JPS5966479A - 蓄冷剤の製造方法 - Google Patents

蓄冷剤の製造方法

Info

Publication number
JPS5966479A
JPS5966479A JP57177395A JP17739582A JPS5966479A JP S5966479 A JPS5966479 A JP S5966479A JP 57177395 A JP57177395 A JP 57177395A JP 17739582 A JP17739582 A JP 17739582A JP S5966479 A JPS5966479 A JP S5966479A
Authority
JP
Japan
Prior art keywords
cold
aqueous solution
methylenebisacrylamide
heat
agent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP57177395A
Other languages
English (en)
Other versions
JPH0124435B2 (ja
Inventor
Satsuki Kitani
木谷 五月
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ESUREN KAKO KK
Original Assignee
ESUREN KAKO KK
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ESUREN KAKO KK filed Critical ESUREN KAKO KK
Priority to JP57177395A priority Critical patent/JPS5966479A/ja
Publication of JPS5966479A publication Critical patent/JPS5966479A/ja
Publication of JPH0124435B2 publication Critical patent/JPH0124435B2/ja
Granted legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 本発明は非シキソトロビソクな粘性を有するコンニャク
状の蓄冷剤の製造方法に関するものである。
近年ニーズの多様化により種々の蓄冷剤が提案され実用
に供されつつあるが、その主流は無機塩類水溶液と高分
子ゲルの組合せで所望の温度特性を得ようとするもので
あり、一般には袋状容器に封入された高粘性体であるが
、ゲルの殆どはシキソトロビソクな性質を有し、完全な
包装でなければ液洩れ等に対し万全とは云えないし、又
このようなゲルを一定形状化することは難しい。一方、
ポリアクリルアミドは非イオン性の水溶性高分子でその
水溶液は構造粘性を有し、塩類の影響を受けることもな
いが、高粘度体はタック性がある。
而るに、三官能基をもつN、N−メチレンビスアクリル
アミドやホルムアルデヒドを若干添加して共重合したポ
リアミドの水溶液は低濃度で高粘性を有し、タンク性も
殆どなく、形状化した弾性体が得られることが判明した
が、この実験結果に基づいて、高濃度塩類水溶液中に於
て重合を試みたが、塩類の種類により若干の差はあって
も実用」二問題のないコンニ中り状の固体形状の蓄冷剤
が得られることが判明した。
以下、本発明の好適実施例を説明する。
(実施例1) 塩化カリウム10%水溶液100gにアクリルアミド3
gとアクリルアミ1゛に対するモルLヒ0゜05%のN
、N−メチレンビスアクリルアミドを溶解し、過硫酸カ
リウムを触媒として30゛Cで重合したところ、約10
分の加り^m ’491で容器形状のコンニャク状弾性
体が得られた。
この物質は一方を持ち上げても変形がなく、タック性も
殆どなかった。又、ナイフ等で切って任意の形状にする
ことも出来、乾燥すれば固体になるが吸水させれば復元
する可逆性も有している。
色調はガラス状東名であり、変形に対する復元性を有し
ている。更に温度特性は、−10℃近辺に転移点をもち
、この温度を持続する時間が「い。
上記の他、塩化ナトリウムや塩化カルシウム、更には塩
化マグオンラムやアンモニウム塩、或いは硫酸塩につい
て実施したが、夫々特有の温度特性を示すと共に、ゲル
の状態は殆ど変化がなかった。
共重合したN、N−メチレンビスアクリルアミドの添加
量については、対アクリルアミドモル比が0.02%以
上が好ましい様で、0.1%程度以上を添加してもそれ
程の粘度上昇を示さなかっIこ。
(実施例2) 実施例1のN、N−メチレンビスアクリルアミドに代え
てホルムアルデヒド35%水溶液0.3gを添加し同様
に重合したものは、実施例1のものと比較してややタッ
ク性が少ない他は全く変りがなく、温度特性も同様であ
り、他の塩類中に於ける場合も変化がなかった。添加す
るホルムアルデヒドは、35%水溶液でアクリルアミド
に対する重量比1%〜100%程度の範囲で添加するこ
とが出来るが、添加量が多くなるに従ってタンク性が減
少するが、余剰感加分は蒸発揮散するので正確に共重合
した量を知ることは難しい。
以上の如(本発明によれば、従来にない固体状の蓄冷剤
が得られると共に、塩類を選択することによって任意の
温度性能を付与し得る。
特許出願人 エスレン化工株式会社

Claims (1)

  1. 【特許請求の範囲】 ■アクリルアミドとN、N−メチレンビスアクリルアミ
    ドの混合水溶液に無機塩類を溶解し、過硫酸塩を触媒と
    して重合することを特徴とする蓄冷剤の製造方法。 ■前記N、N−メチレンビスアクリルアミドをホルトア
    ルデヒドとする前記第0項記載の方法。
JP57177395A 1982-10-08 1982-10-08 蓄冷剤の製造方法 Granted JPS5966479A (ja)