JPH0449514A - Magnetic recording medium and its production - Google Patents
Magnetic recording medium and its productionInfo
- Publication number
- JPH0449514A JPH0449514A JP15751690A JP15751690A JPH0449514A JP H0449514 A JPH0449514 A JP H0449514A JP 15751690 A JP15751690 A JP 15751690A JP 15751690 A JP15751690 A JP 15751690A JP H0449514 A JPH0449514 A JP H0449514A
- Authority
- JP
- Japan
- Prior art keywords
- magnetic recording
- magnetic
- recording medium
- film
- fine particles
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.
Description
【発明の詳細な説明】
〔産業上の利用分野〕
本発明は、磁気ディスク装置などに用いられる磁気記録
媒体の構造及びその製造方法に係り、特に、磁気ヘッド
と磁気記録媒体の吸着を防止して磁気記録媒体の耐摺動
性を向上させる、磁気記録媒体の表面に形成する凹凸形
状、及び該凹凸形状の形成方法に関するものである。[Detailed Description of the Invention] [Industrial Application Field] The present invention relates to the structure of a magnetic recording medium used in a magnetic disk drive and the like and a method for manufacturing the same, and particularly to a method for preventing adhesion between a magnetic head and a magnetic recording medium. The present invention relates to an uneven shape formed on the surface of a magnetic recording medium and a method for forming the uneven shape, which improves the sliding resistance of the magnetic recording medium.
磁気ディスク装置の市場においては、磁気ディスクの高
記録密度化と共に、装置の大容量化・小型化が要求され
ており、対応策の一つとして、磁気記録媒体に対して、
記録・再生を行う磁気ヘッドの浮上間隔は、益々狭めら
れる傾向にある。In the magnetic disk device market, there is a demand for higher recording density of magnetic disks, as well as larger capacity and smaller devices.As one of the countermeasures,
The flying distance of magnetic heads that perform recording and reproduction tends to become narrower and narrower.
これにともない、記録・再生時の磁気ヘッドが磁気記録
媒体面に対して、接触または衝突する確率が高くなり、
その結果、これら磁気記録媒体、または該磁気記録媒体
および磁気ヘッドの双方を損傷させるクラッシュ障害が
増加する。このため、そのような障害を解消した信頼性
の高い磁気記録媒体を得る方法が必要とされている。Along with this, the probability that the magnetic head will come into contact with or collide with the surface of the magnetic recording medium during recording/reproducing increases.
As a result, crash failures that damage these magnetic recording media or both the magnetic recording media and the magnetic head increase. Therefore, there is a need for a method of obtaining a highly reliable magnetic recording medium that eliminates such obstacles.
従来の磁気記録媒体では、特開平1−211236号公
報に記載のように、非磁性体基板上に形成された平滑な
磁気記録膜表面に、例えば、電子線シャワーからなる微
粒子帯電手段によって、基板側に印加した極性と反対極
性に帯電した、保護膜と同材質であるカーボン、アルミ
ナ、シリコン酸化物などの凹凸面形成用微粒子を静電的
に被着させ、引き続き、該凹凸面形成用微粒子が被着さ
れた磁気記録膜の表面に、スパッタリング法などを用い
て、保護膜を被覆後、潤滑膜を形成して耐摺動性の向上
を図ったものがある。In conventional magnetic recording media, as described in Japanese Unexamined Patent Publication No. 1-211236, a smooth magnetic recording film surface formed on a non-magnetic substrate is charged with a fine particle charging means such as an electron beam shower. Fine particles for forming an uneven surface, such as carbon, alumina, silicon oxide, etc., which are made of the same material as the protective film and are charged to the opposite polarity to the polarity applied to the side, are electrostatically deposited, and then the fine particles for forming an uneven surface are applied. There is a method in which a protective film is coated on the surface of a magnetic recording film to which is deposited, using a sputtering method or the like, and then a lubricating film is formed to improve the sliding resistance.
前記した従来の磁気記録媒体では、帯電した微粒子を静
電的な被着方法により磁気記録膜上に被着させる工程で
あるので、予め、微粒子のサイズを選択することはでき
るが、磁気記録膜上への微粒子の被着量、被着密度およ
び分布を高精度に制御することはできない。In the conventional magnetic recording medium described above, the process involves depositing charged fine particles onto the magnetic recording film using an electrostatic deposition method, so the size of the fine particles can be selected in advance; The amount, density and distribution of fine particles deposited on the surface cannot be controlled with high precision.
この原因は、粒子サイズが1μm以下の微小なものにな
ると、微粒子どうしの凝集力が増大して、磁気記録膜上
に微粒子を均一に分散させることが困難になると考えら
れるからである。The reason for this is thought to be that when the particle size becomes as small as 1 μm or less, the cohesive force between the particles increases, making it difficult to uniformly disperse the particles on the magnetic recording film.
