JPS6367464B2 - - Google Patents
Info
- Publication number
- JPS6367464B2 JPS6367464B2 JP56097131A JP9713181A JPS6367464B2 JP S6367464 B2 JPS6367464 B2 JP S6367464B2 JP 56097131 A JP56097131 A JP 56097131A JP 9713181 A JP9713181 A JP 9713181A JP S6367464 B2 JPS6367464 B2 JP S6367464B2
- Authority
- JP
- Japan
- Prior art keywords
- foam
- defective part
- stock solution
- foaming
- plastic
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired
Description
【発明の詳細な説明】
本発明はプラスチツク発泡体において、その成
型時に発生する欠損部を補修する方法の改良に関
するものである。
型時に発生する欠損部を補修する方法の改良に関
するものである。
従来、車輛、家具等のクツシヨン材として使用
されるプラスチツク発泡体又は人形、ボール等の
玩具に使用されるプラスチツク発泡体は通常軟質
或は半硬質のポリウレタン原液を所望型状を有す
るモールド型内に注入し、発泡キユアせしめた
後、該型より取出し成形品をえているものであ
る。然しながらこの場合往々にして発泡原液のバ
ランスのくずれや型温その他が基因して該成形品
の表面に一部の空洞、キレツなどの欠損部を生ず
るものであつた。これらの欠損部は成形品の形
状、大きさにより夫々異なるが通常2〜30%程度
に達するものである。
されるプラスチツク発泡体又は人形、ボール等の
玩具に使用されるプラスチツク発泡体は通常軟質
或は半硬質のポリウレタン原液を所望型状を有す
るモールド型内に注入し、発泡キユアせしめた
後、該型より取出し成形品をえているものであ
る。然しながらこの場合往々にして発泡原液のバ
ランスのくずれや型温その他が基因して該成形品
の表面に一部の空洞、キレツなどの欠損部を生ず
るものであつた。これらの欠損部は成形品の形
状、大きさにより夫々異なるが通常2〜30%程度
に達するものである。
而してこのような欠損部をそのまま放置してお
くと商品価値が著しく低減するため通常該欠損部
をハサミ、ナイフ等によりほぼ円形状にきりと
り、接着剤を塗布した後、予め用意した同径の発
泡体片を埋め込み且つはみ出した部分をカツタ
ー、ハサミ等にて切断して仕上げているものであ
る。
くと商品価値が著しく低減するため通常該欠損部
をハサミ、ナイフ等によりほぼ円形状にきりと
り、接着剤を塗布した後、予め用意した同径の発
泡体片を埋め込み且つはみ出した部分をカツタ
ー、ハサミ等にて切断して仕上げているものであ
る。
従つて補修に要する工程が極めて煩雑であると
共に作業時間を著しく浪費するものであつた。
共に作業時間を著しく浪費するものであつた。
本発明はかかる現状に鑑み鋭意研究を行つた結
果、簡単な操作にて且つ短時間に補修する方法を
見出したものである。即ち本発明方法はプラスチ
ツク発泡体の欠損部を補修する方法において、該
欠損部をそのまま或はその周辺部を切取つた後、
プラスチツク発泡原液を注入して発泡せしめ、必
要に応じて加熱キユアを行つて該欠損部を封止し
た後、余剰部分を切断して平滑面を形成せしめる
ことを特徴とするものである。
果、簡単な操作にて且つ短時間に補修する方法を
見出したものである。即ち本発明方法はプラスチ
ツク発泡体の欠損部を補修する方法において、該
欠損部をそのまま或はその周辺部を切取つた後、
プラスチツク発泡原液を注入して発泡せしめ、必
