JPS6213541A - Method for recovering valuable metal from converter slag - Google Patents

Method for recovering valuable metal from converter slag

Info

Publication number
JPS6213541A
JPS6213541A JP60151347A JP15134785A JPS6213541A JP S6213541 A JPS6213541 A JP S6213541A JP 60151347 A JP60151347 A JP 60151347A JP 15134785 A JP15134785 A JP 15134785A JP S6213541 A JPS6213541 A JP S6213541A
Authority
JP
Japan
Prior art keywords
converter slag
slag
content
melting
reducing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
JP60151347A
Other languages
Japanese (ja)
Inventor
Koichi Nakamura
中村 皓一
Satoru Yamaguchi
悟 山口
Seihachiro Takagi
高木 清八郎
Masahiro Fukuda
正博 福田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hamada Heavy Industries Co Ltd
Nippon Steel Corp
Original Assignee
Hamada Heavy Industries Co Ltd
Nippon Steel Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hamada Heavy Industries Co Ltd, Nippon Steel Corp filed Critical Hamada Heavy Industries Co Ltd
Priority to JP60151347A priority Critical patent/JPS6213541A/en
Publication of JPS6213541A publication Critical patent/JPS6213541A/en
Ceased legal-status Critical Current

Abstract

PURPOSE:To recover a valuable metal in a low-P state by selectively adding SiO2, Al2O3, etc., to converter slag together with a carbonaceous reducing material, by subjecting the above to melting-reducing treatment and by regulating the Mn content in the resulting iron melt. CONSTITUTION:One or more kinds among SiO2, Al2O3 an compounds thereof having excellent property of bonding to CaO are selectively added to the converter slag together with a carbonaceous material such as coke etc., which is subjected to melting-reducing treatment of high temp. By carrying out blending and addition of Mn ores or another operation at the above reducing treatment, the Mn content in the iron melt obtained by melting reduction is adjusted to >=25%. In this way, the valuable metal such as Fe, Mn, V, etc., can be recovered from the converter slag in the low-P state.

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は転炉スラグから有価金属を回収する還元処理方
法に関するものである。
DETAILED DESCRIPTION OF THE INVENTION (Field of Industrial Application) The present invention relates to a reduction treatment method for recovering valuable metals from converter slag.

(従来技術) 近年、製鋼スラグの発生量の低減あるいは極低P鋼を製
造するため、溶銑段階であらかじめ脱S1、脱P処理す
る方法が実用化されている。通常の転炉吹錬では溶鋼ト
ン当り100−130 K9の転炉スラグが発生するの
に対し、溶銑脱P処理すると転炉スラグ量が大幅に低減
されるので、溶銑脱P処理した転炉スラグは第1表に示
すように、20〜30チの酸化鉄、4〜10チのMnO
を含有するは第1表 か、1〜3チのV2O,およびほぼ同量のP2O,を含
有しており、通常の転炉スラグに較べてv、0.が多い
という特徴を有している。これは溶洗に含まれる微量の
Vが吹錬によって酸化され、スラグに移行するに当り、
スラグ量が少ないため富化するものであるが、■は貴重
な元素であり、これを回収することは意義がある。ちな
みに本来のV鉱石がたかだか1〜10%のV含有量であ
ることを考えると溶銑脱P処理した転炉スラグは貴重な
V資源である。
(Prior Art) In recent years, in order to reduce the amount of steelmaking slag generated or to produce extremely low P steel, a method of performing de-S1 and de-P treatment in advance at the hot metal stage has been put into practical use. In normal converter blowing, converter slag of 100-130 K9 is generated per ton of molten steel, but when hot metal is dephosphorized, the amount of converter slag is significantly reduced. As shown in Table 1, 20 to 30 T iron oxide, 4 to 10 T MnO
As shown in Table 1, the slag containing V2O and approximately the same amount of P2O as shown in Table 1, has a v, 0. It is characterized by a large number of This is because a trace amount of V contained in melt washing is oxidized by blowing and transferred to slag.
Although it is enriched because the amount of slag is small, (2) is a valuable element and it is significant to recover it. Incidentally, considering that the original V ore has a V content of at most 1 to 10%, converter slag treated with hot metal deP is a valuable V resource.

