JPS61119331A - Method and device for annealing of casting made of aluminum alloy - Google Patents

Method and device for annealing of casting made of aluminum alloy

Info

Publication number
JPS61119331A
JPS61119331A JP23852184A JP23852184A JPS61119331A JP S61119331 A JPS61119331 A JP S61119331A JP 23852184 A JP23852184 A JP 23852184A JP 23852184 A JP23852184 A JP 23852184A JP S61119331 A JPS61119331 A JP S61119331A
Authority
JP
Japan
Prior art keywords
aluminum alloy
casting
press
strain
press die
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP23852184A
Other languages
Japanese (ja)
Inventor
Yoshizo Yamamoto
山本 由三
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to JP23852184A priority Critical patent/JPS61119331A/en
Publication of JPS61119331A publication Critical patent/JPS61119331A/en
Pending legal-status Critical Current

Abstract

PURPOSE:To anneal exactly the titled casting in a comparatively short time by heating the casting in a state that it has been pressed by a mold, and thereafter, quenching it in the pressed state. CONSTITUTION:A piston rod 5a of a press device A is made to ascend, and a casting 7 is pinched and pressed by a movable mold 6 and a fixed mold 4. Subsequently, in a state that the casting 7 has been pressed, the casting 7 is heated by bringing sheath heaters 8, 9 to an electric conduction, and its state is maintained for a prescribed time. Next, the piston rod 5a is made to descend, the casting 7 is fetched from the press device A, and immediately the casting 7 is installed to a press device B. The piston rod 5a is made to ascend and the casting 7 is pinched and pressed by the movable mold 6 and the fixed mold 4. Subsequently, in a state that the casting 7 has been pressed, cooling water is made to flow through water cooling jackets 10, 11, and its state is maintained until a temperature of the casting 7 becomes a room temperature. When it has descended to a room temperature, the casting 7 is fetched from the press device.

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は、鋳造歪等の歪のあるアルミニウム合金製鋳造
品の歪を矯正する方法、及びその方法の実施に直接使用
する装置に関するものである。
DETAILED DESCRIPTION OF THE INVENTION (Field of Industrial Application) The present invention relates to a method for correcting distortions in aluminum alloy castings that have distortions such as casting distortions, and an apparatus used directly to carry out the method. be.

(従来の技術) 従来、アルミニウムダイカスト鋳造品は、溶湯を金型内
に加圧噴入し、凝固後、押出しピン等により離型し、取
出す作業を繰り返すことにより、連続的に製造されてお
り、その成型サイクルは、およそ20〜30秒である。
(Prior art) Conventionally, aluminum die-casting products have been manufactured continuously by repeatedly injecting molten metal into a mold under pressure, releasing it with an ejector pin after solidification, and taking it out. , the molding cycle is approximately 20-30 seconds.

しかし、このようなアルミニウムダイカスト鋳造品の製
造方法においては、鋳造歪等の歪の発生を完全に防止す
ることは困難で、特に薄肉、偏平なものほど、歪発生の
おそれが大であるゆ(発明が解決しようとする問題点) そのため、従来は、鋳造後に、製品の歪を、手作業のハ
ンマリングにより、矯正していたが、その作業が煩雑で
、かつ熟練を要する等の問題点があった。
However, in this method of manufacturing aluminum die-casting products, it is difficult to completely prevent the occurrence of distortions such as casting distortion, and the risk of distortion is particularly high in thinner and flatter products. (Problems to be Solved by the Invention) Conventionally, distortions in the product were corrected by manual hammering after casting, but this work was complicated and required skill. there were.

また、常温でプレスしただけでは、完全に歪を除去でき
なかったり、又は一時的に歪を除去できても、しばらく
すると元の歪が復元したりする等の問題点がある。
In addition, there are problems in that the strain cannot be completely removed by simply pressing at room temperature, or that even if the strain can be removed temporarily, the original strain returns after a while.

このような問題点は、アルミニウム合金のダイカスト鋳
造の場合だけでなく、砂型や金型を用いる普通の鋳造の
場合においても、共通の問題点となっている。
Such problems are common not only in die casting of aluminum alloys, but also in ordinary casting using sand molds or metal molds.

本発明は、このような問題点を解決することを目的とす
るものである。
The present invention aims to solve these problems.

