JPH0688024A - Polyarylene sulfide resin composition - Google Patents

Polyarylene sulfide resin composition

Info

Publication number
JPH0688024A
JPH0688024A JP15427892A JP15427892A JPH0688024A JP H0688024 A JPH0688024 A JP H0688024A JP 15427892 A JP15427892 A JP 15427892A JP 15427892 A JP15427892 A JP 15427892A JP H0688024 A JPH0688024 A JP H0688024A
Authority
JP
Japan
Prior art keywords
pas
amino group
olefin elastomer
formula
group
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP15427892A
Other languages
Japanese (ja)
Inventor
Naohiro Mikawa
直浩 三川
Satoshi Inoue
井上  敏
Ichigen Watanabe
一玄 渡辺
Tadao Ikeda
忠生 池田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tonen General Sekiyu KK
Original Assignee
Tonen Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tonen Corp filed Critical Tonen Corp
Priority to JP15427892A priority Critical patent/JPH0688024A/en
Publication of JPH0688024A publication Critical patent/JPH0688024A/en
Pending legal-status Critical Current

Abstract

(57)【要約】 【構成】 (A)オレフィン系エラストマーに次式
(1): 【化1】 (式中、RはHまたは炭素数1〜6のアルキル基であ
り、Arは少くとも一つのグリシジルオキシ基を有する
炭素数6〜20の芳香族炭化水素基であり、mは1〜4
の整数を表す)で表されるグリシジル化合物をグラフト
した変性オレフィン系エラストマーと(B)側鎖にアミ
ノ基をもつポリアリーレンサルファイドとからなる樹脂
組成物。 【効果】 ポリアリーレンサルファイドの特性である良
好な耐熱性、機械的強度などを維持したまま、耐衝撃性
が著しく向上した成形品が得られる。
(57) [Summary] [Structure] (A) The following formula (1) for the olefin elastomer: (In the formula, R is H or an alkyl group having 1 to 6 carbon atoms, Ar is an aromatic hydrocarbon group having 6 to 20 carbon atoms having at least one glycidyloxy group, and m is 1 to 4
The modified olefin elastomer grafted with a glycidyl compound represented by the formula (4) and (B) a polyarylene sulfide having an amino group in the side chain. [Effect] A molded article having remarkably improved impact resistance can be obtained while maintaining good heat resistance and mechanical strength, which are the characteristics of polyarylene sulfide.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は、ポリアリーレンサルフ
ァイド樹脂組成物に関する。さらに詳しくは、耐衝撃性
その他の機械的物性に優れていて、構造材料用または機
械部品などとして有用な、変性オレフィン系ポリマーを
含むポリアリーレンサルファイド樹脂組成物に関する。
FIELD OF THE INVENTION The present invention relates to a polyarylene sulfide resin composition. More specifically, it relates to a polyarylene sulfide resin composition containing a modified olefin polymer, which is excellent in impact resistance and other mechanical properties and is useful as a structural material or a mechanical part.

【0002】[0002]

【従来の技術】ポリフェニレンサルファイド(以下、
「PPS」という)によって代表されるポリアリーレン
サルファイド(以下、「PAS」という)は、他の汎用
エンジニアリングプラスチックと比較して高い耐熱性、
耐薬品性、剛性を有しているが、耐衝撃性に劣るという
欠点がある。従って、構造材料用および機械部品として
使用するにはガラス繊維などの補強材を多量に添加しな
ければならない。
2. Description of the Related Art Polyphenylene sulfide (hereinafter referred to as
Polyarylene sulfide (hereinafter referred to as "PAS") represented by "PPS" has higher heat resistance than other general-purpose engineering plastics,
It has chemical resistance and rigidity, but has the drawback of poor impact resistance. Therefore, a large amount of reinforcing material such as glass fiber must be added for use as a structural material and as a mechanical part.

【0003】一般に、耐衝撃性に劣る樹脂の耐衝撃性を
改良する目的でエラストマーを添加してアロイ化する手
法が採られているが、PASの場合多くのエラストマー
との相溶性が高くないため、エラストマーによるアロイ
化は不十分である。PASの耐衝撃性その他の特性を改
善する目的で、PASにα−オレフィン−グリシジルメ
タクリレート共重合体をブレンドすることが提案されて
いる(特開昭61−21156号)が、PAS本来の優
れた特性を損うことなく、耐衝撃性を大巾に改良するこ
とは困難である。
Generally, a method of adding an elastomer to form an alloy for the purpose of improving the impact resistance of a resin having poor impact resistance is used, but in the case of PAS, compatibility with many elastomers is not high. , Alloying with elastomer is insufficient. For the purpose of improving impact resistance and other properties of PAS, it has been proposed to blend PAS with an α-olefin-glycidyl methacrylate copolymer (Japanese Patent Laid-Open No. 61-21156). It is difficult to greatly improve the impact resistance without impairing the properties.

【0004】[0004]

【発明が解決しようとする課題】本発明の目的は、PA
S本来の良好な耐熱性、機械的強度などを維持したま
ま、耐衝撃性が著しく改良されたPAS樹脂組成物を提
供することにある。
The object of the present invention is to provide a PA
An object of the present invention is to provide a PAS resin composition in which impact resistance is remarkably improved while maintaining the original good heat resistance and mechanical strength of S.

【0005】[0005]

【課題を解決するための手段】上記の目的は、側鎖にア
ミノ基をもつPASに、高い相溶性を示す特定の変性オ
レフィン系エラストマーを配合することによって達成さ
れる。すなわち、本発明は、(A)オレフィン系エラス
トマーに次の一般式(1):
The above object can be achieved by blending PAS having an amino group in its side chain with a specific modified olefin elastomer exhibiting high compatibility. That is, the present invention provides the olefin elastomer (A) with the following general formula (1):

【化2】 (式中、RはHまたは炭素数1〜6のアルキル基であ
り、Arは少くとも一つのグリシジルオキシ基を有する
炭素数6〜20の芳香族炭化水素基であり、mは1〜4
の整数を表す)で表されるグリシジル化合物をグラフト
した変性オレフィン系エラストマーと(B)側鎖にアミ
ノ基をもつPASとからなることを特徴とする、変性オ
レフィン系エラストマーを含むポリアリーレンサルファ
イド樹脂組成物を提供する。
[Chemical 2] (In the formula, R is H or an alkyl group having 1 to 6 carbon atoms, Ar is an aromatic hydrocarbon group having 6 to 20 carbon atoms having at least one glycidyloxy group, and m is 1 to 4
A modified olefin-based elastomer grafted with a glycidyl compound represented by the formula (1) and a PAS having an amino group in the side chain (B), a polyarylene sulfide resin composition containing a modified olefin-based elastomer. Provide things.