従来より、転炉スラグを高温で炭素還元すると有価金属
が回収できることが知られているが、一般的には転炉ス
ラグ中に含有しているP2O,を同時に還元して、回収
鉄のPが高くなるので有効に利用できないという欠点が
あり、これを解決するために種々の試みがなされている
。例えば、転炉滓と炭素質還元剤との混合物を同相状態
を保持しながら加熱して転炉滓中に含まれる鉄分を粒鉄
に還元した後、さらに昇温加熱して粒鉄を凝集粗大化す
ることを特徴とする転炉滓の還元処理方法(特開昭56
−123312号公報)。
It has long been known that valuable metals can be recovered by reducing converter slag with carbon at high temperatures; There is a drawback that it is expensive and cannot be used effectively, and various attempts have been made to solve this problem. For example, a mixture of converter slag and a carbonaceous reducing agent is heated while maintaining the same phase state to reduce the iron contained in the converter slag to granular iron, and then the granular iron is coagulated and coarsened by further heating. A method for reducing converter slag characterized by
-123312).

また、炭素および珪素を含む鉄合金の溶融浴を電気弧光
炉内に準備し、これに転炉焼滓を導入して攪拌と加熱を
施すことによシ、転炉廃滓中のP2osまたはV2O,
を還元させ、上記溶融浴から還元スラグを炉外へ排除す
る工程を必要度数にわたり行なうこと、その後、炉内に
残された上記溶融浴中に、その浴温か1450℃以下、
1200℃以上の範囲に到達するのを待って該溶融浴の
1トン当り10〜100 Kpに当る量のソーダ灰を導
入し、談溶融浴中のPまた、さらにはVをソーダ灰系ス
ラグに移行させてから、このスラグを炉外へ排除するこ
と、および、このソーダ灰系スラグを炉外排滓して炉内
゛に残留する溶融浴につき、上記各工程段階を繰返すこ
との結合になることを特徴とする転炉焼滓の脱リン再生
および有価成分回収に供する溶融浴処理方法(特開昭5
7−177911号公報)などが提案されている。
In addition, by preparing a molten bath of an iron alloy containing carbon and silicon in an electric arc furnace, introducing converter slag into it, and subjecting it to stirring and heating, it is possible to remove P2os or V2O from the converter slag. ,
and removing the reduced slag from the molten bath to the outside of the furnace over the necessary number of times;
After waiting for the temperature to reach 1200°C or higher, soda ash in an amount equivalent to 10 to 100 Kp per ton of the molten bath is introduced, and P and even V in the molten bath are converted into soda ash-based slag. After transferring, this slag is removed from the furnace, and this soda ash-based slag is removed from the furnace and the above process steps are repeated for the molten bath remaining in the furnace. A method of treating a molten bath for dephosphorization and regeneration of converter slag and recovery of valuable components, characterized by
7-177911) and the like have been proposed.

しかしながら、前者は転炉スラグ中の酸化鉄を固相状態
で選択的に還元処理してP含有量の低い鉄を得る方法で
あり■については何ら述べられていない。また、熱力学
的にも位温度におけるV2O。
However, the former is a method of selectively reducing iron oxide in the converter slag in a solid state to obtain iron with a low P content, and there is no mention of (2). Also, thermodynamically, V2O at about temperature.

の還元速度はP2O,よりさらに小さいのでVは実質的
に還元されえないと考えられる。一方、後者は転炉スラ
グのP、Vを溶融浴へ還元移行させその後、溶融浴から
ソーダ灰系スラグに再度移行させるなど工程が複雑であ
り、さらに、ソーダ灰系スラグを湿式処理するので特殊
な設備と処理工程を必要とし、能率的でない。
Since the reduction rate of P2O is even lower than that of P2O, it is considered that V cannot be reduced substantially. On the other hand, the latter involves a complicated process in which P and V in the converter slag are reduced and transferred to the molten bath, and then transferred from the molten bath to soda ash slag again.Furthermore, the soda ash slag is wet-processed, so it is a special process. Requires extensive equipment and processing processes, making it inefficient.

(発明の解決しようとする問題点) 本発明は、このような従来法の欠点を解消せんとするも
のであり、転炉スラグからFe、λ(n、Vなどの有価
金属を、P含有量が低く利用しやすい状態で回収する還
元処理方法を目的とするものである。
(Problems to be Solved by the Invention) The present invention aims to eliminate the drawbacks of such conventional methods, and aims to remove valuable metals such as Fe, λ(n, and V) from converter slag by reducing the P content. The purpose of this is to provide a reduction treatment method that recovers waste in a state where it is easy to use and has a low amount of carbon dioxide.

