JPH0978286A - White copper alloy plating solution - Google Patents

White copper alloy plating solution

Info

Publication number
JPH0978286A
JPH0978286A JP26353595A JP26353595A JPH0978286A JP H0978286 A JPH0978286 A JP H0978286A JP 26353595 A JP26353595 A JP 26353595A JP 26353595 A JP26353595 A JP 26353595A JP H0978286 A JPH0978286 A JP H0978286A
Authority
JP
Japan
Prior art keywords
soluble
compound
plating solution
white
copper alloy
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP26353595A
Other languages
Japanese (ja)
Other versions
JP2732044B2 (en
JPH0978286A5 (en
Inventor
Toshiyuki Akaza
敏之 赤座
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
BIKUTORIA KK
Original Assignee
BIKUTORIA KK
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by BIKUTORIA KK filed Critical BIKUTORIA KK
Priority to JP7263535A priority Critical patent/JP2732044B2/en
Publication of JPH0978286A publication Critical patent/JPH0978286A/en
Application granted granted Critical
Publication of JP2732044B2 publication Critical patent/JP2732044B2/en
Publication of JPH0978286A5 publication Critical patent/JPH0978286A5/ja
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To apply a white copper alloy plating having white elegancy and excellent in corrosion resistance, thick plating property or the like by adding a specific quantity of a surfactant, a pyrophosphate, ammonia and specifying free cyanide concn. and pH. SOLUTION: A soluble copper cyanide compound and a soluble palladium compound are added into the white copper alloy plating solution and a soluble zinc compound or a soluble stannic compound are incorporated. Then 0.1-5ml/l surfactant, 0.1-5g/l pyrophosphate and 1-50g/l ammonia are added, and the free cyanide concn. and pH are regulated respectively to 40-60g/l and 11-13. The soluble copper cyanide compound of 40-60g/l expressed in terms of metal copper and the soluble palladium compound of 5-30g/l expressed in terms of metal palladium are incorporated. The soluble zinc compound of 0.1-5g/l expressed in terms of metal zinc is incorporated. The soluble stannic compound of 0.1-5g/l expressed in terms of metal tin is incorporated. Thus, this plating solution can be treated even by a person liable to be suffered from metal allergy.

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【発明が属する技術分野】本発明は、光沢性、耐蝕性等
のある白色優美なメッキを施すことのできる白色銅合金
メッキ液に関するものである。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a white copper alloy plating solution capable of performing elegant white plating having gloss, corrosion resistance and the like.

【0002】[0002]

【従来の技術及び発明が解決しようとする課題】従来よ
り、金属製の眼鏡フレームや腕時計外装部品等に白色メ
ッキを施そうとする場合等にはニッケルメッキ液が多用
されているが、ニッケルは金属アレルギーの主な原因と
なるものであって、金属アレルギーを起こし易い人はニ
ッケルメッキ液により白色メッキが施された物品を利用
することができないという問題があった。
2. Description of the Related Art Conventionally, a nickel plating solution is often used when white plating is applied to metal eyeglass frames, wristwatch exterior parts, etc. This is a main cause of metal allergy, and there is a problem that a person who is liable to cause metal allergy cannot use an article that is white-plated with a nickel plating solution.

【0003】また、銅と亜鉛とを含有せしめた銅合金メ
ッキ液(黄銅メッキ液)や、銅とスズとを含有せしめた
銅合金メッキ液(スペキュラムメッキ液)によっても白
色メッキを施すことができるが、黄銅メッキは耐蝕性が
悪いという不具合があり、一方のスペキュラムメッキは
光沢性、合金比率、メッキ厚づけ性が安定しないという
不具合があるため、これらのメッキ液は用途が限定され
ていた。
White plating can also be performed with a copper alloy plating solution containing copper and zinc (brass plating solution) or a copper alloy plating solution containing copper and tin (speculum plating solution). However, brass plating has a problem that corrosion resistance is poor, and specular plating, on the other hand, has problems that glossiness, alloy ratio, and plating thickening property are not stable, so that these plating solutions have limited applications.