(問題点を解決するための手段) 本発明においては、歪のあるアルミニウム合金製鋳造品
を、押し型により加圧した状態で、加温した後、押し型
により加圧した状態で、急冷することにより、アルミニ
ウム合金製鋳造品の鋳造歪等の歪を、熟練を要するこ・
となく、かつ確実に矯正することができるアルミニウム
合金製鋳造品の歪矯正方法を提供するものである。
(Means for Solving the Problems) In the present invention, a distorted aluminum alloy casting product is heated while being pressurized by a press die, and then rapidly cooled while being pressurized by the press die. As a result, distortion such as casting distortion of aluminum alloy castings can be reduced by skill.
The present invention provides a method for straightening the distortion of an aluminum alloy casting, which can be straightened without any distortion and reliably.

また1本発明においては、アルミニウム合金製鋳造品の
完成形状に対応した形状の押し型をそれぞれ備える2台
のプレス装置からなり、一方のプレス装置には、アルミ
ニウム合金製鋳造品の加温装置を、かつ他方のプレス装
置には、アルミニウム合金製鋳造品の冷却装置を、それ
ぞれ設けてなるアルミニウム合金製鋳造品の歪矯正装置
を提供することにより、上記方法を効率よ〈実施し得る
ようにしである。
In addition, in the present invention, there are two press machines each equipped with a pressing die having a shape corresponding to the finished shape of the aluminum alloy casting, and one of the press machines is equipped with a heating device for the aluminum alloy casting. , and the other press device is provided with a strain straightening device for aluminum alloy castings, each of which is equipped with a cooling device for aluminum alloy castings, thereby making it possible to carry out the above method efficiently. be.

さらに、本発明においては、アルミニウム合金製鋳造品
の完成形状に対応した形状の押し型を備える1台のプレ
ス装置に、アルミニウム合金製鋳造品の加温装置と、ア
ルミニウム合金製鋳造品の冷却装置とを設けてなるアル
ミニウム合金製鋳造品の歪矯正装置を提供することによ
り、上記方法をさらに効率よ〈実施し得るようにしであ
る。
Furthermore, in the present invention, one press device equipped with a pressing mold having a shape corresponding to the completed shape of the aluminum alloy casting product includes a heating device for the aluminum alloy casting product and a cooling device for the aluminum alloy casting product. By providing an apparatus for straightening the strain of an aluminum alloy cast product, the method described above can be carried out more efficiently.

(作用) 歪のあるアルミニウム合金製鋳造品を、押し型により加
圧した状態で、加温すると、歪は除去されるが、この鋳
造品を、押し型から取り出して常温で自然放置しておく
と、鋳造品の温度が下・降するにつれて、元の歪が復元
するおそれがある6本発明のように、鋳造品を、押し型
により加圧した状態で、加温した後、押し型により加圧
した状態で、急冷することにより、上述のような歪が復
元することはなくなる。
(Function) If a distorted aluminum alloy casting is heated while being pressurized by a press mold, the distortion will be removed, but if the cast product is removed from the press mold and left to stand at room temperature. As the temperature of the cast product decreases, the original strain may be restored.6 As in the present invention, the cast product is heated under pressure with a press die, and then By rapidly cooling in a pressurized state, the distortion described above will not be restored.

(実施例) 以下、本発明の一実施例を、添付図面に基づいて説明す
る。
(Example) Hereinafter, an example of the present invention will be described based on the accompanying drawings.

第1図及び第2図は1本発明の第2発明に対応する装置
の一実施例を示す。
1 and 2 show an embodiment of an apparatus corresponding to the second aspect of the present invention.

この装置は、2台のプレス装置(A) (B)からなり
、各プレス装置(A)(B)は、4本の支柱(1)によ
って、四隅を支持された上下1対の水平な上板(2)及
び下板(3)と、上板(2)の下面に固着された固定押
し型(4)と2下板(3)の上面中央に立設され、かつ
上端よりピストンロッド(5a)が進退しうるようにし
た油圧シリンダ装置(5)と、ピストンロッド(5a)
の上端に固着された可動押し型(6)とを、それぞれ備
えている。
This device consists of two press devices (A) and (B), and each press device (A) and (B) consists of a pair of upper and lower horizontal supports supported at their four corners by four columns (1). The plate (2), the lower plate (3), and the fixed press die (4) fixed to the lower surface of the upper plate (2) are erected in the center of the upper surface of the lower plate (3), and the piston rod ( A hydraulic cylinder device (5) that allows the cylinder 5a) to move forward and backward, and a piston rod (5a)
A movable press mold (6) is fixed to the upper end of the mold.