(問題点の解決手段) 本発明者らは上記問題点を解決するため研究を行い、転
炉スラグに炭素質還元剤を添加するとともに一方5i0
2 、 AH,03ならびに、その化合物の一種以上を
選択的に添加して溶融還元処理し、得られる溶融鉄のM
n含有量を25チ以上になるように以下に本発明の詳細
な説明する。
(Means for solving the problems) The present inventors conducted research to solve the above problems, and added a carbonaceous reducing agent to the converter slag, while at the same time
2, M of the molten iron obtained by selectively adding AH,03 and one or more of its compounds and melting reduction treatment.
The present invention will be described below in detail so that the n content is 25 or more.

本発明の第一の特徴は転炉スラグから有価金属を還元回
収するに当り、炭素質還元剤を添加するとともに810
2、AJt203ならびにその化合物の一種以上を選択
的に添加することを前提とする。
The first feature of the present invention is that when reducing and recovering valuable metals from converter slag, a carbonaceous reducing agent is added and 810%
2. It is assumed that AJt203 and one or more of its compounds are selectively added.

一般に還元剤としてはC,Si、Mが広く用いられるが
酸素との親和力が弱いFeO,MnOを還元するには炭
素質還元剤が安価である。
Generally, C, Si, and M are widely used as reducing agents, but carbonaceous reducing agents are inexpensive for reducing FeO and MnO, which have weak affinity with oxygen.

しかしながら、Fe01Mn0に較べると含有量が少な
くかつ、酸素との親和力が強いV2O,を収率よく還元
することは難しい。そこで、V2O5の炭素還元につい
て種々の実験を行なった結果5102、V2O,ならび
にその化合物の一種以上を選択的に添加すると還元収率
が高まることを見出した。この理由は次のように説明で
きる。
However, it is difficult to reduce V2O with a good yield, which has a lower content than Fe01Mn0 and has a strong affinity for oxygen. Therefore, as a result of conducting various experiments regarding carbon reduction of V2O5, it was found that the reduction yield can be increased by selectively adding 5102, V2O, and one or more of their compounds. The reason for this can be explained as follows.

すなわち、実際操巣で得られる転炉スラグには2 c、
o ・Si O,,2CeLO・Fe2O3およびスピ
ネルまたはFe(Mn)o固溶体が代表的な鉱物相とし
て存在しており、P2O,は2CaO: 8102  
中に含有することが知られているが、本発明者等のEP
MA (ElectronProbe Micro A
nalyser)調査結果によると転炉スラグ中のV2
O,は主に、2 CaO・5102および、2CaO・
Fe203に含有しており、CaOと結合していること
を認めている。したがって、CcLOとの結合性が強い
5i02ならびにAL20s を添加するとV2O,と
C,Oの結合が弱まるので還元が容易になる。同様の理
由で8102、A1.2o、を添加するとスラグの脱P
がよくなるので例えば取鍋の酸化防止剤など精錬用フシ
ックスに再生利用することが可能になる。SiO□、N
1tOsの添加量について本発明は特に限定するものC
aOチ ではないが、処理後のスラグ組成が。□。2%+鳩。3
%=0.5〜2.0になる量を添加するのが好ましい。
In other words, the converter slag obtained in actual operation contains 2 c,
o ・SiO,,2CeLO・Fe2O3 and spinel or Fe(Mn)o solid solution are present as typical mineral phases, and P2O, is 2CaO: 8102
Although it is known that EP
MA (Electron Probe Micro A
According to the investigation results, V2 in converter slag
O, is mainly 2CaO・5102 and 2CaO・
It is recognized that it is contained in Fe203 and combined with CaO. Therefore, when 5i02 and AL20s, which have strong bonding properties with CcLO, are added, the bonds between V2O, C, and O are weakened, making reduction easier. For the same reason, adding 8102, A1.2o, dephosphorizes the slag.
This improves oxidation properties, making it possible to reuse it in refining fusics, such as antioxidants for ladles. SiO□,N
The present invention specifically limits the amount of addition of 1 tOs C
Although it is not aOchi, the slag composition after treatment is. □. 2% + pigeon. 3
It is preferable to add the amount such that %=0.5 to 2.0.

この値が2.0以上ではv20.の還元収率が低下、逆
に0.5以下では収率が飽和するので過剰添加になる。
If this value is 2.0 or more, v20. On the other hand, if it is less than 0.5, the yield will be saturated, resulting in excessive addition.

