JPS6445708A - Production of composite carbon nitride - Google Patents
Production of composite carbon nitrideInfo
- Publication number
- JPS6445708A JPS6445708A JP20305587A JP20305587A JPS6445708A JP S6445708 A JPS6445708 A JP S6445708A JP 20305587 A JP20305587 A JP 20305587A JP 20305587 A JP20305587 A JP 20305587A JP S6445708 A JPS6445708 A JP S6445708A
- Authority
- JP
- Japan
- Prior art keywords
- atmosphere
- temperature
- nitrogen
- heated
- powder
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
Description
【発明の詳細な説明】
〔産業上の利用分野〕
本発明は、極めて強靭で高品質な窒素含有サーメットの
製造に必要とする硬質原料の、Ti。[Detailed Description of the Invention] [Industrial Field of Application] The present invention relates to Ti, a hard raw material required for the manufacture of extremely tough and high-quality nitrogen-containing cermets.
’ra、 W、 Moの複合炭窒化物の製造法に関する
。This relates to a method for producing a composite carbonitride of ra, W, and Mo.
本発明による複合炭窒化物を原料とした窒素含有サーメ
ットは例えば高速、高送り条件下で使用する切削工具等
に有効に利用できる。The nitrogen-containing cermet made from composite carbonitrides according to the present invention can be effectively used, for example, in cutting tools used under high-speed and high-feed conditions.
Ti、 Ta、 W、 Moの炭窒化物をN1やCO等
の金属で結合した窒素含有サーメットは、従来の窒素を
含有しないサーメットに比べ、その硬質分散相が著しく
微粒になるため、切削工具としての耐塑性変形性、耐熱
疲労性が大幅に改善されることが知られている(特公昭
49−1364号公報)。
Nitrogen-containing cermets, which bond carbonitrides of Ti, Ta, W, and Mo with metals such as N1 and CO, are known to have significantly improved resistance to plastic deformation and thermal fatigue as cutting tools compared to conventional cermets that do not contain nitrogen, because their hard dispersed phase is remarkably finer (Japanese Patent Publication No. 49-1364).
ところで、この種のサーメットの作製において、真空中
での焼結を行うと、サーメット合金中に含有される炭窒
化物が分解し、いわゆる脱窒現象が起きて窒素添加の効
果が減少したり、また、その際に生じた窒素ガスが焼結
体から充分に抜けずに焼結後にボアとして残存し、いず
れも窒素含有サーメットの工具としての信頼性を著しく
低下させることになる。そのために、上記特公昭49−
1364号公報には、該サーメットを真空中ではなく窒
素雰囲気中で焼結することによシ、窒化物の分解を抑え
るという技術が開示されている。Incidentally, when sintering this type of cermet is performed in a vacuum, the carbonitrides contained in the cermet alloy decompose, causing a so-called denitrification phenomenon that reduces the effect of nitrogen addition. Furthermore, the nitrogen gas generated at that time does not fully escape from the sintered body and remains as a bore after sintering, both of which significantly reduce the reliability of the nitrogen-containing cermet as a tool. For this reason, the above-mentioned Japanese Patent Publication No. 49-
Patent No. 1364 discloses a technique for suppressing the decomposition of nitrides by sintering the cermet in a nitrogen atmosphere rather than in a vacuum.
さらに、含有窒素量が増すと脱窒量も増すため、その抑
制のためには雰囲気窒素圧を80Torr以上必要とす
るが、焼結時の該サーメットからの脱ガスが不充分とな
る欠点があった。Furthermore, as the nitrogen content increases, the amount of denitrification also increases. To suppress this, an atmospheric nitrogen pressure of 80 Torr or higher is required, but this has the drawback of insufficient degassing from the cermet during sintering.
その克服法として、サーメット中に含有される金属元素
の複合炭窒化物を予め製造して、窒素解離圧を下げ、焼
結中の脱窒を極力抑える方法が提案されている(例えば
特公昭56−51201号公報等)。To overcome this problem, a method has been proposed in which a composite carbonitride of the metal elements contained in the cermet is manufactured in advance to lower the nitrogen dissociation pressure and minimize denitrification during sintering (for example, Japanese Patent Publication No. 56-51201).