要に応じて加熱キユアを行つて該欠損部を封止し
た後、余剰部分を切断して平滑面を形成せしめる
ことを特徴とするものである。
本発明方法は発泡体の欠損部にまず液状のプラ
スチツク発泡原液を注入するため該欠損部が如何
なる形状を有するとしても該原液は欠損部の隅々
まで容易に浸み込むように充填することができ
る。従つてこの原液を発泡せしめてなる発泡体は
該欠損部に何等空隙部を生成せしめることなく十
分に封止することが出来る。
スチツク発泡原液を注入するため該欠損部が如何
なる形状を有するとしても該原液は欠損部の隅々
まで容易に浸み込むように充填することができ
る。従つてこの原液を発泡せしめてなる発泡体は
該欠損部に何等空隙部を生成せしめることなく十
分に封止することが出来る。
なお発泡原液としては特に限定するものではな
いが発泡体がポリウレタン発泡体の場合にはポリ
ウレタン原液を使用するものであり、その場合常
温によりキユアしうるコールドキユアタイプのも
のが好ましい。
いが発泡体がポリウレタン発泡体の場合にはポリ
ウレタン原液を使用するものであり、その場合常
温によりキユアしうるコールドキユアタイプのも
のが好ましい。
又欠損部に注入するための発泡原液注出機とし
ては小吐出量のものが望ましくワンシヨツト2
g/sec〜30g/sec程度のものが好ましい。
ては小吐出量のものが望ましくワンシヨツト2
g/sec〜30g/sec程度のものが好ましい。
次に本発明の実施例を図面により説明する。
実施例
第1図に示す如くポリウレタン発泡体からなる
自動車用クツシヨン材1の表面に直径4cm、深さ
2cmの空洞の欠損部2を生成した。この欠損部2
に小吐出量発泡機3にて第1表に示す如き組成か
らなるポリウレタン発泡原液4を10g注入し第2
図に示す如く該原液を発泡せしめた発泡体5にて
封止した。
自動車用クツシヨン材1の表面に直径4cm、深さ
2cmの空洞の欠損部2を生成した。この欠損部2
に小吐出量発泡機3にて第1表に示す如き組成か
らなるポリウレタン発泡原液4を10g注入し第2
図に示す如く該原液を発泡せしめた発泡体5にて
封止した。
第 1 表
三管能OH価28のポリエーテルポリオール
100.0重量部 ジエタノールアミン 2.0 〃 水 3.0 〃 シリコーン油 2.0 〃 ダブコ33LV(アミン触媒) 0.8 〃 トリレンジイソシアネート 36.0 〃 ジフエニルメタンジイソシアネート 10.0 〃 この状態にて5分間放置した後カツターにてそ
の余剰の突出部を第3図に示す如く切断して本発
明方法による補修部をえた。
100.0重量部 ジエタノールアミン 2.0 〃 水 3.0 〃 シリコーン油 2.0 〃 ダブコ33LV(アミン触媒) 0.8 〃 トリレンジイソシアネート 36.0 〃 ジフエニルメタンジイソシアネート 10.0 〃 この状態にて5分間放置した後カツターにてそ
の余剰の突出部を第3図に示す如く切断して本発
明方法による補修部をえた。
本発明方法によれば次の如き効果を有するもの
である。
である。
(1) 作業工程が極めて簡単である。
(2) 生産性が著しく向上する。
(3) 外観を美麗に仕上げることが出来る。
(4) 安価に補修することが出来る。
第1図乃至第3図は本発明方法を実施するため
の工程概略説明図である。 1……発泡体、2……欠損部、3……発泡機、
4……発泡原液、5……補修発泡体。
の工程概略説明図である。 1……発泡体、2……欠損部、3……発泡機、
4……発泡原液、5……補修発泡体。
Claims (1)
- 1 プラスチツク発泡体の欠損部を補修する方法
において、該欠損部をそのまま或はその周辺部を
切取つた後、プラスチツク発報原液を注入して発
泡せしめ、必要に応じて加熱キユアを行つて該欠
損部を封止した後余剰部分を切断して平滑面を形
成せしめることを特徴とする発泡体の補修方法。