次に、本発明は転炉スラグを高温度の溶融状態化鉄の炭
素還元は低温度でも進行するが、Mn01v20.は低
温度では実質的に還元が進まないので、処理温度を14
00〜1500℃以上に高くし、溶融状態で還元する必
要がある。一般に還元によって酸化鉄が激減するとスラ
グの融点が高くなるが、前述したように8102、A1
.O8を添加すると融点が低下するので、1400〜1
500℃で溶融状態が維持できMn01v20.の還元
が容易となる。
Next, the present invention converts converter slag into a high-temperature molten state.Although the carbon reduction of iron proceeds even at low temperatures, Mn01v20. Since reduction does not substantially proceed at low temperatures, the treatment temperature is set at 14.
It is necessary to raise the temperature to 00 to 1500°C or higher and reduce it in a molten state. Generally, when iron oxide is drastically reduced by reduction, the melting point of slag increases, but as mentioned above, 8102, A1
.. Adding O8 lowers the melting point, so 1400~1
The molten state can be maintained at 500°C and Mn01v20. It becomes easy to reduce the amount of

本発明の第三の、かつまた主柱をなす特徴は転炉スラグ
を溶融還元処理して得られる溶融還元鉄5のMn含有量
が25%以上となるように調整することにある。この第
三の特徴は全く本発明者等の実験結果に基ずくものであ
り、転炉スラグに炭素質還元剤を添加するとともに、一
方、5102、Al2O。
The third and main feature of the present invention is that the Mn content of the molten reduced iron 5 obtained by melting and reducing converter slag is adjusted to 25% or more. This third feature is entirely based on the experimental results of the present inventors, and is based on the addition of a carbonaceous reducing agent to the converter slag, and on the other hand, 5102, Al2O.

ならびにその化合物の一種以上を選択的に添加して溶融
還元処理すると、スラグ中のp、o、は85〜98チが
分離除去されて、溶鉄中および排ガス中に移行するが、
ここで溶鉄中のP含有量はMn含有量の影響を強くうけ
ており、第1図に示すような関係のあることが判明した
。第1図から溶融鉄のMn 含有量を25チ以上にすれ
ば溶融鉄のP含有量は1.5%以下になることが知られ
る。これは溶鉄中のMn含有量が高いほどPの溶解能が
低下して排ガス中に移行するPのガス化率が増大するこ
とを示すものであシ、本発明はこの新知見を利用するこ
とによって想到した転炉スラグからP含有量が低い有価
金属を回収する溶融還元処理方法である。
When one or more of these compounds is selectively added and melted and reduced, 85 to 98 p and o in the slag are separated and removed and transferred to the molten iron and exhaust gas.
It has been found that the P content in molten iron is strongly influenced by the Mn content, and there is a relationship as shown in FIG. It is known from FIG. 1 that if the Mn content of the molten iron is set to 25% or more, the P content of the molten iron becomes 1.5% or less. This indicates that the higher the Mn content in molten iron, the lower the P dissolution ability and the higher the gasification rate of P transferred to exhaust gas.The present invention utilizes this new knowledge. This is a smelting reduction treatment method for recovering valuable metals with a low P content from converter slag.

スラグを還元処理して得られる溶融鉄のMn含有量はス
ラグ組成によってほぼ定まるので、これの調整は例えば
転炉吹錬中にMn鉱石を使用するなどしてスラグのMn
O含有量を高める。あるいは溶融還元処理する際にMn
鉱石を配合、添加するなどによって容易に調整できる。
Since the Mn content of molten iron obtained by reducing slag is almost determined by the slag composition, this can be adjusted, for example, by using Mn ore during converter blowing.
Increase O content. Or Mn during melt reduction treatment.
It can be easily adjusted by blending or adding ores.

ちなみに、MnO含有量6.2チの転炉スラグを調整す
ることなく溶融還元処理して得た溶融鉄のMn含有量は
13〜16%であった。
Incidentally, the Mn content of molten iron obtained by melting and reducing converter slag with an MnO content of 6.2% without adjustment was 13 to 16%.

(実施例) 次に本発明の実施例を示す。(Example) Next, examples of the present invention will be shown.