【0004】本出願人は、上記従来技術の有する問題に
鑑みて金属アレルギーを誘発する虞のあるニッケルメッ
キに代え、光沢が良く白色優美であるとともに耐蝕性や
厚づけ性等にも優れた白色メッキを施すことができる銅
合金メッキ液を提供すべく鋭意研究を重ねた結果、本発
明を完成するに至った。
In view of the above-mentioned problems of the prior art, the present applicant has replaced the nickel plating, which may induce metal allergies, with a white color that has good gloss and white grace, as well as excellent corrosion resistance and thickening properties. As a result of intensive studies to provide a copper alloy plating solution capable of plating, the present invention has been completed.

【0005】[0005]

【課題を解決するための手段】即ち、本発明白色銅合金
メッキ液は、可溶性銅シアン化物及び可溶性パラジウム
化合物に加え可溶性亜鉛化合物又は可溶性第二スズ化合
物を含有せしめ、界面活性剤0.1〜5ml/L、ピロ
リン酸塩0.1〜5g/L、アンモニア1〜50g/L
を添加するとともに遊離シアン濃度を40〜60g/
L、pHを11〜13に調整したことを特徴とする。
That is, the white copper alloy plating solution of the present invention contains a soluble zinc compound or a soluble stannic compound in addition to a soluble copper cyanide and a soluble palladium compound, and a surfactant of 0.1 to 10 is used. 5 ml / L, pyrophosphate 0.1-5 g / L, ammonia 1-50 g / L
And the free cyan concentration of 40-60 g /
It is characterized in that L and pH are adjusted to 11 to 13.

【0006】[0006]

【発明の実施の形態】本発明白色銅合金メッキ液に含有
せしめる可溶性銅シアン化物としては、例えば、シアン
化第一銅、シアン化第一銅カリウム、シアン化第一銅ナ
トリウム等を用いることができる。銅シアン化物の含有
量は、金属銅に換算した量で5〜20g/Lであるのが
好ましく、含有量が5g/L未満であると電流効率の低
下をきたしてしまい、20g/Lよりも多くなると銅の
析出が増えてメッキの色調がブロンズ色となってしうた
め好ましくない。
BEST MODE FOR CARRYING OUT THE INVENTION As the soluble copper cyanide contained in the white copper alloy plating solution of the present invention, for example, cuprous cyanide, potassium cuprous cyanide, cuprous cyanide, etc. may be used. it can. The content of copper cyanide is preferably 5 to 20 g / L in terms of metallic copper, and if the content is less than 5 g / L, the current efficiency is lowered, and the content is more than 20 g / L. If the amount is too large, the amount of copper is increased and the color tone of the plating becomes bronze, which is not preferable.

【0007】また、可溶性パラジウム化合物としては、
例えば、硝酸パラジウムアミン、塩化パラジウムアミ
ン、シアン化パラジウム等を用いることができる。パラ
ジウム化合物の含有量は、金属パラジウムに換算した量
で5〜30g/Lであるのが好ましく、含有量が5g/
L未満であると電流効率の低下をきたしてしまい、30
g/Lよりも多くなるとパラジウムの析出が増えてしう
ため好ましくない。
As the soluble palladium compound,
For example, palladium amine nitrate, palladium amine chloride, palladium cyanide and the like can be used. The content of the palladium compound is preferably 5 to 30 g / L in terms of metallic palladium, and the content is 5 g / L.
If it is less than L, the current efficiency will decrease, and
When it is more than g / L, palladium precipitation is likely to increase, which is not preferable.