各可動押し型(6)は、ピストンロッド(5a)の上端
に下面中央部を固着された磁性体よりなる水平板状のベ
ース(6a)と、このベース(6a)の上面に磁着させ
た永久磁石よりなる短円柱状の複数のサポートヘッド(
6b)とからなり、加圧しようとするアルミニウム合金
製鋳造品(以下類に鋳造品という)(7)の下面形状に
合致するように、複数のサポートヘッド(6b)をベー
ス(6a)上において自由に移動し得るようにしである
Each movable push mold (6) has a horizontal plate-shaped base (6a) made of a magnetic material whose lower center part is fixed to the upper end of the piston rod (5a), and a horizontal plate-shaped base (6a) that is magnetically attached to the upper surface of this base (6a). Multiple short cylindrical support heads made of permanent magnets (
6b), and a plurality of support heads (6b) are placed on the base (6a) so as to match the lower surface shape of the aluminum alloy casting product (hereinafter referred to as casting product) (7) to be pressurized. This allows them to move freely.

なお、鋳造品(7)は、この実施例においては、計測器
のカバープレートをなす薄肉、偏平な矩形の逆皿状のダ
イカスト品としである。
In this embodiment, the cast product (7) is a thin, flat, rectangular, inverted dish-shaped die-cast product that forms the cover plate of the measuring instrument.

一方のプレス装置(A)における固定押し型(4)と可
動押し型(6)のベース(6a)とには、鋳造品(7)
の加温装置として、公知のシーズヒータ(8) (9)
がそれぞれ内蔵されている。
The bases (6a) of the fixed press die (4) and the movable press die (6) in one press device (A) are made of cast products (7).
Well-known sheathed heaters (8) (9) are used as heating devices for
are each built-in.

また、他方のプレス装置(B)における固定押し型(4
)と可動押し型(6)のベース(6a)とには、鋳造品
(7)の冷却装置として、冷却水が流通するようにした
水冷ジャケット(10)(11)がそれぞれ設けられて
いる。
In addition, the fixed press mold (4) in the other press device (B)
) and the base (6a) of the movable pressing die (6) are respectively provided with water cooling jackets (10) and (11) through which cooling water flows as a cooling device for the cast product (7).

次に、この装置を用いた本発明のアルミニウム合金製鋳
造品の歪矯正方法の実施要領について説明する。
Next, a description will be given of the method for straightening the strain of an aluminum alloy cast product according to the present invention using this apparatus.

まず、プレス装置(A)における油圧シリンダ装置(5
)を作動させて、可動押し型(6)を下降させ、サポー
トヘッド(6b)上に、歪を有する鋳造品(7)を載せ
た後、油圧シリンダ装置(5)におけるピストンロッド
(5a)を上昇させ、可動押し型(6)と固定押し型(
4)とで鋳造品(7)を挾んで加圧する。
First, the hydraulic cylinder device (5) in the press device (A)
) to lower the movable push mold (6) and place the distorted casting (7) on the support head (6b), then move the piston rod (5a) in the hydraulic cylinder device (5). Raise the movable press die (6) and fixed press die (
4) and pressurize the cast product (7).

次に、鋳造品(7)を加圧したまま、シーズヒータ(8
) (9)に通電して、鋳造品(7)を、約150゜〜
200°Cに加温し、そのままの状態を約2〜3分間維
持する。なお、鋳造品(7)をプレス装置(A)に装着
する前から、予めシーズヒータ(8)(9)に通電して
おいてもよい。
Next, while pressurizing the cast product (7), the sheathed heater (8)
) (9) is energized and the cast product (7) is heated at approximately 150°~
Heat to 200°C and maintain the temperature for about 2-3 minutes. Note that the sheathed heaters (8) and (9) may be energized in advance before the cast product (7) is mounted on the press device (A).

次に、油圧シリンダ装置(5)におけるピストンロッド
(5a)を下降させて、可動押し型(6)と固定押し型
(4)とを開き、鋳造品(7)をプレス装置(A)から
取り出し、即座に、鋳造品(7)を、プレス装置(A)
への装着要領と同様にして、プレス装置(B)に装着し
、プレス装置(B)における油圧シリンダ装置(5)の
ピストンロッド(5a)を上昇させて、可動押し型(6
)と固定押し型(4)とで鋳造品(7)を挾んで加圧す
る。
Next, the piston rod (5a) in the hydraulic cylinder device (5) is lowered to open the movable push die (6) and the fixed push die (4), and the cast product (7) is taken out from the press device (A). , immediately press the casting (7) into the press device (A).
In the same manner as in the installation procedure, attach it to the press device (B), raise the piston rod (5a) of the hydraulic cylinder device (5) in the press device (B), and attach the movable push die (6
) and the fixed pressing mold (4) sandwich the casting (7) and pressurize it.