【0006】本発明のPAS樹脂組成物の調製に使用す
る側鎖にアミノ基をもつPASは、その骨格が次の式
(2)で表されるアリーレンサルファイド結合、または
該アリーレンサルファイド結合(2)を主成分とし、
The PAS having an amino group in the side chain used for preparing the PAS resin composition of the present invention has an skeleton of an arylene sulfide bond represented by the following formula (2), or the arylene sulfide bond (2). As the main component,

【0007】[0007]

【化3】 次の式(3)で示されるエーテル結合、次の式(4)で
示されるスルホン結合、次の式(5)で示されるビフェ
ニル結合、次の式(6)で示される置換フェニルスルフ
ィド結合(但し、式(6)中、R1 はアルキル、ニト
ロ、フェニル、アルコキシ、カルボキシル基を示
す。)、次の式(7)で示される3官能結合で例示され
るような共重合成分から導かれる結合を劣成分として含
有した結合からなり、かつその側鎖にアミノ基が結合し
た構造からなる。但し、当該共重合成分は、30モル%
未満であることが好ましい。
[Chemical 3] An ether bond represented by the following formula (3), a sulfone bond represented by the following formula (4), a biphenyl bond represented by the following formula (5), a substituted phenyl sulfide bond represented by the following formula (6) ( However, in the formula (6), R 1 represents an alkyl, nitro, phenyl, alkoxy, or carboxyl group.), And is derived from a copolymerization component exemplified by the trifunctional bond represented by the following formula (7). It is composed of a bond containing a bond as an inferior component, and has a structure in which an amino group is bonded to its side chain. However, the copolymerization component is 30 mol%
It is preferably less than.

【0008】[0008]

【化4】 本発明の組成物においては、側鎖にアミノ基をもつPA
Sは次の(a)成分と(b)成分とを反応させることに
より合成することができる。 (a)アルカリ金属サルファイド(代表的には硫化ソー
ダ) (b)アミノ基を置換基として有するハロゲン化物 上記において、原料として使用されるアミノ基を置換基
として有するハロゲン化物の例としては、次式で示され
るハロゲン化アミノベンゼンが挙げられる。
[Chemical 4] In the composition of the present invention, PA having an amino group in the side chain is used.
S can be synthesized by reacting the following components (a) and (b). (A) Alkali metal sulfide (typically sodium sulfide) (b) Halide having an amino group as a substituent In the above, an example of a halide having an amino group as a substituent used as a raw material is represented by the following formula: And a halogenated aminobenzene represented by

【化7】 (式中、R2 およびnは前述したものと同一意義を有
し、R2 は水素原子または炭素原子1〜3個のアルキル
基を示し、Yはハロゲン原子を示し、mは1または2を
示す)
[Chemical 7] (In the formula, R 2 and n have the same meanings as described above, R 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, Y represents a halogen atom, and m represents 1 or 2. Show)

【0009】かかるハロゲン化アミノベンゼンの具体例
としては、下記の式で示されるハロゲン化アミノベンゼ
ン化合物が挙げられる。但し、これらの式において、Y
1 の例としては、C1またはBrが挙げられる。
Specific examples of such halogenated aminobenzene include halogenated aminobenzene compounds represented by the following formula. However, in these equations, Y
Examples of 1 include C1 or Br.

【0010】[0010]

【化8】 [Chemical 8]

【0011】本発明の樹脂組成物における(B)成分は
側鎖にアミノ基をもつPASからなるが、(B)成分が
該アミノ基をもつPASのみからなる場合、樹脂組成物
がPAS本来の性質を発現できない場合があるので、ア
ミノ基をもたないPASを併用することが好ましい。
(B)成分には、PAS側鎖に結合したアミノ基が0.
03モル%以上、好ましくは0.1〜25モル%含まれ
るべきである。該アミノ基含有量が0.03モル%未満
では(A)成分の変性オレフィン系エラストマーとの高
い相溶性が得られず、耐衝撃性その他の機械的性質に優
れた成形品を得ることが困難となる。
The component (B) in the resin composition of the present invention is composed of PAS having an amino group in the side chain. When the component (B) is composed only of PAS having the amino group, the resin composition is the original PAS. Since the properties may not be expressed in some cases, it is preferable to use PAS having no amino group together.
In the component (B), an amino group bonded to the PAS side chain is 0.
It should be contained in an amount of at least 03 mol%, preferably 0.1 to 25 mol%. When the amino group content is less than 0.03 mol%, high compatibility with the modified olefin elastomer of component (A) cannot be obtained, and it is difficult to obtain a molded article excellent in impact resistance and other mechanical properties. Becomes

【0012】上記において、アミノ基をもたないPAS
を併用する方法としては、(1)側鎖にアミノ基をもつ
PASとアミノ基をもたないPASを混合して用いる方
法、(2)側鎖にアミノ基をもつPASを製造する上記
の方法において、(b)成分のアミノ基を置換基として
有するハロゲン化物にジハロゲン化物を混合した混合体
を用いて得られるPASを用いる方法が採用され得る。
もちろん、上記(2)の方法によって得られるPAS
に、さらにアミノ基をもたないPASを混合することも
可能である。
In the above, PAS having no amino group
As a method of using in combination, (1) a method in which PAS having an amino group in the side chain and PAS having no amino group are mixed and used, and (2) the above method for producing a PAS having an amino group in the side chain. In the above, a method using PAS obtained by using a mixture obtained by mixing a dihalide with a halide of the component (b) as a substituent can be adopted.
Of course, the PAS obtained by the method (2) above
Further, it is also possible to mix PAS having no amino group.

【0013】アミノ基をもたないPASおよび側鎖にア
ミノ基をもつPASは、いずれも、前記のように式
(2)で表わされる結合、またはこの結合を主成分と
し、前記式(3)〜(7)のいずれかで例示されるよう
な結合を劣成分として含む基本骨格をもつ構造であれば
よい。アミノ基をもたないPASは、(a)アルカリ金
属サルファイド(代表的には硫化ソーダ)と(c)ジハ
ロゲン化物とを反応させることにより合成することがで
きる。ここで、原料として使用されるジハロゲン化物の
例としては、下記の式で示されるジハロゲン化ベンゼン
が挙げられる。
Both the PAS having no amino group and the PAS having an amino group in its side chain have the bond represented by the formula (2) as described above, or the bond represented by the formula (3) as a main component. Any structure having a basic skeleton containing a bond as exemplified by any one of to (7) as a poor component may be used. PAS having no amino group can be synthesized by reacting (a) an alkali metal sulfide (typically sodium sulfide) with (c) a dihalide. Here, examples of the dihalide used as a raw material include dihalogenated benzene represented by the following formula.

【0014】[0014]

【化5】 (式中R2 は炭素原子1〜3個のアルキルもしくはアル
コキシ基を示し、nは0〜3の整数を示し、Xはハロゲ
ン原子を示す)。
[Chemical 5] (In the formula, R 2 represents an alkyl or alkoxy group having 1 to 3 carbon atoms, n represents an integer of 0 to 3, and X represents a halogen atom).

【0015】かかるジハロゲン化ベンゼンの具体例とし
ては、次の式で示される化合物が挙げられる。但し、こ
れらの式において、X1 はハロゲン原子であって、その
例としてClまたはBrが挙げられる。
Specific examples of such dihalogenated benzene include compounds represented by the following formula. However, in these formulas, X 1 is a halogen atom, and examples thereof include Cl or Br.