さらに、該複合炭窒化物の粉末を微粒にするために、酸
化物を出発原料とし、これに炭素粉末を混合し、窒素気
流中にて加熱させるという試みがなされている(例えば
特開昭61−291408号公報等)。Furthermore, in order to make the powder of the composite carbonitride into fine particles, attempts have been made to use an oxide as a starting material, mix it with carbon powder, and heat it in a nitrogen stream (for example, Japanese Patent Publication No. 61-291408).
また、このような従来の複合炭窒化物の製造法は、開放
型ボート送シの連続炉で、窒素を流したままの状態にし
て、ボートを順次送っていく方式で行なうのが一般的で
あった。Furthermore, conventional methods for producing such composite carbonitrides typically involved using an open-type boat-feeding continuous furnace, where nitrogen was continuously flowed through the furnace while boats were sequentially fed through.
しかしながら、従来の酸化物と炭素との混合物に窒素を
流して複合炭窒化物を作製するという方法では、遊離炭
素、酸素が残存し、得られた複合炭窒化物を原料に用い
たサーメットを作製する際の焼結過程における焼結性を
劣化させ、その結果、工具としての特性である耐摩耗性
や靭性を低下させてしまうという問題があった。
However, the conventional method of producing composite carbonitrides by flowing nitrogen through a mixture of oxides and carbon had a problem in that free carbon and oxygen remained, degrading the sinterability during the sintering process when producing cermets using the resulting composite carbonitrides as raw materials, and consequently reducing the wear resistance and toughness, which are the properties of tools.
本発明はこの問題点を解決して、金属酸化物と炭素粉末
を原料として、酸素や遊離炭素の残存を防止し、しかも
微細な粉末で焼結性の良いTi、 Ta、 W、 Mo
の複合炭窒化物の製造法を提案することを目的とするも
のである。This invention solves this problem by using metal oxides and carbon powder as raw materials, preventing the residue of oxygen and free carbon, and producing fine powders with good sinterability of Ti, Ta, W, and Mo.
The objective is to propose a method for producing composite carbonitrides.
〔問題点を解決するための手段及び作用〕上記の問題点
の解決手段を求めて、本発明者らは、酸化物を出発原料
とした複合炭窒化物の生成過程について詳細な検討を行
った。[Means and actions for solving the problems] In search of means to solve the above problems, the present inventors conducted a detailed study on the process of producing composite carbonitrides using oxides as starting materials.
その結果、前記のように連続炉で窒素を流した状態で開
放型ボート送υ方式で、酸化物原料から複合炭窒化物を
作製する従来法は、明らかに製造工程が簡略化されてお
り、かつ酸化物原料自体が元来微粒な粉末であるため、
生成する複合炭窒化物粉末も微粒になる点で有効なもの
であるが、その反応は非常に複雑であることが判った。As a result, the conventional method of producing composite carbonitrides from oxide raw materials using an open-type boat transport method while flowing nitrogen in a continuous furnace, as described above, clearly simplifies the manufacturing process, and the oxide raw materials themselves are originally fine powders.
The resulting composite carbonitride powder is effective in that it is finely granulated, but the reaction itself was found to be extremely complex.
これは、還元反応に加え、炭化、窒化各反応が起こり、
さらに固溶化反応も生じるためであシ、加熱に伴い、ま
ず各酸化物の還元反応がCOガスの発生として進行し、
引き続き窒化、炭化が重なり合うように起こるものであ
るという知見を得た。This involves not only a reduction reaction, but also carbonization and nitriding reactions.
Furthermore, a solid solution reaction also occurs, and as heating progresses, the reduction reaction of each oxide proceeds first as the generation of CO gas.
We gained the insight that nitriding and carbonization occur in an overlapping manner.
