、2−一〜−−−電子ビーム、3
−−−−−一附材、4.−−−−−一溶融部、5−−−
−−一透過電子、6−−−=−非導電体、7−−−−−
−導電体、8−−−−−−アース線、9−一一一一一電
流計、1.0−−−−−−マイクロコンビュ/−−−−
一電j& 2−一一−−電子ヒ私(R1〃 3−−−4 、fJ

Claims (1)

    【特許請求の範囲】
  1. 1、母材を貫通した透過電子を、母材や電子ビーム溶接
    機と絶縁された状態の導電体で受け、該導体からアース
    線へ流れる電流を電流計で測定し、加速電圧、ビーム電
    流や焦点位置などの溶接条件をマイクロコンピュータで
    演算し、所定の溶け込み深さとなるように制御したこと
    を特徴とする電子ビーム溶接法。
JP32897590A 1990-11-30 1990-11-30 電子ビーム溶接法 Pending JPH04200882A (ja)