【0016】[0016]

【化6】 [Chemical 6]

【0017】また、前記アミノ基をもたないPASを併
用する場合の(2)の方法において、ジハロゲン化物
(c)とアミノ基を置換基として有するハロゲン化物
(b)の混合体中のジハロゲン化物(c)とアミノ基を
置換基として有するハロゲン化物(b)との割合は格別
限定されるものではないが、変性オレフィン系エラスト
マーとの相溶性の向上という見地から、該混合体中に
(b)が0.2〜25モル%含まれることが望ましい。
また、この混合体中に2つのハロゲンがパラ位にある化
合物(bおよびc)が85モル%以上含まれることが好
ましい。
Further, in the method (2) in the case of using the PAS having no amino group in combination, the dihalide in the mixture of the dihalide (c) and the halide (b) having an amino group as a substituent is used. The ratio of (c) and the halide (b) having an amino group as a substituent is not particularly limited, but from the viewpoint of improving the compatibility with the modified olefin elastomer, (b) is added to the mixture. ) Is preferably contained in an amount of 0.2 to 25 mol%.
Further, it is preferable that the compound (b and c) having two halogens in the para position is contained in this mixture in an amount of 85 mol% or more.

【0018】アルカリ金属サルファイドと、ジハロゲン
化物、またはジハロゲン化物とアミノ置換基含有ハロゲ
ン化物との混合体との反応に際して、必要に応じて、ジ
ハロゲン化物に対し5モル%以下の範囲内で、トリクロ
ルベンゼンなどのトリハロゲン化物を反応系に添加して
もよい。
In the reaction of an alkali metal sulfide with a dihalide or a mixture of a dihalide and an amino substituent-containing halide, trichlorobenzene may be added, if necessary, within a range of 5 mol% or less based on the dihalide. Trihalides such as may be added to the reaction system.

【0019】重合反応は、極性溶媒中で、好ましくは、
N−メチル−2−ピロリドン(NMP)、ジメチルアセ
トアミドなどのアミド系溶媒やスルホランなどのスルホ
ン系溶媒中で行なうとよい。この際に、重合度を調節す
るために、カルボン酸やスルホン酸のアルカリ金属塩、
水酸化アルカリなどを添加するのが望ましい。好ましい
重合反応の温度および時間は、およそ120〜300℃
で2〜10時間である。反応は不活性ガスの雰囲気下に
行なうのが望ましい。反応終了後、固体生成物をろ別
し、脱イオン水で十分洗浄、乾燥して側鎖にアミノ基を
もつ、または、もたないPASが得られる。
The polymerization reaction is carried out in a polar solvent, preferably
It may be carried out in an amide solvent such as N-methyl-2-pyrrolidone (NMP) or dimethylacetamide or a sulfone solvent such as sulfolane. At this time, in order to adjust the degree of polymerization, an alkali metal salt of carboxylic acid or sulfonic acid,
It is desirable to add alkali hydroxide or the like. The preferable temperature and time of the polymerization reaction are about 120 to 300 ° C.
It takes 2 to 10 hours. It is desirable to carry out the reaction in an inert gas atmosphere. After the completion of the reaction, the solid product is separated by filtration, thoroughly washed with deionized water and dried to obtain PAS having or not having an amino group in the side chain.

【0020】アミノ基をもたないPASは重合後酸素雰
囲気において加熱することにより、あるいは過酸化物な
どの架橋剤を添加して加熱することにより架橋して、よ
り高分子量化したうえ使用することも可能である。本発
明で使用するアミノ基をもたないPASは上記のように
種々のタイプのものが広く使用可能であるが、脱イオン
処理して得たナトリウム含有量が900ppm以下、特
に500ppm以下のPASを用いるのが好ましい。脱
イオン処理としては酸処理が挙げられる。
PAS having no amino group should be crosslinked by heating in an oxygen atmosphere after polymerization, or by adding a crosslinking agent such as peroxide to heat to make it higher molecular weight before use. Is also possible. As the PAS having no amino group used in the present invention, various types of PAS can be widely used as described above, but PAS having a sodium content of 900 ppm or less, particularly 500 ppm or less obtained by deionization treatment can be used. It is preferably used. Examples of the deionization treatment include acid treatment.

【0021】酸処理の代表的な方法は、酸またはその水
溶液にアミノ基をもたないPASを浸漬せしめる方法で
ある。酸処理に際し、適宜撹拌または加熱することも可
能である。酸処理方法の具体例としては、pH4の酢酸
水溶液にPAS粉末を浸漬し、約30分間撹拌する方法
が挙げられる。酸処理を施されたPASは残留している
酸または塩を除去するため、水または温水で数回洗浄す
ることが必要である。洗浄に用いる水は、酸処理による
変性効果を損わぬよう蒸留水または脱イオン水であるこ
とが好ましい。酸処理に用いる酸は、アミノ基をもつ、
または、もたないPASを分解する作用を有しないもの
であれば特に制限はなく、その具体例としては酢酸、塩
酸、硫酸、リン酸、珪酸、炭酸、プロピオン酸が挙げら
れる。なかでも、酢酸および塩酸が好ましく、また、硝
酸はPASを分解劣化させるので好ましくない。
A typical method of acid treatment is to immerse PAS having no amino group in an acid or an aqueous solution thereof. It is also possible to appropriately stir or heat the acid treatment. A specific example of the acid treatment method is a method in which the PAS powder is immersed in an acetic acid aqueous solution having a pH of 4 and stirred for about 30 minutes. The acid-treated PAS needs to be washed several times with water or warm water to remove residual acid or salt. The water used for washing is preferably distilled water or deionized water so as not to impair the denaturing effect of the acid treatment. The acid used for the acid treatment has an amino group,
Alternatively, it is not particularly limited as long as it does not have the action of decomposing undesired PAS, and specific examples thereof include acetic acid, hydrochloric acid, sulfuric acid, phosphoric acid, silicic acid, carbonic acid, and propionic acid. Of these, acetic acid and hydrochloric acid are preferable, and nitric acid is not preferable because it decomposes and deteriorates PAS.

【0022】本発明において使用する変性オレフィン系
エラストマーとは、(i)オレフィン系エラストマー
を、(ii)アクリルアミド基とエポキシ基とを有する特
定のグリシジル化合物により変性してなるものである。
上記(i)オレフィン系エラストマーとは、エチレン
と、プロピレン、1−ブテン、1−ヘキセン、4−メチ
ル−1−ペンテンなどのエチレン以外のα−オレフィン
の1種または2種以上との共重合体ゴムを意味する。上
記エチレンとエチレン以外のα−オレフィンの1種また
は2種以上との共重合体ゴムとしては、典型的にはエチ
レン−ブテン共重合体ゴム(EBR)、エチレン−プロ
ピレン共重合体ゴム(EPR)およびエチレン−プロピ
レン−ジエン共重合体ゴム(EPDM)などが挙げられ
る。エチレン−プロピレン−ジエン共重合体(EPD
M)中のジエンとしては、ジシクロペンタジエン、1,
4−ヘキサジエン、シクロオクタジエン、メチレンノル
ボルネンなどの非共役ジエンまたはブタジエン、イソプ
レンなどの共役ジエンを使用することができる。
The modified olefin elastomer used in the present invention is obtained by modifying (i) an olefin elastomer with (ii) a specific glycidyl compound having an acrylamide group and an epoxy group.
The above (i) olefin elastomer is a copolymer of ethylene and one or more α-olefins other than ethylene such as propylene, 1-butene, 1-hexene, and 4-methyl-1-pentene. Means rubber. The copolymer rubber of ethylene and one or more kinds of α-olefins other than ethylene is typically ethylene-butene copolymer rubber (EBR), ethylene-propylene copolymer rubber (EPR). And ethylene-propylene-diene copolymer rubber (EPDM). Ethylene-propylene-diene copolymer (EPD
The diene in M) is dicyclopentadiene, 1,
Non-conjugated dienes such as 4-hexadiene, cyclooctadiene, methylene norbornene or conjugated dienes such as butadiene and isoprene can be used.