従って、上記従来技術では、磁気記録媒体表面に形成さ
れる凹凸が不均一になることは避けられず、磁気ヘッド
の吸着などを低減するとともに、磁気ヘッドによるクラ
ッシュ障害を防止して、磁気記録媒体の耐摺動性を向上
させることが難しい。Therefore, with the above conventional technology, it is inevitable that the unevenness formed on the surface of the magnetic recording medium becomes non-uniform, so it is possible to reduce the adhesion of the magnetic head, prevent crash failure caused by the magnetic head, and improve the quality of the magnetic recording medium. It is difficult to improve the sliding resistance of
本発明は、上記した問題を解決するため、磁気記録膜上
に微粒子を被着させることによって、磁気記録膜の磁気
特性を劣化させることなく、磁気記録膜上に被着させる
微粒子の被着量、被着密度およびその分布状態を好適な
範囲に高精度に制御して、低粘着性と耐摺動性に優れた
磁気記録媒体、および、その製造方法を提供することを
目的とするものである。In order to solve the above-mentioned problems, the present invention provides a method for depositing fine particles on a magnetic recording film, thereby reducing the amount of fine particles deposited on the magnetic recording film without deteriorating the magnetic properties of the magnetic recording film. The purpose of the present invention is to provide a magnetic recording medium that has low adhesion and excellent sliding resistance by highly precisely controlling the adhesion density and its distribution within a suitable range, and a method for manufacturing the same. be.
上記目的は、磁気記録膜上に磁性体の微粒子を被着し、
保護膜および潤滑膜を、順次形成させる磁気記録媒体に
より、達成できる。The above purpose is to deposit fine particles of magnetic material on a magnetic recording film,
This can be achieved by using a magnetic recording medium in which a protective film and a lubricating film are sequentially formed.
また、上記目的は、磁気記録膜を部分的に磁化した後磁
化した部分に磁性体微粒子を被着させ、その後に、保護
膜を形成する磁気記録膜媒体を作成する製造方法により
達成できる。Further, the above object can be achieved by a manufacturing method for producing a magnetic recording film medium in which a magnetic recording film is partially magnetized, then magnetic fine particles are deposited on the magnetized portion, and then a protective film is formed.
なお、上記の磁性体微粒子は、不定形でもよい。Note that the magnetic fine particles described above may have an amorphous shape.
まず、本発明による磁気記録媒体の作用について説明す
る。First, the operation of the magnetic recording medium according to the present invention will be explained.
非磁性体基板上に形成された平滑な磁気記録膜に、好適
な磁化パターンを形成し、該磁気記録膜上に、例えば、
磁気記録膜と同材質の磁性体微粒子を磁気的に被着し、
引き続き、その表面に保護膜及び潤滑膜を連続して形成
することにより、表面に好適な凹凸形状を有して高耐摺
動性を実現する磁気記録媒体を形成する。A suitable magnetization pattern is formed on a smooth magnetic recording film formed on a non-magnetic substrate, and on the magnetic recording film, for example,
Magnetic fine particles made of the same material as the magnetic recording film are magnetically adhered,
Subsequently, a protective film and a lubricating film are successively formed on the surface, thereby forming a magnetic recording medium that has a suitable uneven shape on the surface and achieves high sliding resistance.
次に、本発明による磁気記録媒体製造方法の作用につい
て説明する。Next, the operation of the magnetic recording medium manufacturing method according to the present invention will be explained.
平滑な磁気記録膜上に磁性体微粒子を被着させるに際し
、被着させる磁性体微粒子の材料組成とサイズを予め選
択し、磁気記録膜に加える磁場の強度によって微粒子の
被着量を制御し、磁化するパターンの選択により磁化し
た部分に選択的に被着する微粒子の被着密度をも高精度
に制御することができる。When depositing magnetic fine particles on a smooth magnetic recording film, the material composition and size of the magnetic fine particles to be deposited are selected in advance, and the amount of deposited fine particles is controlled by the intensity of the magnetic field applied to the magnetic recording film. By selecting a magnetized pattern, it is also possible to control with high precision the density of fine particles that selectively adhere to the magnetized portion.
従って、従来の磁気記録媒体のように耐摺動性に寄与す
る磁気記録媒体表面の凹凸形状が不均一になることはな
い。Therefore, unlike conventional magnetic recording media, the uneven shape of the surface of the magnetic recording medium, which contributes to the sliding resistance, does not become non-uniform.
以下、本発明の実施例を図を用いて詳細に説明する。 Embodiments of the present invention will be described in detail below with reference to the drawings.
第1図(a)は、本実施例の磁気記録媒体の一部の拡大
断面図である。FIG. 1(a) is an enlarged cross-sectional view of a portion of the magnetic recording medium of this example.
第1図(a)に示すように、平滑な非磁性体基板1上に
下地膜2および磁気記録膜3を順次形成する。該磁気記
録膜3に外部磁場を加えて所望のパターンに磁化した後
、磁性体微粒子6を該磁気記録膜3にパターンの通りに
被着させる。As shown in FIG. 1(a), a base film 2 and a magnetic recording film 3 are sequentially formed on a smooth non-magnetic substrate 1. As shown in FIG. After applying an external magnetic field to the magnetic recording film 3 to magnetize it into a desired pattern, magnetic fine particles 6 are deposited on the magnetic recording film 3 according to the pattern.
この後、前記した真空薄膜形成法を用いて、磁性体微粒
子6が被着した該磁気記録膜3上に保護膜4を被覆し、
さらに、その表面に潤滑膜5を形成して磁気記録媒体8
を完成させる。After that, the protective film 4 is coated on the magnetic recording film 3 to which the magnetic fine particles 6 are adhered, using the vacuum thin film forming method described above.
Furthermore, a lubricating film 5 is formed on the surface of the magnetic recording medium 8.
complete.
上記した中で、磁性体微粒子6が被着した磁気記録膜表
面を第1図(b)に模式的に表した。第1図(a)は、
第1図(b)内に点線で示した部分の断面を表している
。Among the above, the surface of the magnetic recording film to which the magnetic fine particles 6 are adhered is schematically shown in FIG. 1(b). Figure 1(a) shows
The cross section of the portion indicated by the dotted line in FIG. 1(b) is shown.
本発明によれば、第1図(b)に示すように、磁場を加
え電荷が集中した部分にのみ磁性体微粒子6が被着する
ので、従来技術のように微粒子の凝集による不均一な被
着は生じない。According to the present invention, as shown in FIG. 1(b), the magnetic particles 6 adhere only to the areas where a magnetic field is applied and the electric charge is concentrated. No wear will occur.
また、第1図(b)とは異なり、ビット7の端部の電荷
の集中した部分をつなぐように磁性体微粒子6が単独、
または複数個が連なって被着する場合が考えられる。In addition, unlike in FIG. 1(b), the magnetic particles 6 are arranged singly so as to connect the areas where the electric charges are concentrated at the ends of the bits 7.
Alternatively, a case may be considered in which a plurality of pieces are deposited in a row.
上記の場合においても、磁化パターンの制御によって、
磁化する部分を所望のパターンに分散させることによっ
て、出力を低下させるような微粒子の被着は回避できる
。Even in the above case, by controlling the magnetization pattern,
By dispersing the magnetized portions in a desired pattern, deposition of fine particles that would reduce output can be avoided.
本発明の磁気記録媒体の製造方法において、磁気記録膜
を所望のパターンにに磁化する方法は、例えば、次のよ
うな方法がある。In the method for manufacturing a magnetic recording medium of the present invention, the following methods can be used, for example, to magnetize the magnetic recording film into a desired pattern.
(1)実際のヘッド・ディスク・アセンブリにて使用す
るヘッドと同一形状で、磁気記録膜に比べ高保磁力を有
する磁気ヘッドを用いて、ヘッド浮上高さを磁気記録媒
体と接触することのない°ヴも゛
十分な間隔、例えば0.3μm以上の高さに設置する。(1) By using a magnetic head that has the same shape as the head used in the actual head-disk assembly and has a higher coercive force than the magnetic recording film, the flying height of the head can be adjusted to avoid contact with the magnetic recording medium. The walls are also installed at sufficient intervals, for example, at a height of 0.3 μm or more.
該ヘッドを磁気記録媒体の半径方向に走行させると同時
に、磁気記録媒体を1回転させ、磁気記録膜を、所望の
磁化量および分布に磁化させる
(以下、この方法を、「実ヘッドを用いる方法」という
。)。The head is moved in the radial direction of the magnetic recording medium, and at the same time, the magnetic recording medium is rotated once to magnetize the magnetic recording film to a desired amount and distribution of magnetization (hereinafter, this method will be referred to as "method using a real head"). ).
(2)基板と同一サイズ、同一形状であり、所望の磁化
パターンを予じめ作成しである円板を、磁気記録膜まで
成膜した基板と重なる位置に好適な間隙を設けて一定時
間設置した後、該円板を基板面に対して、垂直に引き離
すことにより、磁気記録膜を所望のパターンに磁化する
(以下、この方法を、「磁化パターン形成用円板を用い
る方法」という。)。(2) A disk of the same size and shape as the substrate, with a desired magnetization pattern created in advance, is placed for a certain period of time with a suitable gap at a position overlapping the substrate on which the magnetic recording film has been deposited. After that, the magnetic recording film is magnetized into a desired pattern by separating the disk perpendicularly from the substrate surface (hereinafter, this method is referred to as "method using a magnetization pattern forming disk"). .
(3)複数種の微細パターンに作成した櫛形の電磁石を
放射状に組み合わせ、所望の間隙を設け、一定時間磁気
記録膜近傍に設置した後、該櫛形電磁石を媒体面に対し
て、垂直に引き離すことにより、磁気記録膜を所望のパ
ターンに磁化す° 8 。(3) Comb-shaped electromagnets created in multiple types of fine patterns are combined radially, a desired gap is provided, and the comb-shaped electromagnets are placed near the magnetic recording film for a certain period of time, and then the comb-shaped electromagnets are pulled away perpendicularly to the medium surface. The magnetic recording film is magnetized into a desired pattern.
る
(以下、この方法を「櫛形電磁石を用いる方法」という
。)。(Hereinafter, this method will be referred to as the "method using a comb-shaped electromagnet.")
次に、本発明の磁気記録媒体を製造するに際して、例え
ば、上記した方法などを用いて、所望のパターンに磁化
した磁気記録膜上に、磁性体微粒子を被着させる方法と
しては、次のような方法がある。Next, when manufacturing the magnetic recording medium of the present invention, the method of depositing magnetic fine particles on a magnetic recording film magnetized in a desired pattern using, for example, the method described above is as follows. There is a method.