次いで、鋳造品(7)を加圧したまま、水冷ジャケット
(10) (11)に冷却水を流通させて、鋳造品(7
)の温度が常温になるまでそのままの状態を維持する。
Next, cooling water is passed through the water cooling jackets (10) and (11) while the casting product (7) is kept under pressure.
) until the temperature reaches room temperature.

なお、鋳造品(7)をプレス装@(B)に装着する前か
ら、予め水冷ジャケット(10) (11)に冷却水を
流通させておいてもよい。
Note that cooling water may be allowed to flow through the water cooling jackets (10) (11) in advance before the cast product (7) is mounted on the press equipment @(B).

鋳造品(7)の温度が常温まで下降したとき、油圧シリ
ンダ装置(5)におけるピストンロッド(5a)を下降
させて、可動押し型(6)と固定押し型(4)とを開き
、鋳造品(7)をプレス装置(A)から取り出す。
When the temperature of the cast product (7) falls to room temperature, the piston rod (5a) in the hydraulic cylinder device (5) is lowered to open the movable push die (6) and the fixed push die (4), and the cast product (7) is taken out from the press device (A).

このようにして歪を矯正した鋳造品(7)は、常温にお
いて、歪が再度復元することはない。
In the cast product (7) whose distortion has been corrected in this way, the distortion will not be restored again at room temperature.

第3図は、本発明の第3発明に対応する装置の一実施例
を示す。
FIG. 3 shows an embodiment of an apparatus corresponding to the third aspect of the present invention.

この装置は、1台のプレス装置(C)のみからなり、こ
のプレス装置(C)における固定押し型(4′)と可動
押し型(6′)のベース(6a’ )とには、公知のシ
ーズヒータ(8’ ) (9’ )と、水冷ジャケット
(10’ )(11’)とがそれぞれ設けられている。
This device consists of only one press device (C), and the bases (6a') of the stationary press die (4') and the movable press die (6') in this press device (C) are constructed using known methods. Sheathed heaters (8') (9') and water cooling jackets (10') (11') are provided, respectively.

その他の構成は、第1図及び第2図に示す実施例のもの
と同一であり、これらについては、同一の符号を付して
、説明を省略する。
The rest of the structure is the same as that of the embodiment shown in FIGS. 1 and 2, and the same reference numerals are used to omit the explanation.

この第3図に示す装置を用いて1本発明の第1発明の方
法を実施する場合は、鋳造品(7)を、′可動押し型(
6)と固定押し型(4)とで挾んで加圧した後、まず水
冷ジャケット(10’ )(11’ )への冷却水の流
通を停止させて、シーズヒータ(8’)(9’)に通電
して、鋳造品(7)を約150°〜200℃まで加温し
、そのままの状態を約2〜3分維持する。
When carrying out the method of the first aspect of the present invention using the apparatus shown in FIG.
6) and the fixed pressing die (4) and pressurized, first stop the flow of cooling water to the water cooling jackets (10') (11'), and then remove the sheathed heaters (8') (9'). The cast product (7) is heated to about 150° to 200°C by applying electricity, and the state is maintained for about 2 to 3 minutes.

次いで、鋳造品(7)をプレス装置(C)から取り出す
ことなく、可動押し型(6)と固定押し型(4)とで挾
んで加圧したまま、シーズヒータ(8’)(9’)への
通電を停止し、かつ水冷ジャケット(10’ ) (1
1’ )に冷却水を流通させ、鋳造品(7)の温度を常
温まで下降させる。
Next, without taking out the cast product (7) from the press device (C), the sheathed heater (8') (9') is pressed while being sandwiched and pressurized between the movable press die (6) and the fixed press die (4). Stop the power supply to the water cooling jacket (10') (1
1') to lower the temperature of the cast product (7) to room temperature.

その他の実施要領は、第1図及び第2図に示す装置を用
いる場合と同様である。
Other implementation procedures are the same as those using the apparatus shown in FIGS. 1 and 2.