【0023】上記オレフィン系エラストマー中のエチレ
ンの含有量は、概して5〜95重量%であり、好ましく
は10〜90重量%である。エチレンの含有量が5重量
%未満、あるいは95重量%を超えると、エラストマー
としての性質の発現が困難となる。このようなオレフィ
ン系エラストマーの結晶化度は、通常40重量%以下で
ある。
The content of ethylene in the above olefin elastomer is generally 5 to 95% by weight, preferably 10 to 90% by weight. If the ethylene content is less than 5% by weight or more than 95% by weight, it becomes difficult to exhibit properties as an elastomer. The crystallinity of such an olefin elastomer is usually 40% by weight or less.

【0024】本発明において使用するオレフィン系エラ
ストマーの代表的一例であるエチレン−プロピレン共重
合体ゴム(EPR)は、エチレンから誘導される繰り返
し単位の含有率が50〜80モル%、プロピレンから誘
導される繰り返し単位の含有率が20〜50モル%であ
ることが好ましい。より好ましい範囲は、エチレン系繰
り返し単位が60〜70モル%、プロピレン系繰り返し
単位が30〜40モル%である。また、EPRのメルト
フローレート(MFR、230℃、2.16kg荷重)
は0.01〜50g/10分の範囲内にあるのが好まし
く、より好ましくは0.5〜30g/10分である。
The ethylene-propylene copolymer rubber (EPR), which is a typical example of the olefin elastomer used in the present invention, has a content of repeating units derived from ethylene of 50 to 80 mol% and is derived from propylene. The content of the repeating unit is preferably 20 to 50 mol%. A more preferable range is 60 to 70 mol% of ethylene-based repeating units and 30 to 40 mol% of propylene-based repeating units. Also, EPR melt flow rate (MFR, 230 ° C, 2.16 kg load)
Is preferably in the range of 0.01 to 50 g / 10 minutes, more preferably 0.5 to 30 g / 10 minutes.

【0025】オレフィン系エラストマーの他の代表的一
例であるエチレン−ブテン共重合体ゴム(EBR)は、
エチレンから誘導される繰り返し単位の含有率が50〜
90モル%、ブテンから誘導される繰り返し単位の含有
率が10〜50モル%であることが好ましい。より好ま
しい範囲は、エチレン系繰り返し単位が60〜80モル
%、ブテン系繰り返し単位が20〜40モル%である。
また、EBRのメルトフローレート(MFR、230
℃、2.16kg荷重)は0.01〜50g/10分の
範囲内にあるのが好ましく、より好ましくは0.5〜3
0g/10分である。
Ethylene-butene copolymer rubber (EBR), which is another typical example of the olefin elastomer, is
The content of repeating units derived from ethylene is 50-
It is preferable that the content of the repeating unit derived from butene is 90 mol% and the content thereof is 10 to 50 mol%. A more preferable range is 60 to 80 mol% of ethylene-based repeating units and 20 to 40 mol% of butene-based repeating units.
In addition, the EBR melt flow rate (MFR, 230
(° C, 2.16 kg load) is preferably in the range of 0.01 to 50 g / 10 minutes, more preferably 0.5 to 3
It is 0 g / 10 minutes.

【0026】また、オレフィン系エラストマーのさらに
他の代表的一例であるエチレン−プロピレン−ジエン共
重合体(EPDM)は、エチレンから誘導される繰り返
し単位の含有率が40〜70モル%、プロピレンから誘
導される繰り返し単位の含有率が30〜60モル%、お
よびジエンから誘導される繰り返し単位の含有率が1〜
10モル%であることが好ましい。より好ましい範囲
は、エチレン系繰り返し単位が50〜60モル%、プロ
ピレン系繰り返し単位が40〜50モル%、およびジエ
ン系繰り返し単位が3〜6モル%である。さらに、EP
DMのメルトフローレート(MFR、230℃、2.1
6kg荷重)は0.01〜50g/10分の範囲内にあ
るのが好ましく、より好ましくは0.1〜30g/10
分である。
In addition, ethylene-propylene-diene copolymer (EPDM), which is another typical example of the olefin elastomer, has a repeating unit content of 40 to 70 mol% derived from ethylene and is derived from propylene. The content of the repeating unit is 30 to 60 mol%, and the content of the repeating unit derived from a diene is 1 to
It is preferably 10 mol%. More preferable ranges are 50 to 60 mol% of ethylene-based repeating units, 40 to 50 mol% of propylene-based repeating units, and 3 to 6 mol% of diene-based repeating units. Furthermore, EP
DM melt flow rate (MFR, 230 ° C, 2.1
6 kg load) is preferably in the range of 0.01 to 50 g / 10 minutes, more preferably 0.1 to 30 g / 10.
Minutes.

【0027】オレフィン系エラストマーの代表的例であ
るエチレン−プロピレン共重合体(EPR)、エチレン
−ブテン共重合体ゴム(EBR)及びエチレン−プロピ
レン−ジエン共重合体(EPDM)は、基本的には上記
の繰り返し単位からなるものであるが、これらの共重合
体の特性を損なわない範囲内で、たとえば4−メチル−
1−ペンテンなどの他のα−オレフィンから誘導される
繰り返し単位などの他の繰り返し単位を10モル%以下
の割合で含んでもよい。
Ethylene-propylene copolymer (EPR), ethylene-butene copolymer rubber (EBR) and ethylene-propylene-diene copolymer (EPDM), which are typical examples of olefin elastomers, are basically It is composed of the above repeating unit, but within a range not impairing the properties of these copolymers, for example, 4-methyl-
Other repeating units such as repeating units derived from other α-olefins such as 1-pentene may be contained in a proportion of 10 mol% or less.

【0028】本発明においては、所望により、上述した
(i)オレフィン系エラストマーにポリオレフィンを8
0重量%以下混合したオレフィン系エラストマー組成物
も用いることができる。オレフィン系エラストマーに加
えて使用し得るポリオレフィンとしては、エチレン、プ
ロピレン、1−ブテン、1−ヘキセン、4−メチル−1
−ベンテンなどのα−オレフィンの単独重合体、エチレ
ンとプロピレンもしくは他のα−オレフィンとの非エラ
ストマー性共重合体、またはこれらのα−オレフィンの
2種以上の非エラストマー性共重合体、またはこれらの
単独重合体どうし、共重合体どうし、さらには単独重合
体と共重合体とをブレンドしたものを用いることができ
る。
In the present invention, if desired, a polyolefin may be added to the above-mentioned (i) olefin elastomer.
It is also possible to use an olefin elastomer composition in which 0% by weight or less is mixed. As the polyolefin that can be used in addition to the olefin elastomer, ethylene, propylene, 1-butene, 1-hexene, 4-methyl-1
-Homopolymers of α-olefins such as bentene, non-elastomeric copolymers of ethylene and propylene or other α-olefins, or non-elastomeric copolymers of two or more of these α-olefins, or these The homopolymers, the copolymers, and the blend of the homopolymer and the copolymer can be used.