この知見に基き検討したところ、酸素を完全に除去する
ためには、換言すれば酸化物の還元反応を促進するため
には、加熱中に還元雰囲気をつくりだす水素を流すとよ
いことが判明した。Based on this finding, our investigation revealed that in order to completely remove oxygen, or in other words, to promote the reduction reaction of oxides, it is effective to flow hydrogen, which creates a reducing atmosphere, during heating.
そして、充分に酸素が抜けた後で窒素を流すのが理想的
手段であるといえる。しかし、実際には、窒素を流さな
ければ、ある温度から粒成長が始tb、当初の目的であ
る微粒化が充分には図れない。Ideally, nitrogen should be introduced after sufficient oxygen has been removed. However, in reality, without nitrogen, grain growth begins at a certain temperature, and the initial goal of micronization cannot be fully achieved.
本発明者らは、これらの状況に鑑みて、酸化物を原料と
し、酸素除去、遊離炭素の残留防止と微粒化の両方を達
成できるような加熱方法、特に雰囲気条件と温度条件に
ついて研究を重ね、TiO2,Ta1O1,wo、、
MnO2及び炭素粉末を出発原料として混合し、該混合
物を水素雰囲気中で加熱した後、1200℃以上150
0℃以下の温度で窒素雰囲気に切換えて加熱し、引き続
き該窒素雰囲気中で1500℃以上2100℃以下の温
度に保持して反応せしめることを特徴とするTi、 T
a、 W、 Moの複合炭窒化物の製造法である本発明
に到達したのである。In view of these circumstances, the inventors have conducted extensive research on heating methods, particularly atmospheric and temperature conditions, that can use oxides as raw materials and achieve both oxygen removal, prevention of residual free carbon, and atomization.
MnO2 and carbon powder are mixed as starting materials, and the mixture is heated in a hydrogen atmosphere, then heated to 1200°C or higher.
The Ti, T reaction is characterized by switching to a nitrogen atmosphere and heating at a temperature below 0°C, and then continuing to react while maintaining a temperature of 1500°C to 2100°C in the nitrogen atmosphere.
We have arrived at the present invention, which is a method for producing a composite carbonitride of a, W, and Mo.
本発明はTi、 Ta、 W、 Moを、それぞれTi
O2゜Tag os 、 WO3、MoOs という
酸化物で供給し、これに炭素粉末を混合し、これを加熱
処理するに際し、まず還元反応が進行する低温側では水
素雰囲気で加熱し、加熱昇温を続けて1200℃以上1
500℃以下までの温度域に入った時点で雰囲気を窒素
に切換え引き続きこの窒素雰囲気中で1500℃以上2
100℃以下で加熱することにより、炭窒化反応をさせ
てTi、 Ta、 W。This invention uses Ti, Ta, W, and Mo, respectively
The oxides O2°Tag os, WO3, and MoOs are supplied, and carbon powder is mixed with them. When this mixture is heat-treated, it is first heated in a hydrogen atmosphere at the low temperature side where the reduction reaction proceeds, and the heating is continued to raise the temperature to over 1200°C.
Once the temperature drops below 500°C, the atmosphere is switched to nitrogen, and the temperature is then maintained above 1500°C in this nitrogen atmosphere for 2 minutes.
By heating to below 100°C, a carbonitriding reaction occurs, producing Ti, Ta, and W.
MOの複炭窒化物を得る方法である。窒素雰囲気圧力は
50 Torr以上10気圧以下とすることが特に好ま
しい。This is a method for obtaining MO double carbonitrides. It is particularly preferable that the nitrogen atmosphere pressure be between 50 Torr and 10 atmospheres.