(1)磁気記録膜と保護膜とを成膜する真空槽の間に、
磁性体微粒子被着用の槽を設け、該槽内に磁気記録膜ま
で成膜した円板を設置する。この後、磁性体微粒子を槽
内に一定時間噴射し、さらに好適な量および流速で、例
えば、窒素ガスなどの不活性ガスを、磁性体微粒子が被
着した円板上に吹き付けて、余剰微粒子を排除する。(1) Between the vacuum chamber in which the magnetic recording film and the protective film are formed,
A tank for depositing magnetic fine particles is provided, and a disk coated with a magnetic recording film is placed in the tank. After that, the magnetic fine particles are injected into the tank for a certain period of time, and then an inert gas such as nitrogen gas is sprayed at a suitable amount and flow rate onto the disc on which the magnetic fine particles are attached, so that the excess fine particles are removed. eliminate.
(以下、この方法を、「噴射法」という。)。(Hereinafter, this method will be referred to as the "injection method.")
(2)磁性体微粒子を所望の濃度に分散溶解させた、例
えば、分子量70以上の炭化水素類およびそれらのハロ
ゲン化物、分子量60以上のアルコール類、分子量70
以上のエーテル類、分子量50以上のケトン類、分子量
60以上の有機酸およびそれらの誘導体などの有機溶剤
液槽を、例えば窒素ガスなどの不活性ガス雰囲気中に設
置し、磁気記録膜まで成膜した円板を一定時間該溶液中
に浸漬させた後引き上げる。上記した方法を用いて、磁
性体微粒子を磁気記録膜上に被着させた後、加熱または
光照射などの方法により有機溶剤を排除する。(2) Magnetic particles are dispersed and dissolved to a desired concentration, such as hydrocarbons with a molecular weight of 70 or more and their halides, alcohols with a molecular weight of 60 or more, molecular weight 70 or more.
A bath of organic solvents such as the above ethers, ketones with a molecular weight of 50 or more, organic acids with a molecular weight of 60 or more and their derivatives is placed in an inert gas atmosphere such as nitrogen gas, and a magnetic recording film is formed. The disc is immersed in the solution for a certain period of time and then pulled out. After the magnetic fine particles are deposited on the magnetic recording film using the method described above, the organic solvent is removed by heating or light irradiation.
なお、磁性体微粒子を有機溶剤中に分散溶解させるにあ
たり、分散性を向上させるために、ある種の界面活性剤
を好適な濃度で加えても良い
(以下、この方法を「浸漬法」という。)。Note that when dispersing and dissolving magnetic particles in an organic solvent, a certain type of surfactant may be added at a suitable concentration in order to improve dispersibility (hereinafter, this method is referred to as the "immersion method"). ).
本発明の磁気記録媒体を製造するに際して用いる磁性体
微粒子の材料としては、鉄、コバルト、ニッケル、これ
ら単独または複数の合金、これらの単独の酸化物または
複数の酸化物の合金などである。Materials for the magnetic fine particles used in manufacturing the magnetic recording medium of the present invention include iron, cobalt, nickel, alloys of these or a combination of these, single oxides of these, or alloys of multiple oxides.
次に、いくつかの実施例及び比較例の条件にて作成した
磁気記録媒体について088強度を測定し、耐摺動性を
評価した結果を表1及び表2に示す。Next, 088 strength was measured for magnetic recording media prepared under the conditions of some examples and comparative examples, and the results of evaluating the sliding resistance are shown in Tables 1 and 2.
表1
表2
*CS S : Contact 旦tart &
5topマンガン−亜鉛磁気ヘッドを用いて、荷重(た
だし静止時)20gf、回転数3600rpm、磁気記
録媒体の回転開始と回転停止とのスイッチ° 12′
0N−OFF間隔15secの条件にて、クラッシュが
発生するまでの磁気記録媒体の総回転数をC8S強度と
する。C8S強度試験機のモータの回転数の時間変化を
第2図に示す。Table 1 Table 2 *CS S: Contact Tart &
Using a 5top manganese-zinc magnetic head, a crash occurred under the conditions of a load (when stationary) of 20 gf, a rotation speed of 3600 rpm, and a switch for starting and stopping rotation of the magnetic recording medium with a 12' 0N-OFF interval of 15 seconds. The total number of rotations of the magnetic recording medium until the C8S strength is determined. Figure 2 shows the change in the rotational speed of the motor of the C8S strength testing machine over time.
まず、実験例1について説明する。First, Experimental Example 1 will be explained.
φ5.25”アルミニウムーマグネシウム合金基板上に
ニッケル−リン(膜厚10μm)めっき後クロム下地膜
(膜厚450nm)を形成し、該表面上にコバルト−ニ
ッケル磁気記録膜(膜厚45nm)を形成した。After plating nickel-phosphorous (film thickness 10 μm) on a φ5.25” aluminum-magnesium alloy substrate, a chromium base film (film thickness 450 nm) is formed, and a cobalt-nickel magnetic recording film (film thickness 45 nm) is formed on the surface. did.
次に、該磁気記録膜を前記した実ヘッドを用いる方法に
よって磁化した。この後、前記した噴射法を用いて、表
1実験番号1から6に記述した径の球状磁性体微粒子を
、上記磁気記録膜上に均一に被着させた。磁性体微粒子
を被着させた磁気記録膜上に、さらに、CVD法によっ
てカーボン保護膜(膜厚45nm)を形成し、凹凸形状
を有する該保護膜上にパーフロロポリエーテルよりなる
潤滑膜(膜厚8nm)を形成して磁気記録媒体を完成し
た。Next, the magnetic recording film was magnetized by the method using the actual head described above. Thereafter, spherical magnetic fine particles having the diameters listed in Experiment Nos. 1 to 6 in Table 1 were uniformly deposited on the magnetic recording film using the above-described spraying method. A carbon protective film (film thickness: 45 nm) is further formed by CVD on the magnetic recording film on which magnetic fine particles are adhered, and a lubricating film (film) made of perfluoropolyether is formed on the protective film having an uneven shape. 8 nm thick) to complete a magnetic recording medium.
なお、実験番号1.2ではコバルト−ニッケル系合金、
実験番号3.4では鉄−コバルト系合金、実験番号5.
6では鉄−ニッケル系合金の球状磁性体微粒子をそれぞ
れ用いた。In addition, in experiment number 1.2, cobalt-nickel alloy,
Experiment number 3.4 uses iron-cobalt alloy, experiment number 5.
In No. 6, spherical magnetic fine particles of iron-nickel alloy were used.
以上のように作成した磁気記録媒体について測定したC
8S強度は、表1に示すように目標値を達成した。C measured on the magnetic recording medium prepared as above
The 8S strength achieved the target value as shown in Table 1.
次に、実験例2について説明する。Next, Experimental Example 2 will be explained.
上記実験例1と同様に、磁気記録膜まで形成後、前記し
た磁化パターン形成用円板を用いる方法によって該磁気
記録膜を磁化した。As in Experimental Example 1 above, after the magnetic recording film was formed, the magnetic recording film was magnetized by the method using the above-described magnetization pattern forming disk.
該磁気記録膜に実験例1と同様の噴射法を用いて球状磁
性体微粒子を均一に被着させた後、実験例1と同様の工
程によって磁気記録媒体を完成した。After uniformly depositing spherical magnetic fine particles on the magnetic recording film using the same spraying method as in Experimental Example 1, a magnetic recording medium was completed using the same steps as in Experimental Example 1.
被着させた磁性体微粒子の組成、サイズは実験例1と同
様であり、実験例2において作成した磁気記録媒体のC
SS強度は、表1の実験番号1から6と同様、目標値を
達成した。The composition and size of the deposited magnetic fine particles are the same as in Experimental Example 1, and the C of the magnetic recording medium prepared in Experimental Example 2 is
The SS strength achieved the target value as in Experiments Nos. 1 to 6 in Table 1.
次に、実験例3について説明する。Next, Experimental Example 3 will be explained.
上記実験例1と同様に、磁気記録膜まで形成後、前記し
た櫛形電磁石を用いる方法により該磁気記録膜を磁化し
た。As in Experimental Example 1 above, after the magnetic recording film was formed, the magnetic recording film was magnetized by the method using the comb-shaped electromagnet described above.
該磁気記録膜に前記した浸漬法を用いて球状磁性体微粒
子を均一に被着させた後、実験例1と同様の工程を用い
て、磁気記録媒体を完成した。After uniformly depositing spherical magnetic fine particles on the magnetic recording film using the dipping method described above, a magnetic recording medium was completed using the same steps as in Experimental Example 1.
被着させた磁性体微粒子の組成、サイズは実験例1と同
様であり、実験例3において作成した磁気記録媒体のC
8S強度は、表1の実験番号1から6と同様、目標値を
達成した。The composition and size of the deposited magnetic fine particles are the same as in Experimental Example 1, and the C of the magnetic recording medium prepared in Experimental Example 3 is
The 8S intensity achieved the target value as in Experiments Nos. 1 to 6 in Table 1.
次に、実験例4について説明する。Next, Experimental Example 4 will be explained.
上記実験例1と同様に、磁気記録膜まで形成後、実験例
1と同様の実ヘッドを用いる方法により磁気記録膜を磁
化した。As in Experimental Example 1 above, after the magnetic recording film was formed, the magnetic recording film was magnetized by the same method as in Experimental Example 1 using an actual head.
該磁気記録膜に、上記した実験例3と同様の浸漬法を用
いて、針状磁性体微粒子を均一に被着させた後、実験例
1と同様の工程を用いて、磁気記録媒体を完成した。After uniformly depositing acicular magnetic particles on the magnetic recording film using the same dipping method as in Experimental Example 3 described above, a magnetic recording medium was completed using the same process as in Experimental Example 1. did.
なお実験番号15.16.17では酸化鉄、実験番号1
8.19.20では鉄−コバルト系合金の針状磁性体微
粒子を用いた。In addition, in experiment numbers 15, 16, and 17, iron oxide, experiment number 1
In 8.19.20, acicular magnetic fine particles of iron-cobalt alloy were used.
以上のようにして作成した磁気記録媒体について測定し
たC8S強度は、表2に示すように目標値を達成した。The C8S intensity measured for the magnetic recording medium produced as described above achieved the target value as shown in Table 2.
次に、実験例5について説明する。Next, Experimental Example 5 will be explained.
上記実験例1と同様に、磁気記録膜まで形成後、実験例
2と同様の磁化パターン形成用円板を用いる方法によっ
て、磁気記録膜を磁化した。As in Experimental Example 1 above, after the magnetic recording film was formed, the magnetic recording film was magnetized by the same method as in Experimental Example 2, using a disk for forming a magnetization pattern.
該磁気記録膜に上記した実験例4と同様の浸漬法を用い
て針状磁性体微粒子を均一に被着させた後、実験例1と
同様の工程によって磁気記録媒体を完成した。After uniformly depositing acicular magnetic fine particles on the magnetic recording film using the same dipping method as in Experimental Example 4 described above, a magnetic recording medium was completed using the same steps as in Experimental Example 1.
被着させた磁性体微粒子の組成、サイズは実験例4と同
様であり、実験例5において作成した磁気記録媒体のC
8S強度は、表2の実験番号15から20と同様、目標
値を達成した。The composition and size of the deposited magnetic fine particles are the same as in Experimental Example 4, and the C of the magnetic recording medium prepared in Experimental Example 5 is
Similar to experiment numbers 15 to 20 in Table 2, the 8S intensity achieved the target value.
次に、実験例6について説明する。Next, Experimental Example 6 will be explained.
上記実験例1と同様に、磁気記録膜まで形成後、実験例
3と同様の櫛形電磁石を用いる方法によって磁気記録膜
を磁化した。As in Experimental Example 1 above, after the magnetic recording film was formed, the magnetic recording film was magnetized by the same method as in Experimental Example 3 using a comb-shaped electromagnet.
該磁気記録膜に上記した実験例1と同様の噴射法を用い
て針状磁性体微粒子を均一に被着させた後、実験例1と
同様の工程によって磁気記録媒体を完成した。After uniformly depositing acicular magnetic fine particles on the magnetic recording film using the same spraying method as in Experimental Example 1 described above, a magnetic recording medium was completed using the same steps as in Experimental Example 1.
被着させた磁性体微粒子の組成、サイズは実験例4と同
様であり、実験例6において作成した磁気記録媒体のC
SS強度は、表2の実験番号15から20と同様、目標
値を達成した。The composition and size of the deposited magnetic fine particles are the same as in Experimental Example 4, and the C of the magnetic recording medium prepared in Experimental Example 6 is
The SS strength achieved the target value as in Experiments Nos. 15 to 20 in Table 2.
次に、比較例1について説明する。Next, Comparative Example 1 will be explained.
上記実験例1と同様に、磁気記録膜まで形成後、実験例
1と同様の実ヘッドを用いる方法によって磁気記録膜を
磁化した。As in Experimental Example 1 above, after the magnetic recording film was formed, the magnetic recording film was magnetized by the same method as in Experimental Example 1 using an actual head.
該磁気記録膜に上記した実験例1と同様の噴射法を用い
て球状磁性体微粒子を均一に被着させた後、実験例1と
同様の工程によって磁気記録媒体を完成した。After uniformly depositing spherical magnetic fine particles on the magnetic recording film using the same spraying method as in Experimental Example 1 described above, a magnetic recording medium was completed using the same steps as in Experimental Example 1.
被着させた磁性体微粒子の組成は実験例1と同様である
が、サイズ(表1中実験番号7.8)、被着量(同9.
10)及び被着密度(同11.12.13.14)が好
適範囲外であるため、比較例1において作成した磁気記
録媒体のCSS強度は、表1に示すように目標値に達し
なかった。The composition of the deposited magnetic fine particles was the same as in Experimental Example 1, but the size (experiment number 7.8 in Table 1) and the amount of deposition (experiment number 9.8 in Table 1) were different.
10) and adhesion density (11.12.13.14) were outside the preferred range, so the CSS strength of the magnetic recording medium created in Comparative Example 1 did not reach the target value as shown in Table 1. .
次に比較例2について説明する。Next, Comparative Example 2 will be explained.
上記実験例1と同様に、磁気記録膜まで形成後、実験例
2と同様の磁化パターン形成用円板を用いる方法によっ
て磁気記録膜を磁化した。As in Experimental Example 1 above, after the magnetic recording film was formed, the magnetic recording film was magnetized by the same method as in Experimental Example 2, using a disk for forming a magnetization pattern.
該磁気記録膜に、上記した実験例3と同様の浸漬法を用
いて、針状磁性体微粒子を均一に被着させた後、実験例
1と同様の工程によって磁気記録媒体を完成した。After uniformly depositing acicular magnetic fine particles on the magnetic recording film using the same dipping method as in Experimental Example 3 described above, a magnetic recording medium was completed using the same steps as in Experimental Example 1.
被着させた磁性体微粒子の組成は実験例4と同様である
が、サイズ(表2中実験番号21.22)被着量(同2
3.24)及び被着密度(同25.26.27.28)
が好適範囲外であるため、比較例2において作成した磁
気記録媒体のCSS強度は、表2に示すように、目標値
に達しなかった。The composition of the deposited magnetic fine particles is the same as that in Experimental Example 4, but the size (experiment number 21.22 in Table 2) and the amount of deposition (experiment number 21.22 in Table 2) are the same as those in Experimental Example 4.
3.24) and adhesion density (25.26.27.28)
was outside the preferred range, so the CSS strength of the magnetic recording medium produced in Comparative Example 2 did not reach the target value, as shown in Table 2.