【0029】ポリオレフィンを混合する場合、その混合
量はオレフィン系エラストマー+ポリオレフィンを10
0重量%として、80重量%以下、好ましくは50重量
%以下である。ポリオレフィンの混合量が80重量%を
超えると、エラストマーとしての特性が失われる。
When the polyolefin is mixed, the mixing amount is 10 olefin elastomer + polyolefin.
0% by weight is 80% by weight or less, preferably 50% by weight or less. When the amount of the polyolefin mixed exceeds 80% by weight, the properties as an elastomer are lost.

【0030】また、本発明において、オレフィン系ポリ
マーの変性に用いる(ii)変性用モノマーは、下記一般
式(1):
In the present invention, the modifying monomer (ii) used for modifying the olefinic polymer is represented by the following general formula (1):

【化9】 (式中、RはHまたは炭素数1〜6のアルキル基であ
り、Arは少くとも一つのグリシジルオキシ基を有する
炭素数6〜20の芳香族炭化水素基であり、mは1〜4
の整数を表す)で表されるグリシジル化合物である。
[Chemical 9] (In the formula, R is H or an alkyl group having 1 to 6 carbon atoms, Ar is an aromatic hydrocarbon group having 6 to 20 carbon atoms having at least one glycidyloxy group, and m is 1 to 4
Represents the integer) of the glycidyl compound.

【0031】好ましいグリシジル化合物としては、下記
一般式(8)で表わされるものが挙げられる。
Preferred glycidyl compounds include those represented by the following general formula (8).

【化10】 (式中、RはHまたは炭素数1〜6のアルキル基であ
る。)
[Chemical 10] (In the formula, R is H or an alkyl group having 1 to 6 carbon atoms.)

【0032】このようなグリシジル化合物は、例えば特
開昭60−130580号に示されるように、以下のよ
うな方法により製造することができる。まず、少なくと
も1つのフェノール性水酸基を有する芳香族炭化水素
と、N−メチロールアクリルアミドまたはN−メチロー
ルメタアクリルアミド、あるいはN−メチロールメタア
クリルアミドのアルキルエーテル誘導体(以下、これら
をN−メチロールアクリルアミド類という)を酸触媒を
用いて縮合させることにより、下記一般式(9):
Such a glycidyl compound can be produced by the following method, as disclosed in, for example, JP-A-60-130580. First, an aromatic hydrocarbon having at least one phenolic hydroxyl group, N-methylolacrylamide or N-methylolmethacrylamide, or an alkyl ether derivative of N-methylolmethacrylamide (hereinafter, these are referred to as N-methylolacrylamides). By condensation using an acid catalyst, the following general formula (9):

【化11】 (式中、RはHまたは炭素数1〜6のアルキル基であ
り、Ar′は少くとも1つの水酸基を有する炭素数6〜
20の芳香族炭化水素基であり、mは1〜4の整数を表
す。)で表される化合物を製造する。
[Chemical 11] (In the formula, R is H or an alkyl group having 1 to 6 carbon atoms, and Ar ′ is 6 to 6 carbon atoms having at least one hydroxyl group.
20 is an aromatic hydrocarbon group, and m represents an integer of 1 to 4. ) Is produced.

【0033】上記の少なくとも1つのフェノール性水酸
基を有する芳香族炭化水素としては特に制限はないが、
例えばフェノール、o−クレゾール、m−クレゾール、
p−クレゾール、2,6−キシレノール、2,4−キシ
レノ−ル、o−クロルフェノール、m−クロルフェノー
ル、o−フェニルフェノール、p−クロルフェノール、
2,6−ジフェニルフェノールなどのフェノール性化合
物、ヒドロキノン、カテコール、フロログルシノールな
どのポリフェノール性化合物、1−ナフトール、2−ナ
フト−ル、9−ヒドロキシアントラセンなどの多環式ヒ
ドロキシ化合物、2,2−ビス(4−ヒドロキシフェニ
ル)プロパン(ビスフェノール−A)、ビス(4−ヒド
ロキシフェニル)メタンなどのビスフェノール類などが
挙げられる。
The aromatic hydrocarbon having at least one phenolic hydroxyl group is not particularly limited,
For example, phenol, o-cresol, m-cresol,
p-cresol, 2,6-xylenol, 2,4-xylenol, o-chlorophenol, m-chlorophenol, o-phenylphenol, p-chlorophenol,
Phenolic compounds such as 2,6-diphenylphenol, polyphenolic compounds such as hydroquinone, catechol and phloroglucinol, polycyclic hydroxy compounds such as 1-naphthol, 2-naphthol and 9-hydroxyanthracene, 2,2 -Bisphenol such as bis (4-hydroxyphenyl) propane (bisphenol-A) and bis (4-hydroxyphenyl) methane.

【0034】次に、上記一般式(9)で表される化合物
の水酸基をグリシジル化することにより、一般式(1)
で表されるグリシジル化合物を得ることができる。この
グリシジル化は、一般式(9)で表される化合物とエピ
ハロヒドリンとの付加反応を行った後、苛性アルカリに
より脱ハロゲン化水素化することにより行うのが好まし
い。上記エピハロヒドリンとしてはエピクロルヒドリ
ン、エピブロムヒドリン、エピヨードヒドリンなどを用
いることができる。
Next, the hydroxyl group of the compound represented by the general formula (9) is glycidylated to give the general formula (1).
A glycidyl compound represented by can be obtained. This glycidylation is preferably carried out by performing an addition reaction between the compound represented by the general formula (9) and epihalohydrin, and then dehydrohalogenating with caustic alkali. As the above-mentioned epihalohydrin, epichlorohydrin, epibromhydrin, epiiodohydrin, etc. can be used.

【0035】エピハロヒドリンとの付加反応は、相間移
動触媒を用いて行う。相間移動触媒としては、例えばテ
トラブチルアンモニウムブロマイド、トリオクチルメチ
ルアンモニウムクロライド、ベンジルトリエチルアンモ
ニウムクロライドなどの第4級アンモニウム塩、テトラ
フェニルホスホニウムクロライド、トリフェニルメチル
ホスホニウムクロライドなどの第4級ホスニウム塩など
を用いることができる。上記相間移動触媒の使用量は、
一般式(9)で表される化合物を100モル%として、
0.01〜100モル%の範囲であるのが好ましい。特
に好ましい相間移動触媒の使用量は、0.05〜10モ
ル%である。また反応温度および反応時間は50〜12
0℃で5分〜2時間、より好ましくは80〜110℃で
10〜30分である。
The addition reaction with epihalohydrin is carried out using a phase transfer catalyst. As the phase transfer catalyst, for example, a quaternary ammonium salt such as tetrabutylammonium bromide, trioctylmethylammonium chloride or benzyltriethylammonium chloride, or a quaternary phosnium salt such as tetraphenylphosphonium chloride or triphenylmethylphosphonium chloride is used. be able to. The amount of the phase transfer catalyst used is
When the compound represented by the general formula (9) is 100 mol%,
It is preferably in the range of 0.01 to 100 mol%. A particularly preferable amount of the phase transfer catalyst used is 0.05 to 10 mol%. The reaction temperature and reaction time are 50 to 12
It is 5 minutes to 2 hours at 0 ° C, more preferably 10 to 30 minutes at 80 to 110 ° C.

【0036】エピハロヒドリンの付加に続いて、苛性ア
ルカリにより脱ハロゲン化水素化を行う。苛性アルカリ
としては、苛性ソーダ、苛性カリ、水酸化リチウムなど
が使用できる。これらは固体のままか、または水溶液と
して用いることができる。また、脱ハロゲン化水素化の
触媒としては上述の相間移動触媒と同様のものを用いる
ことができる。また上記相間移動触媒以外の触媒も使用
でき、そのような触媒としては、クラウンエーテル類、
エチレングリコール、ジエチレングリコール、トリエチ
レングリコール、テトラエチレングリコール、ポリエチ
レングリコールなどが挙げられる。
The addition of epihalohydrin is followed by dehydrohalogenation with caustic. As the caustic alkali, caustic soda, caustic potash, lithium hydroxide and the like can be used. These can be used as solids or as aqueous solutions. As the dehydrohalogenation catalyst, the same one as the above-mentioned phase transfer catalyst can be used. Further, a catalyst other than the above phase transfer catalyst can also be used, and as such a catalyst, crown ethers,
Examples thereof include ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol and polyethylene glycol.

【0037】上記苛性アルカリの使用量は、一般式
(9)で表される化合物に対して等モル量を使用するの
が好ましい。より好ましくは、1.1〜1.5倍モルを
使用する。また反応温度および反応時間は20〜90℃
で10分〜3時間、より好ましくは40〜70℃で30
分〜20時間である。
The caustic alkali is preferably used in an equimolar amount with respect to the compound represented by the general formula (9). More preferably, 1.1 to 1.5 times the molar amount is used. The reaction temperature and reaction time are 20 to 90 ° C.
10 minutes to 3 hours, more preferably 30 to 40 to 70 ° C
Minutes to 20 hours.

【0038】このようなグリシジル化合物によるオレフ
ィン系エラストマー(またはオレフィン系エラストマー
組成物)の変性(グラフト重合)は、溶液法または溶融
混練法のいずれでも行うことができる。溶融混練法の場
合、オレフィン系エラストマーと上述した変性用のグリ
シジル化合物、および必要に応じて触媒を、押出機や二
軸混練機などに投入し、180〜300℃の温度に加熱
して溶融しながら0.1〜20分混練する。また、溶液
法の場合、キシレンなどの有機溶剤に上記出発物質を溶
解し、90〜200℃の温度で0.1〜100時間撹拌
しながら行う。いずれの場合にも、触媒として通常のラ
ジカル重合用触媒を用いることができ、その具体例とし
ては、過酸化ベンゾイル、過酸化ラウロイル、過酸化ジ
ターシャリーブチル、過酸化アセチル、ターシャリーブ
チルペルオキシ安息香酸、過酸化ジクミル、ペルオキシ
安息香酸、ペルオキシ酢酸、ターシャリーブチルペルオ
キシピバレート、2,5−ジメチル−2,5−ジターシ
ャリーブチルペルオキシヘキシンなどの過酸化物類や、
アゾビスイソブチロニトリルなどのジアゾ化合物類等が
挙げられる。触媒の添加量は変性のグリシジル化合物1
00重量部に対して0.1〜10重量部程度である。な
お、上記グラフト反応時にフェノール系酸化防止剤を添
加することができる。ただし、ラジカル重合用触媒を添
加しない場合には、添加しない方が好ましい。
The modification (graft polymerization) of the olefinic elastomer (or olefinic elastomer composition) with such a glycidyl compound can be carried out by either a solution method or a melt-kneading method. In the case of the melt-kneading method, the olefinic elastomer, the above-mentioned glycidyl compound for modification, and the catalyst as required are charged into an extruder, a twin-screw kneader, or the like, and heated to a temperature of 180 to 300 ° C. to melt. While kneading for 0.1 to 20 minutes. In the case of the solution method, the above-mentioned starting materials are dissolved in an organic solvent such as xylene and the stirring is performed at a temperature of 90 to 200 ° C for 0.1 to 100 hours. In any case, an ordinary radical polymerization catalyst can be used as the catalyst, and specific examples thereof include benzoyl peroxide, lauroyl peroxide, ditertiary butyl peroxide, acetyl peroxide, tert-butyl peroxybenzoic acid. , Peroxides such as dicumyl peroxide, peroxybenzoic acid, peroxyacetic acid, tertiary butyl peroxypivalate, and 2,5-dimethyl-2,5-ditertiary butyl peroxyhexyne,
Examples thereof include diazo compounds such as azobisisobutyronitrile. The amount of catalyst added is modified glycidyl compound 1
It is about 0.1 to 10 parts by weight with respect to 00 parts by weight. A phenolic antioxidant can be added during the graft reaction. However, when the radical polymerization catalyst is not added, it is preferable not to add it.

【0039】前記(ii)グリシジル化合物の配合割合
は、前記(i)オレフィン系エラストマー(またはオレ
フィン系エラストマー組成物)100重量部に対して、
0.01〜30重量部、好ましくは0.1〜10重量部
である。グリシジル化合物の配合量が0.01重量部未
満では、高グラフト率の達成が困難であり、また30重
量部を超えると得られる変性オレフィン系エラストマー
の分子量が低下する。
The mixing ratio of the (ii) glycidyl compound is 100 parts by weight of the (i) olefin-based elastomer (or olefin-based elastomer composition).
It is 0.01 to 30 parts by weight, preferably 0.1 to 10 parts by weight. When the blending amount of the glycidyl compound is less than 0.01 parts by weight, it is difficult to achieve a high graft ratio, and when it exceeds 30 parts by weight, the molecular weight of the modified olefin elastomer obtained is lowered.

【0040】上述したような(a)変性オレフィン系エ
ラストマーと(b)側鎖にアミノ基をもつPAS(アミ
ノ基をもたないPASを併用する場合も含む、以下同
じ)との配合割合は、両者の合計重量に基づき、(a)
変性オレフィン系エラストマーが2〜70重量%、好ま
しくは10〜40重量%であり、(b)該PASが98
〜30重量%、好ましくは90〜60重量%である。
(a)変性オレフィン系エラストマーが2重量%未満で
は(すなわち、(b)側鎖にアミノ基をもつPASを含
むPASが98重量%を越えると)、その配合によるP
ASの耐衝撃性等の物性の改善の効果が充分でなく、ま
た(a)変性オレフィン系エラストマーが70重量%を
越えると(すなわち、(b)上記PASが30重量%未
満では)、PASの特性が損なわれる。
The mixing ratio of (a) the modified olefin elastomer as described above and (b) the PAS having an amino group in the side chain (including the case where PAS having no amino group is used in combination, the same applies hereinafter) is Based on the total weight of both, (a)
The modified olefin elastomer is 2 to 70% by weight, preferably 10 to 40% by weight, and (b) the PAS is 98.
-30% by weight, preferably 90-60% by weight.
When (a) the modified olefin elastomer is less than 2% by weight (that is, when (b) the PAS containing a PAS having an amino group in the side chain exceeds 98% by weight), P by the blending is increased.
If the effect of improving physical properties such as impact resistance of AS is not sufficient and (a) the modified olefin elastomer exceeds 70% by weight (that is, (b) the PAS is less than 30% by weight), The characteristics are impaired.

【0041】本発明のPAS樹脂組成物には、無機フィ
ラー、カーボンブラックなどの充填剤や、その他その改
質を目的として、他の添加剤、例えば熱安定剤、光安定
剤、難燃剤、可塑剤、帯電防止剤、発泡剤、核剤などを
添加することができる。
The PAS resin composition of the present invention contains a filler such as an inorganic filler or carbon black, and other additives such as a heat stabilizer, a light stabilizer, a flame retardant, and a plasticizer for the purpose of modifying the filler. Agents, antistatic agents, foaming agents, nucleating agents and the like can be added.

【0042】このような(a)変性オレフィン系エラス
トマーと(b)PASとからなる本発明の組成物は、
(a)変性オレフィン系エラストマーと(b)側鎖にア
ミノ基をもつPASと必要に応じて添加される各種添加
剤とを、一軸押出機、二軸押出機、バンバリミキサー、
混練ロール、ブラベンダー・プラストグラフ(登録商
標)などの混練機を用いて220〜300℃、好ましく
は240〜280℃で加熱溶融状態で混練することによ
り得ることができる。
The composition of the present invention comprising such (a) modified olefin elastomer and (b) PAS is
A single-screw extruder, a twin-screw extruder, a Banbury mixer, a modified olefin elastomer (a) and (b) a PAS having an amino group in a side chain and various additives to be added as necessary are prepared.
It can be obtained by kneading in a heat-melted state at 220 to 300 ° C., preferably 240 to 280 ° C. using a kneading machine such as a kneading roll or Brabender Plastograph (registered trademark).

【0043】[0043]

〔ブテン含有量80%、メルトフローレート(230
℃、2.16kg荷重)1.5g/10分〕
[Butene content 80%, melt flow rate (230
℃, 2.16kg load) 1.5g / 10 minutes]

(ロ)エチレン−プロピレン共重合体ゴム(EPR) 〔プロピレン含有量70%、メルトフローレート(23
0℃、2.16kg荷重)1.7g/10分〕
(B) Ethylene-propylene copolymer rubber (EPR) [Propylene content 70%, melt flow rate (23
0 ° C, 2.16 kg load) 1.7 g / 10 minutes]

【0044】〔2〕変性用モノマー AXE:下記化学式(8)で表されるグリシジル化合物
(鐘淵化学工業(株)製〕 〔3〕ラジカル発生剤 POX:パーヘキシン2−5B〔日本油脂(株)製〕 〔4〕ポリアリーレンサルファイド (イ)アミノ基をもたないポリ(p−フェニレン)サル
ファイド((株)トープレン製 T−4AG)、Na含
有量1,800ppm (ロ)アミノ基をもたないポリ(p−フェニレン)サル
ファイド((株)トープレン製 T−2に酸処理を施し
たもの、Na含有量290ppm (ハ)側鎖にアミノ基をもつポリ(p−フェニレン)サ
ルファイド 次の方法によって合成した。容量100リットルの撹拌
機付の耐圧反応容器中に、N−メチル−2−ピロリドン
(NMP)80リットルとNa2 S(含水量40重量
%)40.64kg(313.6モル)とNaOH9
9.2gを仕込み、窒素雰囲気中で撹拌しながら約2時
間かけて205℃にまで徐々に昇温させて脱水した。そ
の後、反応系を150℃にまで冷却し、反応系に、パラ
ジクロルベンゼン44.8kg(304モル)と−p−
ジクロルアニリン2.56kg(16モル)と1,2,
4−トリクロルベンゼン160g(0.96モル)を2
5.6kgのNMP中に溶解した溶液を加え、更に1時
間かけて250℃にまで昇温し、2時間反応を行った。
反応終了後、オートクレーブを室温にまで冷却し、内容
物を濾別し、反応生成物である濾過ケーキを50℃で脱
イオン水で3回洗浄し、副生した食塩やその他の未反応
物を除き、100℃で乾燥してPPSを得た。このPP
Sは側鎖にアミノ基をもち、その含有率は3モル%であ
った。
[2] Modification Monomer AXE: Glycidyl compound represented by the following chemical formula (8) (manufactured by Kanegafuchi Chemical Industry Co., Ltd.) [3] Radical generator POX: Perhexin 2-5B [NOF CORPORATION] [4] Polyarylene sulfide (a) Poly (p-phenylene) sulfide having no amino group (T-4AG manufactured by Topren Co., Ltd.), Na content of 1,800 ppm (b) No amino group Poly (p-phenylene) sulfide (manufactured by Topren Co., Ltd. T-2 subjected to acid treatment, Na content 290 ppm (c) Poly (p-phenylene) sulfide having amino group in side chain Synthesized by the following method. In a pressure resistant reactor equipped with a stirrer having a capacity of 100 liters, 80 liters of N-methyl-2-pyrrolidone (NMP) and Na 2 S (water content: 40 wt. %) 40.64 kg (313.6 mol) and NaOH 9
9.2 g was charged and dehydrated by gradually raising the temperature to 205 ° C. over about 2 hours while stirring in a nitrogen atmosphere. Then, the reaction system was cooled to 150 ° C., and 44.8 kg (304 mol) of paradichlorobenzene and -p- were added to the reaction system.
Dichloroaniline 2.56 kg (16 mol) 1,2,
2-trichlorobenzene 160 g (0.96 mol) 2
A solution dissolved in 5.6 kg of NMP was added, the temperature was further raised to 250 ° C. over 1 hour, and the reaction was performed for 2 hours.
After the reaction was completed, the autoclave was cooled to room temperature, the contents were filtered off, and the reaction product, the filter cake, was washed 3 times with deionized water at 50 ° C. to remove by-produced salt and other unreacted substances. It was removed and dried at 100 ° C. to obtain PPS. This PP
S had an amino group in its side chain, and its content was 3 mol%.

【0045】実施例1〜20、比較例1〜12 オレフィン系エラストマーと、表1、表2および表3に
示す各種の変性用モノマーと、さらに表1、表2および
表3に示す量のラジカル発生剤とをヘンシェルミキサー
により、ドライブレンドし、その後30mmφ、L/D
=25の単軸押出機中で、200℃、30rpmで溶融
混練してグラフト重合させた。このようにして得られた
変性オレフィン系エラストマーのメルトフローレート、
変性用モノマーのグラフト率を測定した。結果を表1、
表2および表3に示す。
Examples 1 to 20 and Comparative Examples 1 to 12 Olefin-based elastomers, various modifying monomers shown in Tables 1, 2 and 3, and radicals in the amounts shown in Tables 1, 2 and 3. Dry blend with generator using Henschel mixer, then 30mmφ, L / D
= 25 in a single screw extruder, melt kneading was carried out at 200 ° C. and 30 rpm to carry out graft polymerization. The melt flow rate of the modified olefin elastomer thus obtained,
The graft ratio of the modifying monomer was measured. The results are shown in Table 1,
The results are shown in Table 2 and Table 3.

【0046】次に上記変性オレフィン系エラストマー
と、表1、表2および表3に示す各種PPSとを表1、
表2および表3に示す割合で混合し、20mmφの二軸
押出機により、300℃、400rpmで混練し、樹脂
組成物を得た。このようにして得られた熱可塑性樹脂組
成物の23℃でのデュポン衝撃強度、アイゾット衝撃強
度、曲げ弾性率、曲げ強度、引張降伏強度、引張破断伸
びを測定した。結果を表1、表2および表3に示す。
Next, the above-mentioned modified olefin elastomer and various PPSs shown in Table 1, Table 2 and Table 3 are shown in Table 1,
The resin compositions were obtained by mixing in the proportions shown in Tables 2 and 3 and kneading with a 20 mmφ twin-screw extruder at 300 ° C. and 400 rpm. The DuPont impact strength, Izod impact strength, flexural modulus, flexural strength, tensile yield strength, and tensile elongation at break of the thermoplastic resin composition thus obtained at 23 ° C. were measured. The results are shown in Table 1, Table 2 and Table 3.

【0047】[0047]

【表1】 [Table 1]

【0048】[0048]

【表2】 [Table 2]

【0049】[0049]

【表3】 [Table 3]

【0050】(1)MFR:JIS K7210により
測定。(温度190℃、荷重1.05kg) (2)変性用モノマーのグラフト率:変性オレフィン系
エラストマーを沸騰キシレンに溶解し、不溶分を除去し
た後、メタノールにより溶解成分を沈澱させ、これを5
0μm程度の厚さにプレスし、IRスペクトルを測定
し、AXEのC=O結合の伸縮のピーク(1648cm
-1)と、アイソタクティックPPに特有のピークの一つ
(840cm-1)との比から、算出した。 (3)デュポン衝撃試験:JIS K7211により測
定。 (4)アイゾット衝撃強度:JIS K7110により
測定。 (5)曲げ弾性率および曲げ強度:JIS K7203
により測定。 (6)引張降伏強度:JIS K7113により測定。 (7)引張破断伸び:JIS K7113により測定。
(1) MFR: Measured according to JIS K7210. (Temperature 190 ° C., load 1.05 kg) (2) Grafting ratio of modifying monomer: The modified olefin elastomer is dissolved in boiling xylene, the insoluble matter is removed, and then the dissolved component is precipitated with methanol.
After pressing to a thickness of about 0 μm and measuring the IR spectrum, the peak of stretching of the C═O bond of AXE (1648 cm
-1 ) and one of the peaks (840 cm -1 ) peculiar to isotactic PP was calculated. (3) DuPont impact test: Measured according to JIS K7211. (4) Izod impact strength: Measured according to JIS K7110. (5) Flexural modulus and flexural strength: JIS K7203
Measured by. (6) Tensile yield strength: Measured according to JIS K7113. (7) Tensile elongation at break: Measured according to JIS K7113.

【0051】表1、表2および表3から明らかなよう
に、本発明のPAS樹脂組成物は、耐衝撃性、曲げ弾性
率、引張降伏強度、引張破断伸びのすべてが良好であっ
た。特に、酸処理をしたPPSを用いた場合には、酸処
理をしないPPSを用いた場合と比較して、著しく衝撃
強度に優れていた。これに対し、側鎖にアミノ基をもつ
PPSを含むPPSと未変性のオレフィン系エラストマ
ーとをブレンドした比較例1〜6の熱可塑性樹脂組成物
は、耐衝撃性が悪かった。また、アミノ基をもたない通
常のPPSと変性オレフィン系エラストマーとをブレン
ドした比較例7〜12の熱可塑性樹脂組成物は、PPS
単体と比較すると耐衝撃性は改良されているものの充分
に満足できる水準には到達していなかった。これは、未
変性のオレフィン系エラストマーやアミノ基をもたない
通常のPPSが本発明で用いる変性オレフィン系エラス
トマーや側鎖にアミノ基をもつPPSと比較して、相溶
性の点で劣るためである考えられる。
As is clear from Tables 1, 2 and 3, the PAS resin composition of the present invention had good impact resistance, flexural modulus, tensile yield strength and tensile elongation at break. Particularly, when the acid-treated PPS was used, the impact strength was remarkably excellent as compared with the case where the acid-untreated PPS was used. On the other hand, the thermoplastic resin compositions of Comparative Examples 1 to 6 in which PPS containing PPS having an amino group in the side chain and an unmodified olefin elastomer were blended had poor impact resistance. In addition, the thermoplastic resin compositions of Comparative Examples 7 to 12 in which a normal PPS having no amino group and a modified olefin elastomer are blended have PPS.
Although the impact resistance was improved as compared with the single substance, it did not reach a sufficiently satisfactory level. This is because the compatibility of the unmodified olefin elastomer and the ordinary PPS having no amino group is inferior to the modified olefin elastomer used in the present invention and the PPS having an amino group in the side chain in terms of compatibility. There is possible.

【0052】[0052]

【発明の効果】以上に詳述したように、本発明のPAS
樹脂組成物は、互に相溶性に優れた、アクリルアミド基
とエポキシ基とを有する特定のグリシジル化合物により
変性したオレフィン系エラストマーと、側鎖にアミノ基
をもつPASとからなるため、PASの特性である耐熱
性、機械的強度などを損なうことなく、耐衝撃性の大幅
に向上したものとなっている。このような特性をもつ本
発明のPAS樹脂組成物は、各種エンジニアリングプラ
スチックとして、特に自動車部品、家電部品、工業材料
部品、包装材料など用の成形原料として好適である。
As described above in detail, the PAS of the present invention
Since the resin composition comprises an olefin-based elastomer modified with a specific glycidyl compound having an acrylamide group and an epoxy group and having excellent compatibility with each other, and PAS having an amino group in a side chain, it has characteristics of PAS. The impact resistance is greatly improved without impairing certain heat resistance and mechanical strength. The PAS resin composition of the present invention having such characteristics is suitable as various engineering plastics, particularly as a molding raw material for automobile parts, home electric appliance parts, industrial material parts, packaging materials and the like.

───────────────────────────────────────────────────── フロントページの続き (72)発明者 池田 忠生 埼玉県入間郡大井町西鶴ケ岡一丁目3番1 号 東燃株式会社総合研究所内 ─────────────────────────────────────────────────── ─── Continuation of the front page (72) Inventor Tadao Ikeda 1-3-1 Nishitsurugaoka, Oi-cho, Iruma-gun, Saitama Tonen Research Institute

Claims (1)

【特許請求の範囲】[Claims] 【請求項1】 (A)オレフィン系エラストマーに次の
一般式(1): 【化1】 (式中、RはHまたは炭素数1〜6のアルキル基であ
り、Arは少くとも一つのグリシジルオキシ基を有する
炭素数6〜20の芳香族炭化水素基であり、mは1〜4
の整数を表す)で表されるグリシジル化合物をグラフト
した変性オレフィン系エラストマーと(B)側鎖にアミ
ノ基をもつポリアリーレンサルファイドとからなること
を特徴とするポリアリーレンサルファイド樹脂組成物。
1. An olefin elastomer (A) having the following general formula (1): (In the formula, R is H or an alkyl group having 1 to 6 carbon atoms, Ar is an aromatic hydrocarbon group having 6 to 20 carbon atoms having at least one glycidyloxy group, and m is 1 to 4
A polyarylene sulfide resin composition comprising a modified olefin elastomer grafted with a glycidyl compound represented by the formula (1) and (B) a polyarylene sulfide having an amino group in a side chain.
JP15427892A 1992-05-21 1992-05-21 Polyarylene sulfide resin composition Pending JPH0688024A (en)