実施例l Pe0 ; l 4.9 %、Fe2O,; 9.9%
、CaO、’ 41.3チ、5io2; l 1.6 
%、MnO; 6.2 % 、 Al2O3; 2.8
チ、v、o、 ; 2.3 %、P2O,; 2.7 
%の転炉スラグ33Kgに5i02 ; 95%の軽珪
石10に2とMnO;40%、Fe2O3; 31 %
のMn鉱石7Kfおよびコークス5 Kfを配合して、
よく混合した原料55Kfを容量80KVAの電気炉を
用いて温度1550℃に昇温、溶解した後10分間保持
して出湯し、11Kpの還元溶融鉄を得た。溶融鉄の化
学成分を第2表に示す。
Example l Pe0; l 4.9%, Fe2O,; 9.9%
, CaO,' 41.3chi, 5io2; l 1.6
%, MnO; 6.2%, Al2O3; 2.8
Chi, v, o, ; 2.3 %, P2O,; 2.7
Converter slag 33Kg to 5i02; 95% silica stone 10 to 2 and MnO; 40%, Fe2O3; 31%
Blending 7 Kf of Mn ore and 5 Kf of coke,
55 Kf of well-mixed raw materials were heated to 1550° C. using an electric furnace with a capacity of 80 KVA, melted, held for 10 minutes, and tapped to obtain reduced molten iron of 11 Kp. The chemical composition of molten iron is shown in Table 2.

第2表で明らかなように、本発明方法に基すき転炉スラ
グに軽珪石とMn鉱石およびコークスを添加して溶融還
元処理した結果、P含有量が低いFe−Mn−V  系
の有価金属が回収できた。ちなみに、処理後のスラグ組
成はT、Fe ; 1.24%、MnO;o、s3%、
v2o、 ; o、 02%、p、o、 ; o、 0
7%でCaOチ =1.02であった。
As is clear from Table 2, as a result of adding silica stone, Mn ore, and coke to plow converter slag based on the method of the present invention and melting and reducing it, Fe-Mn-V system valuable metals with low P content were obtained. was able to be recovered. By the way, the slag composition after treatment is T, Fe; 1.24%, MnO; o, s3%,
v2o, ; o, 02%, p, o, ; o, 0
At 7%, CaO was 1.02.

5107%+fiJ!、203チ 実施例2 FeO; 14.9 %、Fe2O3; 9.9%、C
6LO;41.3チ、5i02 ; l 1.6%、M
no;6.2%、A1.2o、; 2.8チ、v2o、
 ; 2.3 %、p2o、 ; 2.7%の転炉スラ
グ34KfにU;lO%、ldl、20. ; 45%
、5i02 ’、 9係のM灰7 KPとMnO; 4
0 %、Fe2O3; 31 %のMn鉱石9 KPお
よびコークス5 Kpを配合して、よく混合した原料5
5に9を容量80 KVAの電気炉を用いて温度155
0℃な昇温、溶解した後10分間保持して出湯し、12
Kpの還元溶融鉄を得た。溶融鉄の化学成分を第3表に
示す。
5107%+fiJ! , 203chi Example 2 FeO; 14.9%, Fe2O3; 9.9%, C
6LO; 41.3chi, 5i02; l 1.6%, M
no; 6.2%, A1.2o; 2.8chi, v2o,
; 2.3%, p2o, ; 2.7% converter slag 34Kf U; lO%, ldl, 20. ; 45%
, 5i02', 9th section M Ash 7 KP and MnO; 4
0%, Fe2O3; 31% Mn ore 9 KP and coke 5 Kp were blended to form a well-mixed raw material 5.
5 to 9 using an electric furnace with a capacity of 80 KVA and a temperature of 155
Raise the temperature to 0℃, hold it for 10 minutes after melting, and pour out the hot water.12
A reduced molten iron of Kp was obtained. The chemical composition of molten iron is shown in Table 3.

