JPS6476902A - Perovskite-type superconductor and superconducting member - Google Patents

Perovskite-type superconductor and superconducting member

Info

Publication number
JPS6476902A
JPS6476902A JP62206359A JP20635987A JPS6476902A JP S6476902 A JPS6476902 A JP S6476902A JP 62206359 A JP62206359 A JP 62206359A JP 20635987 A JP20635987 A JP 20635987A JP S6476902 A JPS6476902 A JP S6476902A
Authority
JP
Japan
Prior art keywords
group
elements
perovskite
oxygen
element selected
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP62206359A
Other languages
Japanese (ja)
Other versions
JP2880163B2 (en
Inventor
大串 哲彌
善則 白楽
久直 尾形
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Hitachi Ltd
Original Assignee
Hitachi Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Hitachi Ltd filed Critical Hitachi Ltd
Priority to JP62206359A priority Critical patent/JP2880163B2/en
Priority to EP88303270A priority patent/EP0287325B1/en
Priority to DE3850800T priority patent/DE3850800T2/en
Priority to US07/181,097 priority patent/US4892862A/en
Publication of JPS6476902A publication Critical patent/JPS6476902A/en
Priority to US07/727,310 priority patent/US5183799A/en
Application granted granted Critical
Publication of JP2880163B2 publication Critical patent/JP2880163B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To produce an excellent perovskite-type superconductor having high superconducting transition temperature, by using a group Ia metallic element, a group IIa element, a group IVa element and oxygen as main components. CONSTITUTION:The objective oxide superconducting material is composed mainly of (1) the 1st element L selected from group Ia metallic element (Li, Na or K) and group IIIa element (Sc, Y or La), (2) the 2nd element A selected from group IIa element (Ba, Sr or Ca), (3) the 3rd element M selected from group IVa element (Ti, Zr or Hf) and group Va element (V, Nb or Ta) and (4) oxygen and expressed by chemical formula (LxA1-x)iMOy wherein x is 0<x<1, i is 1, 3/2 or 2 and y is 0<y<=3 when i=1 and 0<y<=4 when i=3/2 or 2. The sum of the valence of the 1st element L (x) and the sum of the valence of oxygen (y) preferably satisfy the relationship ¦x¦=¦y¦+ or -0.5. Preferably a bivalent state is included in the takable valance of the 3rd element M. A superconductor having a superconducting transition temperature of about >=150 deg.K can be produced by this process.

Description

【発明の詳細な説明】 〔産業上の利用分野〕 本発明は、ペロブスカイト型超電導材及びこれを用いた
超電導部材に係り、特に高覧1超電導転移温度を有する
に好適なアロブスカイト型超電導材及び超電導部材に関
する。
[Detailed Description of the Invention] [Industrial Field of Application] The present invention relates to a perovskite-type superconducting material and a superconducting member using the same, and more particularly to an allovskite-type superconducting material and a superconducting member suitable for having a high superconducting transition temperature of 1.

〔従来の技術〕[Conventional technology]

従来、酸化物系の超電導材料及びその製法については、
ツアイト シュリフト フユーアフィジーク B64 
(1987年)第189頁から第193頁(Zaits
chift fur Physik  B 64(19
86)pp189−193) 、サイエンス235 (
1987年)第567頁から第569頁(Scienc
e、 235 (1987) p p 567−569
)、及びフィジカル レヴユー レターズ5B (19
87年)第908頁から第910頁(Physical
 Review Letters 58 (1987)
pp (908−910)などにおいて論じられている
。
Conventionally, oxide-based superconducting materials and their manufacturing methods have been:
Zeit Schrift Fureafizik B64
(1987) Pages 189 to 193 (Zaits)
chift fur Physik B 64 (19
86) pp189-193), Science 235 (
1987), pp. 567-569 (Scientific
e, 235 (1987) pp 567-569
), and Physical Review Letters 5B (19
1987) pages 908 to 910 (Physical
Review Letters 58 (1987)
This is discussed in pp. (908-910), etc.

〔発明が解決しようとする問題点〕[Problems that the invention aims to solve]

上記従来技術は、100K以上の超電導転移温度を有す
る酸化物超電導材料及びそのm法について配慮がなされ
ておらず、これらの材料を超電導状態で使用する場合に
は、液体窒素温度(78K)レベルに冷却しなければな
らないという問題があった・ 本発明の目的は150に以上の超電導転移温度を有する
ペロブスカイト型超電導材及びこれを用いた超電導部材
を得ることにある。
The above-mentioned conventional technology does not take into consideration oxide superconducting materials having a superconducting transition temperature of 100K or higher, and the m method thereof. When these materials are used in a superconducting state, there is a problem that they must be cooled to the liquid nitrogen temperature level (78K). The object of the present invention is to obtain a perovskite-type superconducting material having a superconducting transition temperature of 150K or higher, and a superconducting component using the same.

〔問題点を解決するための手段〕[Means for solving the problem]

本発明に係る超電導材は、la族元素及びIIIa族元
素の群から選ばれる第1の元素と、II a族元素の群
から選ばれる第2の元素と、IVa族元素及びVa族元
素の群から選ばれる第3の元素と、酸素とを主成分とし
て含む        ペロブスカイト型のものである
。
The superconducting material according to the present invention is a perovskite type mainly composed of a first element selected from the group of lag elements and group IIIa elements, a second element selected from the group of IIa elements, a third element selected from the group of IVa elements and group Va elements, and oxygen.

更に本発明に係る超電導部材は、上記の超電導材を成形
した焼結晶の露出部分を酸素防壁膜(パッシベーション
膜)にて被覆し、或いはこの超電導材の膜状物を他の電
気絶縁材の膜状物と積層したものである。積層に際して
は両膜状物を夫々複数層用いて各層交互に積層すること
が好ましく、また絶縁材も同系統のペロブスカイト型セ
ラミクスであることが望ましい。
Furthermore, the superconducting member according to the present invention is obtained by covering the exposed portion of the sintered crystal formed from the superconducting material with an oxygen barrier film (passivation film), or by laminating this film of superconducting material with a film of another electrical insulating material. When laminating, it is preferable to use multiple layers of each of the film materials and to laminate them alternately, and it is also desirable that the insulating material is a perovskite-type ceramic of the same type.

いずれにせよ上記第3の構成元素の価数合計Xと酸素の
価数合計yとの関係ばIxl=Iyl±0.5 である
ことが望ましく、また第3の元素の取り得る価数の内二
価の状態のものが含まれている方が好ましい。
In any case, it is desirable that the relationship between the sum of the valencies X of the third constituent element and the sum of the valencies y of oxygen be Ixl = Iyl ± 0.5, and it is also preferable that the third element includes a divalent state among its possible valencies.

上記超導電材を化学式にて示せば次式(1) 、 (2
)の通りになる。
The above superconducting material can be expressed by the following chemical formulas: (1), (2)
It will be as follows.

(L++Az−x)*MOy          ”・
”(1)但し、この(1)式で。
(L++Az-x)*MOy”・
(1) However, in this equation (1).

Xは、O<X<1であり。X is such that O < X < 1.

1は、i=1.−、または2であり、 yは、i冨1のとき、O<y≦3 ■=−または2のとき、O< y≦4 (L *A z−x)t Mu−zCu toy   
   ”” (2)但し、この式で、 Xは、O< x < 1であり。
1 is i = 1, -, or 2, and y is O < y ≤ 3 when i = 1, or O < y ≤ 4 when i = - or 2. (L *A z-x)t Mu-zCu toy
(2) However, in this equation, X is O < x < 1.

2は、O< z < 1であり、 iは、i =1 t  oまたは2であり。2 is O < z < 1, and i is i = 1 t o or 2.

yは、i=1のとき、O< y≦3 1=−または2のとき、O< y≦4 本発明材料の特徴は、上記(1)式で示されるペロブス
カイト状結晶構造を有し1式中のL元素はスカンジウム
(Se)、イツトリウム(Y)、まトリウム(IVa)
、カリウム(K)の群がら選ばれるIa族元元素あり、
式中のA元素はバリウム(Ba)、ストロンチウム(S
r)、カルシウ1−(Ca)などのアルカリ土類金属(
lln族)の群から選ばれた少なくとも一つの元素であ
り、更に酸素(0)及び酸素空孔により形成される八面
体結晶構造の中心部に位置する式中のM元素は元素周期
表のVa族元素であるバナジウム(V)、ニオブ(Nb
)、タンタル(Ta)、またはIVa族元素であるチタ
ン(Ti)、ジルコニウム(Zr)、ハフニウム(Hf
)の群から選ばれた少なくとも一つの元素である酸化物
超電導材料にある。上記材料(1)式のものは、前記り
元素の酸化物の粉末。
When i = 1, O < y ≤ 3 When 1 = - or 2, O < y ≤ 4 The characteristic of the material of the present invention is that it has a perovskite-like crystal structure shown in the above formula (1), and the element L in formula 1 is scandium (Se), ytztrium (Y), mathrium (IVa)
Among the group of elements, potassium (K) is selected as a Group Ia element.
In the formula, element A is barium (Ba), strontium (S)
r), alkaline earth metals such as calcium-1-(Ca)
The element M in the formula is at least one element selected from the group (lln), and is located at the center of the octahedral crystal structure formed by oxygen (0) and oxygen vacancies. The element M is a group Va element of the periodic table, such as vanadium (V) or niobium (Nb).
), tantalum (Ta), or the group IVa elements titanium (Ti), zirconium (Zr), hafnium (Hf
The material is an oxide superconducting material which is at least one element selected from the group of ). The material of formula (1) above is a powder of the oxide of the aforementioned element.

A元素の炭酸物の粉末、及びM元素の酸化物またはその
純金属の粉末を所望の化学量論組成で混合し、その混合
粉末を真空中、還元性または弱い酸化性雰囲気中で高温
度に加熱して反応させ、その後その混合反応物を焼結さ
せて製造される。また別の製法として、前記り元素の酸
化物の粉末、A元素の炭酸化物の粉末、及び第2グ酸化
鋼(Cub)粉末を混合し、この混合粉末を真空中また
は還元性或いは弱い酸化性雰囲気中において、900〜
1ooo℃の温度で加熱反応させ、この反応混合粉末に
、M元素の純金属粉末を所望の化学量論量で混合し、こ
の混合物を再び真空中、還元性あるいは弱酸化性雰囲気
中で加熱して反応させ、その後その混合反応物を焼結さ
せて、上記(2)式で示されるペロブスカイト状結晶構
造を有する酸化物超電導材料も得られる。更に応用例と
しては、基板としてケイ1(Si)単結晶、酸化アルミ
ニウム(AjisOj)単結晶、#化ケイ14(Sin
s)単結晶、酸化マグネシウム(M g O)単結晶、
酸化ジルコニウム(ZrOz)単結晶の少なくとも一つ
を用い、この基板上に前記M元素の金属薄膜を形成し、
この上に前記り元素とへ元素の混合物の膜(L x A
 L−X膜、但しO< x < 1 )を堆積させ、次
に熱処理して前記元素を反応させることにより。
It is manufactured by mixing a carbonate powder of element A and an oxide or pure metal powder of element M in a desired stoichiometric composition, reacting the mixed powder by heating it to a high temperature in a vacuum, reducing or weakly oxidizing atmosphere, and then sintering the reacted mixture. Alternatively, as a manufacturing method, the oxide powder of element A, the carbon oxide powder of element M, and the 2G oxide steel (Cub) powder are mixed, and this mixed powder is heated in a vacuum or reducing or weakly oxidizing atmosphere at 900°C.
The reaction is carried out at a temperature of 100°C, and a pure metal powder of element M is mixed with the desired stoichiometric amount. This mixture is then heated again in a vacuum, reducing or weakly oxidizing atmosphere to cause a reaction, and the mixed reaction product is then sintered to obtain an oxide superconducting material having a perovskite-like crystalline structure as shown in equation (2) above. Further application examples include silicon 1 (Si) single crystals, aluminum oxide (AjisOj) single crystals, and silicon 14 (Si) as substrates.
s) Single crystal, magnesium oxide (MgO) single crystal,
Using at least one zirconium oxide (ZrOz) single crystal, a thin metal film of the aforementioned M element is formed on this substrate.
A film (L x A) of a mixture of the aforementioned elements is placed on top of this.
An L-X film (where O < x < 1) is deposited, and then heat-treated to react with the aforementioned elements.