【0008】更に、本発明にあっては上記可溶性銅シア
ン化物及び可溶性パラジウム化合物に加え、可溶性亜鉛
化合物又は可溶性第二スズ化合物をメッキ液中に含有さ
せるが、可溶性亜鉛化合物としては、例えば、シアン化
亜鉛、硫酸亜鉛等を用いることができる。本発明メッキ
液中に亜鉛化合物を含有させる場合、その含有量は、金
属亜鉛に換算した量で0.1〜5g/Lであるのが好ま
しく、含有量が0.1g/L未満であるとメッキの光沢
の低下をきたし、5g/Lよりも多くなるとメッキ応力
が増え、耐蝕性も悪くなってしまうため好ましくない。
Further, in the present invention, a soluble zinc compound or a soluble stannic compound is contained in the plating solution in addition to the soluble copper cyanide and the soluble palladium compound. Examples of the soluble zinc compound include cyanide. Zinc oxide, zinc sulfate or the like can be used. When a zinc compound is contained in the plating solution of the present invention, its content is preferably 0.1 to 5 g / L in terms of metallic zinc, and the content is less than 0.1 g / L. The gloss of the plating is lowered, and if it exceeds 5 g / L, the plating stress increases and the corrosion resistance deteriorates, which is not preferable.

【0009】一方、可溶性第二スズ化合物としては、例
えば、スズ酸ナトリウム、スズ酸カリウム等を用いるこ
とができる。本発明メッキ液中に第二スズ化合物を含有
させる場合、その含有量は、金属スズに換算した量で
0.1〜5g/Lであるのが好ましく、含有量が0.1
g/L未満であると光沢の低下をきたし、5g/Lより
も多くなるとスズの析出が増えてしまいメッキの物性が
悪くなるため好ましくない。
On the other hand, as the soluble stannic compound, for example, sodium stannate, potassium stannate, etc. can be used. When the stannous compound is contained in the plating solution of the present invention, its content is preferably 0.1 to 5 g / L in terms of metal tin, and the content is 0.1.
If it is less than g / L, the gloss will be deteriorated, and if it is more than 5 g / L, the precipitation of tin will increase and the physical properties of the plating will deteriorate, which is not preferable.

【0010】本発明において界面活性剤は光沢安定剤と
して添加され、例えば、ポリオキシエチレンアルキルエ
ーテル型、又はポリオキシエチレンアルキルエーテルリ
ン酸エステル型の非イオン系界面活性剤等を用いること
ができる。界面活性剤の添加量は0.1〜5ml/Lで
あって、0.1ml/L未満であると光沢安定性が悪く
なり、5ml/Lより多くても害はないがそれ以上の効
果が得られず多量に添加する意味がない。
In the present invention, the surfactant is added as a gloss stabilizer, and for example, a polyoxyethylene alkyl ether type or a polyoxyethylene alkyl ether phosphate type nonionic surfactant can be used. The amount of the surfactant added is 0.1 to 5 ml / L, and if it is less than 0.1 ml / L, the gloss stability becomes poor, and if it is more than 5 ml / L, there is no harm, but further effects are obtained. There is no point in adding a large amount because it cannot be obtained.

【0011】また、ピロリン酸塩は金属錯塩安定剤とし
て添加され、その添加量は5〜120g/Lである。ピ
ロリン酸塩の添加量が5g/L未満であると亜鉛化合物
や第二スズ化合物の溶解安定性が悪くなり、120g/
Lよりも多くなると光沢範囲が狭くなってしまうため好
ましくない。
Further, pyrophosphate is added as a metal complex salt stabilizer, and the addition amount is 5 to 120 g / L. If the amount of the pyrophosphate added is less than 5 g / L, the dissolution stability of the zinc compound or the stannic compound becomes poor, and 120 g / L
When it is more than L, the gloss range becomes narrow, which is not preferable.

【0012】アンモニアは色調安定剤として添加され、
その添加量は1〜50g/Lである。アンモニアの添加
量が1g/L未満であるとメッキの色調ムラが発生し易
くなり、50g/Lよりも多くなっても害はないがアン
モニア臭が強くなり作業環境上好ましくない。
Ammonia is added as a color stabilizer,
The added amount is 1 to 50 g / L. When the amount of ammonia added is less than 1 g / L, uneven color tone of the plating is apt to occur, and when it is more than 50 g / L, there is no harm but the ammonia odor becomes strong, which is not preferable in the working environment.

