JPH0459260B2 - - Google Patents
Info
- Publication number
- JPH0459260B2 JPH0459260B2 JP59034160A JP3416084A JPH0459260B2 JP H0459260 B2 JPH0459260 B2 JP H0459260B2 JP 59034160 A JP59034160 A JP 59034160A JP 3416084 A JP3416084 A JP 3416084A JP H0459260 B2 JPH0459260 B2 JP H0459260B2
- Authority
- JP
- Japan
- Prior art keywords
- mol
- tio
- present
- substrate
- paste
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Description
〔発明の技術分野〕
本発明は、回路基板に係り、特に低温焼成可能
な回路基板に関する。
〔発明の技術的背景とその問題点〕
従来から回路基板用のセラミツクス材料として
用いられているものにアルミナがある。このアル
ミナは絶縁性が良好であるため、もつとも一般的
に使用されている。
しかしながらアルミナを用いた場合は、その焼
成温度が1500〜1600℃と高温であるため、使用で
きる導体ペーストに制限が生じていた。例えば導
体ペーストと基板とを同時焼結する多層回路基板
では、アルミナの焼成温度に十分耐え得るような
タングステン、モリブデン等の導体ペーストを用
いる必要があつた。しかしながらW,Moは抵抗
率がAgの1.6×10-6Ω・cmに比べ5.2×10-6Ω・
cm、5.5×10-6Ω・cmと3倍程度大きい。従つて
同じ伝導度の導体路を得るためには、導体幅を3
倍程度にする必要があり、高密度配線ができない
欠点があつた。
また、ガラス成分を加えて焼成温度を下げる試
みもあるが、多層配線の場合のマイグレーシヨン
の問題があり、実用上好ましくない。
このような欠点を除去するため、絶縁性等の特
性を劣化させることなく低温焼成可能な回路基板
の開発が望まれている。
このような要望にこたえて、本発明は先に
BaO,SnO2,B2O3を主成分とする1300℃以下程
度で焼結可能な低温焼結基板を提案した。絶縁抵
抗、誘電率等の電気的特性はAl2O3と同等以上で
あり、かつ低温焼結ができるため非常に有効な材
料である。本発明者等が、この基板材料について
さらに検討を加えたところ、耐水性の点で少々問
題があることがわかつた。
基板の耐水性は、高湿中もしくは水分の存在す
る環境で用いた場合の絶縁特性等を考慮した場合
重要な要素である。
〔発明の目的〕
本発明は以上の点を考慮してなされたもので、
低温焼成が可能で、かつ耐水性に優れた回路基板
を提供することを目的とする。
〔発明の概要〕
本発明は、バリウム、スズ、硼素、チタンを、
BaO,SnO2,B2O3,TiO2換算して、
BaO 8〜54mol%
SnO2 7〜40mol%
B2O3 10〜58mol%
TiO2 5〜48mol%
含有された酸化物焼結体を絶縁体として用いて
いることを特徴とする回路基板である。
このような組成をとることにより焼成温度1300
℃以下の低温焼成可能な回路基板を得ることがで
きる。この基板は熱膨張率αが9×10-6/℃以下
程度と小さいため、Si(4×10-6/℃)と同程度
であり、直接LSIチツプを実装するハイブリツド
基板用に好適である。また他の特性、例えば誘電
率εs12以下程度、誘電損失tanδ1.2×10-3以下程
度、絶縁抵抗ρ0.7×1013Ω・cm以上と回路基板と
して十分な特性を有する。また抗折強度も1700
Kg/cm2以上と十分な強度を有する。この酸化物焼
結体は基板自体として用いても良いし、多層配線
間の層間絶縁層として用いても良い。
本発明において、各組成分は以下の理由で限定
する。
まずSnO2であるが、余り多いと本来半導体の
性質を有するため、絶縁抵抗が低下してしまい、
絶縁性基板としての特性を満足しなくなる。
また誘電損失(tanδ)、比誘電率(εs)も大き
くなり、高密度配線、高周波特性に劣つてしま
う。また少ないと、熱膨張率が大きくなってしま
い、例えばLSIチツプを搭載する場合にチツプの
ソリ、割れ等が生じ易くなる。よつてSnO2に換
算して7〜40mol%の範囲が好ましい。
またBaOであるが、余り多いと、もろくなつ
てしまい基板強度に劣り、少ないと熱膨張率、
tanδが大きくなつてしまう。特にバリウムの少な
い領域でホウ素量が多いと熱膨張率の劣化が顕著
であり、ホウ素量が少ないとtanδの劣化が顕著で
ある。よつてBaOに換算して、8〜54mol%の範
囲が好ましい。
次にB2O3である。ホウ素量が少ないと、本発
明の主目的である低温焼成の効果が得られず、
1300℃以上程度の温度となつてしまう。また多い
と、熱膨張係数が大きくなつてしまう。
よつて、B2O3に換算して10〜58mol%の範囲
が好ましい。
本発明においては、さらにTiO2を含有させる。
このTiO2を含有させることにより、耐環壊性が
非常に向上する。すなわち、一般環境での使用を
考えた場合、湿度の影響を無視することはできな
い。TiO2を含有させることにより、耐湿性が向
上するのである。TiO2に換算して5mol%より少
ないと吸水率が大きく、高湿中、もしくは水分が
存在するような環境で回路基板を用いた場合、絶
縁抵抗が低下してしまう恐れがある。又、48mol
%を超えると、誘電率等の他の特性が劣化してし
まう。
よつて、TiO2に換算して5〜48mol%の範囲
が好ましい。
このように本発明によれば、焼成温度が1300℃
以下の絶縁性基板を得ることができ、Al2O3の場
合のW,Mo等に変え、Ag,Ag−Pd,Ag−Pt等
のAg系ペースト、Cuペースト等のシート抵抗の
小さい低温焼成ペーストを用いることができるた
め高密度配線ができ、非常に有効である。又、焼
成温度を下げることにより、製造時のエネルギー
コストの低下の効果も大である。
又、特にSnO212〜38mol%、BaO11〜36mol
%、B2O314〜45mol%、TiO27〜40mol%範囲
では、焼成温度1100℃以下程度で製造することが
でき、α≦6.5×10-6/℃と優れた特性を有する
基板を低温焼結できるので非常に有効である。
さらにBaO12〜35mol%、SnO211〜32mol%、
TiO210〜36mol%、B2O315〜40mol%のとき、
耐水性に優れ、ガラスエポキシ基板の1/8程度の
吸水率となり、特に好ましい組成範囲である。
本件発明の焼結体中にはBaSn(BO3)2及び
BaSn(BO3)2のSnがTiで置換された相が存在す
る。Ba(Sn0.5Ti0.5)(BO3)2近傍の相が耐水性で
は優れている。BaTi(BO3)2のみでは、導体層と
の同時焼結の際に、金属が拡散してしまい、多層
配線間の短絡の問題が生じる。
従来用いられているAl2O3基板はAl2O3を92〜
93%含有したもので、1500〜1600℃程度の焼結程
度、εs=10.5〜12、tanδ=2〜5×10-3、ρ=0.2
〜5×1013、α8×10-6℃である。
本発明においては、前述のごとく焼結温度で
Al2O3を大幅に下回り、他の特性も同等かそれ以
上のものを得ることができる。
本発明絶縁性基板を用いて、同時焼結により多
層配線基板を形成した例を説明する。
まず、所望のBaO,SnO2,B2O3,TiO2組成比
を有する原料粉末を含有するスラリーを製造す
る。スラリーは原料粉末に、例えばポリビニルブ
チラル等の結合剤、フタール酸オクチル、ポリエ
チレングリコール等の可塑剤、メンヘーテン油等
の解膠剤、エチルアルコール、トリクロロエチレ
ン等の溶媒を加えて製造する。このスラリーを用
い、ドクタープレード法でグリーンシートを製造
する。次いでAg系等の導体ペーストを用い、第
1の導体層を印刷・塗布し乾燥する。続いて所望
のBaO,SnO2,B2O3,TiO2の組成比を有する原
料粉末を含有する絶縁体ペーストを第1の導体層
上に印刷塗布し、乾燥した後、第2の導体層を同
様に形成する。絶縁ペーストは、ブチルカルビト
ールアセテート、テルピネオール、エチルセルロ
ーズ等を添加してペースト状とし、塗布する。
このように、2層配線を施したグリーンシート
を電気炉中で例えば1000℃程度で3hr同時焼成し、
多層配線基板を製造する。
本発明の回路基板は、多層配線を有する同時焼
成用の基板としての用途に特に優れている。本発
明によれば低温焼成が可能な絶縁体層を提供でき
るので、導体層として、従来のW,Mo等にか
え、シート抵抗の小さいAg系、Cu系、Au系、
Ni系等のペーストを用いることができる。特に
ガラス成分を含んでいないため、空孔が少なく、
構造がち密であるため、Ag系を用いてもマイグ
レーシヨン等の問題が起こることもない。従つて
配線密度をあげ、高密度化が可能となる。また、
Ag系ペースト中の例えばPd量を減少させること
もできコスト的にもすぐれた基板を提供できる。
従来Al2O3にW,Mo等の導体ペースト用いた
場合は、還元性雰囲気中で同時焼結を行なう必要
があつたが、Ag,Auを用いることができるた
め、空気中焼成が可能であり、製造容易、コスト
の低下等の効果を得ることもできる。又、基板中
にガラス成分がないため、Agのマイグレーシヨ
ンが生じにくい。
また、この例は印刷多層であるがいわゆるグリ
ーンシート多層でも同様であり、2層以上でも同
様である。
この方法では、まずドクターブレート法て
100μm程度の厚さを有するグリーンシートを作
り、そのシートの片面上に導体パターンを印刷
し、それらのシートを複数枚重ねて、温度50℃程
度、圧力200Kg/cm2程度で加圧積層し、多層配線
を施す。同時焼成は上記と同様である。
また、多層配線基板の場合、基体としては、本
発明の回路基板を用いても良いが、例えばAl2O3
基板、ムライト基板等の他の基体を用いても良
い。
〔発明の効果〕
以上説明したように本発明によれば、1300℃以
下程度、特に800〜1200℃程度の低温で焼成可能
な回路基板を得ることができる。
従つて高密度配線、特に一体焼結による多層配
線基板用として有効である。また熱膨張も小さく
できるため、LSIチツプ等を直接搭載する高密度
ハイブリツドIC用の基板としても有効である。
〔発明の実施例〕
以下に本発明の実施例を説明する。本実施例の
回路基板は以下のようにして製造した。
まず、所望の組成比となるようにBaO,B2O3,
SnO2,TiO2の原料粉末を調合し、この調合され
た粉末をアルミナボールと共にアルミナ製ポツト
に入れ、振動ミルにより16時間程度の湿式粉砕を
行なつた。この原料粉末は、焼結後酸化物に転化
するもの、例えば炭酸塩等で用いても良く、本実
施例ではBaCO3,H3BO3,SnO2,TiO2を用い
た。次いで脱水乾燥を施し、1000〜1400℃で3時
間程度の加熱処理を加えた仮焼の後、再度アルミ
ナ製ポツト中に入れ、30時間程度の湿式粉砕を行
なつた。次に、例えばポリビニールアルコール
(P.V.A)等の粘結剤を加え、造粒し、団粒を製
造した。
その後前記団粒を金型に充填し、1000Kg/cm2程
度の圧力で加圧成形し、大気中830〜1200℃3時
間焼成し、試料を作成した。
試料としては、22mmφ×1mmtの円板状試料、
20×3.5×3.5tmmの棒状試料及び20×10×2mmの角
板状試料を作成し、諸特性を測定した。その結果
を第1表に示す。なお比誘電率(εs)及び誘電損
失(tanδ)、抵抗率(ρ)は、円板状試料の両面
にAgペーストを325メツシユのスクリーン印刷に
より同心円状に印刷し、乾燥後大気中にて750℃
20分間の焼付処理を行ない、22mmφ×15μmの円
形の電極を形成して測定した。εs及びtanδは1M
Hzでの値であり、ρは25℃、湿度50%の条件で
1000V印加してから1分後の値の最低値である。
また熱膨張係数(α)は棒状試料を用い、25〜
500℃の温度変化の条件で測定した。
また吸水率は、プレツシヤークツカーテスト
(121℃、2Kg/cm2、水蒸気中)での値であり、テ
スト前後における単位体積当りの重量変化から得
た値(mg/cm2)である。
第1表から明らかなように、本発明の実施例に
おいては、いずれも1300℃以下の焼成温度を有し
tanδが〜10-4程度、αが〜8×10-4/℃以下程度
と優れた特性を示す。また、いずれの試料も抗折
強度は1500Kg/cm2と優れた値を示した。
特に焼成温度低下の効果が大きく、他の特性で
もAl2O3と同等もしくはそれ以上の値を示す。
又、比較例(試料No.16〜19)からも明らかなよ
うに、TiO2が本発明の範囲をはずれるが、吸水
性が大きく、耐水性に劣ることがわかる。
特に試料No.7および12は、100時間後でも高々
0.5mg/cm2以下であり、非常に優れている。
[Technical Field of the Invention] The present invention relates to a circuit board, and particularly to a circuit board that can be fired at a low temperature. [Technical background of the invention and its problems] Alumina has been conventionally used as a ceramic material for circuit boards. Alumina is commonly used because it has good insulation properties. However, when alumina is used, the firing temperature is as high as 1,500 to 1,600°C, which limits the types of conductor pastes that can be used. For example, in a multilayer circuit board in which a conductive paste and a substrate are simultaneously sintered, it is necessary to use a conductive paste made of tungsten, molybdenum, or the like that can sufficiently withstand the firing temperature of alumina. However, the resistivity of W and Mo is 5.2×10 -6 Ω・compared to 1.6×10 −6 Ω・cm of Ag.
cm, 5.5×10 -6 Ω・cm, which is about three times larger. Therefore, in order to obtain a conductor path with the same conductivity, the conductor width must be increased by 3
It was necessary to approximately double the size, which had the disadvantage that high-density wiring could not be achieved. There have also been attempts to lower the firing temperature by adding a glass component, but this poses a problem of migration in the case of multilayer wiring, and is not preferred in practice. In order to eliminate these drawbacks, it is desired to develop a circuit board that can be fired at low temperatures without deteriorating properties such as insulation. In response to such demands, the present invention first
We proposed a low-temperature sintered substrate whose main components are BaO, SnO 2 and B 2 O 3 and which can be sintered at temperatures below 1300°C. It is a very effective material because its electrical properties such as insulation resistance and dielectric constant are equal to or higher than Al 2 O 3 and can be sintered at low temperatures. When the present inventors further investigated this substrate material, they found that it had some problems in terms of water resistance. The water resistance of the substrate is an important factor when considering insulation properties when used in high humidity or environments where moisture is present. [Object of the invention] The present invention has been made in consideration of the above points, and
The purpose of the present invention is to provide a circuit board that can be fired at low temperatures and has excellent water resistance. [Summary of the invention] The present invention provides barium, tin, boron, titanium,
In terms of BaO, SnO 2 , B 2 O 3 , TiO 2 , the oxide sintered body contains BaO 8-54 mol% SnO 2 7-40 mol% B 2 O 3 10-58 mol% TiO 2 5-48 mol% This circuit board is characterized by being used as an insulator. By adopting such a composition, the firing temperature can be increased to 1300℃.
It is possible to obtain a circuit board that can be fired at a low temperature of .degree. C. or lower. This substrate has a small coefficient of thermal expansion α of about 9×10 -6 /℃ or less, which is comparable to that of Si (4×10 -6 /℃), making it suitable for use as a hybrid substrate on which LSI chips are directly mounted. . It also has other properties, such as dielectric constant εs12 or less, dielectric loss tan δ1.2×10 -3 or less, and insulation resistance ρ0.7×10 13 Ω·cm or more, which are sufficient for use as a circuit board. Also, the bending strength is 1700
It has sufficient strength at over Kg/cm 2 . This oxide sintered body may be used as the substrate itself, or as an interlayer insulating layer between multilayer wiring. In the present invention, each component is limited for the following reasons. First of all, SnO 2 has the properties of a semiconductor, so if it is too large, the insulation resistance will decrease.
The characteristics as an insulating substrate will no longer be satisfied. Furthermore, the dielectric loss (tan δ) and relative permittivity (ε s ) also increase, resulting in poor high-density wiring and high-frequency characteristics. If it is too small, the coefficient of thermal expansion will increase, making it more likely that the chip will warp or crack, for example, when mounting an LSI chip. Therefore, it is preferably in the range of 7 to 40 mol% in terms of SnO2 . Also, with regard to BaO, if there is too much, the substrate will become brittle and the strength will be poor, while if there is too little, the coefficient of thermal expansion will decrease.
tanδ becomes large. Particularly in a region with little barium, if the amount of boron is large, the thermal expansion coefficient will deteriorate significantly, and if the amount of boron is small, the deterioration of tan δ will be noticeable. Therefore, it is preferably in the range of 8 to 54 mol% in terms of BaO. Next is B2O3 . If the amount of boron is small, the effect of low-temperature firing, which is the main objective of the present invention, cannot be obtained,
The temperature will reach over 1300℃. If the amount is too large, the coefficient of thermal expansion will become large. Therefore, it is preferably in the range of 10 to 58 mol% in terms of B 2 O 3 . In the present invention, TiO 2 is further contained.
By containing this TiO 2 , ring breakage resistance is greatly improved. That is, when considering use in a general environment, the influence of humidity cannot be ignored. Inclusion of TiO 2 improves moisture resistance. If it is less than 5 mol % in terms of TiO 2 , the water absorption rate will be high, and if the circuit board is used in high humidity or an environment where moisture is present, there is a risk that the insulation resistance will decrease. Also, 48mol
%, other properties such as dielectric constant will deteriorate. Therefore, it is preferably in the range of 5 to 48 mol% in terms of TiO2 . According to the present invention, the firing temperature is 1300°C.
The following insulating substrates can be obtained, and in place of W, Mo, etc. in the case of Al 2 O 3 , low-temperature firing with low sheet resistance such as Ag-based pastes such as Ag, Ag-Pd, Ag-Pt, and Cu pastes can be used. Since paste can be used, high-density wiring can be achieved, which is very effective. Furthermore, by lowering the firing temperature, energy costs during production can be reduced significantly. Also, especially SnO 2 12-38 mol%, BaO 11-36 mol%
%, B 2 O 3 14 to 45 mol %, and TiO 2 7 to 40 mol %, it can be manufactured at a firing temperature of about 1100°C or less, and a substrate with excellent characteristics of α≦6.5×10 -6 /°C can be produced. It is very effective because it can be sintered at a low temperature. In addition, BaO 12-35 mol%, SnO 2 11-32 mol%,
When TiO 2 is 10-36 mol% and B 2 O 3 is 15-40 mol%,
It has excellent water resistance and has a water absorption rate of about 1/8 that of glass epoxy substrates, which is a particularly preferable composition range. The sintered body of the present invention contains BaSn(BO 3 ) 2 and
A phase exists in which Sn in BaSn(BO 3 ) 2 is replaced with Ti. The phase near Ba(Sn 0.5 Ti 0.5 ) (BO 3 ) 2 has excellent water resistance. If BaTi(BO 3 ) 2 is used alone, the metal will diffuse during co-sintering with the conductor layer, causing the problem of short circuits between multilayer wiring. The conventionally used Al 2 O 3 substrate has Al 2 O 3 of 92~
Contains 93%, sintering at about 1500 to 1600℃, ε s = 10.5 to 12, tan δ = 2 to 5 × 10 -3 , ρ = 0.2
~5×10 13 and α8×10 −6 °C. In the present invention, as mentioned above, the sintering temperature is
It is significantly lower than Al 2 O 3 and has other properties that are equivalent to or better than Al 2 O 3. An example will be described in which a multilayer wiring board is formed by simultaneous sintering using the insulating substrate of the present invention. First, a slurry containing raw material powder having a desired composition ratio of BaO, SnO 2 , B 2 O 3 , and TiO 2 is produced. The slurry is produced by adding, for example, a binder such as polyvinyl butyral, a plasticizer such as octyl phthalate or polyethylene glycol, a peptizer such as menhathene oil, and a solvent such as ethyl alcohol or trichloroethylene to the raw material powder. Using this slurry, a green sheet is manufactured by the doctor blade method. Next, a first conductor layer is printed and applied using a conductor paste such as Ag-based conductor paste, and dried. Subsequently, an insulating paste containing raw material powder having a desired composition ratio of BaO, SnO 2 , B 2 O 3 , and TiO 2 is printed and coated on the first conductor layer, and after drying, a second conductor layer is applied. is formed in the same way. The insulating paste is made into a paste by adding butyl carbitol acetate, terpineol, ethyl cellulose, etc., and then applied. In this way, the green sheet with the two-layer wiring is simultaneously fired in an electric furnace at about 1000℃ for 3 hours,
Manufactures multilayer wiring boards. The circuit board of the present invention is particularly suitable for use as a co-firing board having multilayer wiring. According to the present invention, it is possible to provide an insulating layer that can be fired at low temperatures, so instead of using conventional W, Mo, etc., Ag-based, Cu-based, Au-based, etc.
A Ni-based paste or the like can be used. In particular, since it does not contain glass components, there are fewer pores,
Since the structure is dense, problems such as migration will not occur even if Ag-based materials are used. Therefore, it is possible to increase the wiring density and achieve higher density. Also,
For example, the amount of Pd in the Ag-based paste can be reduced, and a cost-effective substrate can be provided. Conventionally, when a conductor paste such as W or Mo was used for Al 2 O 3 , it was necessary to perform simultaneous sintering in a reducing atmosphere, but since Ag and Au can be used, sintering in air is possible. Therefore, it is possible to obtain effects such as ease of manufacture and reduction in cost. Furthermore, since there is no glass component in the substrate, migration of Ag is less likely to occur. Further, although this example is a printed multilayer, the same applies to a so-called green sheet multilayer, and the same applies to two or more layers. In this method, first the doctor blast method is used.
A green sheet with a thickness of about 100 μm is made, a conductor pattern is printed on one side of the sheet, and multiple sheets are stacked and laminated under pressure at a temperature of about 50°C and a pressure of about 200 kg/ cm2 . Perform multilayer wiring. Simultaneous firing is the same as above. Further, in the case of a multilayer wiring board, the circuit board of the present invention may be used as the base, but for example, Al 2 O 3
Other substrates such as substrates, mullite substrates, etc. may also be used. [Effects of the Invention] As explained above, according to the present invention, it is possible to obtain a circuit board that can be fired at a low temperature of about 1300°C or lower, particularly about 800 to 1200°C. Therefore, it is effective for high-density wiring, especially for multilayer wiring boards formed by integral sintering. Furthermore, since thermal expansion can be reduced, it is also effective as a substrate for high-density hybrid ICs on which LSI chips and the like are directly mounted. [Embodiments of the Invention] Examples of the present invention will be described below. The circuit board of this example was manufactured as follows. First, BaO, B 2 O 3 ,
Raw material powders of SnO 2 and TiO 2 were mixed, and the mixed powders were put into an alumina pot together with alumina balls, and wet-pulverized for about 16 hours using a vibrating mill. This raw material powder may be one that is converted into an oxide after sintering, such as a carbonate, and in this example, BaCO 3 , H 3 BO 3 , SnO 2 , and TiO 2 were used. Next, it was dehydrated and dried, and after calcining with heat treatment at 1,000 to 1,400°C for about 3 hours, it was placed again in an alumina pot and wet-pulverized for about 30 hours. Next, a binder such as polyvinyl alcohol (PVA) was added and granulated to produce aggregates. Thereafter, the aggregates were filled into a mold, pressure-molded at a pressure of about 1000 kg/cm 2 , and fired in the atmosphere at 830 to 1200° C. for 3 hours to prepare a sample. The sample is a disc-shaped sample of 22 mmφ x 1 mmt,
A rod-shaped sample of 20 x 3.5 x 3.5 tmm and a square plate-shaped sample of 20 x 10 x 2 mm were prepared, and various properties were measured. The results are shown in Table 1. The relative dielectric constant (ε s ), dielectric loss (tan δ), and resistivity (ρ) were determined by printing Ag paste in concentric circles on both sides of a disk-shaped sample using 325-mesh screen printing, and drying it in the air. 750℃
A baking process was performed for 20 minutes, and a circular electrode of 22 mmφ x 15 μm was formed and measured. ε s and tan δ are 1M
The value is in Hz, and ρ is at 25℃ and 50% humidity.
This is the lowest value one minute after applying 1000V.
In addition, the coefficient of thermal expansion (α) is 25~
Measurements were made under the condition of a temperature change of 500℃. In addition, the water absorption rate is the value obtained in the Pressure Shacker test (121°C, 2Kg/cm 2 , in water vapor), and is the value obtained from the weight change per unit volume before and after the test (mg/cm 2 ). . As is clear from Table 1, all of the examples of the present invention had a firing temperature of 1300°C or less.
It exhibits excellent properties with tan δ of about 10 -4 and α of about 8×10 -4 /°C or less. Furthermore, all the samples exhibited an excellent bending strength of 1500 Kg/cm 2 . In particular, it has a large effect in lowering the firing temperature, and shows values equal to or higher than Al 2 O 3 in other properties. Furthermore, as is clear from the comparative examples (sample Nos. 16 to 19), although TiO 2 is outside the scope of the present invention, it is found to have high water absorption and poor water resistance. In particular, samples Nos. 7 and 12 were at best even after 100 hours.
It is 0.5 mg/cm 2 or less, which is very good.
【表】【table】
【表】【table】
【表】
次に本発明絶縁性基板を用いて、同時焼結によ
り多層配線基板を形成した実施例を説明する。
まず、所望のBaO,SnO2,B2O3,TiO2組成比
を有する原料粉末を含有するスラリーを製造す
る。スラリーは原料粉末に、例えばポリビニルブ
チラル等の結合剤、フタール酸オクチル、ポリエ
チレングリコール等の可塑剤、メンヘーデン油等
の解膠剤、エチルアルコール、トリクロロエチレ
ン等の溶媒を加えて製造する。このスラリーを用
い、ドクターブレード法でグリーンシートを製造
する。次いでAg系等の導体ペーストを用い、第
1の導体層を印刷・塗布し乾燥する。続いて所望
のBaO,SnO2,B2O3,TiO2の組成比を有する原
料粉末を含有する絶縁体ペーストを第1の導体層
上に印刷塗布し、乾燥した後、第2の導体層を同
様に形成する。絶縁ペーストは、ブチルカルビト
ールアセテート、テルピネオール、エチルセルロ
ーズ等を添加してペースト状とし、塗布する。
このように、2層配線を施したグリーンシート
を電気炉中で1000℃程度で3hr同度焼成し、多層
配線基板を製造した。
第2表に、この多層配線基板の諸特性を示す。
同表中密着強度は引張試験用ワイヤを半田付で第
2の導体層に固着し、インストロン引張試験機を
用いて測定した(引張測定0.5cm/min)基板と
導体層との密着の度合である。またワイヤボンデ
イング性はAu、Al系の25μmφのボンデイング
ワイヤの導体層との接着の強度を示したものであ
る。また同表中試料No.は、第1表における組成比
のセラミツル原料粉を用いたことを示す。また各
特性は10個の試料の平均値である。
なお第3表に、第2表で用いた導体ペーストの
諸特性を示す。
密着強度、ボンデイング特性は、それぞれ1
Kg/mm2以上、5g以上で実用上問題はなく、各実
施例ともに十分満足している。またシート抵抗も
導体ペーストの設定値のものを得ることができ
た。
また、同時焼成時の焼成温度は組成によつても
異なるが、800〜1200℃程度が好ましい。余り高
くするとBが蒸発しやすくなり、均一な基板を得[Table] Next, an example will be described in which a multilayer wiring board was formed by simultaneous sintering using the insulating substrate of the present invention. First, a slurry containing raw material powder having a desired composition ratio of BaO, SnO 2 , B 2 O 3 , and TiO 2 is produced. The slurry is produced by adding, for example, a binder such as polyvinyl butyral, a plasticizer such as octyl phthalate or polyethylene glycol, a peptizer such as menhaden oil, and a solvent such as ethyl alcohol or trichloroethylene to the raw material powder. Using this slurry, a green sheet is manufactured by a doctor blade method. Next, a first conductor layer is printed and applied using a conductor paste such as Ag-based conductor paste, and dried. Subsequently, an insulating paste containing raw material powder having a desired composition ratio of BaO, SnO 2 , B 2 O 3 , and TiO 2 is printed and coated on the first conductor layer, and after drying, a second conductor layer is applied. is formed in the same way. The insulating paste is made into a paste by adding butyl carbitol acetate, terpineol, ethyl cellulose, etc., and then applied. In this way, the green sheet with the two-layer wiring was fired in an electric furnace at about 1000°C for 3 hours to produce a multilayer wiring board. Table 2 shows various characteristics of this multilayer wiring board.
The adhesion strength in the same table is the degree of adhesion between the substrate and the conductor layer, which was measured using an Instron tensile tester (tensile measurement 0.5 cm/min) after fixing a tensile test wire to the second conductor layer by soldering. It is. Further, wire bonding property indicates the strength of adhesion between a 25 μm diameter Au or Al based bonding wire and a conductor layer. In addition, the sample No. in the same table indicates that the ceramic vine raw material powder having the composition ratio shown in Table 1 was used. Moreover, each characteristic is the average value of 10 samples. Table 3 shows various properties of the conductor paste used in Table 2. Adhesion strength and bonding properties are each 1
Kg/mm 2 or more, 5 g or more, there is no practical problem, and each example is fully satisfied. Also, the sheet resistance could be obtained at the set value of the conductor paste. Further, the firing temperature during simultaneous firing varies depending on the composition, but is preferably about 800 to 1200°C. If the temperature is too high, B will easily evaporate, making it difficult to obtain a uniform substrate.
【表】【table】
【表】【table】
【表】
ることが困難だからである。また1200℃以上では
Au、Ag等がセラミツク中に拡散してしまい良好
なシート抵抗が得られなくなるからである。
従来Al2O3にW,Mo等の導体ペーストを用い
た場合は、還元性雰囲気中で同時焼結を行なう必
要があつたが、Ag,Auを用いることができるた
め空気中焼成が可能であり、製造容易、コストの
低下等の効果を得ることもできる。[Table] This is because it is difficult to Also, at temperatures above 1200℃
This is because Au, Ag, etc. will diffuse into the ceramic, making it impossible to obtain good sheet resistance. Conventionally, when conductor pastes such as W and Mo were used for Al 2 O 3 , it was necessary to perform simultaneous sintering in a reducing atmosphere, but since Ag and Au can be used, sintering in air is possible. Therefore, it is possible to obtain effects such as ease of manufacture and reduction in cost.
Claims (1)
SnO2,B2O3,TiO2に換算して BaO 8〜54mol% SnO2 7〜40mol% B2O3 10〜58mol% TiO2 5〜48mol% 含有された酸化物焼結体を絶縁体として用いる
ことを特徴とする回路基板。[Claims] 1. Barium, tin, boron, titanium as BaO,
BaO 8 to 54 mol% SnO 2 7 to 40 mol% B 2 O 3 10 to 58 mol% TiO 2 5 to 48 mol % The contained oxide sintered body is used as an insulator A circuit board characterized by being used as a circuit board.