このように酸化物を出発原料に用いることで、微粉末が
得られ、また、酸化物の還元反応は水素雰囲気中で充分
に進行できるので、酸素含有量を著しく低下させること
ができ、かつ、酸素はCOガスとして抜けるため、炭化
するために必要な量の炭素以外に還元のために混合して
おいた炭素も、その役割を果して抜けてゆく。その結果
、残留酸素や遊離炭素の著しく少ない良質な複合炭窒化
物が得られる。By using oxides as starting materials in this way, fine powder can be obtained. Furthermore, since the reduction reaction of oxides can proceed sufficiently in a hydrogen atmosphere, the oxygen content can be significantly reduced. Moreover, since the oxygen escapes as CO gas, the carbon mixed in for reduction, in addition to the amount of carbon necessary for carbonization, also fulfills its role and escapes. As a result, high-quality composite carbonitrides with significantly low levels of residual oxygen and free carbon can be obtained.
従って、本発明の複合炭窒化物を用いてサーメットを作
製すると、非常に焼結性が良く、切削特性においても耐
摩耗性、靭性、耐熱亀裂性の極めて優れた、信頼性の高
い合金が得られるのである。Therefore, when a cermet is fabricated using the composite carbonitride of the present invention, a highly reliable alloy is obtained that exhibits excellent sinterability, wear resistance, toughness, and thermal crack resistance in terms of cutting properties.
以下、本発明における一般的方法と制限理由を述べる。The general methods and limitations of the present invention are described below.
1)水素雰囲気加熱条件
水素雰囲気圧力は10−”Torr以上10気圧以下と
する。10−3Torr未満では酸素除去の効果がなく
、10気圧を越えてもその効果に差異がない上に、高圧
製造設備となり設備的に無駄が生じるので好ましくない
。この雰囲気に保持する時間については、特に制限する
ところはない。1) Hydrogen Atmosphere Heating Conditions: The hydrogen atmosphere pressure should be between 10⁻³ Torr and 10 atmospheres. Below 10⁻³ Torr, there is no effect in removing oxygen, and above 10 atmospheres, there is no difference in effect, and it becomes a high-pressure manufacturing facility, which is undesirable as it results in equipment waste. There are no particular restrictions on the duration of holding in this atmosphere.
2)昇温速度
常温(加熱処理開始)から1500℃以上2100℃以
下の最高到達温度までの全温度域で1〜b
小さいと粒成長するし、100℃/分より大きいと、酸
素、遊離炭素を充分に除去することができない。2) Heating rate: If the heating rate is too small, grain growth will occur, and if it is greater than 100°C/min, oxygen and free carbon cannot be sufficiently removed.
5)窒素供給開始温度 1200℃以上1500℃以下で窒素供給を開始する。5) Nitrogen supply initiation temperature Nitrogen supply should be initiated at a temperature between 1200°C and 1500°C.
1200℃未満で供給すると、該複合炭窒化物中に酸素
が残留し、1500℃を越えても窒素供給しないでおく
と粒成長をきたし、合金の硬度を低下させることになる
ので好ましくない。If nitrogen is supplied at a temperature below 1200°C, oxygen will remain in the composite carbonitride, and if nitrogen is not supplied even when the temperature exceeds 1500°C, grain growth will occur, which will reduce the hardness of the alloy, and is therefore undesirable.
4)加熱処理中の窒素雰囲気圧力
30 Torr以上10気圧以下とする。30Torr
未満では窒素供給による微細化の効果が得られず、また
10気圧を越えてもその効果に差異はないに加え、設備
的に無駄が生じるので好ましくない。4) The nitrogen atmosphere pressure during heat treatment shall be between 30 Torr and 10 atmospheres.
Below 10 atmospheres, the atomization effect from nitrogen supply is not obtained, and exceeding 10 atmospheres does not make any difference in effect, and is also undesirable because it results in wasted equipment.
5)反応温度
窒素雰囲気中で1500℃以ム2100℃以下で保持し
反応させる。1500℃未満では固溶が不充分で好まし
くなく、一方% 2100℃を越えると粒生長が著しく
なるので好ましくない。5) Reaction temperature: The reaction should be carried out in a nitrogen atmosphere at a temperature between 1500°C and 2100°C. Below 1500°C, solid solution is insufficient and undesirable, while above 2100°C, grain growth becomes excessive and is also undesirable.