この第3図に示す装置を用いる場合は、プレス装置(C
)が1台で足りること、及び鋳造品(7)を加圧したま
ま、加温から急冷に切換えることができ。
When using the apparatus shown in Fig. 3, press equipment (C
) is sufficient, and it is possible to switch from heating to quenching while keeping the cast product (7) under pressure.

かつ鋳造品(7)のプレス装置への掛は替えの手間を省
くことができる等の利点がある。
In addition, there is an advantage that it is possible to save the effort of changing the casting product (7) on the press device.

なお、以上の実施例においては、鋳造品(7)の加温装
置として、公知のシーズヒータ(8) (9)を用い、
かつ鋳造品(7)の冷却装置として、冷却水が流通する
ようにした水冷ジャケット(10)(11)を用いてい
るが、加温装置として1例えば高周波加熱装置や、熱風
を鋳造品に吹き付けるようにした加温装置等を用いたり
、冷却装置として、冷風を鋳造品に吹き付けるようにし
た空冷式の冷却装置や、その他の冷却装置を用いてもよ
い。
In addition, in the above embodiment, a known sheathed heater (8) (9) is used as a heating device for the cast product (7),
In addition, as a cooling device for the cast product (7), water cooling jackets (10) and (11) through which cooling water flows are used, but as a heating device, for example, a high-frequency heating device or a device that blows hot air onto the cast product is used. A heating device or the like may be used, or an air-cooled cooling device that blows cold air onto the casting, or other cooling device may be used as the cooling device.

(発明の効果) 第1発明の方法によると、アルミニウム合金製鋳造品の
歪を、熟練を要することなく、比較的短時間の間に、確
実に矯正することができ1手作業によるハンマリング矯
正のような失敗のおそれも少ない等の利点がある。
(Effects of the Invention) According to the method of the first invention, distortions in aluminum alloy castings can be reliably corrected in a relatively short period of time without requiring any skill.1 Manual hammering correction There are advantages such as less risk of failure.

、また、第2発明の装置を用いれば、作業を手際よく、
連続的に行なうことができ1作業効率がよい等の利点が
ある。
, Also, if the device of the second invention is used, the work can be done quickly,
It has the advantage that it can be carried out continuously and has good one-work efficiency.

さらに、第3発明の装置を用いれば、装置全体を小型化
できるとともに、アルミニウム合金製鋳造品のプレス装
置への掛は替え手数を少なくすることができ、かつ自動
化が容易である等の利点がある。
Furthermore, if the apparatus of the third invention is used, the entire apparatus can be made smaller, and there are other advantages such as the reduction in the number of changes to the pressing apparatus for aluminum alloy castings, and the ease of automation. be.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図は、本発明の第2発明の装置の一実施例を示す縦
断正面図、 第2図は、第1図のx−X線に沿う拡大矢示図。 第3図は、本発明の第3発明の装置の一実施例を示す縦
断の縦断正面図である。 (A) CB) (C)プレス装置   (1)支 柱
(2)上 板        (3)下 板(4) (
4’ )固定押し型    (5)油圧シリンダ装置(
5a)ピストンロンド   (6) (6″)可動押し
型(6a) (6a’ )ベース     (6b)サ
ポートヘッド(7)アルミニウム合金製鋳造品 (8) (8’ > (9) (9″)シーズヒータ(
10) (10’ )(11) (11’ )水冷ジャ
ケット第1図 第2図      第3因
FIG. 1 is a longitudinal sectional front view showing an embodiment of the apparatus according to the second aspect of the present invention, and FIG. 2 is an enlarged arrow view taken along line XX in FIG. 1. FIG. 3 is a longitudinal sectional front view showing an embodiment of the apparatus according to the third aspect of the present invention. (A) CB) (C) Press device (1) Support column (2) Upper plate (3) Lower plate (4) (
4') Fixed push type (5) Hydraulic cylinder device (
5a) Piston rond (6) (6″) Movable push die (6a) (6a’) Base (6b) Support head (7) Aluminum alloy casting (8) (8’ > (9) (9″) Seed heater(
10) (10') (11) (11') Water cooling jacket Figure 1 Figure 2 Factor 3

Claims (10)