第3表 第3表から明らかなように、本発明方法に基ずき転炉ス
ラグにAl灰とMn鉱石およびコークスを添加して溶融
還元処理した結果、P含有量が低いFe−Mn −V系
の有価金属が回収できた。ちなみに処理後のスラグ組成
はT、Fe ; 1.22%、MnO;0.57%、v
2o、 :  0.04 %、p、o、 :  0.1
1 %で、実施例3 FeO: 14.4%、Fe2O3; 7.3 %、C
aO”、 43.8係、5102 ;10.9 %、M
nO; 12.5 %、Al2O5:2.2チ、v2o
、 ;  1.9チ、p、o、; 2.1%の吹錬中に
Mn鉱石を使用したMnO含有量が高い転炉スラグ32
に2に5i02 ; 95%の軽珪石9 KPとU;X
Oチ、A1.203 ; 45チ、5i02 ; 9襲
のM灰9 Kgおよびコークス3 KPを添加して、よ
く混合した原料53KPを容量80 KVAの電気炉を
用いて温度1550℃に昇温、溶解した後10分間保持
して出湯し、s、s Kyの溶融還元鉄を得た。溶融鉄
の化学成分を第4表に示す。
Table 3 As is clear from Table 3, as a result of melting and reducing converter slag by adding Al ash, Mn ore, and coke based on the method of the present invention, Fe-Mn-V with low P content was obtained. Valuable metals in the system were recovered. By the way, the slag composition after treatment is T, Fe; 1.22%, MnO; 0.57%, v
2o, : 0.04%, p,o, : 0.1
1%, Example 3 FeO: 14.4%, Fe2O3; 7.3%, C
aO", 43.8 section, 5102; 10.9%, M
nO; 12.5%, Al2O5: 2.2chi, v2o
Converter slag with high MnO content using Mn ore during blowing 32
2 to 5i02; 95% light silica 9 KP and U;
Ochi, A1.203; 45chi, 5i02; 9 kg of M ash and 3 KP of coke were added, and 53 KP of the well-mixed raw material was heated to 1550°C using an electric furnace with a capacity of 80 KVA. After melting, the mixture was held for 10 minutes and tapped to obtain molten reduced iron of s and s Ky. The chemical composition of the molten iron is shown in Table 4.

第4表 第4表から明らかなように、本発明方法に基すきMnO
含有量が高い転炉スラグに軟珪石とM灰およびコークス
を添加して溶融還元処理した結果、P含有量が低いFe
−Mn−V系の有価金属が回収できた。ちなみに、処理
後のスラグ組成はT、Fe;1.15%、MnO; 0
.50%、v2o、 ; o、 02%、た。
Table 4 As is clear from Table 4, MnO based on the method of the present invention
As a result of adding soft silica stone, M ash, and coke to converter slag with a high content and melting and reducing it, Fe with a low P content was produced.
-Mn-V-based valuable metals were recovered. By the way, the slag composition after treatment is T, Fe; 1.15%, MnO; 0
.. 50%, v2o; o, 02%.

(発明の効果) 以上のように、本発明は転炉スラグからFe、Mn、V
  などの有価金属を、P含有量が低い状態′で回収す
ることを可能とする還元処理方法である。
(Effects of the Invention) As described above, the present invention can extract Fe, Mn, and V from converter slag.
This is a reduction treatment method that makes it possible to recover valuable metals such as P in a state where the P content is low.

実施例から知られるように回収金属は安価なFe −M
n −V合金として実用に供せられるものであり、回収
メリットの向上に寄与する効果大なるものがある。
As is known from the examples, the recovered metal is inexpensive Fe-M.
It can be put to practical use as an n-V alloy, and has great effects that contribute to improving recovery benefits.

また、これを原料として例えば酸化、還元法あるいは湿
式法などの従来技術を用い高品位の合金鉄を製造するこ
とが出来る。
Furthermore, high-grade ferroalloy can be produced from this raw material using conventional techniques such as oxidation, reduction, or wet methods.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は転炉スラグを溶融還元処理実験において発生し
た溶融還元銑中の[Mn%〕とl”Pl)との関係を示
すグラフである。
FIG. 1 is a graph showing the relationship between [Mn%] and l''Pl) in molten reduced pig iron generated in a converter slag smelting reduction treatment experiment.

Claims (1)

【特許請求の範囲】[Claims] 転炉スラグに炭素質還元剤を添加するとともに、一方、
SiO_2、Al_2O_3ならびにその化合物の一種
以上を選択的に添加して溶融還元処理し、得られる溶融
鉄のMn含有量が25%以上になるように調整すること
を特徴とする転炉スラグから有価金属を回収する方法。
While adding a carbonaceous reducing agent to the converter slag,
Valuable metals from converter slag characterized by selectively adding one or more of SiO_2, Al_2O_3 and their compounds and subjecting the resulting molten iron to a melting reduction treatment so that the Mn content of the resulting molten iron is adjusted to 25% or more. How to recover.
JP60151347A 1985-07-11 1985-07-11 Method for recovering valuable metal from converter slag Ceased JPS6213541A (en)