6)最高到達温度での保持時間
10分以上5時間以下が好ましい。10分未満では還元
反応が不充分であり、5時間を越えると粒成長をきたす
ので好ましくない。6) The holding time at the highest temperature reached is preferably 10 minutes to 5 hours. Less than 10 minutes results in insufficient reduction reaction, and more than 5 hours is undesirable as it leads to grain growth.
以下、実施例により本発明を具体的に説明する。The present invention will be specifically described below with reference to examples.
実施例1
TiO1粉末、Tag(%粉末、WO,粉末、MOO!
粉末とC粉末を混合して水練り造粒し、1400℃まで
1気圧の水素雰囲気中で加熱の後、 PN、 = 30
0 ’rorrの窒素雰囲気に切換え、1750℃で1
時間保持し、本発明の複合炭窒化物Af、得た。なお、
加熱処理開始から1750℃までの昇温速度は10℃/
分で行なった。Example 1 TiO1 powder, Tag (% powder, WO, powder, MOO!
The powder and C powder were mixed and granulated with water, then heated to 1400°C in a hydrogen atmosphere at 1 atmosphere, followed by PN, = 30
Switch to a nitrogen atmosphere of 0 'rorr, and set to 1750°C.
The compound carbonitride Af of the present invention was obtained by holding it for a period of time.
The heating rate from the start of the heat treatment to 1750°C was 10°C/
It was done in minutes.
比較として、同様に造粒したものをPN!= 500
Torrの窒素雰囲気下で1750℃まで10℃/分の
昇温速度で加熱し、この条件で1時間保持した比較量B
を得た。For comparison, a similarly granulated product was prepared as PN! = 500.
Comparative quantity B was heated to 1750°C at a heating rate of 10°C/min under a Torr nitrogen atmosphere and held under these conditions for 1 hour.
I obtained it.
A、B各試料の分析結果を第1表に示す。The analysis results for samples A and B are shown in Table 1.
第1表から、本発明品Aと比較量Bは粒度では殆んど差
がないものの、本発明品Aでは遊離炭素及び酸素量が著
しく減少していることが、明らかに判る。Table 1 clearly shows that although there is almost no difference in particle size between product A and comparative quantity B, product A of the present invention shows a significant decrease in free carbon and oxygen content.
得られた複合炭窒化物A、BにそれぞれNi。Ni was added to the obtained composite carbonitrides A and B, respectively.
COを重量ずつ添加して、サーメット合金を作製すべ(
,1450℃で1時間焼結した。得られた合金は、本発
明品Aを原料としたものには巣が殆んど存在しなかった
のに対し、比較量Bを原料としたものは、AOAタイプ
(超硬工具協会規格CIS O06B −1983)の
巣が認められた。To produce a cermet alloy, add CO in increments by weight.
The alloy was sintered at 1450°C for 1 hour. The alloy obtained using product A of the present invention as the raw material contained almost no porosity, whereas the alloy obtained using comparative quantity B as the raw material showed AOA type porosity (CIS O06B-1983 standard of the Japan Carbide Tool Association).
冥施例2
Ti:Ta:W:Mo=0.75 :α10:[110
:α05゜C:N=(L55:(L45.非金属成分/
金属成分の比が1.0となるように第1表のように金属
又は酸化物、炭化物、炭窒化物を混合し、各試料につい
て1250℃まで200 Torrの水素雰囲気中で加
熱後、1250℃からはPN!= 1俄圧で窒素を導入
し雰囲気に切換え、この雰囲気で、1750℃で1時間
保持した。加熱処理開始から1750℃までの昇温は1
2℃/分で行なった。得られた本発明品Cと比較量り、
Eの複合炭窒化物についての分析結果を第2表に示す。Example 2 Ti:Ta:W:Mo=0.75 :α10:[110
:α05°C:N=(L55:(L45. Nonmetallic component/
As shown in Table 1, metals, oxides, carbides, and carbonitrides were mixed so that the ratio of metal components was 1.0. Each sample was heated to 1250°C in a hydrogen atmosphere of 200 Torr, and then, from 1250°C, nitrogen was introduced at PN⁻¹ = 1 oz pressure to switch to a nitrogen atmosphere. The samples were then held at 1750°C for 1 hour. The temperature increase from the start of the heat treatment to 1750°C was 1
The process was carried out at 2°C/min. The obtained product C of the present invention was measured in comparison with the results.
The analysis results for composite carbonitride E are shown in Table 2.
この結果、本発明品Cは酸化物原料を用いず金属粉を用
いた比較量りに比べ粒度が非常に小さくまた炭窒化物、
炭化物を原料とする比較品已に比べて酸素量はやや多い
ものの遊離炭素は少なく1粒度は非常に小さいことが判
る。すなわち本発明品が最も微細であることが認められ
た。As a result, product C of the present invention has a much smaller particle size compared to the comparative product using metal powder without using oxide raw materials, and also contains carbonitrides.
Compared to comparative products made from carbides, the oxygen content is slightly higher, but the amount of free carbon is low, and the particle size is extremely small. In other words, the present invention was found to be the finest.
実施例3
T10鵞、 Ta鵞01. WOI、 MoO31Cの
各粉末を第3表の如く配合し400 Torrの水素中
で加熱、還元し、第3表に示した条件で炭窒化処理を施
した。このときの昇温速度は10℃/分、PN、は全て
500 Torrとした。得られた木発明品F〜I及び
比較量J〜0の複合炭窒化物の分析結果も合せて第3表
に示す。Example 3: Powders of T10 Goose, Ta Goose 01, WOI, and MoO31C were blended as shown in Table 3 and heated and reduced in 400 Torr hydrogen to perform carbonitriding treatment under the conditions shown in Table 3. The heating rate at this time was 10°C/min, and PN was set to 500 Torr in all cases. The analysis results of the resulting composite carbonitrides of wood inventions F to I and comparative amounts J to 0 are also shown in Table 3.
実施例4 実施例1〜3で得た複合炭窒化物A、B。Example 4 Compound carbonitrides A and B obtained in Examples 1 to 3.
E 、 H、M 、 Nを原料として用い、これ等にN
i、Coを10重量%ずつ添加し、混合してプレス後、
1450℃%PN2 = 5 Torθ窒素雰囲気下で
1時間焼結してサーメット合金を作製した。E, H, M, and N are used as raw materials, and N is added to these.
Add 10% each of i and Co by weight, mix, and press,
A cermet alloy was fabricated by sintering 1450°C %PN2 = 5 Torθ under a nitrogen atmosphere for 1 hour.
得られた合金をそれぞれP、Q、R,S、T。The resulting alloys are designated P, Q, R, S, and T.
Uとする。各合金の硬度、抗折力を第4表に示す。Let U be the correct value. The hardness and flexural strength of each alloy are shown in Table 4.
第4表
さらに原料E、Nを用いて、硬度を向上させるべく、N
i、Co添加量を7重量%ずつにして、1450℃、P
NI = 5 Torrで時間焼結し、合金V、Wを得
た。これ等の合金の硬度、抗折力を第5表に示すが、抗
折力が著しく低下した。Table 4: Furthermore, using raw materials E and N, in order to improve hardness, N
i. Add 7% by weight of Co each, and heat at 1450°C, P
NI was sintered at 5 Torr for a specified time to obtain alloys V and W. The hardness and flexural strength of these alloys are shown in Table 5, but the flexural strength was significantly reduced.
第5表
次に上記p−wの合金について、下記の条件で切削試験
を行った。試験結果を第6表に示すが1本発明の複合炭
窒化物を原料とした合金がフランク摩耗量、断続切削で
の欠損数、フライス断続切削での熱亀裂発生本数のいず
れの項目においても優れていることが判る。Table 5 shows that cutting tests were performed on the above p-w alloy under the following conditions. The test results are shown in Table 6, and it can be seen that the alloy made from the composite carbonitride of the present invention is superior in all items, including flank wear amount, number of chips in intermittent cutting, and number of thermal cracks initiation in intermittent milling.