【0013】更に、本発明ではメッキ液中の遊離シアン
濃度が40〜60g/Lとなるように調整するが、遊離
シアン濃度が40g/L未満ではメッキの光沢が安定せ
ず、60g/Lよりも多くなるとメッキの色調がブロン
ズ色となってしまうため好ましくない。
Further, in the present invention, the free cyan concentration in the plating solution is adjusted to 40 to 60 g / L, but if the free cyan concentration is less than 40 g / L, the gloss of the plating is not stable, and if the free cyan concentration is less than 60 g / L, If too much, the color tone of the plating becomes bronze, which is not preferable.

【0014】また、本発明メッキ液のpHは11〜13
になるように調整するが、pHが11未満の場合は亜鉛
化合物や第二スズ化合物の溶解安定性や、メッキの光沢
性が悪くなり、pHが13よりも大きくなるとメッキの
色調がブロンズ色となってしまうため好ましくない。
The plating solution of the present invention has a pH of 11-13.
However, when the pH is less than 11, the dissolution stability of zinc compounds and stannic compounds and the gloss of the plating become poor, and when the pH is more than 13, the plating tone becomes a bronze color. It is not preferable because it becomes.

【0015】このような本発明白色銅合金メッキ液を用
いて被メッキ物に白色メッキを施すには、例えば、電圧
1〜10V、電流密度0.1〜10A/dm2 等の条件
で、従来公知の方法により行うことができる。
To perform white plating on an object to be plated using such a white copper alloy plating solution of the present invention, for example, a voltage of 1 to 10 V and a current density of 0.1 to 10 A / dm 2 have been used. It can be performed by a known method.

【0016】[0016]

【実施例】次に具体的実施例を挙げて本発明をより詳細
に説明するが、本発明はこれらに限定されるものではな
い。
The present invention will be described in more detail with reference to specific examples, but the present invention is not limited thereto.

【0017】〔実施例1〕長さ10cm×幅15cm×
厚み0.1cmの黄銅素材からなる板状の試験片に、ア
ルカリ脱脂(マクダット社:WSP)、電解脱脂(マク
ダット社:DEW)、酸浸積(5重量%硫酸)の順に一
般の銅合金用の処理と同様の前処理を施した後、下記組
成の本発明白色銅合金メッキ液を用いて、当該メッキ液
の温度を55℃とし、電圧3V、電流密度2A/dm2
で30分間陰極電解してメッキを施したところ、試験片
上に良好な光沢を有する白色優美なメッキ被膜が5μm
の厚さで形成された。また、メッキの施された試験片を
180度折り曲げたところ、メッキ被膜には割れも入ら
ず、剥離もなく耐摩耗性も良好なものであった。
Example 1 Length 10 cm x Width 15 cm x
For a general copper alloy, a 0.1 cm-thick plate-shaped test piece made of brass material was alkali degreased (McDat: WSP), electrolytic degreased (McDat: DEW), and acid immersion (5 wt% sulfuric acid) in that order. After performing the same pretreatment as the above treatment, using the white copper alloy plating solution of the present invention having the following composition, setting the temperature of the plating solution to 55 ° C., voltage 3 V, current density 2 A / dm 2
After 30 minutes of cathodic electrolysis and plating, a white elegant plating film with good luster on the test piece of 5 μm
Formed with a thickness of. Further, when the plated test piece was bent 180 degrees, the plating film had no cracks, no peeling, and good wear resistance.

【0018】 <白色銅合金メッキ液組成> シアン化銅 ・・・・・・12g/L(金属銅換算) 塩化パラジウムアミン ・・・・・・50g/L(金属パラジウム換算) シアン化亜鉛 ・・・・・・1.0g/L(金属亜鉛換算) 界面活性剤 ・・・・・・0.1ml/L ピロリン酸カリウム ・・・・・・20g/L アンモニア ・・・・・・ 2g/L 遊離シアン ・・・・・・50g/L pH ・・・・・・12<White copper alloy plating solution composition> Copper cyanide: 12 g / L (converted to metallic copper) Palladium amine chloride: 50 g / L (converted to metallic palladium) Zinc cyanide:・ ・ ・ ・ 1.0g / L (calculated as metallic zinc) Surfactant ・ ・ ・ ・ 0.1ml / L Potassium pyrophosphate ・ ・ ・ ・ ・ ・ 20g / L Ammonia ・ ・ ・ ・ ・ ・ 2g / L Free cyan: 50 g / L pH: 12