【特許請求の範囲】[Claims] (1)歪のあるアルミニウム合金製鋳造品を、押し型に
より加圧した状態で、加温した後、押し型により加圧し
た状態で、急冷することを特徴とするアルミニウム合金
製鋳造品の歪矯正方法。
(1) Distorted aluminum alloy castings characterized by heating the aluminum alloy castings under pressure with a press die, and then rapidly cooling them under pressure with the press die. Correction method.
(2)加温時の押し型と、急冷時の押し型とが互いに独
立した別個のものである特許請求の範囲第(1)項に記
載のアルミニウム合金製鋳造品の歪矯正方法。
(2) The method for straightening the distortion of an aluminum alloy cast product according to claim (1), wherein the pressing mold for heating and the pressing mold for quenching are independent and separate from each other.
(3)加温時の押し型と、急冷時の押し型とが同一のも
のである特許請求の範囲第(1)項に記載のアルミニウ
ム合金製鋳造品の歪矯正方法。
(3) The method for straightening the strain of an aluminum alloy casting as set forth in claim (1), wherein the pressing mold for heating and the pressing mold for quenching are the same.
(4)アルミニウム合金製鋳造品の完成形状に対応した
形状の押し型をそれぞれ備える2台のプレス装置からな
り、一方のプレス装置には、アルミニウム合金製鋳造品
の加温装置を、かつ他方のプレス装置には、アルミニウ
ム合金製鋳造品の冷却装置を、それぞれ設けてなるアル
ミニウム合金製鋳造品の歪矯正装置。
(4) Consisting of two press machines, each equipped with a pressing mold of a shape corresponding to the finished shape of the aluminum alloy casting, one of the press machines is equipped with a heating device for the aluminum alloy casting, and the other is equipped with a heating device for the aluminum alloy casting. A strain straightening device for aluminum alloy castings, in which each pressing device is provided with a cooling device for the aluminum alloy castings.
(5)加温装置が、ヒータである特許請求の範囲第(4
)項に記載のアルミニウム合金製鋳造品の歪矯正装置。
(5) Claim No. 4, wherein the heating device is a heater.
) Strain correction device for cast aluminum alloy products.
(6)加温装置が、高周波加熱装置である特許請求の範
囲第(4)項に記載のアルミニウム合金製鋳造品の歪矯
正装置。
(6) The strain straightening device for aluminum alloy castings according to claim (4), wherein the heating device is a high-frequency heating device.
(7)冷却装置が、水冷ジャケットである特許請求の範
囲第(4)項乃至第(6)項のいずれかに記載のアルミ
ニウム合金製鋳造品の歪矯正装置。
(7) The strain straightening device for an aluminum alloy cast product according to any one of claims (4) to (6), wherein the cooling device is a water cooling jacket.
(8)各プレス装置における押し型が、固定押し型と可
動押し型とからなり、その少なくとも一方が、磁性体よ
りなるベースと、該ベースに磁着された永久磁石よりな
るサポートヘッドとからなる特許請求の範囲第(4)項
乃至第(7)項のいずれかに記載のアルミニウム合金製
鋳造品の歪矯正装置。
(8) The press die in each press device consists of a fixed press die and a movable press die, at least one of which consists of a base made of a magnetic material and a support head made of a permanent magnet magnetically attached to the base. A strain correction device for aluminum alloy castings according to any one of claims (4) to (7).
(9)アルミニウム合金製鋳造品の完成形状に対応した
形状の押し型を備える1台のプレス装置に、アルミニウ
ム合金製鋳造品の加温装置と、アルミニウム合金製鋳造
品の冷却装置とを設けてなるアルミニウム合金製鋳造品
の歪矯正装置。
(9) A single press machine equipped with a pressing mold of a shape corresponding to the completed shape of the aluminum alloy casting product is equipped with a heating device for the aluminum alloy casting product and a cooling device for the aluminum alloy casting product. Strain straightening device for aluminum alloy castings.
(10)プレス装置における押し型が、固定押し型と可
動押し型とからなり、その少なくとも一方が、磁性体よ
りなるベースと、該ベースに磁着された永久磁石よりな
るサポートヘッドとからなる特許請求の範囲第(9)項
に記載のアルミニウム合金製鋳造品の歪矯正装置。
(10) A patent in which the press die in the press device consists of a fixed press die and a movable press die, at least one of which includes a base made of a magnetic material and a support head made of a permanent magnet magnetically attached to the base. A strain correction device for aluminum alloy castings according to claim (9).
JP23852184A 1984-11-14 1984-11-14 Method and device for annealing of casting made of aluminum alloy Pending JPS61119331A (en)