以上の実験例および比較例に記述したように、磁気記録
膜上に被着させる磁性体微粒子の径が5〜80nm(針
状微粒子の場合長さが20nm〜1.5μm)、微粒子
被着量(磁気記録膜の全面積に占める微粒子被着面積)
が0.5%〜5%、微粒子被着密度が半径方向の微粒子
被着部分の間隔として1μm〜400μm、周方向の微
粒子被着部分の間隔として1μm〜100μmの範囲内
にて作成した実験例1から実験例6の磁気記録媒体は、
C8S強度が目標値の20に回以上を達成した。As described in the above experimental examples and comparative examples, the diameter of the magnetic fine particles deposited on the magnetic recording film is 5 to 80 nm (in the case of acicular fine particles, the length is 20 nm to 1.5 μm), and the amount of fine particles deposited is 5 to 80 nm. (Fine particle adhesion area in total area of magnetic recording film)
Experimental examples created with a particle adhesion density of 1 μm to 400 μm in the radial direction, and 1 μm to 100 μm in the circumferential direction. The magnetic recording media of Experimental Examples 1 to 6 are as follows:
The C8S intensity achieved the target value of 20 times or more.
これに対し、比較例1.2に示すように上記した好適範
囲外の条件にて作成した磁気記録媒体では、C8S強度
が12に回以下に低下して磁気記録媒体の耐摺動性が劣
化した。On the other hand, as shown in Comparative Example 1.2, in a magnetic recording medium prepared under conditions outside the above-mentioned preferred range, the C8S strength decreased to 12 times or less, and the sliding resistance of the magnetic recording medium deteriorated. did.
具体的には、実験番号7.21に記述したように、被着
させる磁性体微粒子のサイズが上記好適範囲よりも小さ
い場合は、完成した磁気記録媒体表面に形成された凹凸
の大きさが不十分となり、該凹凸によるヘッドと媒体の
吸着防止効果が減少してC8S強度が低下すると考えら
れる。Specifically, as described in Experiment No. 7.21, if the size of the magnetic fine particles to be deposited is smaller than the above-mentioned preferred range, the size of the unevenness formed on the surface of the completed magnetic recording medium may be inappropriate. It is considered that this becomes sufficient, and the effect of preventing adhesion between the head and the medium due to the unevenness decreases, resulting in a decrease in C8S strength.
実験番号8.22に記述したように、被着させる磁性体
微粒子のサイズが上記好適範囲よりも大きい場合は、完
成された磁気記録媒体表面に過剰な大きさの凹凸が形成
され、ヘッド接触時の衝撃が増大してC8S強度が低下
すると考えられる。As described in Experiment No. 8.22, if the size of the magnetic fine particles to be deposited is larger than the above-mentioned preferred range, excessively large irregularities will be formed on the surface of the completed magnetic recording medium, causing problems when the head makes contact. It is thought that the C8S strength decreases as the impact increases.
実験番号9.12.14.23.26.28に記述した
ように、磁性体微粒子の被着量が好適範囲よりも多い場
合、または被着密度が好適範囲よりも高密度である場合
は、ヘッドが接触する面積が増大してヘッドと媒体の吸
着を防止する効果よりも、ヘッドが媒体と接触してクラ
ッシュする確率の方が高くなるためにC8S強度が低下
すると考えられる。As described in Experiment No. 9.12.14.23.26.28, if the amount of magnetic fine particles deposited is higher than the preferred range, or if the deposit density is higher than the preferred range, It is thought that the C8S strength decreases because the probability of the head coming into contact with the medium and crashing becomes higher than the effect of preventing adhesion between the head and the medium due to an increase in the contact area of the head.
実験番号10.11.13.24.25.27、に記述
したように、磁性体微粒子の被着量が好適範囲よりも少
ない場合、または被着密度が好適範囲よりも低密度であ
る場合は、ヘッドと媒体の吸着を防止するための凹凸量
が不十分となりC8S強度が低下すると考えられる。As described in Experiment No. 10.11.13.24.25.27, if the amount of magnetic fine particles deposited is less than the preferred range, or if the deposit density is lower than the preferred range, , it is thought that the amount of unevenness to prevent the head and the medium from adhering is insufficient, resulting in a decrease in C8S strength.
なお、上記した実験例および比較例に記述した以外に、
以下に記述するような変更も可能である。In addition to what was described in the experimental examples and comparative examples above,
Changes as described below are also possible.
(1)非磁性体基板として、表面にアルマイト処理を施
したアルミニウム基板、ガラス基板などを用いる。(1) As the non-magnetic substrate, an aluminum substrate, a glass substrate, etc. whose surface has been subjected to an alumite treatment is used.
(2)磁気記録膜としてコバルト、コバルト−クロム系
合金、コバルト−白金系合金などを用いる。(2) Cobalt, cobalt-chromium alloy, cobalt-platinum alloy, etc. are used as the magnetic recording film.
(3)磁気ヘッドとして酸化ジルコニウム、アルミナチ
タンカーバイトなどからなる磁気ヘッドを用いる。(3) A magnetic head made of zirconium oxide, alumina titanium carbide, etc. is used as the magnetic head.
(4)磁気記録媒体上に被着させる磁性体微粒子として
上記した(2)の磁気記録媒体材料からなる微粒子を用
いる。(4) Fine particles made of the magnetic recording medium material described in (2) above are used as magnetic fine particles to be deposited on the magnetic recording medium.
(5)保護膜としてシリコン化合物、窒化物等を用いる
。(5) A silicon compound, nitride, etc. is used as the protective film.
(6)磁気記録膜及び保護膜をスパッタリング法にて形
成する。(6) Form a magnetic recording film and a protective film by sputtering.
(7)潤滑膜材料として脂肪酸化を用いる。(7) Use fatty acid conversion as a lubricating film material.