【0019】〔実施例2〕シアン化亜鉛の代わりにスズ
酸ナトリウムを5g/L(金属スズ換算)含有させた以
外は実施例1で用いたメッキ液と同様のメッキ液を用
い、実施例1と同様の方法で試験片にメッキを施したと
ころ、試験片上に良好な光沢を有する白色優美なメッキ
被膜が5μmの厚さで形成された。また、メッキの施さ
れた試験片を180度折り曲げたところ、メッキ層には
割れも入らず、剥離もなく耐摩耗性も良好なものであ
り、実施例1と同様の結果を得ることができた。
Example 2 The same plating solution as that used in Example 1 was used except that sodium stannate was added in an amount of 5 g / L (as metal tin) instead of zinc cyanide. When a test piece was plated in the same manner as in (1), a white graceful plated film having good gloss was formed on the test piece in a thickness of 5 μm. Further, when the plated test piece was bent 180 degrees, cracks did not occur in the plated layer, peeling did not occur, and wear resistance was good, and the same results as in Example 1 could be obtained. It was

【0020】〔比較例1〕実施例1のメッキ液から界面
活性剤を除いた以外は実施例1で用いたメッキ液と同様
のメッキ液を用い、実施例1と同様の方法で試験片にメ
ッキを施したところ、試験片上には白色のメッキ被膜が
形成されたが、かかるメッキ被膜は光沢性に乏しく、部
分的にムラのあるものであり、実施例1とは大きく異な
る結果であった。
Comparative Example 1 A test piece was prepared in the same manner as in Example 1 using the same plating solution as that used in Example 1 except that the surfactant was removed from the plating solution of Example 1. When plating was performed, a white plating film was formed on the test piece, but the plating film was poor in gloss and partially uneven, and the results were significantly different from those of Example 1. .

【0021】〔比較例2〕実施例1のメッキ液からアン
モニアを除いた以外は実施例1で用いたメッキ液と同様
のメッキ液を用い、実施例1と同様の方法で試験片にメ
ッキを施したところ、試験片上には白色のメッキ被膜が
形成されたが、かかるメッキ被膜は光沢性に乏しく、部
分的にムラのあるものであり、実施例1とは大きく異な
る結果であった。
Comparative Example 2 A test piece was plated in the same manner as in Example 1 using the same plating solution as that used in Example 1 except that ammonia was removed from the plating solution of Example 1. When applied, a white plating film was formed on the test piece, but the plating film was poor in gloss and partially uneven, and the results were significantly different from those of Example 1.

【0022】〔比較例3〕実施例1のメッキ液からピロ
リン酸カリウムを除いた以外は実施例1で用いたメッキ
液と同様のメッキ液を用い、実施例1と同様の方法で試
験片にメッキを施したところ、試験片上には白色のメッ
キ被膜が形成されたが、その後メッキ液が濁り、更に再
度別の試験片に同じ条件でメッキを施したところ、今度
はメッキ被膜の光沢がなくなり、安定しない結果となっ
てしまい、実施例1とは大きく異なる結果であった。
Comparative Example 3 A test piece was prepared in the same manner as in Example 1 except that potassium pyrophosphate was removed from the plating solution of Example 1 using the same plating solution as that used in Example 1. When plating was performed, a white plating film was formed on the test piece, but then the plating solution became turbid, and when another test piece was plated again under the same conditions, the glossiness of the plating film disappeared this time. However, the result is not stable, which is a result greatly different from that of the first embodiment.

