JPH01224960A - 光磁気記録媒体 - Google Patents

光磁気記録媒体

Info

Publication number
JPH01224960A
JPH01224960A JP5107088A JP5107088A JPH01224960A JP H01224960 A JPH01224960 A JP H01224960A JP 5107088 A JP5107088 A JP 5107088A JP 5107088 A JP5107088 A JP 5107088A JP H01224960 A JPH01224960 A JP H01224960A
Authority
JP
Japan
Prior art keywords
magneto
recording layer
optical recording
spatterning
recording medium
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP5107088A
Other languages
English (en)
Inventor
Masabumi Nakada
正文 中田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
NEC Corp
Original Assignee
NEC Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by NEC Corp filed Critical NEC Corp
Priority to JP5107088A priority Critical patent/JPH01224960A/ja
Publication of JPH01224960A publication Critical patent/JPH01224960A/ja
Pending legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。

Description

【発明の詳細な説明】 〔産業上の利用分野] 本発明は、書換え可能な光磁気ディスクなどに用いられ
、磁気カー回転効果あるいは、ノア2デー効果などの磁
気光学効果を用いて読出すことのできる光磁気記録媒体
に関する。
〔従来の技術〕
従来、情報を熱磁気的に記録し、磁気光学的に再生する
光磁気記録媒体は、透明な樹脂基板上あるいは、ガラス
基板上に誘電体からなる保護層。
垂直磁化膜の記録層、金属膜からなる反射層などを様々
の組み合わせで、ススブタ法あるいは蒸着法により成膜
したものである。このうち、垂直磁化膜としてはGdT
bFe、DyFe、GdCo、TbCo。
TbDyFe、TbFeCo  などの希土類−鉄属遷
移金属の非晶質合金薄膜が量産に適し、かつ読出しノイ
ズが少ないこと等から有望とされている。
基板と記録層の間の中間層は、記録層である垂直磁化膜
の酸化防止と、カーエ/ハ/ス効果の双方を目的として
形成されAI!N、SiN等の窒化物。
S io 、 S iozなどの酸化物のほか、ZnS
、MgFz。
SiCなどの種々の誘電体が用いられている。
〔発明が解決しようとする課題〕
記録層に用いられる垂直磁化膜は、酸化によってその垂
直磁気異方性を失なうことが多い。特に、希土類−鉄属
遷移金属系の垂直磁化膜の場合、希土類金属が酸化しや
すいために、空気中に数日放置するだけでその垂直磁気
異方性に劣化が認められる。
この酸化を防ぐことを目的として、記録層を誘電体から
なる保護層で挟み込むことが行われており、効果をあげ
ている。しかし、保護層に存在するピンホール、基板の
傷、ごみ等の欠陥から発生する記録層の酸化を完全に防
止することは困難である。このため、記録層自体の耐腐
食性を向上させる必要がある。
記録層の耐腐食性向上のために、希土類−鉄属遷移金属
合金に非磁性元素の添加が行われている。
添加元素としては、不動態形成元素であるlf2゜Ti
 、Cr  や、貴金属系元素であるAu、Ag’、P
t等が検討されているが、いずれの元素の場合も1種類
の元素だけでは、十分な長期信頼性を得ることはできな
い。
本発明の目的は、磁気記録層の耐腐食性を向上させ、長
時間経過しても特性の劣化しない長期信頼性の優れた光
磁気記録媒体を提供することにある。
〔課題を解決するための手段〕 本発明の光磁気記録媒体は、膜面と垂直方向に磁化容易
軸を有し、希土類と鉄属遷移元素とTaとTi?含む磁
性合金?記録層として構成される。
〔作用〕
希土類−鉄属遷移金属の非晶質合金薄膜にTaとTiの
2種類の不動態形成元素を添加することにより、カー回
転角1反対車を低下させることなく、耐腐食性を大きく
向上できること?見い出した。
〔実施例〕
次に、本発明の実施例について図面を参照して説明する
第1図は本発明の一実施例?示す断面図である。
ガラス基板1の上に、中間層(スパッタによる窒化ケイ
素膜)2を80nm の厚さに、光磁気記録層(スパッ
タによるTbFeCo+M)3を80nmの厚さに、保
護層(スパッタによる窒化ケイ素膜)4を80nrn 
 の厚さに順次形成する。ここで1MはPL、Ti、C
r、Taの4種類の元素の少くとも一種を示す。
上記の構成の試料を、80Cの温水に2日間漬け、媒体
表面に発生した孔食の密度と、試料の外周端部から発生
した腐食の数の比較を行なった。
第2図は添加元素の種類と孔食の密度の関係を示す相関
図である。
孔食の密度は、添加元素の種類により2桁以上具なり、
Ti、Cr、Ta、Pt添加なしの順に小さい。
第3図は添加元素の種類と外周端部からの腐食数の関係
を示す相関図である。
腐食数は、Ta、 Cr、 Ti、 Pt、添加なしの
順に少ない。Ta添加により、外周端部からの腐食が完
全に防止できることが注目される。
第4元素の添加により、いずれの元素でも耐候性は向上
している力ζ一種類の元素の添加では、孔食と、外周端
部の腐食の両方を防止することはできなかった。そこで
、孔食に対して最も効果のあったTiと、外周端部の腐
食に対して最も効果のあったTaの2種類を同時にTb
FeCo1C添加し、同様の実験を行なった。その結果
、孔食と外周端部の腐食の両者?同時に〃防止すること
ができた。
上記効果は、他の希土類と鉄属遷移元素からなる磁性合
金9例えばGdTbFe、GdTbFeCo。
DyTbFe  などに対しても同様に見られた。
〔発明の効果〕
以上説明したように本発明は、耐食性の優れた記録層を
用いたので、従来の光磁気記録媒体に比べて長期信頼性
が改善されるという効果を有する。
【図面の簡単な説明】
第1′図は本発明の一実施例を示す断面図、第2図は添
加元素と孔食の密度との関係を示す相関図。 第3図はl添加元素と外周端部からの腐食の数との関係
を示す相関図である。 1・・・・・・ガラス基板、2・・・・・・中間層、3
・・・・・・光磁気記録層、4・・・・・・保護層。 代理人 弁理士  内 原   晋 M 1 図 グし  Pt   ’7う°   Cと   ;〜λ刃
艷7J[]i果 犀 Z 凹

Claims (1)

    【特許請求の範囲】
  1.  膜面と垂直方向に磁化容易軸を有し、希土類元素と鉄
    族遷移元素とTaとTiを含む磁性合金を記録層とする
    ことを特徴とする光磁気記録媒体。
JP5107088A 1988-03-03 1988-03-03 光磁気記録媒体 Pending JPH01224960A (ja)