前記基板上に上記(1)式で示されるペロブスカイト状
結晶構造を有する酸化物超電導薄膜を形成することも可
能であるし、前記M:ycNの金属テープまたは基板上
に、前記り元素とA元素の混合物の上記(1)式で示さ
れるペロブスカイト状結晶構造を有する酸化物超電導材
料を得ることも可能である。
It is also possible to form an oxide superconducting thin film having a perovskite-like crystalline structure represented by formula (1) on the substrate, and it is also possible to obtain an oxide superconducting material having a perovskite-like crystalline structure represented by formula (1) of a mixture of element ri and element A on the metal tape or substrate of M:ycN.

加えて、基板としてケイ1t(Si)単結晶、酸化アル
ミニウム(AflzOa)単結晶、酸化ケイ素(Sif
t)単結晶、酸化マグネシウム(M g O)単結晶、
酸化ジルコニウム(ZrOz)、QL結品の少なくとも
一つを用い、この基板上に前記M元素の金属薄膜を形成
し、この上に前記り元素及びA元素と銅(Ou)及びl
l111素(0)を含む非晶質または多結晶質[(L+
+At−x)icuOy膜]を堆積させ。
In addition, silicon 1t (Si) single crystal, aluminum oxide (AflzOa) single crystal, and silicon oxide (SiF) can be used as substrates.
t) Single crystal, magnesium oxide (MgO) single crystal,
Using at least one of zirconium oxide (ZrOz) and QL crystals, a metal thin film of the aforementioned M element is formed on this substrate, and the aforementioned element and element A, copper (Ou) and l are placed thereon.
Amorphous or polycrystalline material containing l111 element (0) [(L+
A film [+At-x)icuOy film] is deposited.

その後熱処理により前記M7G素を(LxAt−x);
CuO1膜中に拡散させることにより、上記(2)式で
示されるペロブスカイト状結晶構造を有する酸化物超電
導膜を形成する製法も有効である。
Subsequently, the M7G element is subjected to heat treatment (LxAt-x);
A method for forming an oxide superconducting film having a perovskite-like crystalline structure, as shown in equation (2) above, by diffusing it into a CuO1 film is also effective.

更に本発明は上記各構成元素に加えて銅、フッ素、塩素
、窒素等他の少量元素を含んでいても差し支えない、銅
は製法の過程で残留することもある。フッ素等が併存す
る場合、最も望ましい形態は、下式(3)で示されるペ
ロブスカイト状結晶構造を有し、式中のL元素は、スカ
ンジウム(Sc)。
Furthermore, the present invention may also contain small amounts of other elements such as copper, fluorine, chlorine, and nitrogen in addition to the above constituent elements, although copper may remain as a residue during the manufacturing process. When fluorine and other elements are present, the most desirable form is a perovskite-like crystal structure shown in formula (3) below, where element L is scandium (Sc).

イツトリウム(Y)、ランタン(La)などのランタノ
イド元素並びにリチウム(Li)などの1a族金属元素
の群の中から選ばれた少なくとも一つの元素であり、式
中のへ元素はバリウム(Ba)。
It is at least one element selected from the group of lanthanide elements such as ytztrium (Y) and lanthanum (La), and group 1a metallic elements such as lithium (Li), where the element h in the formula is barium (Ba).

ストロンチウム(Sr)、カルシウム(Ca)などのア
ルカリ土類金属元素の群から選ばれた少なくとも一つの
元素であり、さらに酸14(0)及び酸素空孔により形
成される八面体結晶構造の中心部に位置する式中のM元
素は元素周期表のVa族元素であるバナジウム(V)、
ニオブ(Nb)。
At least one element selected from the group of alkaline earth metal elements such as strontium (Sr) and calcium (Ca), and furthermore, the element M in the formula, located at the center of the octahedral crystal structure formed by acid 14(0) and oxygen vacancies, is vanadium (V), a group Va element of the periodic table.
Niobium (Nb).

タンタル(Ta)、またはIVa族元素であるタチン(
Ti)、ジルコニウム(Zr)、ハフニウム(Hf)の
群から選ばれた少なくとも一つの元素であるペロブスカ
イト型超電導材料で、前記酸素(0)の一部及び全部を
をふフ素(F)、塩素(Cm)。
Tantalum (Ta), or tatin, an element of group IVa (
A perovskite-type superconducting material comprising at least one element selected from the group consisting of Ti, zirconium (Zr), and hafnium (Hf), wherein some and all of the oxygen (O) is composed of fluorine (F) and chlorine (Cm).

窒素(N)により構成する製法によフて達成される。前
記り元素の酸化物の粉末、A元素のふフ化物あるいは塩
化物の粉末、及びM元素の酸化物まr;はその純金属の
粉末を所望の化学量論組成で混合し、その混合粉末を酸
化性雰囲気中で高温度に加熱して反応させ、その後その
混合反応物を焼結させて、下記(3)式で示されるペロ
ブスカイト状結晶構造を有するペロブスカイト型超電暮
材料を製造することが妨ましい。
This is achieved by a manufacturing method consisting of nitrogen (N). It is difficult to produce a perovskite-type superelectronic material having a perovskite-like crystalline structure shown in equation (3) below by mixing the oxide powder of the aforementioned element, the fluoride or chloride powder of element A, and the oxide or pure metal powder of element M in a desired stoichiometric composition, heating the mixed powder to a high temperature in an oxidizing atmosphere to react, and then sintering the mixed reactant.

更に、ふっ素ガス或いは塩素ガスを含む酸化性雰囲気中
で熱処理し、その後同じ雰囲気中で除冷する製法や、酸
化性雰囲気中で熱処理し、その後イオンプランチーシー
ン法により、ふフ素或いは塩素イオンを注入する製法も
有効である。
Furthermore, methods involving heat treatment in an oxidizing atmosphere containing fluorine gas or chlorine gas, followed by sequestering in the same atmosphere, or heat treatment in an oxidizing atmosphere followed by implantation of fluorine or chloride ions using the ion planty-sene method are also effective.

(LxAt−x)tMOa−JGh       −(
3)但し、この式で。
(LxAt-x)tMOa-JGh -(
3) However, using this formula.

Xは、O< x < 1であり、 iは、i=1.3/2.または2 j及びkは、i=1のとき、i+k=31=−のとき 
j+k=7/2 i=1のときj+k:4 であり、 δは、酸素の欠損量、 Gは、ふフ素(F)、塩素(CQ)あるいは窒−14(
N)である。
X is O < x < 1, i is i = 1, 3/2, or 2, and j and k are when i = 1, i + k = 31 = -
j + k = 7/2. When i = 1, j + k = 4, where δ is the amount of oxygen deficiency, and G is fluorine (F), chlorine (CQ), or nitrogen-14.
N) is the answer.

〔作用〕[Effect]

上記ペロブスカイト状結晶構造を有する本発明の酸化物
超電導材料は、M元素であるVa族元素あるいはIV 
a族元素の原子をその中心にもつ、6個の酸素原子の八
面体構造を基本構成とするもので、この材料は前記八面
体を構成する酸素の欠損。
The oxide superconducting material of the present invention having the above-described perovskite crystal structure is an M element, which is a group Va element or IV
The basic structure is an octahedron of six oxygen atoms, with an atom of a group A element at its center, and this material is characterized by vacancies in the oxygen atoms that make up the octahedron.

即ち酸素空孔が1つあるいは複数個存在するので、その
酸素の欠損により、温度150に以上においても超電導
電子対を形成するに必要な強い引力相互作用が発生して
いるものと予想される。
In other words, since there is one or more oxygen vacancies, it is expected that the absence of oxygen generates a strong attractive interaction necessary for the formation of superconducting pairs even at temperatures above 150°C.

また、本発明によれば、L元素、A元素及びM元素を所
定の化学量論組成比で含む混合物を真空中還元性あるい
は弱い酸化性雰囲気中で高温加熱し、反応させることに
より、前記混合物の非晶質または多結晶質の酸化物の粉
末を得、これを成形し、焼結することにより前記酸化物
の多結晶質あるいは結晶質の上記(1)または(2)式
に示すような酸化物超電導材料が得られる。
Furthermore, according to the present invention, a mixture containing elements L, A, and M in predetermined stoichiometric ratios is heated at a high temperature in a vacuum reducing or weakly oxidizing atmosphere to cause a reaction, thereby obtaining an amorphous or polycrystalline oxide powder of the mixture. This powder is then molded and sintered to obtain a polycrystalline or crystalline oxide superconducting material of the oxide as shown in formula (1) or (2) above.

さらに、本発明の他の製法によれば、L元素、A元素及
びM元素を所定の化学量論組成比で含む膜を、テープ上
、ま冬戸板上に形成し、これを真空中、還元性あるいは
弱い酸化性雰囲気中で熱処理することにより反応させ、
多結晶質あるいは結晶質の上記(1)または(2)式に
示すような酸化物超電導材料が得られる。
Furthermore, according to another method of the present invention, a film containing elements L, A, and M in predetermined stoichiometric composition ratios is formed on a tape or a wooden board, and this film is reacted by heat treatment in a vacuum, reducing or weakly oxidizing atmosphere.
Polycrystalline or crystalline oxide superconducting materials as shown in equation (1) or (2) above can be obtained.

Va族、TVaVa族元素数の価数を操り得る。The valence of elements in the Va and TVaVa groups can be manipulated.

価数が多いもの(例えばN b xの如く酸素元素比率
が多いもの)は一般に安定であり1元素単体或いは低酸
素化合物も酸化雰囲気での加熱により通常は最も酸素の
価数の多いものとなる。従って特に望ましい原料セラミ
クスはNbO,Tag。
Materials with a high valency (for example, Nbx, which has a high oxygen element ratio) are generally stable, and even single-element or low-oxygen compounds usually become the material with the highest oxygen valency when heated in an oxidizing atmosphere. Therefore, particularly desirable raw material ceramics are NbO and Tag.

VO,ZrO,Tie、HfO等である。いずれにせよ
これらの価数のものがペロブスカイト成形体中に残存す
ることにより、当該成形体中では価数の移動(例えば2
価(−)5価)が起こり。
These include VO, ZrO, Tie, HfO, etc. In any case, the presence of these valencies in the perovskite molded body causes valency transfer (for example, 2
A valence (-5) occurs.

これが安定性を高めると推定される。This is presumed to increase stability.

上記のように酸素と第1〜第3元素との価数合計を±0
.5 の範囲で等しくすることが望ましいが、±0.5
 の意味するところは酸素欠陥の若干の過不足は差し支
えなく実質的に等老しくなれば良いということである。
As described above, the sum of the valencies of oxygen and the first to third elements is ±0.
It is desirable to make them equal within the range of 5, but ±0.5 is acceptable.
This means that a slight excess or deficiency of oxygen is acceptable, as long as the organism is essentially equal in age.

上記(1)式中のMは更に(M’ t−zM’ 2)(
但し、この式で、0≦z〈1)で表わされ、M′元素は
、元素周期表のVa族元素であるバナジウム、ニオブ、
タンタル、またはlVaの族元素であるチタン、ジルコ
ニウム、ハフニウムの群から選ばれた一つの元素であり
、M#元素は、前記Va族元素、IVaVa族元素は銅
(Cu)の中から選ばれた少なくとも一つの元素である
ことも有効である。
In equation (1) above, M is further expressed as (M't-zM' 2) (
However, in this equation, 0 ≤ z < 1), and the element M' is a group Va element in the periodic table, such as vanadium, niobium,
It is also valid that the M# element is one element selected from the group of elements in tantalum, iVa, titanium, zirconium, and hafnium, and the M# element is at least one element selected from the group Va elements, and the iVaVa elements are copper (Cu).

また(1)式中のAは(A’ x、、−mA’ *)(
但し、この式で、O≦dく1)で表わされ、A′または
A“元素はそれぞれバリウム、ストロンチウム−カルシ
ウムなどのアルカリ土類金属元素の群から選ばれた一つ
の元素が有効である。
Also, in equation (1), A is (A' x, -mA' *) (
However, in this equation, O ≤ d < 1) and A′ or A'' must be one element selected from the group of alkaline earth metal elements such as barium and strontium-calcium.

本発明による新材料を例示すれば次の通りである。Examples of the new materials according to the present invention are as follows:

(LaxSrz−x)tM’ CuzOy   (0,
6≦x < 0 、9 )(LaxSrt−x)tM’
 t−zcuoy  (0,4≦X≦0.6)(YxB
az−x)zM’z−zcuzoy  (0,4≦X≦
0.6)所IWABOa型としてLiBagNba07
所謂AzBOa型としてLiBaNb0所1rlfAa
Bxos型としてLiBazNbzos一方、F、CQ
、N等の元素を併有する場合には望ましくは上記の(3
)式の構造を有し1M元素であるVa族元素あるいはr
VaVa族元素子をその中心にもつ、6個のイオン配置
に、酸素原子。
(LaxSrz-x)tM' CuzOy (0,
6≦x<0, 9)(LaxSrt-x)tM'
t-zcuoy (0,4≦X≦0.6)(YxB
az-x)zM'z-zcuzoy (0,4≦X≦
0.6) LiBagNba07 as IWABOa type
The so-called AzBOa type is LiBaNb01rlfAa
As a Bxos type, LiBazNbzos, on the other hand, F, CQ
When elements such as N are also present, preferably the above (3
) A group Va element or r that has the structure of the formula and is a 1M element
It has a VaVa group element at its center, with an oxygen atom in a six-ion configuration.

酸素欠損及びふフ素、塩素、あるいは窒素原子を配置さ
せることにより、化学的に安定で、かつ温度150に以
上においても超電導電子対を形成するに必要な強い引力
相互作用が発生できる。
By creating oxygen vacancies and arranging fluorine, chlorine, or nitrogen atoms, it is possible to generate chemically stable materials that also exhibit the strong attractive interactions necessary for forming superconducting pairs, even at temperatures above 150°C.

〔実施例〕[Examples]

以下、本発明の詳細な説明する。The present invention will now be described in detail.

本発明の酸化物超電導材料は第1図、第2図に示すよう
なペロブスカイト状結晶構造を有している。この図は単
位格子を示しており、その化学式%式%(1) で表わせる。この式で、XはO< x < 1であり、
■はl =11  ?または2であり、yは、i=1の
ときO<y≦3.i=−または2のときO< y≦4で
ある。また、(1)式中のL元素はスカンジウム(Sc
)、イツトリウム(Y)、またはランタン(La)など
のランタノイド元素或いはリチウム(LX)、ナトリウ
ム(IVa)、カリウム(K)のIa族金属元素の中か
ら選ばれた少なくとも一つの元素であり1式中のA元素
はバリウム(Ba)、ストロンチウム(Sr)、カルシ
ウム(Ca)などのアルカリ土類金属元素の中から選ば
れた一少なくとも一つの元素であり、さらに酸素(0)
及び酸素空孔により形成される八面体結晶構造の中心部
に位置する式中のM元素は元素周期表のVa族元素であ
るバナジウム(V)、ニオブ(Nb)、タンタル(Ta
)、またはIVaVa族元素るチタン(Ti)、ジルコ
ニウム(7,r)、ハフニウム(Hf)の中から選ばれ
た少なくとも一つの元素である。(1)式中のMには6
個の酸素が図に示すように八面体形に配位している。こ
の6個の酸素のうち1個あるいは2個が抜けることによ
り、Mをその面心にもつ4個の酸素の四角い面、あるい
は2個の酸素と2個の酸素空孔の作る四角い面が複数層
現われ、これらは2次元的に結晶体中でつながっている
。この2次元的に連続した四角い面の発生に伴い、超電
導電子対を形成するに必要な強い引力相互作用が発生し
、こうして発生した超電導電子対は、前記2次元的に連
続しう た四角い面に沿って流会域のと予想される。ここでM元
素として、Va族のバナジウム(V)、ニオブ(Nb)
、タンタル(Ta)あるいはIVa族のチタン(Ti)
、ジルコニウム(Zr)、ハフニウム(Hf)の群から
選ばれた1個あるいは複数の元素を含むようにする。こ
れによって、前記酸素の抜け、即ち酸素空孔の形成が促
進され、前記M元素をその面心にもつ酸素の2次元的な
四角い連続面が形成される。
The oxide superconducting material of the present invention has a perovskite-like crystal structure as shown in Figures 1 and 2. This figure shows the unit cell, which can be represented by the chemical formula %(1). In this formula, X is O < x < 1,
■ is l = 11 or 2, and y is O < y ≤ 3 when i = 1, and O < y ≤ 4 when i = - or 2. Also, the element L in equation (1) is scandium (Sc
), ytztrium (Y), or lanthanide elements such as lanthanum (La), or group Ia metallic elements such as lithium (LX), sodium (IVa), and potassium (K), and element A in one formula is at least one element selected from alkaline earth metallic elements such as barium (Ba), strontium (Sr), and calcium (Ca), and furthermore oxygen (O)
And the element M in the formula, located at the center of the octahedral crystal structure formed by oxygen vacancies, is a group Va element of the periodic table: vanadium (V), niobium (Nb), tantalum (Ta
(1) M is 6
The oxygen atoms are coordinated in an octahedral shape as shown in the figure. When one or two of these six oxygen atoms are removed, multiple layers of square faces appear, each consisting of four oxygen atoms with M as its center, or square faces formed by two oxygen atoms and two oxygen vacancies. These layers are connected two-dimensionally within the crystal. The formation of these two-dimensionally continuous square faces generates strong attractive interactions necessary for the formation of superconducting pairs, and these superconducting pairs are expected to flow along the aforementioned two-dimensionally continuous square faces. Here, as element M, we have vanadium (V) and niobium (Nb) from the Va group.
, tantalum (Ta) or titanium (Ti) of the IVa group
The material contains one or more elements selected from the group consisting of zirconium (Zr) and hafnium (Hf). This promotes the removal of oxygen, i.e., the formation of oxygen vacancies, and creates a two-dimensional, square continuous surface of oxygen with the M element at its center.

(1)式中のM元素が二元系元素、即ち(M’ x−z
M’ z)(但しこの式でOS z < 1 )で表わ
せる酸化物超電導材料としてもよい、この場合、M′元
素は、元素周期表のVa族元素である勇バナジウム、ニ
オブ、タンタル、またはIVa族元素であるチタン、ジ
ルコニウム、ハフニウムの中から選ばれた一つの元素で
あり、M1元素は。
(1) In equation (1), element M is a binary element, i.e., (M' x - z
It may also be an oxide superconducting material that can be expressed as M' z) (where OS z < 1 in this formula), in which case the element M' is one element selected from the group Va elements of the periodic table, such as vanadium, niobium, tantalum, or the group IVa elements such as titanium, zirconium, hafnium, and the element M1 is.

前記Va族元素またはIVa族元素の他に銅(Cu)を
選択することも可能である。
In addition to the aforementioned Group Va or Group IVa elements, copper (Cu) can also be selected.

また、(1)式中のA元素が二元系元素、即ちツ   
シ (A’ z−mA’−)(但シコノ式でo≦d<o)で
表わせる酸化物超電導材料としてもよい、この場合、A
′またはA′元素はそれぞれバリウム、ストロンチウム
1カルシウムなどのアルカリ土類金属元素の中から選ば
れた一つの元素である。
Furthermore, element A in equation (1) is a binary element, i.e., a t
It may also be an oxide superconducting material that can be expressed as シ(A'z-mA'-) (where o ≤ d < o in the Sicono formula), in this case A
Element ' or A' is an element selected from among alkaline earth metal elements such as barium and strontium-1 calcium.

上述した本実施例の酸化物超電導材料の好適な例として
は次の各式で表わせるものが挙げられる。
A suitable example of the oxide superconducting material of the above-described embodiment can be expressed by the following formulas.

(L a、ls rn−x)zM’ 5−zc uzo
y(L ass rt−x)M’  t−zc uzo
y(YIIB  ax−x)M’  z−zcuzoy
これら各式でXは、0.4≦x < 0 、6であるこ
とが望ましく、特にx40.5  が良い。
(L a,ls rn-x)zM' 5-zc uzo
y(L ass rt-x) M' t-zc uzo
y(YIIB ax-x)M'z-zcuzoy
In each of these equations, it is desirable that X be 0.4 ≤ x < 0 or 6, and x 40.5 is particularly good.

一方、化学式が上記(3)式で示されるものはL元素、
へ元素共(1)、(2)式と同じ群がら選ばれ、加えて
、酸素(0)、酸素空孔及びふフ!I(F)、塩素(C
0,窒素(N)の中から選ばれた一つの元素であるG元
素より形成される八面体結晶構造の中心部に位置する式
中のM元素は元素周期表のVa族元素であるバナジウム
(V)、ニオブ(Nb)。
On the other hand, elements whose chemical formula is represented by equation (3) above are L elements.
The elements are selected from the same group as in formulas (1) and (2), in addition to oxygen (0), oxygen vacancies and fluorine (F), chlorine (C).
The element M in the formula, located at the center of the octahedral crystal structure formed from element G, which is one element selected from among 0 and nitrogen (N), is vanadium (V) or niobium (Nb), which are elements of group Va in the periodic table.

タンタル(Ta)、またはIVa族元素であるタチン(
Ti)、ジルコニウム(Zr)、ハフニウム(Hf)の
群から選ばれた少なくとも一つの元素である。(3)式
中のMには6個の酸素、酸素欠損。
Tantalum (Ta), or tatin, an element of group IVa (
It is at least one element selected from the group consisting of Ti, zirconium (Zr), and hafnium (Hf). (3) In equation (3), M has six oxygen atoms and oxygen vacancies.

Gyr、iAが図に示すように八面体形に配位している
。
Gyr and iA are arranged in an octahedron shape as shown in the figure.

こうして、酸素とM元素の線が1次元的に結晶中でつな
がるようになる。この1次元的に連続した酸素とM元素
の発生に伴い、超電導電子対を形成するに必要な強い引
力相互作用が発生し、こうして発生した超電導電子対は
、前記1次元的に連続した線に沿って流れるものと予想
される。ここで。
Thus, lines of oxygen and element M become connected in a one-dimensional manner within the crystal. The generation of these one-dimensionally continuous oxygen and element M molecules generates a strong attractive interaction necessary for the formation of superconducting pairs, and these superconducting pairs are expected to flow along the aforementioned one-dimensionally continuous lines. Here...

M元素として、■d族のバナジウム(V)、ニオブ(N
b)、タンタル(Ta)、またはIVa族のタチン(T
i)、ジルコニウム(Zr)、ハフニウム(Hf)の群
から選ばれた1個あるいは複数の元素を含むようにする
。ふフ素(F)、塩#(CB)。
As M elements, vanadium (V) and niobium (N) of the group d are included.
b) Tantalum (Ta), or Tachin of the IVa group (T
i) To include one or more elements selected from the group consisting of zirconium (Zr) and hafnium (Hf). Fluorine (F), salt # (CB).

窒素(N)の中から選ばれたG元素を導入することによ
り、化学的に結晶が安定化し、かつM元素と酸素の1次
元的な連続が規則的に形成される。
By introducing element G, selected from nitrogen (N), the crystal is chemically stabilized, and a regular one-dimensional continuity of element M and oxygen is formed.

次に1本発明のペロブスカイト型超電導材料の製法につ
いての実施例を説明する。
Next, an example of the method for producing the perovskite-type superconducting material of the present invention will be described.

(L a 冨S r t−x)nN b Oyで表わせ
るペロブスカイト状結晶構造を有する酸化物超電導材料
の製法について説明する。酸化ランタン(Lashs)
(Nb)の粉末を所定の化学量論組成に秤量し。
This document describes a method for producing oxide superconducting materials having a perovskite-like crystal structure that can be represented as (L a 冨S r t-x)nN b Oy. Lanthanum oxide (Lashs)
The powder of (Nb) is weighed to the predetermined stoichiometric composition.

その混合粉末を酸化性雰囲気中で、約900〜1500
℃で数時間加熱して反応させる。この時。
The mixed powder is heated in an oxidizing atmosphere for approximately 900 to 1500 degrees Celsius.
Heat at °C for several hours to allow the reaction to occur. At this time...

NbOを使用する場合は1300〜1500℃Nbを使
用する場合は900〜1100℃が好ましい6次に、そ
の混合反応物を粉砕し、これを適当な形状にプレス成形
し、前記反応温度よりもやや高い温度で、焼結すること
によって、所望の形状の酸化物超電導材料を得ることが
できる。
When using NbO, a temperature of 1300 to 1500°C is preferred, and when using Nb, a temperature of 900 to 1100°C is preferred. Next, the mixed reaction product is pulverized, pressed into an appropriate shape, and sintered at a temperature slightly higher than the reaction temperature to obtain an oxide superconducting material of the desired shape.

なお、本実施例により製造された焼結体;(Lao、5
Sro、a)tNboaをX線回折法で測定したところ
、2θが24.6@、31.1@、33.6@、43.
2” s 47.9@、54.6°、55.4”、65
.4@ にビークを示し、結晶質化しており、かつ焼結
体の色調は黒色に近かった。
Furthermore, the sintered body produced by this embodiment; (Lao, 5
When Sro, a)tNboa was measured by X-ray diffraction, the 2θ values were 24.6@, 31.1@, 33.6@, and 43.
2”s 47.9@, 54.6°, 55.4”, 65
The peak was observed at 4@, indicating crystalline formation, and the sintered body was close to black in color.

本発明の確認によれば、本発明系統の材料の20は上記
(1)式がi=2の場合(所!!W(L−A):M=2
:1の場合)は上記(Lao、5Sro、a)zNbo
aと同様の20が出る。
According to the confirmation of the present invention, the material 20 of the present invention system is when the above equation (1) is i=2 (where W(L-A):M=2
: In case 1) the above (Lao, 5Sro, a) zNbo
The same result as in a, 20, will appear.

(L a X S r’ x−xh N b Oyで表
わせるペロブスカイト状結晶構造を有する酸化物超電導
材料の製法についても、上記と同様に実施できる。−例
としてこの製法で得られたLa5rNbOy (3’は
4と推定される)のEPMA分析の結果を第2図に示す
。所定の20、後述の超電導特性、並びに第3図の分析
値より1本実施例に係る酸化物が上記組成のペロブスカ
イト型超電導材であることが同定される。尚、図中の(
1)はLaLβ2.4583人、(2)はL a L 
a 2.6851人、(3)はLaLβ2.4583人
、(4)はNbLβ5.4914人、(5)はNbLα
5.7235人、(6)はSrLβ6.6234人、(
7)はS r L α6.8624人1(8)はL a
 L a 2.6651人を示す。
The same method can be used to produce an oxide superconducting material having a perovskite-like crystal structure that can be represented as (La X S r' x-xh N b Oy). As an example, Figure 2 shows the results of EPMA analysis of La5rNbOy (3' is presumed to be 4) obtained by this method. From the predetermined 20, the superconducting properties described later, and the analytical values in Figure 3, it is identified that the oxide according to this embodiment is a perovskite-type superconducting material with the above composition.
1) is LaLβ 2.4583 people, (2) is La L
a) 2.6851 people, (3) LaLβ 2.4583 people, (4) NbLβ 5.4914 people, (5) NbLα
5.7235 people, (6) SrLβ 6.6234 people, (
7) is S r L α6.8624 people 1 (8) is La a
L a represents 2.6651 people.

このLa5rNbO4を例にとれば焼成直後の特性は第
4図の通りであり、第4図の測定の為−旦200Kまで
試料温度を下げたものを再度抵抗測定す4れば、第5図
の通りとなり、再現性もあり。
Taking La5rNbO4 as an example, the characteristics immediately after firing are as shown in Figure 4. If the sample temperature is lowered to 200K for the measurement shown in Figure 4 and the resistance is measured again, the results are as shown in Figure 5, and the results are reproducible.

かつ比較的安定となる。第5図が示す通り本実絶倒品は
315にで電気抵抗が下がり始め、300にで電気抵抗
がゼロとなり、測定上の若干のノイズ域をはずしても2
55にで完全に抵抗ゼロとなる。一方各回にχ(%)で
示した通り、マイスナ効果も確認された。χは帯磁率で
あり、完全超電導(Nb4.2K)基準に対する帯磁性
の比率であって、これが負を示せばすなわちマイスナ効
果を具備することになる。尚、電流条件は3 m A 
/ rtAである。
Furthermore, it becomes relatively stable. As shown in Figure 5, in this actual product, the electrical resistance begins to decrease at 315, and the electrical resistance becomes zero at 300, and even excluding the slight noise range in the measurement, 2
At 55, the resistance becomes completely zero. Meanwhile, the Meissner effect was also confirmed, as indicated by χ (%) in each test. χ is the magnetic susceptibility, the ratio of magnetic susceptibility to perfect superconductivity (Nb 4.2K), and a negative value indicates the presence of the Meissner effect. The current condition was 3 mA.
/ This is rtA.

尚、このように温度サイクルをかけることにより所定の
超電導特性を得るよう瀾整することも可能である。更に
所定の特性を示す温度域を限定して超電導応用機器を使
用することも可能であり、第5図の300にの位置のよ
うに完全抵抗ゼロに一時的にでもなる領域があればこの
領域での使用、あるいはこの領域を利用して(上温域・
下温域にて抵抗が変化することから)スイッチング材と
しての使用も好ましい。
Furthermore, by applying temperature cycles in this manner, it is possible to adjust the temperature to obtain the desired superconducting characteristics. It is also possible to use superconducting equipment within a limited temperature range where the desired characteristics are exhibited. For example, if there is a region where the resistance temporarily becomes zero, as shown at position 300 in Figure 5, it is possible to use the equipment in this region, or utilize this region (upper temperature range).
(Since its resistance changes in the lower temperature range), it is also suitable for use as a switching material.

(YxBaz−x)NbOyで表わせるペロブスカイト
状結晶構造を有する酸化物超電導材料の製法の場合には
、出発原料粉末として酸化イツトリウム(Y z Os
 ) 、炭酸おバリウム(BaCO2)、酸化ニオブ(
N b zo s)または純金属のニオブ(Nb)を所
定の組成に秤量し、これを混合後、高温で反応熱処理を
行う、こうして得られた反応混合物の粉末を成形し、焼
結することによって、酸化物超電導材料を得ることがで
きる。
In the case of a method for producing oxide superconducting materials having a perovskite-like crystalline structure that can be represented as (YxBaz-x)Nboy, ytztrium oxide (Y z Os) is used as the starting material powder.
), barium carbonate (BaCO2), niobium oxide (
By weighing Nb (Nb zo s) or pure metallic niobium (Nb) to a predetermined composition, mixing them, and then performing a reaction heat treatment at a high temperature, an oxide superconducting material can be obtained by molding the resulting reaction mixture powder and sintering it.

なお1本実施例((Y o、a B lio、e) N
 b OJ)により製造された焼結体をX線回折法で測
定したところ、2θが22.7@、32.7@、38.
5°、40.3°、46.6” 、47.5°、58.
2’、58.9” 、68.8”にピークを示し、結晶
化し2θ(上記(1)式のi=1の場合)は上記(Y、
Bax−1)NbOyとほぼ同様に20は32.6@3
8.5°、40.4″’、47.0°、58.5@など
にピークを示し、結晶化しており、かつ焼結体の色調は
黒已に近かった。
Note 1. This embodiment ((Y o, a B lio, e) N
When sintered bodies manufactured by (b) OJ) were measured by X-ray diffraction, the 2θ values were found to be 22.7@, 32.7@, and 38.
5°, 40.3°, 46.6°, 47.5°, 58°.
Peaks are observed at 2', 58.9'', and 68.8'', and crystallization occurs, with 2θ (when i=1 in equation (1) above) being the same as above (Y,
Bax-1) Similar to Nbyoy, 20 is 32.6@3
Peaks were observed at 8.5°, 40.4″', 47.0°, and 58.5°, indicating crystallization, and the sintered body was close to black.

L元素に2種以上用いても本発明のものが得られる1例
えば((ScaYz−a)bBaz−b))NbO8(
Xは7と推定)である、ここでa、bは夫々0<a、b
<1である。M料粉末はこの場合、5ozoa、YzO
a、BaC0a 、並びにN )) O或いは純Nb 
(純Nbなら還元雰囲気での処理を要す)である、i=
1の場合の20が得られる。
The present invention can be obtained even if two or more L elements are used. For example, ((ScaYz-a)bBaz-b))NbO8(
X is estimated to be 7, where a and b are 0 < a, b
< 1. In this case, the M powder is 5 oz a, Y oz O
a, BaC0a, and N)) O or pure Nb
(If it is pure Nb, it requires treatment in a reducing atmosphere) i =
In case 1, we get 20.

こうして得られたペロブスカイト・の代表例は、(L 
i aB a n−a)N b Oであり、2θはi 
= 1の系と同様である。
A representative example of the perovskite obtained in this way is (L
i aB a n-a)N b O, and 2θ is i
This is similar to system 1.

(LaxSrx−x)7.royで表わせるペロブスカ
イト状結晶構造を有する酸化物超電導材料の製法の場合
には、出発〃x料粉末として、LBzOs。
In the case of a method for producing oxide superconducting materials having a perovskite-like crystalline structure that can be represented by (LaxSrx-x)7.roy, the starting material powder is LBzOs.

5rCOst酸化ジルコニウム(ZrOz)または純金
属のジルコニウム(Zr)を所定の組成に秤量し、これ
を混合後、高温で反応熱処理を行う。
5rCOst zirconium oxide (ZrOz) or pure metallic zirconium (Zr) is weighed to a predetermined composition, mixed, and then subjected to a reaction heat treatment at a high temperature.

こうして得られた反応混合物の粉末を形成し、焼結する
ことによって、酸化物超電導材料を得ることができる。
By forming a powder from the reaction mixture obtained in this way and sintering it, an oxide superconducting material can be obtained.

(YxBat−x)Zroyで表わせるペロブスカイト
状結晶構造を有する酸化物超電導材料の製法の場合には
出発原料粉末としてYzOa) 11 a Cog、Z
rOまたはZrを所定の組成に秤量し、これを混合後、
高温で反応熱処理を行う、こうして得られた反応混合物
の粉末を成形し、焼結することによって、酸化物超電導
材料を得ることができる。
In the case of a method for producing oxide superconducting materials having a perovskite-like crystalline structure that can be represented as (YxBat-x)Zroy, the starting raw material powders are YzOa) 11 a Cog, Z
Weigh rO or Zr to a predetermined composition, mix them,
By performing a reaction heat treatment at a high temperature, molding the resulting reaction mixture powder, and sintering it, an oxide superconducting material can be obtained.

(L a、s rt−x)T a Oyで表わせるペロ
ブスカイト状結晶構造を有する酸化物超電導材料の製法
の場合には、出発原料粉末としてLa5hs、5rCO
a、酸化タンタル(Taxes、Tag)または純金属
のタンタル(Ta)を所定の組成に秤量し、これを混合
後、高温で反応熱処理を行う。
In the case of a method for producing an oxide superconducting material having a perovskite-like crystalline structure that can be represented as (La, s rt-x)Ta Oy, the starting raw material powders are La5hs, 5rCO
a. Tantalum oxide (Taxes, Tag) or pure metallic tantalum (Ta) is weighed to a predetermined composition, mixed, and then subjected to a reaction heat treatment at a high temperature.

こうして得られた反応混合物の粉末を成形し、焼結する
ことによって、酸化物超電導材料を得ることができる。
By molding and sintering the powder of the reaction mixture obtained in this way, an oxide superconducting material can be obtained.

(YXB a z−x)T a Oyで表わせるペロブ
スカイト状結晶構造を有する酸化物超電導材料の製法の
場合には、YzOa、BaCO5、TaxOaまたはT
aOまたはTaの組合せで同様に製造できる。
In the case of a method for producing oxide superconducting materials having a perovskite-like crystal structure that can be represented as (YXB a z-x)T a Oy, YzOa, BaCO5, TaxOa, or T
It can be manufactured similarly using a combination of aO or Ta.

以上説明したことから、(L貢At−X)IMOFで表
わされるペロブスカイト状結晶構造を有する酸化物超電
導材料の製法においては、上述した実施例のように、L
元素としてその酸化物(YzOa。
As explained above, in the method for producing an oxide superconducting material having a perovskite-like crystal structure represented as (L-At-X)IMOF, as in the above-described example, L
As an element, its oxide (YzOa).

Latom、5osoa、Yb5os、ErzoaeH
o−ts On、Dynes)を用い、へ元素としてそ
の炭酸化物(B a COa、 S r Co8. C
a Co8)を、モしてM元素としては、その酸化物(
vO9Nbe、Tag、TazOa、Tie、Ti0z
。
Latom, 5osoa, Yb5os, ErzoaeH
Using o-ts On, Dynes, and as the element, its carbon oxide (Ba Coa, S r Co8, C)
a Co8) is used as the element M, and its oxide (
vO9Nbe, Tag, TazOa, Tie, Ti0z
.

Zro、Zrose HfO,HfOx等)或イハ(−
の純金属粉末(V、Nb、Ta、Ti、Zr。
Zro, Zrose HfO, HfOx, etc.) or Iha (-
Pure metal powders (V, Nb, Ta, Ti, Zr).

Hf)を使用することにより製造できる。It can be manufactured using Hf.

(L翼(A’ t−ah’ −)漁−x ) t M 
Oy (但し、0≦dく1)で表おされるペロブスカイ
ト状結晶構造においては、前述した(LヨAx−x)s
MOyの中のA元素を2元素系とするもので、例えば、
(L ax(S rz、Ca−)s−1I)tMOyの
場合は、La5OseS r COs、 Ca COs
の粉末、及びM元素の酸化物または純金属の粉末を所定
の組成に秤量し、これと混合後、高温で反応熱処理を行
う、こうして得られた反応混合物を成形し、焼結するこ
とにより酸化物超電導材料を得ることができる。
(L wing (A't-ah' -) fishing-x) t M
In the perovskite crystal structure represented by Oy (where 0 ≤ d < 1), the aforementioned (LyoAx-x)s
This is a system in which element A within MOy is a two-element system, for example,
(In the case of La ax(S rz, Ca-)s-1I)tMOy, La5OseS r COs, Ca COs
A powder of element M and a powder of an oxide or pure metal of element M are weighed to a predetermined composition, mixed, and then subjected to a reaction heat treatment at a high temperature. The resulting reaction mixture is then molded and sintered to obtain an oxide superconducting material.

(LxAi−x)tM’ 五−zM’ toyで表わさ
れるペロブスカイト状結晶構造においては、前述した(
 L x A l−11)I M Oyの中のM元素を
2元素系とするもので、例えば、(LxAx−x)tN
bt−zZrzoyの場合は、L元素の酸化物の粉末、
A元素の炭酸化物の粉末、及びNbO,ZrOs  (
あるいはNb。
In the perovskite-like crystal structure represented by (LxAi-x)tM'↔zM' toy, the aforementioned (
L x A l-11)I M Oy is a system of two elements, for example, (LxAx-x)tN
In the case of bt-zZrzoy, the oxide powder of element L,
A element carbon oxide powder, and NbO, ZrOs (
Or Nb.

Zr)の粉末を所定の組成に秤量・混合し、これを高温
で反応熱処理を行う、こうして、得られた反応混合物を
成形し、焼結することにより酸化物超電導材料を得るこ
とができる。
By weighing and mixing Zr powder to a predetermined composition and then subjecting it to a high-temperature reaction heat treatment, the resulting reaction mixture can be molded and sintered to obtain an oxide superconducting material.

(L a x S r t−x)sN b Oa−墨F
hで表わせるペロブスカイト状結晶構造を有するものに
ついて説明する。酸化ランタン(Lashs)粉末、ふ
フ化ストロンチウム(SrFz)粉末、及び酸化ニオブ
(N b O)粉末を所定の化学量論組成に秤量し、そ
の混合粉末を酸化性雰囲気中またはふっ素ガスを含む酸
化性雰囲気中で、800℃〜1000℃で数時間加熱し
て反応させる6次に、その混合反応物を粉砕し、これを
適当な形状にプレス成形し。
(L a x S r t-x)sN b Oa-Black F
A perovskite-like crystalline structure that can be represented by h will be described. Lanthanum oxide (Lashs) powder, strontium fluoride (SrFz) powder, and niobium oxide (NbO) powder are weighed to a predetermined stoichiometric composition, and the mixed powder is reacted by heating it at 800°C to 1000°C for several hours in an oxidizing atmosphere or an oxidizing atmosphere containing fluorine gas. The mixed reaction product is then pulverized and pressed into an appropriate shape.

前記反応温度よりもやや高い温度で、焼結することによ
って、所望の形状のペロブスカイト型超電導セラミクス
を得ることができる。
By sintering at a temperature slightly higher than the aforementioned reaction temperature, perovskite-type superconducting ceramics of the desired shape can be obtained.

(Y x B 5−x)zN b Oa−I F hで
表わせるペロブスカイト状結晶構造を有するものの製法
の場合には、出発原料粉末として酸化イツトリウム(Y
zO+s) #ふフ化バリウム(BaFz)*酸化ニオ
ブ(N b O)または純金属のニオブ(Nb)を所定
の組成に秤量し、これを混合後、高温で反応熱処理を行
う、こうして得られた反応粉末を成形し、焼結すること
によって、ペロブスカイト型超電導セラミクスを得るこ
とができる。
In the case of a method for producing a perovskite-like crystalline structure that can be represented as (Y x B 5-x)zN b Oa-I F h, yztrium oxide (Y) is used as the starting material powder.
Barium fluoride (BaFz) is obtained by weighing niobium oxide (N₂b₂O) or pure metallic niobium (Nb) to a predetermined composition, mixing them, and then performing a reaction heat treatment at a high temperature. The resulting reaction powder is then molded and sintered to obtain perovskite-type superconducting ceramics.

(YxBat−x)tNboJjcQhで表わせるペロ
ブスカイト状結晶構造を有するものの製法の場合には、
出発原料粉末として酸化イヅトリウム(YxOs)、塩
化バリウム(BaCflx)、酸化ニオブ(N b O
)を所定の組成に秤量し、これを混合後、高温で反応熱
処理を行う、こうして、得られた反応粉末を成形し、焼
結することによフて。
In the case of a method for producing a material having a perovskite-like crystal structure that can be represented as (YxBat-x)tNboJjcQh,
The starting material powders are izutrium oxide (YxOs), barium chloride (BaCflx), and niobium oxide (NbO).
The following steps are performed: weighing the ingredients to a predetermined composition, mixing them, and then performing a reaction heat treatment at a high temperature; the resulting reaction powder is then molded and sintered.

ペロブスカイト型超電導セラミクスを得ることができる
。
Perovskite-type superconducting ceramics can be obtained.

以上説明したことから、(LxAl−x)tMOa−1
Ghで表わせるペロブスカイト状結晶構造を有する超電
導材料の製法においては、上述した実施例のように、L
元素としてその酸化物(Y to s* L a to
 JltSczos、Ybzoa伊E rzoa、Ho
zOaeD yzOa、Gdzoaなど)を用い、へ元
素としてはそのふフ化物(BaFz、5rFz、CaF
z )あるいはその塩化物(BaCQz、5r(lit
。
Based on the above explanation, (LxAl-x)tMOa-1
In the method for producing a superconducting material having a perovskite-like crystal structure that can be represented by Gh, as in the above-described example, L
As an element, its oxide (Y to s* La to
JltSczos, YbzoaItalyE rzoa, Ho
(e.g., zoaeD, yzoa, Gdzoa) are used, and the element is its fluoride (BaFz, 5rFz, CaF)
z) or its chloride (BaCQz, 5r(lit
.

CaCΩ2)を、モしてM元素としてはその酸化物(N
bO,VO,ZrOx、Tiesなど)を使用すること
により製造できる。また、へ元素としては、その炭酸化
物(B a Co8. S r CO8゜Ca CO’
s )とそのふフ化物あるいは塩化物の混合物でもよい
、また、M元素として、そのふフ化物、塩化物あるいは
窒化物を出発原料としてもよ11゜ ところで、原料混合粉末の反応温度、反応時間などの反
応雰囲気条件、その後の焼結条件は、使用元素の違い、
組成比の違い、粉末の状態などによって変化するので、
適宜選択されなければならない拳苧ことは言うまでもな
い、特に1M元素の純金属粉末を使用する場合、酸化性
雰囲気ではその反応が急激であるため、還元性雰囲気で
熱処理することが望ましい、また、雰囲気条件はG元素
がふっ素の場合にはふフ素を含む酸化性雰囲気、またG
元素が塩素の場合には塩素を含む酸化性雰囲気が望まし
い。
CaCΩ2) is used as the element M, and its oxide (N
It can be produced using elements such as bO, VO, ZrOx, and Ties. Furthermore, as the element, its carbon oxides (Ba, a, Co8, S, r, CO8, Ca, CO') can be used.
s) may be a mixture of its fluoride or chloride, or its fluoride, chloride or nitride may be used as the starting material for element M.11°By the way, the reaction atmosphere conditions such as the reaction temperature and reaction time of the raw material mixed powder, and the subsequent sintering conditions will differ depending on the elements used.
It varies depending on differences in composition ratio, powder state, etc.
Needless to say, the appropriate heat treatment must be selected, especially when using pure metal powder of element 1M. Since the reaction is rapid in an oxidizing atmosphere, it is desirable to heat treat in a reducing atmosphere. Furthermore, the atmospheric conditions should be an oxidizing atmosphere containing fluorine when element G is fluorine, and G
If the element is chlorine, an oxidizing atmosphere containing chlorine is desirable.

さて、焼結後には、G元素(F、CQ、N)が所望の組
成比より少ない場合には、後にイオンプランテーシ1ン
などにより、G元素のイオンを注入してもよい。
Now, if, after sintering, the amount of G elements (F, CQ, N) is less than the desired composition ratio, ions of the G elements may be implanted later using an ion plantation or the like.

上記の製法により得られた(LaxSrx−x)zNb
oy。
(LaxSrx-x)zNb obtained by the above manufacturing method
oy.

(ここで、0〈y≦4.x=0.5 )、及び(Y)I
B a 1−31)N b Oy 、  (ここで、x
=0.5゜0 < y≦3)の焼結体の電気抵抗の温度
特性を第6図に示す、これらの特性は、化学量論組成比
熱処理条件(焼成温度パターン、焼成時の雰囲気、アニ
ール熱処理条件など)により大きく変化するので、第6
図は単なる例示にすぎない、1!l!気抵抗は一温度の
減少に従い、約280により急激に減少し、完全に電気
抵抗が零になるのは約250にである。即ち、約280
Kから超電導状態になり始め、約250にで完全に超電
導状態へ転移したことになる。この場合、転移幅は30
にと非常に大きいが、焼結時の熱処理条件や、焼結後の
アニール熱処理により、更に、転移幅を小さくすること
ができる。
(Here, 0 <y ≤ 4, x = 0.5), and (Y)I
B a 1-31) N b Oy, (where x
Figure 6 shows the temperature characteristics of the electrical resistance of a sintered body with a temperature of 0.5°0 < y ≤ 3). These characteristics change significantly depending on the stoichiometric composition specific heat treatment conditions (firing temperature pattern, atmosphere during firing, annealing heat treatment conditions, etc.).
The diagram is merely an example; 1. Electrical resistance decreases rapidly with each decrease in temperature, by approximately 280, and becomes completely zero at approximately 250. That is, approximately 280
The superconducting state begins at K, and complete transition to the superconducting state occurs at approximately 250. In this case, the transition width is 30.
Although the transition is very large, the transition width can be further reduced by adjusting the heat treatment conditions during sintering and by performing annealing heat treatment after sintering.

原料混合粉末の反応温度や焼結時の熱処理温度は、(L
xAt−x)iMt−zCuzoy  (但し、O< 
zく1)のように、M元素をCuで置換することにより
、低減できる。このとき、超電導特性に大きな劣化はな
い。
The reaction temperature of the raw material mixture powder and the heat treatment temperature during sintering are (L
xAt-x)iMt-zCuzoy (However, O<
As shown in z<1), this can be reduced by substituting the M element with Cu. In this case, there is no significant degradation in superconductivity.

上記の製法により得られたLax S rt Nb0x
−3F x及びYo、aB a o、aNbozjc 
Qの焼結体の電気抵抗の温度特性を第7図に示す、これ
らの特性は、出発化学量論組成比、熱処理条件(焼成温
度パターン、焼成時の雰囲気、アニール熱処理条件など
)により、大きく変化するので、第7図は単なる例示に
すぎない、ft電気抵抗、温度の減少に従い、約320
により急激に減少し、約300にで完全に電気抵抗が零
になる。即ち、約3001(から超電導状態になり始め
、約300にで完全に超電導状態へ転移したことになる
。この場合、転移幅はさくすることができる。また、こ
れらの物質は、化学的に充分安定であり、上記超電導特
性は、経年変化はほとんどない。
Lax S rt Nb0x obtained by the above manufacturing method
-3F x and Yo, aB ao, aNbozzjc
Figure 7 shows the temperature characteristics of the electrical resistance of the sintered body of Q. These characteristics vary greatly depending on the starting stoichiometric composition ratio and heat treatment conditions (sintering temperature pattern, atmosphere during sintering, annealing heat treatment conditions, etc.), so Figure 7 is merely an example. The ft electrical resistance decreases by approximately 320 as the temperature decreases.
The resistance decreases rapidly, and at approximately 300, the electrical resistance becomes completely zero. That is, it begins to enter a superconducting state at approximately 3001, and completely transitions to a superconducting state at approximately 300. In this case, the transition width can be narrowed. Furthermore, these materials are chemically stable, and the above superconducting properties hardly change over time.

次に、実施例のペロブスカイト型超電導材料の薄膜の製
造法の具体的な一例を説明する。上記焼結法により得ら
れたセラミクスをターゲットとして用い、アルゴンガス
雰囲気中あるいは適当な酸素分圧及びふ′)索あるいは
塩素分圧をもつアルゴンガス雰囲気中ではスパッタリン
グによフて、AQ*Os単結晶あるいはAnzOsセラ
ミクスの基板上に、所望の形状及び厚みの膜を堆積でき
る。
Next, a specific example of a method for manufacturing a thin film of the perovskite-type superconducting material of the example will be described. Using the ceramic obtained by the above sintering method as a target, a film of a desired shape and thickness can be deposited on a substrate of AQ*Os single crystal or AnzOs ceramic by sputtering in an argon gas atmosphere or in an argon gas atmosphere with an appropriate oxygen partial pressure and chlorine partial pressure.

また、微妙な膜厚調整、化学量論組成比の調整が必要な
場合には1分子線エピタキシー法により膜を堆積できる
。その他、膜形成法として従来から知られている物理的
方法、化学的方法及び物理化学的方法を利用できること
は言うまでもない、また、膜形成後、G元素の不足分は
後でイオンプランテーションなどの方法により、補給で
きる。
Furthermore, if precise adjustment of film thickness or stoichiometric composition ratio is required, the film can be deposited using single-molecule beam epitaxy. Needless to say, conventional physical, chemical, and physicochemical methods for film formation can also be used. Additionally, any deficiencies in element G after film formation can be replenished later by methods such as ion plantation.

前記、Cuを含む材料の具体的な製造方法のプロセスの
一例を第8図で説明する。L元素の酸化物粉末、A元素
の炭酸化物粉末及び第2酸化銅CuO粉末を所定の組成
となるように秤量し、この混合粉末を酸化性雰囲気中に
おいて900〜1000℃で加熱反応させる。この反応
混合粉末に1M元素であるVa族元@ (v、’Nb、
Ta)あるいはIVa族元素(Ti、Zr、Hf)の中
より選ばれた1つまたは複数の純金属粉末を所望の化学
量論組成量を秤量し、混合する。このようにして得た前
工程混合粉末を再度、真空中、還元性あるいは弱い酸化
性雰囲気(この場合の雰囲気は、例えば2価のNbOが
5価のNbzOsに酸化されない程度)中で加熱反応処
理を行うことにより、(LxAt−x)tMt−zcu
toyの粉末を得ることができる。こうして得られた最
終反応粉末をプレス成形し、焼結することにより、適当
な形状を有する酸化物超電導材料を製造できる。また、
上記の前工程反応混合粉末あるいは最終反応粉末を銅な
どの金属管へ充填したり、金属テープに膜として付着さ
せて1反応焼結することにより、本発明の酸化物超電導
材料で製作した超電導線を製造できる。
Figure 8 illustrates an example of a specific manufacturing process for the Cu-containing material. The oxide powder of element L, the carbon oxide powder of element A, and the copper oxide CuO powder are weighed to a predetermined composition, and this mixed powder is heated and reacted in an oxidizing atmosphere at 900-1000°C. This reaction mixed powder is then mixed with the 1M element, which is a group Va element (v, 'Nb,
One or more pure metal powders selected from Ta) or group IVa elements (Ti, Zr, Hf) are weighed in the desired stoichiometric composition and mixed. The resulting pre-processed powder is then subjected to a heating reaction again in a vacuum, in a reducing or weakly oxidizing atmosphere (in this case, the atmosphere should not be such that, for example, divalent NbO is not oxidized to pentavalent NbzOs), thereby producing (LxAt-x)tMt-zcu
A toy powder can be obtained. By press-molding and sintering the final reaction powder thus obtained, an oxide superconducting material with a suitable shape can be manufactured. Furthermore,
By filling the above-mentioned pre-reaction mixed powder or final reaction powder into a metal tube such as copper, or by attaching it as a film to a metal tape and performing a single-reaction sintering, a superconducting wire made of the oxide superconducting material of the present invention can be manufactured.

尚、反応焼結熱処理後は酸化性雰囲気中でアニール熱処
理することが望ましい。
Furthermore, it is desirable to perform annealing heat treatment in an oxidizing atmosphere after the reaction sintering heat treatment.

次に、本発明の酸化物超電材料の薄膜の形成法の具体的
な一例を説明する。上記の焼結法により得られた磁器を
ターゲットとして用い、アルゴンガス雰囲気中あるいは
適当な酸素分圧をもつアルゴンガス雰囲気中でのスパッ
タリングによって、Si単結晶、AasOn単結晶、S
 x O2単結晶、MgO単結晶、Zr0z単結晶、あ
るいはこれらの多結晶体の基板上に本発明の酸化物超電
導薄膜を直接、所望の形状及び厚みの膜を堆積できる。
Next, a specific example of a method for forming a thin film of the oxide superelectric material of the present invention will be described. Using the porcelain obtained by the above sintering method as a target, a Si single crystal, an AasOn single crystal, and S are formed by sputtering in an argon gas atmosphere or an argon gas atmosphere with an appropriate oxygen partial pressure.
The oxide superconducting thin film of the present invention can be directly deposited on a substrate of x O2 single crystal, MgO single crystal, Zr0z single crystal, or polycrystalline material thereof, in a desired shape and thickness.

また、微妙な膜厚調整、化学量論組成比の調整が必要な
場合には1分子線エピタキシー法により膜を堆積できる
。その他、膜形成法として従来から知られている物理的
方法、化学的方法も利用できることは言うまでもない、
いずれの場合においても、膜成長条゛件を最適化するこ
とにより、第6図で示したような超電導特性を得ること
ができる。
Furthermore, when precise adjustments to film thickness or stoichiometric composition ratios are required, films can be deposited using single-molecule beam epitaxy. Needless to say, conventional physical and chemical methods for film formation can also be used.
In either case, by optimizing the film growth conditions, superconducting properties as shown in Figure 6 can be obtained.

以上説明したような基板上に直接所望の化学量論組成を
もつ酸化物超電導薄膜を形成する方法以外に、第9図に
示すようにAMMgO単結晶どの基板1に先ずM元素の
金属薄膜2を成長させ、次にL元素及びA元素の適当な
化学量論組成比をもつ膜3を堆積させ、その後熱処理に
より金属薄膜2とa3を反応させ、この膜2,3の部分
の一部または全部を本発明に係わる酸化物゛超電導薄膜
4に転化することができる。このとき、先にL元素及び
A元素のrf43を堆積し、次にM金属薄膜2を成長さ
せて、熱処理しても同様の効果が得られる。
In addition to the method of directly forming an oxide superconducting thin film with a desired stoichiometric composition on a substrate as described above, as shown in Figure 9, a metal thin film 2 of element M can be grown first on an AMMgO single crystal substrate 1, then a film 3 having an appropriate stoichiometric composition ratio of elements L and A can be deposited, and then the metal thin film 2 and a3 can be reacted by heat treatment to convert part or all of these films 2 and 3 into the oxide superconducting thin film 4 according to the present invention. At this time, a similar effect can be obtained by first depositing rf43 of elements L and A, then growing the M metal thin film 2, and then heat treating.

基板上の電気配線に本発明の超電導材料の薄膜を使用す
る場合、電気絶縁性のセラミクス基板の上に所望のパタ
ーン形状の膜をスクリーン印刷し、これを焼付けること
も可能である。同様に、多層配線されたセラミクス基板
を製作することもできる。
When using a thin film of the superconducting material of the present invention for electrical wiring on a substrate, it is also possible to screen print a film with a desired pattern shape onto an electrically insulating ceramic substrate and then bake it. Similarly, multilayer-wired ceramic substrates can also be fabricated.

テープ状の酸化物超電導材料を製造する場合には、M元
素(V、Nb、Ta、Ti、Zr、Hf)の金属テープ
上に、L元素(ランタノイド元素の群から選ばれた一つ
の元素)及びA元素(Ba。
When manufacturing tape-shaped oxide superconducting materials, an L element (one element selected from the group of lanthanide elements) and an A element (Ba) are added to a metal tape of an M element (V, Nb, Ta, Ti, Zr, Hf).

Sr、Ca)の適当な化学量論組成LxA+−x、但し
、(0< x < L )の膜を、スパッタ法などの従
来から知られた膜堆積法や粉末塗布焼付法などで付着さ
せ、その後の熱処理工程により、M元素の金属テープの
一部あるいは全部と反応させる方法がよい、この場合、
銅、銅合金あるいはステンレス錆などの金属線をベース
材料として、まずLxAt−xの膜をその表面に形成し
、その上にM元素の金属膜を堆積し、その後の熱処理工
程により、反応させることにより、本発明の酸化物超電
導線を製造できる。このとき、L x A t−x膜と
M元素の金属膜を交互に複数層形成することにより、熱
処理時の反応性を著しく向上させることができる。
A suitable stoichiometric composition LxA+-x of Sr(Ca), where (0 < x < L), is deposited using conventional film deposition methods such as sputtering or powder coating and baking, and then reacted with part or all of the metal tape of element M in a subsequent heat treatment step. In this case,
The oxide superconducting wire of the present invention can be manufactured by first forming an LxAt-x film on the surface of a metal wire such as copper, copper alloy, or stainless steel rust as a base material, depositing a metal film of element M on top of it, and then reacting them through a subsequent heat treatment process. In this case, by alternately forming multiple layers of the LxAt-x film and the metal film of element M, the reactivity during heat treatment can be significantly improved.

(LxAt−x)iMx−zCuzoyで表わせるペロ
ブスカイト状結晶構造を有する酸化物超電導薄膜を形成
する場合には、AQxOs単結晶などの基板上に、先ず
M元素の金属膜を形成し、この上に(L x A t−
x) t Cu Oyの膜を不活性雰囲気中で堆積し、
その後真空中あるいは酸化性雰囲気中で熱処理すること
により、M元素の金属原子が拡散し、Cu原子と置換す
る過程により達成される。そのため、前記2種類の膜、
即ちノM元素の金属膜と(LxAz−x)icuOyの
酸化物の膜を交互に複数層形成した後に、熱処理により
、Cu原子とM元素の原子の置換を高めることができる
。また。
When forming an oxide superconducting thin film having a perovskite-like crystalline structure that can be represented as (LxAt-x)iMx-zCuzoy, first a metal film of element M is formed on a substrate such as an AQxOs single crystal, and then (LxAt-x)iMx-zCuzoy is formed on top of this.
x) A film of t Cu Oy is deposited in an inert atmosphere.
Subsequently, by heat treatment in a vacuum or oxidizing atmosphere, the metal atoms of element M diffuse and replace the Cu atoms, thereby achieving this process. Therefore, the two types of films,
In other words, after alternately forming multiple layers of a metal film of element M and an oxide film of (LxAz-x)icuOy, heat treatment can be used to enhance the substitution of Cu atoms with elements M.

(LXAI−x)lCuOyの酸化物セラミクスを基板
として、M元素の金属膜を形成し、熱処理するなど。
For example, a metal film of element M is formed on an oxide ceramic of (LXAI-x)lCuOy as a substrate, and then heat-treated.

いろいろな手法であることは言うまでもない。Needless to say, there are various methods.

本発明によれば、いずれの実施例においても。According to the present invention, in all embodiments:

超電導転移温度が150に以上の酸化物超電導材料を得
ることは容易でり、200に以上の転移温度を示すもの
、更には第6図に示すように250に以上の転移温度を
示す酸化物超電導材料を容易に得ることができる。
It is easy to obtain oxide superconducting materials with a superconducting transition temperature of 150°C or higher, and even easier to obtain materials exhibiting a transition temperature of 200°C or higher, and furthermore, oxide superconducting materials exhibiting a transition temperature of 250°C or higher, as shown in Figure 6.

尚、第8図においては熱処理雰囲気を還元性としている
が、真空中でも酸化性雰囲気でも差し支えない、但し、
酸化性雰囲気の場合は例えば原料のNbOがNbzOa
にならない程度、すなわち原料IVa、VB族酸酸化組
成分酸化数(価数、酸素比率)が高まらぬ範囲に止める
必要がある。
Note that while Figure 8 shows a reducing atmosphere for the heat treatment, a vacuum or oxidizing atmosphere is also acceptable; however,
In an oxidizing atmosphere, for example, the starting material NbO becomes NbzOa
It is necessary to keep the oxidation state (valence, oxygen ratio) of the raw material IVa and VB group acid oxidation components within a range that does not increase to an excessive degree.

m造されたペロブスカイトの構成成分の各価数の関係は
例示すると次表の通りである。
The relationship between the valencies of the constituent components of the perovskite is illustrated in the following table.

上記のように酸素の総価数と他元素の総分数が実質的に
バランスしていれば安定な(劣化しにくい)ものが得ら
れる。尚、この為には若干の酸素欠陥の過不足は差し支
えなくよって両総価数の差は±0.5の範囲ならば有効
となる。実際には得移動する状態にあり、かつ少なくと
も低価数(前記の例では2価)のものを備えることが望
ましい。
As described above, a stable (less degradable) product can be obtained if the total valency of oxygen and the total fractions of other elements are substantially balanced. For this purpose, a slight excess or deficiency of oxygen is acceptable, and therefore, a difference of ±0.5 between the two total valencies is valid. In practice, it is desirable to have oxygen in a mobile state and at least at a low valency (2 in the above example).

アニーリングとは酸化性雰囲気でも還元性雰囲気でも良
い。
Annealing can be performed in either an oxidizing or reducing atmosphere.

この他得られる超電導材の劣化を防止すべく、原料の適
正な化学量論的組成比の選択と、イオン半径や電気的中
性についても配慮を要する。
Furthermore, to prevent degradation of the resulting superconducting material, it is necessary to select an appropriate stoichiometric composition ratio of raw materials, and to consider ionic radius and electrical neutrality.

第10図は本発明の一実施例に係る超電導部材であり、
上述の易酸化性の問題を解決すべく本例では酸素防止膜
5を用いている。即ち基板1上に配設した超電導薄膜4
の露出部分(即ち側面及び上面)全体に酸素防止膜5を
被覆する。酸素防止膜5の具体例としては銅や合成樹脂
等がなければ。
Figure 10 shows a superconducting member according to one embodiment of the present invention.
To address the aforementioned problem of easy oxidation, an oxygen-blocking film 5 is used in this example. Specifically, a superconducting thin film 4 is disposed on the substrate 1.
The entire exposed portion (i.e., the sides and top) is covered with an oxygen-preventive film 5. Specific examples of the oxygen-preventive film 5 include copper, synthetic resin, etc.

要するに外部の酸素の侵入でペロブスカイト中の残留低
価数原子が酸化されることを防止する機能を具備する。
In short, it has the function of preventing the oxidation of residual low-valent atoms in the perovskite due to the intrusion of external oxygen.

応用例として本発明材料を線材化する際のクラツド材(
表面層、外側層)に酸素防壁膜を施こしても良い。
As an example of application, the cladding material used when forming the material of the present invention into wire (
An oxygen barrier film may be applied to the surface layer and outer layer.

第11図は本発明の超電導材を薄膜化させたもの複数枚
の各間に絶縁シート7を介在させたものでこの絶縁シー
トは超電導材料同様、ペロブス力。
Figure 11 shows a plurality of thin films of the superconducting material of the present invention, with an insulating sheet 7 interposed between each film. This insulating sheet, like the superconducting material, exhibits the Perovs force.

イト系のものが適する。これは両者の格子定数や結晶構
造がペロブスカイトという点で同−若しくは近似してい
る為に界面状態が良くなるからである。尚各シートの厚
さは10〜20人が適する。
Ito-type materials are suitable. This is because the lattice constants and crystal structures of both materials are the same or approximate in that they are perovskite, resulting in a good interface. The appropriate sheet thickness is 10 to 20 people.

絶縁シートの具体例としては5rTiOaやL i N
 b Oaであり、特に後者は本発明超電導材として含
Nb材を使用した場合に親和性がある故有効である。
Specific examples of insulating sheets include 5rTiOa and LinN.
b is Oa, and the latter is particularly effective because it has affinity when Nb-containing material is used as the superconducting material of the present invention.

〔発明の効果〕[Effects of the invention]

本発明によれば、超電導転移温度を150に以上とする
ことができる酸化物超電導材料が得られるので、超電導
状態を保つのに、液体窒素温度レベルなどの極低温環境
を必要としない超電導材料が得られるという効果がある
。
According to the present invention, an oxide superconducting material can be obtained that can achieve a superconducting transition temperature of 150 or higher. This has the effect of providing a superconducting material that does not require an extremely low-temperature environment, such as liquid nitrogen temperature, to maintain the superconducting state.

【図面の簡単な説明】[Brief explanation of the drawing]

第1図、第2図は夫々本発明材料の結晶構造を示す図、
第3図は本発明材料の一例のEPMA分析のデータを示
す特性図、第4図、第5図、第6図、第7図は夫々本発
明材料の実施例による電気抵抗〜温度関係の特性図、第
8図、第9図は夫々本発明の製法例を示す工程図、第1
0図、第11図は夫々本発明部材の実施例断面図である
。 さ 一1J′ 」ツ 図面の浄S(内容に変更なし) 茅 1 図 井 、Z図 茅 3 図 1.so;4   2.oθA2.りθ;    3.
1#);弄斗口 1塵T(に) 茅5図 XJL贋T(K) 季乙国 0     10θ     2θ0   30o  
  ≠りρ羞匙T(に) ギア図 ”    /III     111)    l1l
)    41/温47(K) W−75図 弄91!1 ↓ (反77″熱々町 1・・・l臥 卆・・月1瞬喪 芽/υ図      弄11図 n(1和62年 特許願 第 206359  号2、
発明の名称 ペロブスカイト型超電導材、並びに超電導部材3、補正
をする者 事件との関係  特 許 出 願 人 住 所  鹿児島県鹿児島市鴨池新町26番1−140
4氏名   大小 哲彌 名 称  (510)  株式会社 日 立 展 作 
所5、補正命令の日付(全送日) 昭和62年10月2
0日6、補正の対象   明細書の全文、並びに図面の
全図。 容に変更なし)。
Figures 1 and 2 show the crystal structure of the material of the present invention, respectively.
Figure 3 is a characteristic diagram showing EPMA analysis data of an example of the material of the present invention, Figures 4, 5, 6, and 7 are characteristic diagrams of the electrical resistance-temperature relationship according to an example of the material of the present invention, Figures 8 and 9 are process diagrams showing an example of the manufacturing method of the present invention,
Figures 0 and 11 are cross-sectional views of embodiments of the present invention, respectively. Figure 11 and 11 are cross-sectional views of the present invention. (No changes to the content) Figure 1, Figure 3 Figure 1. so; 4 2. oθA2. riθ; 3.
1 #); Toku mouth 1 dust T (ni) 5 pieces of grass
≠riρspoonT(ni) Gear diagram” /III 111) l1l
) 41/Warm 47 (K) W-75 figure 91! 1 ↓ (Anti 77″ hot town 1...l 卆...month 1 instant mourning bud/υ figure 11 figure n (1wa 62 Patent Application No. 206359 2,
Title of Invention: Perovskite-type superconducting material and superconducting member 3; Relationship to the case; Patent applicant's address: 26-1-140 Kamoike-shinmachi, Kagoshima City, Kagoshima Prefecture
4 Names Large and Small Tetsuya Name (510) Created by Tenno Hitachi Co., Ltd.
5. Date of Correction Order (Total Delivery Date): October 2, 1987
On day 06, the amendments were made to the entire text of the specification and all of the drawings. (No changes to the content.)

Claims (1)

【特許請求の範囲】 1、 I a族金属元素及びIIIa族元素の群から選ばれる
第1の元素と、IIa族元素の群から選ばれる第2の元素
と、IVa族元素及びVa族元素の群から選ばれる第3の
元素と、酸素とを主たる成分として含むことを特徴とす
るペロブスカイト型超電導材。 2、前記第1乃至第3の構成元素の価数合計xと酸素の
価数合計yとの関係が|x|=|y|±0.5であるこ
とを特徴とする特許請求の範囲第1項記載のペロブスカ
イト型超電導材。 3、前記第3の元素はその取り得る価数の内少なくとも
二価の状態を備えていることを特徴とする特許請求の範
囲第1項または第2項記載のペロブスカイト型超電導材
。 4、前記第3の元素はニオブ、ジルコニウム、タンタル
、チタン、バナジウムから選ばれるものであることを特
徴とする特許請求の範囲第1項乃至第3項いずれか記載
のペロブスカイト型超電導材。 5、前記第1乃至第3の構成元素の他に加わる残部元素
は銅、フッ素、窒素、及び/または塩素であることを特
徴とする特許請求の範囲第1項乃至第3項いずれか記載
のペロブスカイト型超電導材。 6、 I a族金属元素及びIIIa族元素の群から選ばれる
第1の元素とIIa族元素の群から選ばれる第2の元素と
、IVa族元素及びVa族元素の群から選ばれる第3の元
素と、酸素とを含むペロブスカイト型超電導材の露出部
分を酸素防壁膜、及び/またはパッシベーション膜にて
被覆することを特徴とする超電導部材。 7、 I a族金属元素及びIIIa族元素の群から選ばれる
第1の元素と、IIa族元素の群から選ばれる第2の元素
と、IVa族元素及びVa族元素の群から選ばれる第3の
元素と、酸素とを含むペロブスカイト型超電導材から形
成される薄膜と電気絶縁材から形成される薄膜とを交互
に積層して成ることを特徴とする超電導部材。 8、前記絶縁材はペロブスカイト型セラミクスであるこ
とを特徴とする特許請求の範囲第6項記載の超電導部材
。 9、下式で示されるペロブスカイト状結晶構造を有し、
式中のL元素は、スカンジウム(Sc)、イットリウム
(Y)、ランタン(La)などのランタノイド元素、並
びに I a族金属元素の群から選ばれた少なくとも一つ
の元素であり、式中のA元素はバリウム(Ba)、スト
ロンチウム(Sr)、カルシウム(Ca)などのアルカ
リ土類金属元素の群から選ばれた少なくとも一つの元素
であり、さらに酸素(O)、及び酸素空孔により形成さ
れる八面体結晶構造の中心部に位置する式中のM元素は
元素周期表のVa族元素であるバナジウム(V)、ニオ
ブ(Nb)、タンタル(Ta)、またはIVa族元素であ
るタチン(Ti)、ジルコニウム(Zr)、ハフニウム
(Hf)の群から選ばれた少なくとも一つの元素である
ペロブスカイト型超電導材において、前記酸素及び酸素
空孔の一部をふつ素(F)塩素(Cl)あるいは窒素(
N)で構成するようにしたことを特徴とするペロブスカ
イト型超電導材。 (L_xA_1___x)_iMO_j__δG_k・
・・(1)但し、この式で、 xは、0<x<1であり、 iは、i=1、3/2、または2であり、 j及びkは、i=1のときj+k=3 i=3/2のときj+k=7/2 i=2のときj+k=4 である。 δは、酸素の欠損量、Gは、ふつ素(F)、塩素(Cl
)あるいは窒素(N)である。
[Claims] 1. A perovskite-type superconducting material characterized by comprising as its main components a first element selected from the group of Group Ia metallic elements and Group IIIa elements, a second element selected from the group of Group IIa elements, a third element selected from the group of Group IVa elements and Group Va elements, and oxygen. 2. The perovskite-type superconducting material according to claim 1, characterized in that the relationship between the sum of the valencies x of the first to third constituent elements and the sum of the valencies y of oxygen is |x| = |y| ± 0.5. 3. The perovskite-type superconducting material according to claim 1 or 2, characterized in that the third element has at least one divalent state among its possible valencies. 4. The perovskite-type superconducting material according to any one of claims 1 to 3, characterized in that the third element is selected from niobium, zirconium, tantalum, titanium, and vanadium. 5. A perovskite-type superconducting material according to any one of claims 1 to 3, characterized in that the remaining elements added in addition to the first to third constituent elements are copper, fluorine, nitrogen, and/or chlorine. 6. A superconducting member characterized in that the exposed portion of a perovskite-type superconducting material containing a first element selected from the group of Group Ia metallic elements and Group IIIa elements, a second element selected from the group of Group IIa elements, a third element selected from the group of Group IVa elements and Group Va elements, and oxygen is covered with an oxygen barrier film and/or a passivation film. 7. A superconducting member characterized by being formed by alternately laminating a thin film made of a perovskite-type superconducting material containing a first element selected from the group of Group Ia metallic elements and Group IIIa elements, a second element selected from the group of Group IIa elements, a third element selected from the group of Group IVa elements and Group Va elements, and oxygen, and a thin film made of an electrical insulating material. 8. The superconducting member according to claim 6, characterized in that the insulating material is a perovskite-type ceramic. 9. Having a perovskite-like crystal structure shown in the following formula,
In a perovskite-type superconducting material, element L in the formula is at least one element selected from the group of lanthanide elements such as scandium (Sc), yttrium (Y), and lanthanum (La), and group Ia metallic elements; element A in the formula is at least one element selected from the group of alkaline earth metallic elements such as barium (Ba), strontium (Sr), and calcium (Ca); and element M in the formula, located at the center of the octahedral crystal structure formed by oxygen (O) and oxygen vacancies, is at least one element selected from the group of group Va elements of the periodic table such as vanadium (V), niobium (Nb), and tantalum (Ta), or group IVa elements such as tatin (Ti), zirconium (Zr), and hafnium (Hf), wherein some of the oxygen and oxygen vacancies are replaced with fluorine (F), chlorine (Cl), or nitrogen (
A perovskite-type superconducting material characterized by being composed of N. (L_xA_1___x)_iMO_j___δG_k
... (1) However, in this equation, x is 0 < x < 1, i is i = 1, 3/2, or 2, and j and k are j + k = 3 when i = 1, j + k = 7/2 when i = 3/2, and j + k = 4 when i = 2. δ is the amount of oxygen deficiency, G is fluorine (F), chlorine (Cl)
) or nitrogen (N).
JP62206359A 1987-04-13 1987-08-21 Perovskite type superconducting member Expired - Lifetime JP2880163B2 (en)