【0023】〔比較例4〕実施例1のメッキ液からシア
ン化亜鉛を除いた以外は実施例1で用いたメッキ液と同
様のメッキ液を用い、実施例1と同様の方法で試験片に
メッキを施したところ、試験片上には白色のメッキ被膜
が形成されたが、かかるメッキ被膜は光沢性に乏しく、
部分的にムラのあるものであり、実施例1とは大きく異
なる結果であった。
[Comparative Example 4] A test piece was prepared in the same manner as in Example 1 except that zinc cyanide was removed from the plating solution of Example 1 using the same plating solution as that used in Example 1. When plating was performed, a white plating film was formed on the test piece, but the plating film had poor gloss,
It was partially uneven, and the result was significantly different from that of Example 1.

【0024】〔比較例5〕実施例2のメッキ液からスズ
酸ナトリウムを除いた以外は実施例1で用いたメッキ液
と同様のメッキ液を用い、実施例1と同様の方法で試験
片にメッキを施したところ、試験片上には白色のメッキ
被膜が形成されたが、かかるメッキ被膜は光沢性に乏し
く、部分的にムラのあるものであり、実施例2とは大き
く異なる結果であった。
Comparative Example 5 A test piece was prepared in the same manner as in Example 1 using the same plating solution as that used in Example 1 except that sodium stannate was removed from the plating solution of Example 2. When plating was performed, a white plating film was formed on the test piece, but the plating film was poor in gloss and partially uneven, and the result was significantly different from that of Example 2. .

【0025】[0025]

【発明の効果】以上説明したように、本発明白色銅合金
メッキ液は金属アレルギーの原因となるニッケルを含ん
でいないため金属アレルギーを起こし易い人でも容易に
扱うことができるのみならず、メッキの色調を著しく異
ならせず光沢が良く白色優美であるとともに耐蝕性や厚
づけ性等にも優れた白色の銅合金メッキを施すことがで
きるというものである。
As described above, since the white copper alloy plating solution of the present invention does not contain nickel which causes metal allergy, it is not only easy for a person who is prone to metal allergy to handle, but also the plating It is possible to apply a white copper alloy plating that does not significantly change the color tone and has a good gloss and a white grace, as well as excellent corrosion resistance and thickening properties.

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】可溶性銅シアン化物及び可溶性パラジウム
化合物に加え可溶性亜鉛化合物又は可溶性第二スズ化合
物を含有せしめ、界面活性剤0.1〜5ml/L、ピロ
リン酸塩0.1〜5g/L、アンモニア1〜50g/L
を添加するとともに遊離シアン濃度を40〜60g/
L、pHを11〜13に調整したことを特徴とする白色
銅合金メッキ液。
1. A soluble copper compound and a soluble stannic compound are contained in addition to a soluble copper cyanide and a soluble palladium compound, and a surfactant of 0.1 to 5 ml / L, a pyrophosphate of 0.1 to 5 g / L, Ammonia 1-50g / L
And the free cyan concentration of 40-60 g /
A white copper alloy plating solution having L and pH adjusted to 11 to 13.
【請求項2】可溶性銅シアン化物を金属銅換算で5〜2
0g/L、可溶性パラジウム化合物を金属パラジウム換
算量で5〜30g/L含有せしめた請求項1記載の白色
銅合金メッキ液。
2. A soluble copper cyanide of 5 to 2 in terms of metallic copper.
The white copper alloy plating solution according to claim 1, which contains 0 g / L and a soluble palladium compound in an amount of 5 to 30 g / L in terms of metallic palladium.
【請求項3】可溶性亜鉛化合物を金属亜鉛換算で0.1
〜5g/L含有せしめた請求項1、又は2記載の白色銅
合金メッキ液。
3. A soluble zinc compound is 0.1 in terms of metallic zinc.
The white copper alloy plating solution according to claim 1 or 2, wherein the white copper alloy plating solution contains 5 g / L.
【請求項4】可溶性スズ化合物を金属スズ換算で0.1
〜5g/L含有せしめた請求項1、又は2記載の白色銅
合金メッキ液。
4. The soluble tin compound is 0.1 in terms of metallic tin.
The white copper alloy plating solution according to claim 1 or 2, wherein the white copper alloy plating solution contains 5 g / L.
JP7263535A 1995-09-18 1995-09-18 White copper alloy plating solution Expired - Lifetime JP2732044B2 (en)