条件1. 連続切削
被削材 80M440 (HB=280)切削速度
150m/min
送シ α36 wsx / rev切シ込み
1.5■
チップ形状 5NGN 120408ホμダー F
NllR−44A
切削時間 10分間
条件2 断続切削
被削材 SCM 455 (HB=260)、4驚
切削速度 120 m/win
送9 α24■/ rev
切シ込み 2.0霞
チップ形状 5N()N120408
ホルダー FNllR−44A
切削時間 欠損まで。最大2分間。Condition 1. Continuous cutting work material 80M440 (HB=280) Cutting speed 150m/min Feed rate α36 wsx / rev cutting depth
1.5 ■ Tip shape 5NGN 120408H μD F
NIIIR-44A Cutting time 10 minutes Condition 2 Intermittent cutting Workpiece material SCM 455 (HB=260), 4 Cutting speed 120 m/win Feed 9 α24■/ rev Cutting depth 2.0 Kasumi Chip shape 5N()N120408 Holder FNIIIR-44A Cutting time Until chipping. Maximum 2 minutes.
条件五 フライス断続切削
被削材 S CM 455 (HB=250)70
■×180−の角材
切削速度 300m/min
送シ cL15■/刃
切り込み 2.0m
チップ形状 5NGN12040B
ホルダー DNF4160R
切削時間 15分間
第6表
1;tF
〔発明の効果〕
以上説明したように、本発明の複合炭窒化物の製造法は
、微細な粉末で、かつ酸素や遊離炭素の著しく少ない良
質なTi、 Ta、 W、 Moの複合炭窒化物が得ら
れるという効果がある。さらに本発明によるTi、 T
a、 W、 Moの複合炭窒化物の粉末を用いてサーメ
ットを作製すると、非常に焼結性が良く、切削工具特性
においても耐摩耗性、靭性、耐熱亀裂性に極めて優れた
合金になるという効果がある。Condition 5: Workpiece material cut intermittently with milling cutter: S CM 455 (HB=250) 70
■×180- Square bar cutting speed 300 m/min Feed cL15■/Blade depth of cut 2.0 m Chip shape 5NGN12040B Holder DNF4160R Cutting time 15 minutes Table 6 1; tF [Effects of the invention] As described above, the method for producing composite carbonitrides of the present invention has the effect of obtaining high-quality composite carbonitrides of Ti, Ta, W, and Mo in the form of fine powder and with significantly low levels of oxygen and free carbon. Furthermore, according to the present invention, Ti, T
When a cermet is made using a composite carbonitride powder of a, W, and Mo, it exhibits excellent sinterability and results in an alloy with extremely superior wear resistance, toughness, and thermal crack resistance in terms of cutting tool properties.
Claims (2)
_3及び炭素粉末を出発原料として混合し、該混合物を
水素雰囲気中で加熱した後、1200℃以上1500℃
以下の温度で窒素雰囲気に切換えて加熱し、引き続き該
窒素雰囲気中で1500℃以上2100℃以下の温度に
保持して反応せしめることを特徴とするTi、Ta、W
、Moの複合炭窒化物の製造法。(1) TiO_2, Ta_2O_5, WO_3, MoO
Mix _3 and carbon powder as starting materials, heat the mixture in a hydrogen atmosphere, and then heat to 1200°C or 1500°C.
The Ti, Ta, and W materials are characterized by being heated in a nitrogen atmosphere at the following temperatures, and then being maintained at a temperature of 1500°C to 2100°C in the nitrogen atmosphere for the reaction.
A method for producing Mo composite carbonitrides.
10気圧以下とする特許請求の範囲第1項に記載される
Ti、Ta、W、Mo複合炭窒化物の製造法。(2) A method for producing a Ti, Ta, W, Mo composite carbonitride as described in claim 1, wherein the nitrogen atmosphere pressure during the heat treatment is 30 Torr or more and 10 atmospheres or less.