(8)上記各膜の膜厚を好適な所望の膜厚とする。(8) The thickness of each of the above films is set to a suitable desired thickness.
以上詳述したように本発明によれば、磁気記録媒体表面
に好適な凹凸形状が形成されるので、磁気ヘッドを磁気
記録媒体表面上に浮」ニさせて記録・再生を行う際に、
該磁気記録媒体面に磁気ヘッドのスライダが潤滑膜を介
して吸着することがなくなり、該媒体の回転開始時ある
いは回転停止時などにおける、前記した吸着に起因する
クラッシュを防止して、耐摺動性に優れた磁気記録媒体
を提供できるという効果がある。As detailed above, according to the present invention, a suitable uneven shape is formed on the surface of the magnetic recording medium, so when recording and reproducing with the magnetic head floating above the surface of the magnetic recording medium,
The slider of the magnetic head is no longer attracted to the surface of the magnetic recording medium through the lubricant film, preventing crashes caused by the above-mentioned attraction when the medium starts or stops rotating, and improves sliding resistance. This has the effect of providing a magnetic recording medium with excellent properties.
第1図(a)は磁気記録媒体の拡大断面図、第1図(b
)は磁気記録膜の表面を示す説明図、第2図はCSS強
度評価試験機のモータ回転数の時間変化を示す説明図で
ある。
1・・・非磁性体基板、 2・・・下地膜、3・・
・磁気記録膜、 4・・保護膜、5・・・潤滑膜
、 6 ・磁性体微粒子、7・・・記録単
位(ビット)。FIG. 1(a) is an enlarged sectional view of a magnetic recording medium, FIG. 1(b)
) is an explanatory diagram showing the surface of the magnetic recording film, and FIG. 2 is an explanatory diagram showing the change over time in the motor rotation speed of the CSS strength evaluation tester. 1... Non-magnetic substrate, 2... Base film, 3...
- Magnetic recording film, 4... Protective film, 5... Lubricating film, 6 - Magnetic fine particles, 7... Recording unit (bit).
Claims (1)
順次形成されてなる磁気記録媒体において、前記磁気記
録膜上に磁性体の微粒子を被着し、保護膜および潤滑膜
を、順次形成させることを特徴とする磁気記録媒体。 2、磁気記録膜を部分的に磁化した後、粒子を磁化した
部分に磁性体微粒子を被着させ、その後に、保護膜を形
成することを特徴とする磁気記録媒体製造方法。 3、磁性体微粒子を被着させるために磁化する磁気記録
膜表面の面積が記録面の全面積の0.1%〜5%である
ことを特徴とする請求項1記載の磁気記録媒体。 4、磁性体微粒子を被着させる部分の間隔が、磁気記録
媒体の半径方向には1μm〜400μm、磁気記録媒体
の周方向には1μm〜100μmであることを特徴とす
る請求項1または3記載の磁気記録媒体。 5、磁気記録膜に被着させる磁性体微粒子の形状が球状
または針状であることを特徴とする請求項1、3または
4記載の磁気記録媒体。 6、磁性体微粒子の形状が球状である場合は、径が5n
m〜80nmであり、磁性体微粒子の形状が針状である
場合は、径が5nm〜80nm、長さが20nm〜1.
5μm、であることを特徴とする請求項5記載の磁気記
録媒体。 7、ニッケル−リン基板またはガラス基板上に、コバル
トを主成分とする金属磁気記録膜、カーボンを主成分と
する保護膜、フッ化炭素およびその誘導体を主成分とす
る潤滑膜を順次、形成して構成されることを特徴とする
請求項3、4、5または6記載の磁気記録媒体。[Claims] 1. In a magnetic recording medium in which a magnetic recording film, a protective film, and a lubricating film are sequentially formed on a non-magnetic substrate, fine particles of a magnetic material are deposited on the magnetic recording film, A magnetic recording medium characterized by sequentially forming a protective film and a lubricating film. 2. A method for manufacturing a magnetic recording medium, which comprises partially magnetizing a magnetic recording film, depositing magnetic particles on the magnetized portions, and then forming a protective film. 3. The magnetic recording medium according to claim 1, wherein the area of the surface of the magnetic recording film that is magnetized for adhering the magnetic fine particles is 0.1% to 5% of the total area of the recording surface. 4. According to claim 1 or 3, the distance between the parts to which the magnetic fine particles are adhered is 1 μm to 400 μm in the radial direction of the magnetic recording medium and 1 μm to 100 μm in the circumferential direction of the magnetic recording medium. magnetic recording media. 5. The magnetic recording medium according to claim 1, 3 or 4, wherein the magnetic fine particles deposited on the magnetic recording film have a spherical or acicular shape. 6. If the shape of the magnetic particles is spherical, the diameter is 5n.
m to 80 nm, and when the shape of the magnetic fine particles is acicular, the diameter is 5 nm to 80 nm, and the length is 20 nm to 1.
6. The magnetic recording medium according to claim 5, wherein the magnetic recording medium has a thickness of 5 μm. 7. On a nickel-phosphorous substrate or a glass substrate, sequentially form a metal magnetic recording film mainly composed of cobalt, a protective film mainly composed of carbon, and a lubricating film mainly composed of fluorocarbon and its derivatives. 7. The magnetic recording medium according to claim 3, wherein the magnetic recording medium is comprised of: