JPH0487631A - Method for adjusting shape of solid particles - Google Patents
Method for adjusting shape of solid particlesInfo
- Publication number
- JPH0487631A JPH0487631A JP20293590A JP20293590A JPH0487631A JP H0487631 A JPH0487631 A JP H0487631A JP 20293590 A JP20293590 A JP 20293590A JP 20293590 A JP20293590 A JP 20293590A JP H0487631 A JPH0487631 A JP H0487631A
- Authority
- JP
- Japan
- Prior art keywords
- solid particles
- rotating
- shape
- high speed
- circular
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
Description
【発明の詳細な説明】
[産業上の利用分野コ
本発明は、自動車、産業機械、宇宙機器などに使用する
構造部品の成形用原料、溶射、塗装用原料、セメント用
高炉スラグ及び製紙用重質度カルなどからなる固体粒子
の形状調製方法に関するものである。Detailed Description of the Invention [Industrial Fields of Application] The present invention is applicable to raw materials for forming structural parts used in automobiles, industrial machinery, space equipment, etc., raw materials for thermal spraying and coating, blast furnace slag for cement, and heavy duty materials for paper manufacturing. This invention relates to a method for preparing the shape of solid particles made of solid particles.
[従来の技術]
従来の微小固体粒子の球形化処理方法として、特開昭6
2−221434号公報をあげることができる(第7図
参照)。[Prior art] As a conventional method for spheroidizing fine solid particles, Japanese Patent Application Laid-open No. 6
2-221434 (see FIG. 7).
この球形化処理方法は、衝撃式打撃手段を用いて行なう
ようにしたものであり、この衝撃式打撃手段はケーシン
グa内に回転軸すにより高速回転する回転盤Cを設け、
この回転盤Cの外周に多数の衝撃ピンdを設け、前記衝
撃ピンdの最外周軌道面に沿い、かつそれに対して一定
の空間に置いて周設された衝突リングeからなる。This spherical processing method is carried out using an impact type impact means, and this impact type impact means is provided with a rotary disk C that rotates at high speed by a rotating shaft in a casing a,
A large number of impact pins d are provided on the outer periphery of the rotary disk C, and an impact ring e is disposed around the outermost orbital surface of the impact pins d and spaced therefrom.
なお、fは開閉弁、qは衝撃室、hは循環回路である。In addition, f is an on-off valve, q is a shock chamber, and h is a circulation circuit.
そして、開閉弁士を閉じた状態で回転盤Cを回転させる
と、この回転盤Cの回転に伴って気流が生じ、この気流
の遠心力に基づくファン効果によって衝撃室q、循環回
路りを巡って自己循環の流れが形成される。When the turntable C is rotated with the on-off valve closed, an airflow is generated as the turntable C rotates, and a fan effect based on the centrifugal force of this airflow circulates around the shock chamber q and the circulation circuit. A self-circulating flow is formed.
一方、貯槽iに貯溜した微小固体粒子を計量フィーダj
、ホッパkを経て前記衝撃式粉砕機の気流循環サイクル
中に投入する。On the other hand, the fine solid particles stored in storage tank i are transferred to weighing feeder j.
, hopper k and then into the air circulation cycle of the impact crusher.
投入された微小固体粒子は、衝撃ピンdによって打撃作
用を受け、ざらに衝突リングeに衝突して圧縮作用を受
ける。The injected minute solid particles are subjected to a striking action by the impact pin d, and roughly collide with the impact ring e, where they are compressed.
次いで、該微小固体粒子は循環ガスとともに循環回路り
を循環して再び衝撃室qに戻り、再度打撃作用を受ける
。Next, the fine solid particles circulate through the circulation circuit together with the circulating gas and return to the impact chamber q, where they are again subjected to the impact action.
このような衝撃作用が何回も繰り返されるうちに、球形
化される。As this impact action is repeated many times, it becomes spherical.
以上の球形化が終了すると開閉弁fを開き、球形化され
た微小固体粒子(製品)を排出する。When the above spheronization is completed, the on-off valve f is opened and the spheroidized fine solid particles (products) are discharged.
排出された微小固体粒子は、排風機nの吸引力によって
、サイクロンI、パックフィルタmに誘導された後、補
集される。The discharged minute solid particles are guided to the cyclone I and the pack filter m by the suction force of the exhaust fan n, and then collected.
[発明が解決しようとする課題]
しかしながら、前記衝撃式打撃手段の回転lcの周速度
は、機械的強度上からあまり大きくとれない為、微小固
体粒子にその周速度以上の打撃力を加えることができな
い。このため、微小固体粒子(以下固体粒子という)の
球形化度は十分とは言えない。勿論打撃回数を増やせば
ある程度は解決されるか、それだけ時間を要することと
なる。[Problems to be Solved by the Invention] However, the peripheral speed of the rotation lc of the impact-type impacting means cannot be set to be very high due to mechanical strength reasons, so it is difficult to apply impact force higher than the peripheral speed to the fine solid particles. Can not. For this reason, the degree of sphericity of the fine solid particles (hereinafter referred to as solid particles) cannot be said to be sufficient. Of course, increasing the number of hits will solve the problem to some extent, or it will take more time.
また、1つの気流循環サイクルであるため、1回当たり
の処理量が小さい。Moreover, since it is one airflow circulation cycle, the throughput per cycle is small.
本発明は、上記のような従来技術の問題点に鑑みてなさ
れたものであり、固体粒子同志の対向衝突と強力な撹拌
・混合によって著しく形状調製度かつ均質度の高い製品
を得るとともに処理量を著しく向上することができる固
体粒子の形状調製方法を提供することを目的とする。The present invention has been made in view of the problems of the prior art as described above, and uses opposing collisions of solid particles and strong stirring/mixing to obtain products with extremely high degree of shape control and homogeneity, and to increase throughput. An object of the present invention is to provide a method for preparing the shape of solid particles, which can significantly improve the shape of solid particles.
[課題を解決するための手段]
上記目的を達成するために、本発明の固体粒子の形状調
製方法は、2つの円形部が並列した筒状ケーシングの円
部内に、外周に複数個の羽根を具備しかつ同一方向に高
速回転する一対の回転ロータを設けた2軸型高速回転調
製機の上方から供給された固体粒子を、前記回転ロータ
とともに回転する羽根により発生する渦流とともに高速
周回させ、該高速周回の交流部おいて対向衝突及び混合
・撹拌して形状調製したのち、下方から排出するように
したことである。[Means for Solving the Problems] In order to achieve the above object, the solid particle shape preparation method of the present invention includes a method of preparing a solid particle shape by forming a plurality of blades on the outer periphery within a circular part of a cylindrical casing in which two circular parts are arranged in parallel. Solid particles supplied from above a two-shaft high-speed rotation preparation machine equipped with a pair of rotating rotors that rotate at high speed in the same direction are rotated at high speed together with a vortex generated by blades that rotate together with the rotation rotors. After the shape is adjusted by colliding oppositely and mixing and stirring in the high-speed circulating exchange section, the material is discharged from below.
形状調製とは、固体粒子の形状を整えること、すなわち
、立方体又は直方体の固体粒子の角を取ってたまご形又
は近似球形にすること、また、鋭利な突起やあばた状の
くぼみを持った不定形固体粒子の該突起を除去するか折
り曲げ、または、あばた状のくぼみを平滑にすること、
さらに薄片状や円孤形棒状の不定形固体粒子を折り曲げ
て丸まったものにすることをいう。Shape adjustment refers to adjusting the shape of solid particles, that is, cutting the corners of cubic or rectangular solid particles to make them egg-shaped or approximately spherical, or shaping them into irregular shapes with sharp protrusions or pock-like depressions. removing or bending the protrusions or smoothing the pock-like depressions of the solid particles;
Furthermore, it refers to bending flaky or arcuate rod-shaped amorphous solid particles into a round shape.
固体粒子としては、溶射用。粉末冶金用等の金属粉、塗
装用、射出成形用等の高分子材料粉等であり、その粒径
は1ミクロン〜1mの範囲に属するものである。As solid particles, for thermal spraying. These include metal powder for powder metallurgy, etc., and polymer material powder for painting, injection molding, etc., and the particle size thereof is in the range of 1 micron to 1 m.
[作用コ
固体粒子を2軸型高速回転調製機の上方からケーシング
内に投入する。[Operation] Solid particles are introduced into the casing from above the two-shaft high-speed rotation preparation machine.
投入された固体粒子は、同一方向に高速回転する向回転
ロータとともに回転する羽根によって回転ロータの外周
と円形部の間にそれぞれ発生する渦流(循環気流)にそ
れぞれ巻き込まれて高速周回する。そして固体粒子を含
む両渦流は向回転ロタの中央で交わる。この交流部にお
いて、固体粒子同志が激しく対向衝突・摩擦し、この衝
突力によって固体粒子は形状調製されるが、このときの
衝突力はほぼ倍加されるため、固体粒子の形状調製が確
実に行われる。しかも、この交流部では渦流同志の衝突
によって乱流状態となるため、前記固体粒子は強力に撹
拌・混合されることとなり再び固体粒子同志の衝突・摩
擦が起こり、2次的に形状調製される。The injected solid particles are caught in vortices (circulating air currents) generated between the outer periphery of the rotor and the circular portion by the vanes that rotate together with the counter-rotating rotor that rotates in the same direction at high speed, and circulate at high speed. Both vortices containing solid particles intersect at the center of the counterrotating rotor. In this exchange part, the solid particles violently collide and rub against each other, and the shape of the solid particles is adjusted by this collision force, but since the collision force at this time is almost doubled, the shape of the solid particles can be adjusted reliably. be exposed. Moreover, in this exchange section, the collision of the eddy currents creates a turbulent state, so the solid particles are strongly stirred and mixed, causing collision and friction between the solid particles again, resulting in secondary shape adjustment. .
次いで、この交流部で衝突及び撹拌・混合された粒子は
、何れかの回転ロータに巻き込まれ、それぞれの渦流に
乗って一周した後、再び粒子同志の衝突及び撹拌・混合
が行われるのである。Next, the particles collided, stirred, and mixed in this exchange section are drawn into one of the rotating rotors, ride the respective vortices, and go around once, after which the particles collide, stir, and mix again.
このような衝突及び撹拌・混合を一定時間繰り返すこと
により、すべての固体粒子が均等に形状調製されて丸味
を帯びたものとなるのである。By repeating such collision, stirring, and mixing for a certain period of time, all the solid particles are uniformly shaped and become rounded.
そして、形状調製された固体粒子は該調製機の下方から
製品として排出される。The shape-adjusted solid particles are then discharged as a product from the bottom of the preparation machine.
[実施例]
以下、本発明の調製方法に用いる装置の実施例を図面を
参照して説明する。[Example] Hereinafter, an example of an apparatus used in the preparation method of the present invention will be described with reference to the drawings.
第1図〜第2図において、固体粒子をピン1から定量フ
ィーダ2にて切り出し、供給シュート5を経て2軸型高
速回転調製機6に投入する。ここで所定時間処理した後
、製品を排風機9の吸引力により排出シュート7を経て
集塵機8にて捕集し、製品ピン10に貯蔵する。In FIGS. 1 and 2, solid particles are cut out from a pin 1 using a metering feeder 2, and fed into a two-shaft type high-speed rotation preparation machine 6 via a supply chute 5. After processing for a predetermined time, the product is collected by the dust collector 8 through the discharge chute 7 by the suction force of the exhaust fan 9, and stored in the product pin 10.
前記2軸型高速回転調製機6の詳細を述べると、次のよ
うである。The details of the two-shaft type high-speed rotation preparation machine 6 are as follows.
11は筒状ケーシングで、その断面は2つの円形部12
.13が連通する如く並列したひようたん形であり、そ
の中央部の上下にそれぞれ供給口14および排出口15
を設ける。11 is a cylindrical casing, the cross section of which has two circular parts 12
.. 13 are arranged in parallel so as to communicate with each other, and there are a supply port 14 and a discharge port 15 at the top and bottom of the central part, respectively.
will be established.
16.17はそれぞれ円形部12.13に配設した回転
ロータで、外周に複数個の羽根18,19が設けられ、
軸20,21.により高速回転するようになっている。Reference numerals 16 and 17 denote rotating rotors arranged in circular parts 12 and 13, each having a plurality of blades 18 and 19 on the outer periphery.
Shafts 20, 21. This allows it to rotate at high speed.
22は円形部12.13と回転ロータ16.17の間の
隙間である。22 is a gap between the circular portion 12.13 and the rotating rotor 16.17.
23は供給口14を塞ぐ着脱自在の上栓体で、この上栓
体に円形部12.13に突出する内向きの凸部32aを
形成する。凸部23aは両側部が円形部12.13の円
弧と同一円弧面24.25であり、頂部が平面26であ
る。Reference numeral 23 denotes a removable upper plug that closes the supply port 14, and an inward convex portion 32a that projects from the circular portion 12.13 is formed on this upper plug. The convex portion 23a has arc surfaces 24.25 on both sides that are the same as the arc of the circular portion 12.13, and a flat surface 26 on the top.
このようにしてなる上栓体23は、供給シート5の壁の
後方を利用して固定し、着脱するようになっている。The upper plug body 23 formed in this manner is fixed using the rear part of the wall of the supply sheet 5, and is adapted to be attached and detached.
27は排出口15を塞ぐ着脱自在の下栓体で、この下栓
体に円形部12.13内に突出する内向きの凸部27a
を形成する。凸部27aは前記上栓体23と同様に両側
部が円形部12.13の円弧と同一円弧面28.29で
あり、頂部が平面30である。Reference numeral 27 denotes a removable lower plug that closes the outlet 15, and the lower plug has an inward convex portion 27a that projects into the circular portion 12.13.
form. Like the upper stopper body 23, the convex portion 27a has arcuate surfaces 28, 29 on both sides that are the same as the arc of the circular portion 12, 13, and has a flat surface 30 at the top.
このようにしてなる下栓体27は、該下栓体に固定した
レバー31をケーシング11に固定したブラケット32
にピン33を介して支承され、該ピン33を支点として
回動するようになっている。The lower plug body 27 constructed in this way has a lever 31 fixed to the lower plug body and a bracket 32 fixed to the casing 11.
It is supported through a pin 33 and rotates about the pin 33 as a fulcrum.
34は加熱又は冷却ジャケットであり、必要により設け
ることかできる。34 is a heating or cooling jacket, which may be provided if necessary.
次に実施例の作用を説明する。Next, the operation of the embodiment will be explained.
下栓体27を閉じたまま、上栓体23を取り出して供給
口14を開く(第3図参照)。While the lower plug body 27 is kept closed, the upper plug body 23 is taken out and the supply port 14 is opened (see FIG. 3).
この状態から、前記した如く固体粒子を供給口14を経
て一定量ケーシング11内に投入した後、上栓体23を
嵌めて供給口14を閉じる。 次いで、両回転ロータ1
6,17を同一方向に高速回転させる。From this state, after a certain amount of solid particles are introduced into the casing 11 through the supply port 14 as described above, the upper stopper 23 is fitted to close the supply port 14. Next, the double rotating rotor 1
6 and 17 are rotated at high speed in the same direction.
この回転ロータ16,17とともに回転する羽根18.
19によって回転ロータ16の外周と円形部12の間に
第1渦流35及び回転ロータ17の外周と円形部13の
間に第2渦流36が発生する。A blade 18 that rotates together with the rotating rotors 16 and 17.
19, a first vortex 35 is generated between the outer periphery of the rotating rotor 16 and the circular portion 12, and a second vortex 36 is generated between the outer periphery of the rotating rotor 17 and the circular portion 13.
両渦流35.36の発生とともに、投入された固体粒子
は前記両渦流に別れて巻き込まれて高速周回し、両回転
ロータ16,17の中央で交わり、この交流部37にお
いて、固体粒子同志が激しく対向衡突・摩擦する。すな
わち、このときの衝突力はほぼ倍加されるため、固体粒
子は確実に形状調製されるとともに、交流部37では渦
流同志の衝突によって乱流状態となるため、前記固体粒
子は強力に撹拌・混合されることとなって、固体粒子同
志の摩擦か起こり形状調製がさらに促道される。With the generation of the two vortices 35 and 36, the injected solid particles are separated into the two vortices and rotated at high speed, intersecting at the center of both rotating rotors 16 and 17, and in this alternating current section 37, the solid particles violently interact with each other. Opposite collision/friction. That is, since the collision force at this time is almost doubled, the shape of the solid particles is reliably adjusted, and in the alternating current section 37, the vortices collide with each other to create a turbulent flow state, so the solid particles are strongly agitated and mixed. This causes friction between the solid particles and further facilitates shape adjustment.
次いで、この交流部37で衝突及び撹拌・混合された固
体粒子は、第1渦流35から第2渦流36へ、また第2
渦流36から第1渦流35へと巻き込まれ、それぞれの
渦流35.36にのって一周した後、再び固体粒子同志
の衝突及び撹拌・混合が行われるのである。Next, the solid particles collided, stirred, and mixed in this exchange section 37 are transferred from the first vortex 35 to the second vortex 36, and then to the second vortex 36.
After being drawn into the first vortex 35 from the vortex 36 and going around once on each vortex 35, 36, the solid particles collide with each other and are stirred and mixed again.
このような衝突及び撹拌・混合を繰り返すことによって
、すべての固体粒子が均等に衝突・摩擦作用を受けて形
状調製され均質なものとなるのである。By repeating such collisions, stirring, and mixing, all solid particles are uniformly subjected to collisions and frictional effects, and their shapes are adjusted and become homogeneous.
τ定時間処理して固体粒子の形状調製が終わると、下栓
体27を回動して排出口15を開くとともに回転ロータ
16,17を逆方向に低速回転させて製品を排出する(
第4図参照)。これで−回の形状調製を終える。When the shape of the solid particles has been adjusted by processing for a certain period of time, the lower stopper 27 is rotated to open the discharge port 15, and the rotors 16 and 17 are rotated at low speed in the opposite direction to discharge the product (
(See Figure 4). This completes the -th round of shape preparation.
なお、前記実施例では、両回転ロータ16,17の直径
を同一としたが、例えば回転ロータ16の直径に対して
回転ロータ17のそれを小径とするとともに、該回転ロ
ータ17の回転数を増速することにより、固体粒子の保
有空間が広くなり、これによって1回当りの処理量を大
きくすることができる。In the embodiment described above, both the rotors 16 and 17 have the same diameter, but for example, the diameter of the rotor 17 is made smaller than that of the rotor 16, and the rotation speed of the rotor 17 is increased. By increasing the speed, the holding space for solid particles becomes wider, and thereby the throughput per one time can be increased.
第5図は他の実施例を示し、上栓体23の凸部23aの
円弧面25及び下栓体27の凸部27aの円弧面28を
斜めに切り落として切落部38゜39を形成したもので
ある。FIG. 5 shows another embodiment in which the arcuate surface 25 of the convex portion 23a of the upper plug body 23 and the circular arcuate surface 28 of the convex portion 27a of the lower plug body 27 are cut off diagonally to form cut portions 38° and 39. It is something.
これによって交流部37の空間が広くなり、それだけ粒
子の撹拌・混合効果が増すとともに固体粒子の衝突点が
偏よることから、渦流への固体粒子の巻き込みが確実に
行われる。この場合、切落部38.39と回転ロータ1
6,17の回転方向は図示に限定されるものではなく、
逆回転させてもよい。As a result, the space in the exchange section 37 becomes wider, which increases the effect of stirring and mixing the particles, and the collision points of the solid particles are shifted, so that the solid particles are reliably drawn into the vortex. In this case, the cutout portion 38, 39 and the rotating rotor 1
The rotation directions of 6 and 17 are not limited to those shown in the drawings,
It may also be rotated in the opposite direction.
さらに、第6図は他の実施例を示し、この場合、上栓体
23の凸部23aの円弧面24.25を斜めに切り落し
て直線面40.41となし、両面により略V字形とした
ものである。同様に、下栓体27の凸部27aの円弧面
28.29を切り落して直線面42.43となし、両面
により略V字形としたものである。この場合も交流部3
7の空間がさらに広くなる。Further, FIG. 6 shows another embodiment, in which the arcuate surface 24.25 of the convex portion 23a of the upper plug body 23 is cut off diagonally to form a straight surface 40.41, and both surfaces form a substantially V-shape. It is something. Similarly, the arcuate surfaces 28, 29 of the convex portion 27a of the lower plug body 27 are cut off to form linear surfaces 42, 43, and both surfaces form a substantially V-shape. In this case as well, AC section 3
7 space becomes even wider.
なお、前記溶射(プラズマ)用金属粉の場合、流動性が
よくなるので、溶射しやすくなる。また、粉末冶金用金
属粉の場合、最適の嵩比重にコントロールすることがで
きる。また、粉体塗装用高分子粒子の場合、流動性がよ
くなるので、均一な厚さの塗装が可能となる。さらに、
割出成形用高分子粒子の場合、流動性がよくなるので、
他の添加材料との均一な混合が得られる。In addition, in the case of the metal powder for thermal spraying (plasma), the fluidity is improved, making thermal spraying easier. Moreover, in the case of metal powder for powder metallurgy, bulk specific gravity can be controlled to an optimum value. In addition, in the case of powder coating polymer particles, the fluidity is improved, making it possible to coat with a uniform thickness. moreover,
In the case of polymer particles for index molding, fluidity is improved, so
Uniform mixing with other additive materials is obtained.
[発明の効果]
本発明は、以上のように構成されるので、以下に記載さ
れるような効果を奏する。[Effects of the Invention] Since the present invention is configured as described above, it produces the following effects.
2つの円形部が並列した筒状ケーシングの円部内に、外
周に複数個の羽根を具備しかつ同一方向に高速回転する
一対の回転ロータを設けた2軸型高速回転調製機の上方
から供給された固体粒子を、前記回転ロータとともに回
転する羽根により発生する渦流とともに高速周回させ、
該高速周回の交流部おいて対向衝突及び混合・撹拌して
形状調製したのち、下方から排出するようにしたから、
固体粒子は確実に形状調製されるとともに該交流部にお
ける強力な撹拌・混合作用による形状調製が促進される
こととなって、著しく丸味を帯びた、しかも均質度の高
い製品を得ることができ、かつ1回当たりの処理量も大
巾に増大する。The oil is supplied from above to a two-shaft high-speed rotation adjusting machine, which has a pair of rotating rotors equipped with a plurality of blades on the outer periphery and rotating at high speed in the same direction in a circular part of a cylindrical casing in which two circular parts are arranged in parallel. rotating the solid particles at high speed with a vortex generated by blades rotating together with the rotating rotor,
After the shape is adjusted by opposing collisions and mixing and stirring in the high-speed circulating exchange section, the material is discharged from below.
The shape of the solid particles is reliably adjusted, and the shape adjustment is promoted by the strong stirring and mixing action in the exchange section, making it possible to obtain a product that is extremely round and highly homogeneous. In addition, the amount of processing per process also increases significantly.
また、粒子同志の衝突により調製するものであるから、
調製機は従来のものに比べて、磨耗が極めて少なく長寿
命となる。In addition, since it is prepared by collision of particles,
Compared to conventional machines, the preparation machine has significantly less wear and has a longer lifespan.
第1図は本発明の固体粒子の調製方法の一実施例に係る
調製装置を示す全体概略図、第2図は同実施例に係る調
製機を示す縦断面図、第3図は同実施例に係る調製機へ
の投入状態を示す縦断面図、第4図は同実施例に係る調
製機からの排出状態を示す縦断面図、第5図〜第6図は
本発明の他の実施例に係る調製機の縦断面図、第7図は
従来例を示¥概略図である。
6・・・・・・2軸型高速回転調製機FIG. 1 is an overall schematic diagram showing a preparation apparatus according to an embodiment of the method for preparing solid particles of the present invention, FIG. 2 is a longitudinal sectional view showing a preparation machine according to the same embodiment, and FIG. FIG. 4 is a vertical cross-sectional view showing the state of discharging from the preparation machine according to the same embodiment, and FIGS. 5 to 6 are other embodiments of the present invention. FIG. 7 is a schematic diagram showing a conventional example. 6...2-shaft high-speed rotation preparation machine
Claims (1)
に、外周に複数個の羽根を具備しかつ同一方向に高速回
転する一対の回転ロータを設けた2軸型高速回転調製機
の上方から供給された固体粒子を、前記回転ロータとと
もに回転する羽根により発生する渦流とともに高速周回
させ、該高速周回の交流部おいて対向衝突及び混合・撹
拌して形状調製したのち、下方から排出するようにした
ことを特徴とする固体粒子の形状調製方法。(1) Above the two-shaft high-speed rotation adjusting machine, which has a pair of rotating rotors that have multiple blades on the outer periphery and rotate at high speed in the same direction, inside a circular part of a cylindrical casing in which two circular parts are arranged in parallel. The solid particles supplied from the rotating rotor are made to circulate at high speed along with the vortex generated by the blades rotating together with the rotating rotor, and are collided with each other in the alternating current part of the high-speed circulation, and are mixed and stirred to adjust their shape, and then are discharged from below. A method for preparing the shape of solid particles, characterized in that: